Heat transfer printing receiving sheet and preparation method thereof
By designing the thermal insulation layer and the printing layer in the thermal transfer receiving sheet, the thermal welding and image durability problems are solved, and high optical density and stable image output are achieved.
Patent Information
- Application Number
- CN202411298619.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-18
- Publication Date
- 2025-02-07
- Estimated Expiration
- 2044-09-18
AI Technical Summary
The existing thermal transfer technology is prone to thermal welding during high-speed printing, and the resulting images have poor light resistance, weather resistance, wear resistance, durability, and low optical density.
A thermal transfer receiving sheet is designed, which includes a thermal insulation layer, a printing layer, a substrate and a back coating. The thermal insulation layer consists of a binder and hollow particles, which have thermal insulation and buffering properties; the printing layer uses a thermal sublimation ribbon with a dye layer to form an image by thermal sublimation.
It effectively prevents thermal welding of thermal transfer sheets and thermal sublimation ribbons, improves the optical density and durability of the image, and has good dye stability under high temperature and high humidity conditions.
Smart Images

Figure CN119388898A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of thermal transfer consumables, and in particular to a thermal transfer receiving sheet and a preparation method thereof. Background Art
[0002] In recent years, the sublimation transfer recording method, which forms an image on a thermal transfer receiving sheet by heating a ribbon having a thermal transfer layer containing a sublimable dye formed on a support such as a polyester film using a heating medium such as a thermal print head or laser, has attracted attention. Thermal sublimation printing technology is used as an information recording unit in various fields. According to such a thermal sublimation printing method, a full-color gradation image can be formed in a very short time, and intermediate colors and full colors with excellent reproducibility and grayscale can be obtained, forming a high-quality image equivalent to a silver halide photo.
[0003] The thermal sublimation printing method can control the amount of dye transfer in units of dots according to the applied energy, so the grayscale of the image formed is excellent. However, the image formed is different from the usual printing ink. The colorant is not a pigment but a low molecular weight dye, which has the disadvantages of poor light resistance, weather resistance, wear resistance and durability. In addition, in recent years, the speed of thermal sublimation printers has increased, and the temperature applied to the thermal head is high, resulting in thermal fusion of the thermal transfer sheet and the thermal sublimation ribbon. In order to solve the problem of thermal fusion, the existing technology increases the softening point of the resin constituting the receiving layer, but this will lead to a decrease in the optical density of the resulting pattern. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a thermal transfer receiving sheet and a preparation method thereof. In the thermal transfer receiving sheet of the present invention, the heat insulating layer has the properties of heat insulation and buffering, preventing the substrate from being heat-melted and having good adhesion; the printing layer is formed by heat sublimation of a heat sublimation ribbon with a dye layer to form an image, which is used as a material for forming the printing layer. Even when the printing speed is high, the thermal transfer sheet and the heat sublimation ribbon can be prevented from being heat-melted, and the demoulding property with the heat sublimation ribbon is also good, aging-resistant and able to improve the optical density of the printed image.
[0005] The technical solution of the present invention to solve the above technical problems is as follows:
[0006] The first object of the present invention is to provide a thermal transfer receiving sheet, comprising a printing layer, a heat insulating layer, a substrate and a back coating layer arranged in sequence from top to bottom;
[0007] The back coating layer comprises the following raw materials in parts by weight: 13-16 parts of a first resin, 2-3 parts of a filler, 0.1-0.5 parts of polyethylene glycol, and 0.01-0.05 parts of lithium chloride.
[0008] The heat insulation layer is composed of the following raw materials in parts by weight: 9-11 parts of adhesive and 4-7 parts of hollow particles;
[0009] The printing layer comprises the following raw materials in parts by weight: 19-22 parts of a second resin, 0.1-1 parts of aromatic hydrocarbon-modified polysiloxane, 0.1-1 parts of polyethylene glycol, and 0.1-1 parts of a polyisocyanate curing agent.
[0010] The beneficial effects of adopting the solution of the present invention are:
[0011] (1) In the heat insulating layer of the present invention, the adhesive and the hollow particles are matched to make the heat insulating layer have the performance of heat insulation and buffering, and the matching ratio between the hollow particles and the adhesive is limited to prevent the substrate from being heat-melted and have good adhesion. The printing layer is a necessary structure in the thermal transfer receiving sheet of the present invention. On the printing layer, the thermal sublimation ribbon with a dye layer forms an image through thermal sublimation. As the material used to form the printing layer, the material used is easy to accept sublimation dyes and is easy to form an image on the thermal transfer receiving sheet; the back coating layer is arranged on the opposite side of the printing layer of the substrate, which plays the role of improving the conveying performance of the thermal transfer receiving sheet, preventing the substrate from curling, and preventing static electricity.
[0012] (2) The thermal transfer receiving sheet prepared by the present invention can ensure that the dye does not escape under high temperature and high humidity conditions, and the overall Od value is significantly higher than that before addition, and has good aging resistance, light resistance, weather resistance, wear resistance and durability.
[0013] (3) The present invention limits the proportion of hollow particles to adhesive. If the content of hollow particles is too little relative to the adhesive, the voids in the thermal insulation layer will be reduced, and the thermal insulation and cushioning functions cannot be fully exerted. If the content is too much relative to the adhesive, the adhesion will be reduced, affecting the adhesion between the layers.
[0014] Furthermore, the substrate is at least one of a heat-resistant resin and paper;
[0015] The heat-resistant resin is at least one of polyester, polyarylate, polycarbonate, polyurethane, polyimide, polyetherimide, cellulose derivatives, polyethylene, ethylene-vinyl acetate copolymer, polypropylene, polystyrene, acrylic acid, polyvinyl chloride, polyvinylidene chloride, polyvinyl alcohol, polyvinyl butyral, and nylon;
[0016] The paper is at least one of capacitor paper, glass paper, sulfate paper, synthetic paper, high-quality paper, art paper, coated paper, cast coated paper, synthetic rubber latex impregnated paper, and fiber paper.
[0017] The beneficial effect of adopting the above further scheme is that the substrate of the present invention can withstand the heat applied during image formation, has mechanical properties that do not hinder handling, and can be appropriately selected according to the type of thermal transfer receiving sheet.
[0018] Furthermore, the synthetic paper is at least one of polystyrene synthetic paper and polyolefin synthetic paper.
[0019] Furthermore, the heat-resistant resin further includes an auxiliary agent.
[0020] Furthermore, the particle size of the hollow particles is 0.3-1.6 μm.
[0021] Furthermore, the thickness of the substrate is 30-300 μm, the thickness of the heat insulation layer is 1-10 μm, the thickness of the back coating layer is 1-20 μm, and the thickness of the printing layer is 1-10 μm.
[0022] The beneficial effect of adopting the above further solution is that the thickness of the thermal transfer receiving sheet can be guaranteed within this thickness range, and at the same time, the adhesion to the substrate and the heat resistance are good.
[0023] Furthermore, the thickness of the substrate is 100-250 μm, the thickness of the heat insulating layer is 1-5 μm, the thickness of the back coating layer is 3-10 μm, and the thickness of the printing layer is 1-5 μm.
[0024] Furthermore, the filler is at least one of an acrylic filler, a polyamide filler, a fluorine-based filler, an organic filler, an inorganic filler, and a conductive filler.
[0025] Furthermore, the organic filler may be polyethylene wax, zinc stearate, etc.; the inorganic filler may be talcum powder, silicon dioxide, gas silica, etc.; the conductive filler may be metal oxide, polyaniline sulfonic acid, etc.
[0026] Furthermore, the first resin is at least one of acrylic resin, cellulose resin, polycarbonate resin, polyvinyl alcohol resin, polyvinyl butyral resin, polyamide resin, polystyrene resin, polyester resin, and halogenated polymer.
[0027] The beneficial effect of adopting the above further scheme is that the back coating prepared by the above material can prevent the substrate from curling and static electricity. The resin with good heat resistance of Tg of 70°C or above is preferred. When the Tg of the resin is lower than this value, the heat resistance is obviously insufficient and it is easy to age.
[0028] Furthermore, the second resin is at least one of polyolefin resins, halogenated resins, ethylene resins, polyester resins, polystyrene resins, polyamide resins, olefin and vinyl polymer copolymer resins, cellulose resins, polycarbonate, vinyl chloride-vinyl acetate copolymers, polyvinyl butyral resins, and silicone resins.
[0029] The beneficial effect of adopting the above further solution is that the addition of the second resin of the present invention in the printing layer can react and chelate with the heat diffusive dye, ensuring that the dye does not overflow and escape under high temperature and high humidity conditions and has good stability.
[0030] Furthermore, the average molecular weight of the second resin is 10,000-70,000.
[0031] The beneficial effects of adopting the above further scheme are: when the molecular weight is low, the toughness of the printing layer is poor, and the addition of the second resin in the printing layer can react and chelate with the heat diffusive dye to ensure that the dye does not escape under high temperature and high humidity conditions, and has good stability. When the molecular weight of the second resin is low, the toughness of the printing layer is poor, and the dye is easy to escape, and the effect of the resin with higher molecular weight and Tg is more obvious, but when the molecular weight is too large, the stability of the printing layer is poor.
[0032] Furthermore, the molecular weight of the second resin is 50,000-60,000.
[0033] A second object of the present invention is to provide a method for preparing a thermal transfer receiving sheet, comprising the following steps:
[0034] S1: Prepared liquid: Back coating liquid: Add heat-resistant resin and filler into solvent to dissolve to prepare back coating liquid for standby use; Printing liquid: Add second resin into solvent to dissolve to prepare printing liquid for standby use; Heat insulation liquid: Add adhesive and hollow particles into solvent to dissolve to prepare heat insulation liquid for standby use;
[0035] S2: applying corona; providing a substrate, and applying corona on at least one side of the substrate;
[0036] S3: coating; coating the back coating liquid on the corona-charged side of the substrate, and then drying to form a back coating layer for standby use; then coating the heat insulating liquid on the side of the substrate away from the back coating layer, and then drying to form a heat insulating layer; finally coating the printing liquid on the side of the heat insulating layer away from the substrate, and then drying to form a printing layer, thereby obtaining a thermal transfer receiving sheet.
[0037] The beneficial effect of adopting the above further scheme is that the thermal transfer receiving sheet prepared by the above preparation method has low production cost and simple and feasible process.
[0038] Further, in step S1, the solvent is at least one of 2-butanone and toluene;
[0039] In step S3, a gravure coater is used to coat the back coating liquid, a gravure coater is used to coat the heat insulation liquid, and a gravure coater is used to coat the printing liquid. The coating speed is 100-150 m / min. The drying temperature is 60-100°C. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 Schematic diagram of the layer structure of the thermal transfer receiving sheet of the present invention.
[0041] In the accompanying drawings, the components represented by the reference numerals are listed as follows:
[0042] 1-substrate, 2-back coating, 3-thermal insulation layer, 4-printing layer. DETAILED DESCRIPTION
[0043] The principles and features of the present invention are described below, and the examples are only used to explain the present invention and are not used to limit the scope of the present invention. If no specific technology or conditions are specified in the embodiments, the technology or conditions described in the literature in this field or the product instructions are used. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased through regular channels.
[0044] Example 1: Preparation of thermal transfer receiving sheet
[0045] S1: Preparation of liquid: Back coating liquid: 0.5 parts of zinc stearate (SAK-ZS-PLB Singapore Samyak), 0.3 parts of polyethylene glycol (PEG-600 Youso Chemical), 15 parts of polyvinyl butyral resin (S-LEC BX-1 Japan Sekisui Chemical), 0.03 parts of lithium chloride, 2 parts of gas silicon (OK607 Evonik Chemical) add 45 parts of isopropanol and 40 parts of toluene to make a back coating liquid for standby use;
[0046] Printing liquid: 20 parts of vinyl chloride-vinyl acetate copolymer (H15-42 Wacker Chemical, Germany) with an average molecular weight of 35000-50000, a vinyl chloride content of 86%, and a glass transition temperature Tg of 70°C, 0.5 parts of aromatic modified polysiloxane (AFCONA-3252 Efcona Chemical), 1 part of polyethylene glycol (PEG-600 Youso Chemical), and 0.5 parts of polyisocyanate curing agent (TFD-90SB Asahi Chemical, Japan) are added to 37.4 parts of 2-butanone and 37.4 parts of toluene to dissolve to prepare a printing liquid for standby use;
[0047] Insulation liquid: 10 parts of styrene butadiene emulsion (101# Yoshida Chemical), 5 parts of hollow ball pigment with an average particle size of 1.6 μm (ROPAQUE TM TH-2000 Dow), 5 parts of isopropyl alcohol, mix evenly to make a heat insulation liquid for later use;
[0048] S2: Corona: Use foamed polypropylene (PP) sheet and apply EVA hot melt adhesive coating liquid on the PP sheet to make the thickness of the PP sheet 3g / m when dry. 2 , PP sheet and 140g / m 2 The substrate paper (purchased from Jinguan Paper) is laminated on both sides, with PE coating on the back, and the thickness when dry is 5g / m 2 , drying at 110° C. for 1 minute to obtain a substrate 1 having a layer structure of foamed PP / adhesive layer / substrate paper / PE; applying a corona on one side of the substrate 1;
[0049] S3: Coating: Use a gravure coater to coat the back coating liquid on the corona-charged side of the substrate 1 at a coating speed of 130m / min, with a coating thickness of 5μm, and then dry it at 80°C to form a back coating layer 2 for standby use; then use a gravure coater to coat the heat insulation liquid on the side of the substrate 1 away from the back coating layer 2 at a coating speed of 130m / min, with a coating thickness of 2μm, and then dry it at 80°C to form a heat insulation layer 3; finally, use a gravure coater to coat the printing liquid on the side of the heat insulation layer 3 away from the substrate 1 at a coating speed of 130m / min, with a coating thickness of 6μm, and then dry it at 80°C to form a printing layer 4, thereby obtaining a thermal transfer receiving sheet.
[0050] Example 2: Preparation of thermal transfer receiving sheet II
[0051] S1: Preparation of liquid: Back coating liquid: 0.5 parts of zinc stearate (SAK-ZS-PLB Singapore Samyak), 0.3 parts of polyethylene glycol (PEG-600 Youso Chemical), 15 parts of polyvinyl butyral resin (S-LEC BX-1 Japan Sekisui Chemical), 0.03 parts of lithium chloride, 2 parts of gas silicon (OK607 Evonik Chemical) add 45 parts of isopropanol and 40 parts of toluene to make a back coating liquid for standby use;
[0052] Printing liquid: 18 parts of vinyl chloride-vinyl acetate copolymer (H15-42 Wacker Chemical, Germany) with an average molecular weight of 35000-50000, a vinyl chloride content of 86%, and a glass transition temperature Tg of 70°C, 2 parts of polyvinyl butyral resin (BA-20S Sekisui Chemical, Japan), 0.5 parts of aromatic modified polysiloxane (AFCONA-3252 Efcona Chemical), 1 part of polyethylene glycol (PEG-600 Youso Chemical), and 0.5 parts of polyisocyanate curing agent (TFD-90SB Asahi Chemical, Japan) are added to 37.4 parts of 2-butanone and 37.4 parts of toluene to dissolve to prepare a printing liquid for standby use;
[0053] Insulation liquid: 10 parts of styrene butadiene emulsion (101# Yoshida Chemical), 5 parts of hollow ball pigment with an average particle size of 1.6 μm (ROPAQUE TM TH-2000 Dow), 5 parts of isopropyl alcohol, mix evenly to make a heat insulation liquid for later use;
[0054] S2: Corona: Use foamed polypropylene (PP) sheet and apply EVA hot melt adhesive coating liquid on the PP sheet to make the thickness of the PP sheet 3g / m when dry. 2 , PP sheet and 140g / m 2 The substrate paper (purchased from Jinguan Paper) is laminated on both sides, with PE coating on the back, and the thickness when dry is 5g / m 2 Drying at 110° C. for 1 minute to obtain a substrate 1 having a layer structure of foamed PP / adhesive layer / substrate paper / PE; applying corona on one side of the substrate 1;
[0055] S3: Coating: Use a gravure coater to coat the back coating liquid on the corona-charged side of the substrate 1 at a coating speed of 130m / min, with a coating thickness of 3μm, and then dry it at 80°C to form a back coating layer 2 for standby use; then use a gravure coater to coat the heat insulation liquid on the side of the substrate 1 away from the back coating layer 2 at a coating speed of 130m / min, with a coating thickness of 1μm, and then dry it at 80°C to form a heat insulation layer 3; finally, use a gravure coater to coat the printing liquid on the side of the heat insulation layer 3 away from the substrate 1 at a coating speed of 130m / min, with a coating thickness of 4μm, and then dry it at 80°C to form a printing layer 4, thereby obtaining a thermal transfer receiving sheet.
[0056] Example 3: Preparation of thermal transfer receiving sheet
[0057] S1: Preparation of liquid: Back coating liquid: 0.5 parts of zinc stearate (SAK-ZS-PLB Singapore Samyak), 0.3 parts of polyethylene glycol (PEG-600 Youso Chemical), 15 parts of polyvinyl butyral resin (S-LEC BX-1 Japan Sekisui Chemical), 0.03 parts of lithium chloride, 2 parts of gas silicon (OK607 Evonik Chemical) add 45 parts of isopropanol and 40 parts of toluene to make a back coating liquid for standby use;
[0058] Printing liquid: 20 parts of vinyl chloride-vinyl acetate copolymer (SOLBIN-C Nissin Chemical), 0.5 parts of aromatic hydrocarbon modified polysiloxane (AFCONA-3252 Efcona Chemical), 1 part of polyethylene glycol (PEG-600 Youso Chemical), 0.5 parts of polyisocyanate curing agent (TFD-90SB Asahi Chemical Co., Ltd., Japan) were added to 37.4 parts of 2-butanone and 37.4 parts of toluene to dissolve and prepare the printing liquid for use;
[0059] Insulation liquid: 10 parts of styrene butadiene emulsion (101# Yoshida Chemical), 5 parts of hollow ball pigment with an average particle size of 1.6 μm (ROPAQUE TM TH-2000 Dow), 5 parts of isopropyl alcohol, mix evenly to make a heat insulation liquid for later use;
[0060] S2: Corona: Use foamed polypropylene (PP) sheet and apply EVA hot melt adhesive coating liquid on the PP sheet to make the thickness of the PP sheet 3g / m when dry. 2 , PP sheet and 140g / m 2 The substrate paper is laminated on both sides, and the back side is PE coated. The thickness when dry is 5g / m 2 Drying at 110° C. for 1 minute to obtain a substrate 1 having a layer structure of foamed PP / adhesive layer / substrate paper / PE; applying corona on one side of the substrate 1;
[0061] S3: Coating: Use a gravure coater to coat the back coating liquid on the corona-charged side of the substrate 1 at a coating speed of 130m / min, with a coating thickness of 6μm, and then dry it at 80℃ to form a back coating layer 2 for standby use; then use a gravure coater to coat the heat insulation liquid on the side of the substrate 2 away from the back coating layer 2 at a coating speed of 130m / min, with a coating thickness of 1-3μm, and then dry it at 80℃ to form a heat insulation layer 3; finally, use a gravure coater to coat the printing liquid on the side of the heat insulation layer 3 away from the substrate 1 at a coating speed of 130m / min, with a coating thickness of 4-7μm, and then dry it at 80℃ to form a printing layer 4, thereby obtaining a thermal transfer receiving sheet.
[0062] Example 4: Preparation of thermal transfer receiving sheet
[0063] S1: Preparation of liquid: Back coating liquid: 0.5 parts of zinc stearate (SAK-ZS-PLB Singapore Samyak), 0.3 parts of polyethylene glycol (PEG-600 Youso Chemical), 15 parts of polyvinyl butyral resin (S-LEC BX-1 Japan Sekisui Chemical), 0.03 parts of lithium chloride, 2 parts of gas silicon (OK607 Evonik Chemical) add 45 parts of isopropanol and 40 parts of toluene to make a back coating liquid for standby use;
[0064] Printing liquid: 20 parts of vinyl chloride-vinyl acetate copolymer (SOLBIN-C Nissin Chemical), 0.5 parts of silicone resin (BYK-323 Germany Bick), 1 part of polyethylene glycol (PEG-600 Youso Chemical), 0.5 parts of polyisocyanate curing agent (TFD-90SB Japan Asahi Chemical) were added to 37.4 parts of 2-butanone and 37.4 parts of toluene to dissolve and prepare the printing liquid for use;
[0065] Insulation liquid: 10 parts of styrene butadiene emulsion (101# Yoshida Chemical), 5 parts of hollow ball pigment with an average particle size of 1.6 μm (ROPAQUE TM TH-2000 Dow), 5 parts of isopropyl alcohol, mix evenly to make a heat insulation liquid for later use;
[0066] S2: Corona: Use foamed polypropylene (PP) sheet and apply EVA hot melt adhesive coating liquid on the PP sheet to make the thickness of the PP sheet 3g / m when dry. 2 , PP sheet and 140g / m 2 The substrate paper (purchased from Jinguan Paper) is laminated on both sides, with PE coating on the back, and the thickness when dry is 5g / m 2 Drying at 110° C. for 1 minute to obtain a substrate 1 having a layer structure of foamed PP / adhesive layer / substrate paper / PE; applying corona on one side of the substrate 1;
[0067] S3: Coating: Use a gravure coater to coat the back coating liquid on the corona-charged side of the substrate 1 at a coating speed of 130m / min, with a coating thickness of 3-6μm, and then dry it at 80℃ to form a back coating layer 2 for standby use; then use a gravure coater to coat the heat insulation liquid on the side of the substrate away from the back coating layer 2 at a coating speed of 130m / min, with a coating thickness of 1-3μm, and then dry it at 80℃ to form a heat insulation layer 3; finally, use a gravure coater to coat the printing liquid on the side of the heat insulation layer 3 away from the substrate 1 at a coating speed of 130m / min, with a coating thickness of 4-7μm, and then dry it at 80℃ to form a printing layer 4, thereby obtaining a thermal transfer receiving sheet.
[0068] Example 5: Preparation of thermal transfer receiving sheet
[0069] S1: Preparation of liquid: Back coating liquid: 0.5 parts of zinc stearate (SAK-ZS-PLB Singapore Samyak), 0.3 parts of polyethylene glycol (PEG-600 Youso Chemical), 15 parts of polyvinyl butyral resin (S-LEC BX-1 Japan Sekisui Chemical), 0.03 parts of lithium chloride, 2 parts of gas silicon (OK607 Evonik Chemical) add 45 parts of isopropanol and 40 parts of toluene to make a back coating liquid for standby use;
[0070] Printing liquid: 20 parts of vinyl chloride-vinyl acetate copolymer (H40-60 Wacker Chemical, Germany) with an average molecular weight of 100,000-140,000, a vinyl chloride content of 61%, and a glass transition temperature Tg of 62°C, 0.5 parts of aromatic modified polysiloxane (AFCONA-3252 Efcona Chemical), 1 part of polyethylene glycol (PEG-600 Youso Chemical), and 0.5 parts of polyisocyanate curing agent (TFD-90SB Asahi Chemical, Japan) are added to 37.4 parts of 2-butanone and 37.4 parts of toluene to dissolve to prepare a printing liquid for standby use;
[0071] Insulation liquid: 10 parts of styrene butadiene emulsion (101# Yoshida Chemical), 5 parts of hollow ball pigment with an average particle size of 1.6 μm (ROPAQUE TM TH-2000 Dow), 5 parts of isopropyl alcohol, mix evenly to make a heat insulation liquid for later use.
[0072] S2: Corona: Use foamed polypropylene (PP) sheet and apply EVA hot melt adhesive coating liquid on the PP sheet to make the thickness of the PP sheet 3g / m when dry. 2 , PP sheet and 140g / m 2 The substrate paper (purchased from Jinguan Paper) is laminated on both sides, with PE coating on the back, and the thickness when dry is 5g / m 2 Drying at 110° C. for 1 minute to obtain a substrate 1 having a layer structure of foamed PP / adhesive layer / substrate paper / PE; applying corona on one side of the substrate 1;
[0073] S3: Coating: Use a gravure coater to coat the back coating liquid on the corona-charged side of the substrate 1 at a coating speed of 130m / min, with a coating thickness of 3-6μm, and then dry it at 80℃ to form a back coating layer 2 for standby use; then use a gravure coater to coat the heat insulation liquid on the side of the substrate away from the back coating layer 2 at a coating speed of 130m / min, with a coating thickness of 1-3μm, and then dry it at 80℃ to form a heat insulation layer 3; finally, use a gravure coater to coat the printing liquid on the side of the heat insulation layer 3 away from the substrate 1 at a coating speed of 130m / min, with a coating thickness of 4-7μm, and then dry it at 80℃ to form a printing layer 4, thereby obtaining a thermal transfer receiving sheet.
[0074] Comparative Example 1: Preparation of thermal transfer receiving sheet
[0075] The difference between this comparative example and Example 1 is only the change in the raw materials for preparing the thermal insulation liquid, and the remaining preparation raw materials and steps are the same as those in Example 1. Step S1 is specifically as follows:
[0076] S1: Prepare solution:
[0077] Back coating liquid: 0.5 parts of zinc stearate (SAK-ZS-PLB Singapore Samyuk), 0.3 parts of polyethylene glycol (PEG-600 Youso Chemical), 15 parts of polyvinyl butyral resin (S-LEC BX-1 Japan Sekisui Chemical), 0.03 parts of lithium chloride, 2 parts of gas silicon (OK607 Evonik Chemical) add 45 parts of isopropanol and 40 parts of toluene to make a back coating liquid for use;
[0078] Printing liquid: 20 parts of vinyl chloride-vinyl acetate copolymer (H15-42 Wacker Chemical, Germany), 0.5 parts of aromatic modified polysiloxane (AFCONA-3252 Efcona Chemical), 1 part of polyethylene glycol (PEG-600 Youso Chemical), 0.5 parts of polyisocyanate curing agent (TFD-90SB Asahi Chemical, Japan) were added to 37.4 parts of 2-butanone and 37.4 parts of toluene to dissolve and prepare the printing liquid for use;
[0079] Insulation liquid: 10 parts of styrene butadiene emulsion (101# Yoshida Chemical), 5 parts of hollow ball pigment with an average particle size of 0.4 μm (ROPAQUE TM HP-380 Dow), 5 parts isopropyl alcohol, mix evenly to make a heat insulation liquid for later use.
[0080] Comparative Example 2: Preparation of thermal transfer receiving sheet
[0081] The difference between this comparative example and Example 1 is that no heat insulating liquid and heat insulating layer are prepared, and the remaining preparation materials and steps are the same as those of Example 1. Step S1 is as follows:
[0082] S1: Prepare solution:
[0083] Back coating liquid: 0.5 parts of zinc stearate (SAK-ZS-PLB Singapore Samyuk), 0.3 parts of polyethylene glycol (PEG-600 Youso Chemical), 15 parts of polyvinyl butyral resin (S-LEC BX-1 Japan Sekisui Chemical), 0.03 parts of lithium chloride, 2 parts of gas silicon (S-LEC BX-1 Japan Sekisui Chemical) add 45 parts of isopropanol and 40 parts of toluene to make a back coating liquid for use;
[0084] Printing liquid: 20 parts of vinyl chloride-vinyl acetate copolymer (H15-42 Wacker Chemical, Germany), 0.5 parts of aromatic modified polysiloxane (AFCONA-3252 Efcona Chemical), 1 part of polyethylene glycol (PEG-600 Youso Chemical), 0.5 parts of polyisocyanate curing agent (TFD-90SB Asahi Chemical, Japan) were added to 37.4 parts of 2-butanone and 37.4 parts of toluene to dissolve and prepare the printing liquid for use;
[0085] S2: Corona: Use foamed polypropylene (PP) sheet and apply EVA hot melt adhesive coating liquid on the PP sheet to make the thickness of the PP sheet 3g / m when dry. 2 , PP sheet and 140g / m 2 The substrate paper (purchased from Jinguan Paper) is laminated on both sides, with PE coating on the back, and the thickness when dry is 5g / m 2 Drying at 110° C. for 1 minute to obtain a substrate 1 having a layer structure of foamed PP / adhesive layer / substrate paper / PE; applying corona on one side of the substrate 1;
[0086] S3: coating; using a gravure coater to coat the back coating liquid on the corona-charged side of the substrate 1 at a coating speed of 130 m / min, the coating thickness is 5 μm, and then drying at 80°C to form a back coating layer 2 for standby use; finally, using a gravure coater to coat the printing liquid on the side of the back coating layer 3 away from the substrate at a coating speed of 130 m / min, the coating thickness is 6 μm, and then drying at 80°C to form a printing layer 4, thus obtaining a thermal transfer receiving sheet.
[0087] Comparative Example 3: Preparation of thermal transfer receiving sheet
[0088] The difference between this comparative example and Example 1 is that the back coating liquid and the back coating layer are not prepared, and the remaining preparation materials and steps are the same as those of Example 1. Step S1 is as follows:
[0089] S1: Prepare solution:
[0090] Printing liquid: 20 parts of vinyl chloride-vinyl acetate copolymer (H15-42 Wacker Chemical, Germany), 0.5 parts of aromatic modified polysiloxane (AFCONA-3252 Efcona Chemical), 1 part of polyethylene glycol (PEG-600 Youso Chemical), 0.5 parts of polyisocyanate curing agent (TFD-90SB Asahi Chemical, Japan) were added to 37.4 parts of 2-butanone and 37.4 parts of toluene to dissolve and prepare the printing liquid for use;
[0091] Insulation liquid: 10 parts of styrene butadiene emulsion (101# Yoshida Chemical), 5 parts of hollow ball pigment with an average particle size of 1.6 μm (ROPAQUE TM TH-2000 Dow), 5 parts of isopropyl alcohol, mix evenly to make a heat insulation liquid for later use;
[0092] S2: Corona: Use foamed polypropylene (PP) sheet and apply EVA hot melt adhesive coating liquid on the PP sheet to make the thickness of the PP sheet 3g / m when dry. 2 , PP sheet and 140g / m 2 The substrate paper (purchased from Jinguan Paper) is laminated on both sides, with PE coating on the back, and the thickness when dry is 5g / m 2 Drying at 110° C. for 1 minute to obtain a substrate 1 having a layer structure of foamed PP / adhesive layer / substrate paper / PE; applying corona on one side of the substrate 1;
[0093] S3: coating; using a gravure coater to coat the insulation liquid on the side of the substrate 1 away from the electrostatic discharge at a coating speed of 130 m / min, the coating thickness is 2 μm, and then drying at 80°C to form an insulation layer 3; using a gravure coater to coat the printing liquid on the side of the insulation layer 3 away from the substrate 1 at a coating speed of 130 m / min, the coating thickness is 6 μm, and then drying at 80°C to form a printing layer 4, thus obtaining a thermal transfer receiving sheet.
[0094] Comparative Example 4: Preparation of thermal transfer receiving sheet
[0095] The difference between this comparative example and Example 2 is that the raw materials used for the printing liquid are different. The BA-20S resin with an average molecular weight of 15000-25000 and a glass transition temperature Tg of 84°C is replaced with a BA-55HH resin with a Tg (glass transition temperature) of 92°C and a molecular weight of 50000-60000. The remaining preparation raw materials and steps are the same as those in Example 1. The specific steps are as follows:
[0096] S1: Preparation of liquid: Back coating liquid: 0.5 parts of zinc stearate (SAK-ZS-PLB Singapore Samyak), 0.3 parts of polyethylene glycol (PEG-600 Youso Chemical), 15 parts of polyvinyl butyral resin (S-LEC BX-1 Japan Sekisui Chemical), 0.03 parts of lithium chloride, 2 parts of gas silicon (OK607 Evonik Chemical) add 45 parts of isopropanol and 40 parts of toluene to make a back coating liquid for standby use;
[0097] Printing liquid: 18 parts of vinyl chloride-vinyl acetate copolymer (H15-42 Wacker Chemical, Germany), 2 parts of polyvinyl butyral resin (BA-55HH, Sekisui Chemical, Japan), 0.5 parts of aromatic modified polysiloxane (AFCONA-3252, Efcona Chemical), 1 part of polyethylene glycol (PEG-600, Youso Chemical), 0.5 parts of polyisocyanate curing agent (TFD-90SB, Asahi Chemical, Japan) were added to 37.4 parts of 2-butanone and 37.4 parts of toluene to dissolve and prepare the printing liquid for use;
[0098] S2: Corona: Use foamed polypropylene (PP) sheet and apply EVA hot melt adhesive coating liquid on the PP sheet to make the thickness of the PP sheet 3g / m when dry. 2 , PP sheet and 140g / m 2 The substrate paper (purchased from Jinguan Paper) is laminated on both sides, with PE coating on the back, and the thickness when dry is 5g / m 2 Drying at 110° C. for 1 minute to obtain a substrate 1 having a layer structure of foamed PP / adhesive layer / substrate paper / PE; applying corona on one side of the substrate 1;
[0099] S3: coating; use a gravure coater to coat the back coating liquid on the corona-charged side of the substrate 1 at a coating speed of 130m / min, with a coating thickness of 5μm, and then dry it at 80°C to form a back coating layer 2 for standby use; then use a gravure coater to coat the heat-insulating liquid on the side of the substrate 1 away from the back coating layer 2 at a coating speed of 130m / min, with a coating thickness of 2μm, and then dry it at 80°C to form a heat-insulating layer 3; finally, use a gravure coater to coat the printing liquid on the other side of the substrate 1 at a coating speed of 130m / min, with a coating thickness of 6μm, and then dry it at 80°C to form a printing layer 4, thereby obtaining a thermal transfer receiving sheet.
[0100] Test example: performance test
[0101] The samples prepared in Examples 1-4 and Comparative Examples 1-5 were printed using a DNP DS620 thermal sublimation printer. The original DNP DS620 ribbon was used for printing and artificial accelerated weathering aging test. The artificial accelerated weathering test was carried out in accordance with the GB / T 1865-2009 standard. The maximum optical density, color difference ΔE, and Od retention were tested using an X-Rite color densitometer and a colorimeter.
[0102] Table 1
[0103]
[0104] From Table 1, we can get:
[0105] Under high temperature and high humidity conditions (90%, 60°C), the back coating layer has a significant effect on improving the Od retention rate of the thermal transfer receiving sheet; the sufficient void structure in the thermal insulation layer can play a role in improving the Od value. The smaller the particle size of the hollow particles in the thermal insulation layer, the denser the overall voids and the higher the Od value; the addition of polyvinyl butyral resin in the printing layer can react and chelate with the heat-diffusive dye to ensure that the dye does not escape under high temperature and high humidity conditions. The overall Od value is significantly higher than before addition, and the effect of resins with higher molecular weight and Tg is more obvious.
[0106] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A thermal transfer receiving sheet, characterized in that: The thermal transfer receiving sheet comprises a printing layer, a heat insulating layer, a substrate and a back coating layer arranged in sequence from top to bottom; The back coating layer comprises the following raw materials in parts by weight: 13-16 parts of the first resin, 2-3 parts of the filler, 0.1-0.5 parts of polyethylene glycol, and 0.01-0.05 parts of lithium chloride; The heat insulation layer is composed of the following raw materials in parts by weight: 9-11 parts of adhesive and 4-7 parts of hollow particles; The printing layer comprises the following raw materials in parts by weight: 19-22 parts of a second resin, 0.1-1 parts of aromatic hydrocarbon-modified polysiloxane, 0.1-1 parts of polyethylene glycol, and 0.1-1 parts of a polyisocyanate curing agent.
2. A thermal transfer receiving sheet according to claim 1, characterized in that: The substrate is at least one of a heat-resistant resin and paper; The heat-resistant resin is at least one of polyester, polyarylate, polycarbonate, polyurethane, polyimide, polyetherimide, cellulose derivatives, polyethylene, ethylene-vinyl acetate copolymer, polypropylene, polystyrene, acrylic acid, polyvinyl chloride, polyvinylidene chloride, polyvinyl alcohol, polyvinyl butyral, and nylon; The paper is at least one of capacitor paper, glass paper, sulfate paper, synthetic paper, high-quality paper, art paper, coated paper, cast coated paper, synthetic rubber latex impregnated paper, and fiber paper.
3. A thermal transfer receiving sheet according to claim 1, characterized in that: The particle size of the hollow particles is 0.3-1.6 μm.
4. A thermal transfer receiving sheet according to claim 1, characterized in that: The thickness of the substrate is 30-300 μm, the thickness of the heat-insulating layer is 1-10 μm, the thickness of the back coating layer is 1-20 μm, and the thickness of the printing layer is 1-10 μm.
5. A thermal transfer receiving sheet according to claim 1, characterized in that: The filler is at least one of acrylic filler, polyamide filler, fluorine filler, organic filler, inorganic filler and conductive filler.
6. A thermal transfer receiving sheet according to claim 1, characterized in that: The first resin is at least one of acrylic resin, cellulose resin, polycarbonate resin, polyvinyl alcohol resin, polyvinyl butyral resin, polyamide resin, polystyrene resin, polyester resin, and halogenated polymer.
7. A thermal transfer receiving sheet according to claim 1, characterized in that: The second resin is at least one of polyolefin resins, halogenated resins, ethylene resins, polyester resins, polystyrene resins, polyamide resins, olefin and vinyl polymer copolymer resins, cellulose resins, polycarbonate, vinyl chloride-vinyl acetate copolymers, polyvinyl butyral resins, and silicone resins.
8. A thermal transfer receiving sheet according to claim 1, characterized in that: The average molecular weight of the second resin is 10,000-70,000.
9. A method for preparing a thermal transfer receiving sheet according to any one of claims 1 to 8, characterized in that: The following steps are involved: S1: Prepared liquid: Back coating liquid: Add heat-resistant resin and filler into solvent to dissolve to prepare back coating liquid for standby use; Printing liquid: Add second resin into solvent to dissolve to prepare printing liquid for standby use; Heat insulation liquid: Add adhesive and hollow particles into solvent to dissolve to prepare heat insulation liquid for standby use; S2: applying corona; providing a substrate, and applying corona on at least one side of the substrate; S3: coating; coating the back coating liquid on the corona-charged side of the substrate, and then drying to form a back coating layer for standby use; then coating the heat insulating liquid on the side of the substrate away from the back coating layer, and then drying to form a heat insulating layer; finally coating the printing liquid on the side of the heat insulating layer away from the substrate, and then drying to form a printing layer, thereby obtaining a thermal transfer receiving sheet.
10. The method for preparing a thermal transfer receiving sheet according to claim 9, characterized in that: In step S1, the solvent is at least one of 2-butanone and toluene; In step S3, a gravure coater is used to coat the back coating liquid, a gravure coater is used to coat the heat insulation liquid, and a gravure coater is used to coat the printing liquid. The coating speed is 100-150 m / min. The drying temperature is 60-100°C.
Citation Information
Patent Citations
Thermal transfer image receiving sheet and method for producing same
CN106536211A
Thermal transfer recording medium
JP2015016701A
Combination of thermal transfer sheet and thermal transfer image-receiving sheet, and image forming method
JP2015066775A
Image-receiving sheet for sublimation transfer
JP2018176458A
Thermal transfer image receiving sheet and manufacturing method thereof
JP2020055192A
Cited By
Thermal sublimation foaming thermal transfer ribbon and preparation method thereof
CN120024140A
Thermal transfer printing receiving sheet and application thereof
CN121043520A