Organopolysiloxane compound

The organopolysiloxane compound addresses the heat dissipation challenges in electronic components by enhancing filler dispersibility and solubility in phenyl-modified silicones, ensuring high thermal conductivity and maintaining fluidity, thus overcoming the limitations of existing silicone-based heat dissipation materials.

WO2024214485A1PCT designated stage expired Publication Date: 2024-10-17SHIN ETSU CHEMICAL CO LTD

Patent Information

Application Number
PCT/JP2024/010323
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-11
Filing Date
2024-03-15
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Highly integrated electronic components face heat dissipation challenges due to heat generation, and silicone-based heat dissipation materials with high thermal conductivity require increased filler content, which reduces fluidity and increases viscosity, especially with phenyl-modified silicones, leading to poor workability and solubility issues.

Method used

Development of an organopolysiloxane compound with a specific general formula, acting as a silane coupling agent (wetter), that enhances the dispersibility and solubility of thermally conductive fillers in phenyl-modified silicones, maintaining fluidity and suppressing viscosity increases even with high filler content.

Benefits of technology

The organopolysiloxane compound effectively improves the dispersibility and solubility of thermally conductive fillers in phenyl-modified silicones, maintaining fluidity and preventing viscosity increases, enabling the creation of thermally conductive silicone compositions with high filler content.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024010323_17102024_PF_FP_ABST
    Figure JP2024010323_17102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention is an organopolysiloxane compound characterized by being represented by general formula (1) (in the formula, R1 is independently an aromatic hydrocarbon group having 6 to 10 carbon atoms, R2 is independently an alkyl group having 1 to 10 carbon atoms, R3 is an alkyl group having 1 to 4 carbon atoms, a is 2 or 3, and n is an integer of 2 ≤ n ≤ 60). Provided thereby is a new organopolysiloxane compound that acts as a wetting agent enabling a high thermal conductive filler to highly fill a phenyl-modified silicone.
Need to check novelty before this filing date? Find Prior Art

Description

organopolysiloxane compounds

[0001] The present invention relates to an organopolysiloxane compound.

[0002] The performance of electronic components, such as highly integrated circuits like CPUs, is significantly degraded by heat generation during use. To solve this problem, heat-dissipating materials are used, which improve heat transfer efficiency when introduced into the air gap between the heat-generating and cooling components. Silicone heat-dissipating materials, in particular, are used in a wide range of fields due to their high heat resistance, weather resistance, and electrical insulation properties inherent to silicone. In addition, as electronic devices have become increasingly miniaturized and highly integrated in recent years, it is important to more efficiently cool the generated heat, which has led to a demand for heat-dissipating materials with high thermal conductivity.

[0003] The thermal conductivity of materials containing silicone oil and thermally conductive fillers is affected by the thermal conductivity of the thermally conductive filler itself when the volume fraction of the thermally conductive filler exceeds 0.6. Therefore, increasing the thermal conductivity of heat-dissipating materials is crucial. However, simply increasing the filler content significantly reduces the fluidity of the conductive grease, making it difficult to process. To solve this problem, a method has been proposed in which the thermally conductive filler is surface-treated with a silane coupling agent (wetter) to disperse it in the silicone base oil and maintain the fluidity of the thermally conductive grease.

[0004] Phenyl-modified silicones, which have a structure in which some methylsilicones have been replaced with phenyl groups, have better heat resistance, cold resistance, and oxidation resistance than methylsilicones. Furthermore, because they have high gas barrier properties and a high refractive index, phenyl-modified silicones are used in cosmetics, light-emitting diode encapsulants, and other applications (Patent Documents 1 and 2). Therefore, by using phenyl-modified silicones as base oils and applying them to heat-dissipating materials, properties that cannot be achieved with methylsilicones can be expected. On the other hand, because the introduction of phenyl groups makes the silicone skeleton rigid, there is a problem of a significant increase in viscosity, especially in high-phenyl-modified silicones (Patent Document 3).

[0005] Therefore, when a phenyl-modified silicone is used as a base oil and a thermally conductive filler is added to form a grease, the fluidity of the thermally conductive grease is significantly reduced. Furthermore, organopolysiloxanes having trialkoxysilyl groups, which are often used as wetters, have poor solubility in phenyl-modified silicones (Patent Documents 4 and 5). Therefore, there has been a need for the development of a wetter that is highly soluble in phenyl-modified silicones and that can suppress an increase in viscosity when a thermally conductive filler is added.

[0006] Japanese Patent Application Laid-Open No. 2004-162039 Japanese Patent Application Laid-Open No. 2007-039621 Japanese Patent Application Laid-Open No. 2004-262919 Japanese Patent Application Laid-Open No. 2004-262972 Japanese Patent Application Laid-Open No. 2005-162975

[0007] An object of the present invention is to provide a novel organopolysiloxane compound that acts as a wetter that allows resin materials, particularly phenyl-modified silicones, to be highly loaded with a highly thermally conductive filler.

[0008] In order to achieve the above object, the present invention provides the following novel organopolysiloxane compound.

[0009] That is, the present invention provides a compound represented by the following general formula (1): (In the formula, R 1 are independently aromatic hydrocarbon groups having 6 to 10 carbon atoms, and R 2 are independently alkyl groups having 1 to 10 carbon atoms, and R 3 is an alkyl group having 1 to 4 carbon atoms; a is 2 or 3, and n is an integer satisfying the condition 2≦n≦60.

[0010] Such organopolysiloxanes are suitable as wetters, and for example, phenyl-modified silicones can be highly loaded with highly thermally conductive fillers.

[0011] R shown in the above general formula (1) 1 is a phenyl group, and R 2 is preferably a methyl group. From the viewpoint of organopolysiloxane synthesis, these groups are preferred.

[0012] The present invention provides a wetter comprising the organopolysiloxane described above. By using the organopolysiloxane described above in the wetter, it is possible to further disperse the thermally conductive filler in the phenyl-modified silicone.

[0013] The organopolysiloxane of the present invention is useful as a silane coupling agent (wetter) that improves the dispersibility of thermally conductive fillers in phenyl-modified silicones. Therefore, a phenyl-modified silicone composition containing the organopolysiloxane of the present invention has a reduced viscosity and maintains fluidity, even when it contains a large amount of thermally conductive filler. Therefore, when the organopolysiloxane of the present invention is incorporated into a silicone composition, a thermally conductive silicone composition can be obtained in which an increase in viscosity is suppressed, even when the thermally conductive filler is highly loaded.

[0014] The organopolysiloxane synthesized in Example 1 29 This is a Si-NMR chart.

[0015] The present inventors have searched for organopolysiloxanes suitable for wetters that enable resin materials, particularly phenyl-modified silicones, to be highly loaded with highly thermally conductive fillers, and have found that those represented by the following general formula (1) are useful for this purpose, leading to the completion of the present invention. (In the formula, R 1 are independently aromatic hydrocarbon groups having 6 to 10 carbon atoms, and R 2 are independently alkyl groups having 1 to 10 carbon atoms, and R 3 is an alkyl group having 1 to 4 carbon atoms; a is 2 or 3, and n is an integer satisfying the condition 2≦n≦60.

[0016] The present invention will be described in detail below.

[0017] In the above general formula (1), R 1 are independently monovalent aromatic hydrocarbon groups having 6 to 10 carbon atoms. 1Specific examples of include aryl groups such as phenyl, tolyl, xylyl, and mesityl groups, and among these, phenyl is preferred from the viewpoint of ease of synthesis.

[0018] In the above general formula (1), R 2 is an alkyl group having 1 to 10 carbon atoms, more preferably 1 to 5, and even more preferably 1 to 3 carbon atoms. 2 Examples of alkyl groups include methyl, ethyl, propyl, isopropyl, butyl, tert-butyl, pentyl, hexyl, octyl, nonyl, and decyl groups, and of these, methyl and ethyl groups are particularly preferred from the viewpoint of ease of synthesis of the organopolysiloxane compound of the present invention.

[0019] In the above general formula (1), R 3 is an alkyl group having 1 to 4 carbon atoms. 3 Examples of the alkyl group include methyl, ethyl, propyl, isopropyl, butyl, and tert-butyl groups. Of these, methyl and ethyl groups are particularly preferred from the viewpoint of the hydrolysis property of the organopolysiloxane compound of the present invention. Furthermore, in the above general formula (1), a is an integer of 2 or 3, but is preferably 3 from the viewpoint of ease of synthesis of the organopolysiloxane compound of the present invention and economic efficiency.

[0020] In the general formula (1), n ​​is an integer satisfying the following conditions: 2≦n≦60, more preferably 9≦n≦30, and even more preferably 12≦n≦18. If n is outside the above range, compatibility with the phenyl-modified silicone will decrease significantly, which is not preferred.

[0021] Specific examples of organopolysiloxanes represented by the general formula (1) include, but are not limited to, the following compounds: In the formulas shown below, "Me" represents a methyl group and "Ph" represents a phenyl group.

[0022] The organopolysiloxane represented by the general formula (1) above can be synthesized, for example, according to the following reaction formula.

[0023] Reaction scheme:

[0024] n in the formula is 29 Identified by Si-NMR.

[0025] An organopolysiloxane compound as shown in general formula (1) above is synthesized by heating and stirring triarylsilanol and hexamethylcyclotrisiloxane (hereinafter sometimes referred to as cyclic siloxane) in acetonitrile solvent in the presence of bis(1,2-benzenediolate)phenylsilicate benzyltetramethylammonium salt (BTMAS, formula above) as a catalyst, and then reacting with ethyl 2-(trimethoxysilyl)propionate (ECMS, formula above) as a reaction terminator. A polar solvent such as acetonitrile (MeCN) or N,N-dimethylformamide (DMF) is preferred as the solvent for this reaction. The reaction temperature is typically 60 to 65°C, and the reaction time is approximately 2 hours for each step.

[0026] By changing the equivalent weight of cyclic siloxane relative to triarylsilanol, the length (n) of the main chain of the organopolysiloxane compound, i.e., the degree of polymerization, can be adjusted.

[0027] The resulting organopolysiloxane exhibits high solubility in phenyl-modified silicone.

[0028] The present invention will be specifically described below with reference to examples, but is not limited to these. In the following examples, the kinematic viscosity is a value measured at 25°C using a Canon-Fenske viscometer according to JIS Z8803:2011. The refractive index is a value measured at 25°C using an Abbe refractometer according to JIS K0062:1992. D In the following formula, Me represents a methyl group, and Ph represents a phenyl group.

[0029] Example 1 A 500 mL round separable flask was equipped with a stirrer, thermometer, and coil condenser via a four-neck separable cover. Cyclic siloxane (201.2 g, 0.904 mol) and acetonitrile (100 g) were added to the separable flask, and the mixture was heated and stirred at 65°C to dissolve the cyclic siloxane. After the cyclic siloxane was completely dissolved, triphenylsilanol (50 g, 0.181 mol) and BTMAS (426.8 mg, 0.0904 mmol) were added, and the reaction solution was heated and stirred at 65°C for 2 hours. The progress of the reaction was 1 After tracking with H-NMR spectroscopy and confirming the disappearance of the cyclic siloxane signal, the reaction terminator ECMS (80.4 g, 0.362 mol) was added, and the mixture was heated and stirred at 65°C for an additional 2 hours. After confirming the disappearance of the peak corresponding to silanol by infrared spectroscopy, methanol was added to the reaction solution, and the mixture was heated and stirred at 65°C for an additional 1 hour. The reaction solution was returned to room temperature, washed with methanol, and the oil layer was extracted. The solvent and low molecular weight siloxane contained in the resulting oil layer were removed under reduced pressure, yielding 178.7 g (yield: 71%) of an organopolysiloxane compound. This compound was a colorless, transparent liquid with a kinematic viscosity of 35 mm 2 ・s -1 The refractive index was 1.44. 29 Si-NMR spectrum analysis revealed that it had the following structure (see FIG. 1). 29 Si-NMR spectrum (99.37 MHz, CDCl 3 , 25°C): δ=-19.2 (SiMe 2 ), -19.5(SiPh 3 ) -20.8 to -21.8 (SiMe 2 ), -84.8(Si(OMe) 3 ).

[0030] [Example 2] An organopolysiloxane compound was obtained in the same manner as above, except that 10 equivalents of cyclic siloxane were used relative to triphenylsilanol. This compound was a colorless, transparent liquid with a kinematic viscosity of 64 mm 2 ・s -1 The refractive index was 1.42. 29Si-NMR spectral analysis revealed the following structure: 29 Si-NMR spectrum (99.37 MHz, CDCl 3 , 25°C): δ=-19.2 (SiMe 2 ), -19.5(SiPh 3 ) -20.8 to -21.8 (SiMe 2 ), -84.8(Si(OMe) 3 ).

[0031] [Example 3] An organopolysiloxane compound was obtained in the same manner as above, except that 3 equivalents of phenyl-modified cyclic siloxane were used relative to trimethylsilanol. This compound was a colorless, transparent liquid with a kinematic viscosity of 61 mm 2 ・s -1 The refractive index was 1.46. 29 Si-NMR spectral analysis revealed the following structure: 29 Si-NMR spectrum (99.37 MHz, CDCl 3 , 25°C): δ=-19.2 (SiMe 2 ), -19.5(SiPh 3 ) -20.8 to -21.8 (SiMe 2 ), -84.8(Si(OMe) 3 ).

[0032] [Compatibility Test] When the following organosiloxane (B-5) was dispersed in a phenyl-modified silicone at a concentration of 25%, clouding and layer separation occurred. Furthermore, when the phenyl-modified organosiloxane (B-4) was dispersed under the same conditions as above, clouding and layer separation did not occur. On the other hand, when the novel organosiloxanes of Examples 1 to 3 were dispersed under the same conditions, clouding occurred but layer separation did not occur. Therefore, it can be said that the novel organosiloxanes exhibit compatibility with phenyl-modified silicones, although not as well as the phenyl-modified organosiloxane (B-4).

[0033] The compositions of Examples 4 to 9 and Comparative Examples 1 to 5 were obtained by mixing components (A) to (C) described below in the composition ratios shown in Tables 1 and 2.

[0034] Example 4 A thermally conductive phenyl-modified silicone composition was obtained by mixing A-1 as component (A), B-1 as component (B), and component (C). Mixing was carried out by placing plastic containers containing weighed-out components (A) to (C) in a rotation-revolution mixer (product name: Awatori Rentaro, manufactured by THINKY Corporation) and mixing at room temperature at 2,000 rpm for 1 minute twice. The resulting mixture was then cooled to room temperature and the viscosity was measured.

[0035] Example 5 A thermally conductive phenyl-modified silicone composition was prepared in the same manner as in Example 4, except that component (B) was changed from B-1 to B-2, and the viscosity was measured.

[0036] Example 6 A thermally conductive phenyl-modified silicone composition was prepared in the same manner as in Example 4, except that component (B) was changed from B-1 to B-3, and the viscosity was measured.

[0037] Comparative Example 1 A composition of Comparative Example 1 was prepared in the same manner as in Example 4, except that the component (B) was changed from B-1 to B-4, and the viscosity was measured.

[0038] Comparative Example 2 A composition of Comparative Example 2 was prepared in the same manner as in Example 4, except that the component (B) was changed from B-1 to B-5, and the viscosity was measured.

[0039] Comparative Example 3 A composition of Comparative Example 3 was prepared in the same manner as in Example 4, except that the component (B) was changed from B-1 to B-6, and the viscosity was measured.

[0040] Example 7 A thermally conductive phenyl-modified silicone composition was prepared in the same manner as in Example 4, except that component (A) was changed from A-1 to A-2, and the viscosity was measured.

[0041] Example 8 A thermally conductive phenyl-modified silicone composition was prepared in the same manner as in Example 4, except that component (A) was changed from A-1 to A-3, and the viscosity was measured.

[0042] Example 9 Thermally conductive phenyl-modified silicone compositions were prepared in the same manner as in Example 4, but with the composition and amount of component (C) changed (C-1 was changed to C-4), and viscosity measurements were carried out.

[0043] Comparative Example 4 A composition of Comparative Example 4 was prepared in the same manner as in Example 4, except that A-2 was added as component (A) in addition to A-1, and component (B) was not added, and the viscosity was measured.

[0044] Comparative Example 5 A composition of Comparative Example 5 was prepared in the same manner as in Example 4, except that the component (B) was not added and the content of the component (C) was changed, and the viscosity was measured.

[0045] (A) Organosiloxane A-1: ​​Represented by the following formula, having a kinematic viscosity of 700 mm 2 ・s -1 Organosiloxane

[0046] A-2: Represented by the following formula, kinematic viscosity is 380 mm 2 ・s -1 Phenyl-modified organosiloxane

[0047] A-3: Represented by the following formula, kinematic viscosity is 2,000 mm 2 ・s -1 Phenyl-modified organosiloxane

[0048] (B) Wetter B-1: Organosiloxane synthesized in Example 1 and represented by the following formula:

[0049] B-2: Organosiloxane synthesized in Example 2, represented by the following formula:

[0050] B-3: Organosiloxane synthesized in Example 3, represented by the following formula:

[0051] B-4: Organosiloxane represented by the following formula

[0052] B-5: Organosiloxane represented by the following formula:

[0053] B-6: Organosiloxane represented by the following formula

[0054] (C) Thermally conductive filler C-1: spherical alumina powder (average particle size 45 μm) C-2: spherical alumina powder (average particle size 10 μm) C-3: irregular alumina powder (average particle size 2 μm) C-4: irregular aluminum nitride powder (average particle size 30 μm)

[0055] [Production Method] Components (A) to (C) were mixed as follows to obtain compositions of the Examples and Comparative Examples: Plastic containers containing weighed components (A) to (C) were placed in a centrifugal mixer (trade name: Awatori Rentaro, manufactured by THINKY Corporation) in the composition ratios (by weight) shown in Tables 1 and 2, and the mixture was mixed at room temperature at 2,000 rpm for 1 minute twice, and then cooled to room temperature.

[0056] [Test Methods] The properties of the resulting compositions were measured using the following test methods, and the results are shown in the table below.

[0057] [Viscosity Measurement] The obtained composition was measured using a viscosity / viscoelasticity measuring device (trade name: MARS40 (Thermo Fisher Scientific Co., Ltd.)) at a rotation speed of 10 s -1 The viscosity at 23°C was measured using parallel plates with a gap of 0.5 mm.

[0058] The results in Tables 1 and 2 demonstrate that phenyl-modified silicone compositions containing the organopolysiloxane of the present invention have reduced viscosity, allowing for higher loadings of thermally conductive filler. In particular, despite the use of the high-viscosity A-3 as Component A in Example 8 and the use of a different Component C in Example 9, the viscosity increase of the composition was suppressed compared to Comparative Example 2. On the other hand, when B-4 (Comparative Example 1), which does not fall within the range represented by general formula (1), or B-5 (Comparative Example 2), which does not have a triphenylsiloxy group at the molecular chain terminal, was used, the viscosity of the composition increased. Furthermore, the viscosity of compositions not containing Component (B) (Comparative Examples 4 and 5) increased significantly. On the other hand, when B-6, which does not contain a phenyl group, was used (Comparative Example 3), the viscosity of the composition did not increase.

[0059] This specification includes the following aspects: [1]: An organopolysiloxane compound characterized by being represented by the following general formula (1): (In the formula, R 1 are independently aromatic hydrocarbon groups having 6 to 10 carbon atoms, and R 2 are independently alkyl groups having 1 to 10 carbon atoms, and R 3 is an alkyl group having 1 to 4 carbon atoms; a is 2 or 3, and n is an integer of 2≦n≦60.) [2]: In the general formula (1), R 1 is a phenyl group, R 2 [3]: A wetter comprising the organopolysiloxane compound according to [1] or [2] above, wherein R is a methyl group.

[0060] The present invention is not limited to the above-described embodiments. The above-described embodiments are merely examples, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and that exhibits similar effects is included within the technical scope of the present invention.

Claims

1. The following general formula (1): (In the formula, R 1 are each independently an aromatic hydrocarbon group having 6 to 10 carbon atoms; R 2 are independently an alkyl group having 1 to 10 carbon atoms; R 3 is an alkyl group having 1 to 4 carbon atoms; a is 2 or 3, and n is an integer satisfying 2≦n≦60.

2. The above R 1 is a phenyl group, and the R 2 2. The organopolysiloxane compound according to claim 1, wherein is a methyl group.

3. A wetter comprising the organopolysiloxane compound according to claim 1 or 2.

Citation Information

Patent Citations

  • Sealer composition for use in optical element, sealed structure, and optical element

    JP2004162039A

  • Cosmetic composition containing hydrocarbon oil and silicone oil

    JP2004262919A

  • Heat conductive silicone composition

    JP2004262972A

  • Heat conductive silicone composition

    JP2005162975A

  • Heat-conductive silicone oil composition, heat-dissipation agent and electronic device

    JP2007039621A

Cited By

  • Thermosoftening thermally conductive composition

    WO2025239281A1