Polarizing film, image display device, polarized sunglasses, and method for producing polarizing film

A thin polarizing film made with polyvinyl alcohol resin and specific azo compounds, using a specialized manufacturing process, addresses the issues of decolorization and thermal shrinkage in harsh environments, ensuring stable polarizing properties and dimensional stability for image display devices and polarized sunglasses.

WO2024214690A1PCT designated stage expired Publication Date: 2024-10-17NITTO DENKO CORP +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/014372
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-13
Filing Date
2024-04-09
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Conventional polarizing films used in image display devices and polarized sunglasses suffer from decolorization and thermal shrinkage when exposed to harsh environments, such as high temperature and high humidity, leading to deteriorated polarizing properties and size variations.

Method used

A polarizing film with a thickness of 10 μm or less, composed of a polyvinyl alcohol resin and azo compounds with specific ureido and naphthyl groups, is developed, along with a manufacturing method involving laminate production, dry and wet stretching, and dyeing steps to enhance durability and prevent decolorization and thermal shrinkage.

Benefits of technology

The polarizing film effectively suppresses decolorization and thermal shrinkage, maintaining excellent polarizing properties and dimensional stability, even in humid conditions, while improving puncture strength and flexibility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024014372_17102024_PF_FP_ABST
    Figure JP2024014372_17102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided are: a polarizing film capable of suppressing discoloration and heat shrinkage; and a method for producing a polarizing film. The polarizing film according to an embodiment of the present invention is 10 μm or less and contains a polyvinyl alcohol-based resin, wherein the polarizing film contains at least a first dye that is an azo compound having the ureido skeleton represented by formula (1) or a salt of the azo compound.
Need to check novelty before this filing date? Find Prior Art

Description

Polarizing film, image display device, polarized sunglasses, and method for manufacturing polarizing film

[0001] The present invention relates to a polarizing film, an image display device, polarized sunglasses, and a method for manufacturing a polarizing film.

[0002] Polarizing plates including a polarizing film are optical components used in image display devices and polarized sunglasses, and for example, polarizing plates including a polarizing film containing iodine, a dichroic material, and a polyvinyl alcohol-based resin are known (see, for example, Patent Document 1). However, the polarizing plate described in Patent Document 1 may suffer from discoloration (color loss) and a deterioration in polarization properties, or may suffer from thermal shrinkage and size fluctuations, when placed in a harsh environment such as a high-temperature, high-humidity environment for a long period of time.

[0003] International Publication No. 2010 / 100917

[0004] The present invention has been made to solve the above-mentioned problems of the conventional art, and a main object of the present invention is to provide a polarizing film, an image display device, polarized sunglasses, and a method for manufacturing a polarizing film, which are capable of suppressing the occurrence of discoloration and thermal shrinkage.

[0005] [1] A polarizing film according to an embodiment of the present invention is a polarizing film having a thickness of 10 μm or less, which contains a polyvinyl alcohol-based resin and at least a first dye which is an azo compound having a ureido skeleton represented by the following formula (1) or a salt thereof: In formula (1), Ay 1 and Ay 2 each independently represents a naphthyl group which may have a substituent, or a phenyl group which may have a substituent; s and t each independently represent 0 or 1, and either s or t is 1; Ry 1 ~Ry 8each independently represents a hydrogen atom or a substituent; the phenyl group which may have a substituent is a phenyl group which has at least one substituent selected from the group consisting of a sulfo group, a carboxy group, an alkoxy group having 1 to 4 carbon atoms and having a sulfo group, an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a halogen atom, a nitro group, an amino group, an alkyl-substituted amino group having 1 to 4 carbon atoms, and an alkyl-substituted acylamino group having 1 to 4 carbon atoms; and the naphthyl group which may have a substituent is a naphthyl group which may have a substituent selected from the group consisting of a hydroxy group, an alkoxy group having 1 to 4 carbon atoms and having a sulfo group, and a sulfo group; Ry 1 , Ry 2 , Ry 7 , Ry 8 are each independently a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, or an alkoxy group having 1 to 4 carbon atoms; Ry 3 ~Ry 6 are each independently a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, or an alkoxy group having 1 to 4 carbon atoms and a sulfo group. [2] In the polarizing film according to [1] above, the polyvinyl alcohol-based resin may have an orientation function of 0.30 or less. [3] The polarizing film according to [1] or [2] above may further contain a second dye which is an azo compound represented by the following formula (2) or a salt thereof, and a third dye which is an azo compound represented by the following formula (3) or a salt thereof: In formula (2), Ar 11 represents a phenyl group having a substituent or a naphthyl group having a substituent, Rr 11 ~Rr 16 each independently represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, or an alkoxy group having 1 to 4 carbon atoms and a sulfo group; 11represents an amino group optionally having a substituent selected from the group consisting of an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a sulfo group, an amino group, and a substituted amino group; a benzoyl group optionally having a substituent selected from the group consisting of an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a sulfo group, an amino group, and a substituted amino group; a phenylamino group optionally having a substituent selected from the group consisting of an alkoxy group having 1 to 4 carbon atoms, a sulfo group, an amino group, and a substituted amino group; a benzoylamino group optionally having a substituent selected from the group consisting of an alkoxy group having 1 to 4 carbon atoms, a sulfo group, an amino group, and a substituted amino group; a phenylazo group optionally having a substituent selected from the group consisting of an alkoxy group having 1 to 4 carbon atoms, a sulfo group, a hydroxy group, an amino group, and a substituted amino group; or a naphthotriazole group optionally having a substituent selected from the group consisting of an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a sulfo group, an amino group, and a substituted amino group; 15 and Rr 16 each independently represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, or an alkoxy group having 1 to 4 carbon atoms; when m1 and n1 are 0, Rr 11 and Rr 12 each independently represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, or an alkoxy group having 1 to 4 carbon atoms and a sulfo group. In formula (3), A is Ar in formula (2). 11 or the following general formula (4): (In formula (4), A 1 represents a nitro group or an amino group), and R 1 ~R 4 , R 6 is Rr in the formula (2) 11 ~Rr 14 X is the same as Xr 11and m and n are each 0 or 1. [4] An in-vehicle liquid crystal display device according to another aspect of the present invention includes the polarizing film according to any one of [1] to [3] above. [5] An image display device according to yet another aspect of the present invention includes the polarizing film according to any one of [1] to [3] above. [6] Polarized sunglasses according to yet another aspect of the present invention include the polarizing film according to any one of [1] to [3] above. [7] A method for producing a polarizing film according to yet another aspect of the present invention includes a laminate production step, a dry stretching step, a dyeing step, a wet stretching step, and a drying shrinkage step, in this order. In the laminate production step, a coating liquid containing a polyvinyl alcohol-based resin is applied to a long thermoplastic resin substrate to produce a laminate including a polyvinyl alcohol-based resin layer and the thermoplastic resin substrate. In the dry stretching step, the laminate is stretched in air. In the dyeing step, the polyvinyl alcohol-based resin layer after the dry stretching step is dyed with a first dye which is an azo compound having a ureido skeleton represented by formula (1) or a salt thereof. In the wet stretching step, the polyvinyl alcohol-based resin layer after the dyeing step is stretched in a stretching bath. In the drying shrinking step, the polyvinyl alcohol-based resin layer after the wet stretching step is shrunk in a width direction perpendicular to the longitudinal direction while being transported in the longitudinal direction, to adjust the thickness to 10 μm or less. [8] In the method for producing a polarizing film according to the above item [7], the stretching ratio in the dry stretching step may be 2.1 times or more, and the stretching ratio in the wet stretching step may be 2.0 times or less.

[0006] According to the embodiments of the present invention, it is possible to realize a polarizing film, an image display device, and polarized sunglasses that can suppress the occurrence of discoloration and thermal shrinkage.

[0007] Fig. 1 is a schematic cross-sectional view of an optical laminate including a polarizing film according to one embodiment of the present invention. Fig. 2 is a schematic cross-sectional view of an optical laminate including a polarizing film according to another embodiment of the present invention. Fig. 3 is a schematic cross-sectional view of an optical laminate including a polarizing film according to yet another embodiment of the present invention.

[0008] Representative embodiments of the present invention will be described below, but the present invention is not limited to these embodiments. In addition, in order to clarify the explanation, the width, thickness, shape, etc. of each part may be shown schematically in the drawings compared to the embodiments, but these are merely examples and do not limit the interpretation of the present invention.

[0009] (Definition of Terms and Symbols) The definitions of terms and symbols used in this specification are as follows. (1) Refractive Index (nx, ny, nz) "nx" is the refractive index in the direction in which the in-plane refractive index is maximum (i.e., the slow axis direction), "ny" is the refractive index in the in-plane direction perpendicular to the slow axis (i.e., the fast axis direction), and "nz" is the refractive index in the thickness direction. (2) In-Plane Retardation (Re) "Re(λ)" is the in-plane retardation measured with light having a wavelength of λ nm at 23°C. For example, "Re(550)" is the in-plane retardation measured with light having a wavelength of 550 nm at 23°C. Re(λ) is calculated by the formula: Re(λ) = (nx - ny) × d, where d (nm) is the thickness of the layer (film). (3) Thickness Direction Retardation (Rth) "Rth(λ)" is the retardation in the thickness direction measured with light having a wavelength of λ nm at 23°C. For example, "Rth(550)" is the retardation in the thickness direction measured with light having a wavelength of 550 nm at 23°C. Rth(λ) is calculated by the formula: Rth(λ) = (nx - nz) × d, where d (nm) is the thickness of the layer (film). (4) Nz Coefficient The Nz coefficient is calculated by Nz = Rth / Re. (5) Angle When an angle is referred to in this specification, the angle includes both clockwise and counterclockwise angles with respect to a reference direction. Thus, for example, "45°" means ±45°. (6) Substantially Parallel or Orthogonal The expressions "substantially orthogonal" and "approximately orthogonal" include cases where the angle between two directions is 90° ±10°, preferably 90° ±7°, and more preferably 90° ±5°. The expressions "substantially parallel" and "approximately parallel" include the case where the angle between two directions is 0°±10°, preferably 0°±7°, and more preferably 0°±5°. Furthermore, in this specification, when simply referring to "orthogonal" or "parallel," this can include a state of being substantially orthogonal or substantially parallel.

[0010] A. Overview of Polarizing Film FIG. 1 is a schematic cross-sectional view of an optical laminate including a polarizing film according to one embodiment of the present invention. The polarizing film 11 contains a polyvinyl alcohol-based resin (hereinafter sometimes referred to as a PVA-based resin) and an organic dye. The thickness of the polarizing film 11 is 10 μm or less, preferably 8 μm or less, and more preferably 6 μm or less. The polarizing film 11 is dyed with an organic dye other than iodine. This can impart excellent polarization properties (optical properties; single transmittance and / or polarization degree) to the polarizing film and suppress discoloration in a humid environment (typically, a relative humidity of 80% or more). In particular, discoloration can be stably suppressed even at the edges of the polarizing film, where discoloration is relatively likely to occur in a humid environment. Therefore, the polarizing film 11 has excellent durability. Furthermore, since the thickness of the polarizing film is equal to or less than the above upper limit, thickness unevenness is small, visibility is excellent, and thermal shrinkage of the polarizing film can be suppressed, thereby improving the dimensional stability of the polarizing film. Furthermore, it is preferable that the thickness of the polarizing plate can be reduced. The lower limit of the thickness of the polarizing film is typically 1 μm.

[0011] The orientation function of the PVA-based resin contained in the polarizing film 11 is, for example, 0.40 or less, preferably 0.38 or less, more preferably 0.35 or less, even more preferably 0.30 or less, and particularly preferably 0.28 or less. When the orientation function of the PVA-based resin contained in the polarizing film is equal to or less than the above upper limit, the thermal shrinkage of the polarizing film can be stably suppressed. The lower limit of the orientation function of the PVA-based resin contained in the polarizing film is typically 0.20. The orientation function of the PVA-based resin can be determined, for example, by attenuated total reflection (ATR) measurement using a Fourier transform infrared spectrophotometer (FT-IR) and polarized light as the measurement light. Specifically, the measurement is performed with the stretching direction of the polarizing film parallel and perpendicular to the polarization direction of the measurement light, and the absorbance spectrum at 2941 cm -1 The intensity I is calculated according to the following formula using the intensity of 3330 cm -1 is used as the reference peak, and 2941 cm -1 / 3330cm -1The value is: When f = 1, it is perfectly oriented, and when f = 0, it is random. Also, 2941 cm -1 The peak is due to the main chain (-CH 2 It is believed that the absorption is due to the vibration of f = (3 < cos 2 θ>-1) / 2 = (1-D) / [c(2D+1)] = -2 x (1-D) / (2D+1) where, c = (3cos 2 β-1) / 2, 2941 cm -1 In the case of vibration of β = 90°, θ: angle of the molecular chain with respect to the stretching direction, β: angle of the transition dipole moment with respect to the molecular chain axis, D = (I ⊥ ) / (I / / ) (In this case, the more the PVA molecules are oriented, the larger D becomes.) I ⊥ : Absorption intensity when the polarization direction of the measurement light and the stretching direction of the polarizing film are perpendicular I / / : Absorption intensity when the polarization direction of the measurement light and the stretching direction of the polarizing film are parallel

[0012] Furthermore, when the orientation function of the PVA-based resin contained in the polarizing film 11 is equal to or less than the above upper limit, the piercing strength of the polarizing film can be improved. The piercing strength of the polarizing film 11 is, for example, 25.0 gf / μm or more, preferably 30.0 gf / μm or more, more preferably 35.0 gf / μm or more, even more preferably 40.0 gf / μm or more, and particularly preferably 45.0 gf / μm or more. When the piercing strength of the polarizing film is equal to or greater than the above lower limit, tearing of the polarizing film along the absorption axis direction can be significantly suppressed. As a result, a polarizing film (and, consequently, a polarizing plate and an optical laminate) with excellent flexibility can be obtained. The piercing strength indicates the crack resistance of the polarizing film when pierced with a predetermined strength. The piercing strength can be expressed, for example, as the strength (breaking strength) at which the polarizing film breaks when a predetermined needle is attached to a compression tester and the needle is pierced into the polarizing film at a predetermined speed. The puncture strength means the puncture strength per unit thickness (1 μm) of the polarizing film, and the upper limit of the puncture strength is, for example, 80 gf / μm.

[0013] The organic dye usable in the present invention may be any suitable dye having dichroism and excellent dyeability to polyvinyl alcohol-based resins, such as polymethine dyes, cyanine dyes, merocyanine dyes, rhodacyanine dyes, trinuclear merocyanine dyes, allopolar dyes, hemicyanine dyes, styryl dyes, and azo dyes. Among these, azo dyes are preferred from the viewpoints of dichroism in polarizing films and durability against discoloration in humid environments.

[0014] Examples of organic dyes of azo dyes include the azo compounds described on pages 98-100 of "Applications of Functional Dyes" (edited by Irie Masahiro, CMC Publishing), C.I. Direct. Yellow 12, C.I. Direct. Yellow 28, C.I. Direct. Yellow 44, C.I. Direct. Orange 26, C.I. Direct. Orange 39, C.I. Direct. Orange 107, C.I. Direct. Red 2, C.I. Direct. Red 31, C.I. Direct. Red 79, C.I. Direct. Red 81, C.I. Direct. Examples of suitable dichroic dyes include C.I. Direct. Red 247, C.I. Direct. Green 80, C.I. Direct. Green 59, and organic dyes described in JP-A 2001-33627, JP-A 2002-296417, JP-A 2003-215338, WO2004 / 092282, JP-A 2001-056412, JP-A 2001-027708, JP-A 11-218611, and JP-A 11-218610. Examples of suitable dichroic dyes include free acids, alkali metal salts (e.g., Na salts, K salts, and Li salts), ammonium salts, salts of amines, and complex salts (e.g., Cu complexes, Ni complexes, and Co complexes). Such azo compounds generally have unique hues, such as yellow, red, or blue, when used alone, and are therefore used alone or in combination of two or more types depending on the optical properties and hue of the desired polarizing film. Such organic dye-based polarizing films have high optical properties and can be adjusted to any hue, thereby improving the display quality of image display devices that use them. The display quality referred to here refers to the contrast, brightness, saturation, and hue of the displayed image, as well as the hue and appearance of the reflected color on a black screen when no image is displayed.

[0015] In general, a polarizing film using the organic dye described above can suitably employ a PVA-based resin as an alignment substrate from the viewpoint of exhibiting high optical properties. An organic dye-based polarizing film is generally formed by wet-adsorbing the organic dye into a PVA-based resin and stretching the resin.

[0016] From the viewpoint of the optical properties of the polarizing film, particularly the dyeability and orientation of the PVA-based resin used in the polarizing film, the polarizing film preferably contains, as an organic dye, at least a first dye which is an azo compound having a ureido skeleton represented by the following formula (1) or a salt thereof. The first dye does not impair the dyeability and orientation properties inherent to the dye even in the PVA-based resin, and therefore contributes to the development of high polarization properties across the visible light range. Furthermore, because the first dye has the ability to develop high polarization properties, it is possible to maintain desired optical properties even when the stretching ratio for dye orientation is appropriately reduced.

[0017] Furthermore, in one embodiment, the polarizing film preferably contains, in addition to the first dye, a second dye which is an azo compound represented by the following formula (2) or a salt thereof, and a third dye which is an azo compound represented by the following formula (3) or a salt thereof, as organic dyes. A polarizing film containing such multiple organic dyes can be adjusted to a desired hue, and can have suitable polarization characteristics for image display devices that require high display quality.

[0018] In one embodiment, the polarizing film contains at least a first dye which is an azo compound having a ureido skeleton represented by the following formula (1) or a salt thereof. In formula (1), Ay 1 and Ay 2 each independently represents a naphthyl group which may have a substituent, or a phenyl group which may have a substituent; s and t each independently represent 0 or 1, and either s or t is 1; Ry 1 ~Ry 8each independently represents a hydrogen atom or a substituent; the phenyl group which may have a substituent is a phenyl group which has at least one substituent selected from the group consisting of a sulfo group, a carboxy group, an alkoxy group having 1 to 4 carbon atoms and having a sulfo group, an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a halogen atom, a nitro group, an amino group, an alkyl-substituted amino group having 1 to 4 carbon atoms, and an alkyl-substituted acylamino group having 1 to 4 carbon atoms; and the naphthyl group which may have a substituent is a naphthyl group which may have a substituent selected from the group consisting of a hydroxy group, an alkoxy group having 1 to 4 carbon atoms and having a sulfo group, and a sulfo group; Ry 1 , Ry 2 , Ry 7 , Ry 8 are each independently a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, or an alkoxy group having 1 to 4 carbon atoms; Ry 3 ~Ry 6 are each independently a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, or an alkoxy group having 1 to 4 carbon atoms and a sulfo group. When the organic dye contains the first dye, the heat shrinkage of the polarizing film can be stably suppressed, and the polarization properties of the polarizing film can be improved.

[0019] In one embodiment, the polarizing film further contains, in addition to the first dye, a second dye which is an azo compound represented by the following formula (2) or a salt thereof, and a third dye which is an azo compound represented by the following formula (3) or a salt thereof: In formula (2), Ar 11 represents a phenyl group having a substituent or a naphthyl group having a substituent, Rr 11 ~Rr 16 each independently represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, or an alkoxy group having 1 to 4 carbon atoms and a sulfo group; 11represents an amino group optionally having a substituent selected from the group consisting of an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a sulfo group, an amino group, and a substituted amino group; a benzoyl group optionally having a substituent selected from the group consisting of an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a sulfo group, an amino group, and a substituted amino group; a phenylamino group optionally having a substituent selected from the group consisting of an alkoxy group having 1 to 4 carbon atoms, a sulfo group, an amino group, and a substituted amino group; a benzoylamino group optionally having a substituent selected from the group consisting of an alkoxy group having 1 to 4 carbon atoms, a sulfo group, an amino group, and a substituted amino group; a phenylazo group optionally having a substituent selected from the group consisting of an alkoxy group having 1 to 4 carbon atoms, a sulfo group, a hydroxy group, an amino group, and a substituted amino group; or a naphthotriazole group optionally having a substituent selected from the group consisting of an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a sulfo group, an amino group, and a substituted amino group; 15 and Rr 16 each independently represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, or an alkoxy group having 1 to 4 carbon atoms; when m1 and n1 are 0, Rr 11 and Rr 12 each independently represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, or an alkoxy group having 1 to 4 carbon atoms and a sulfo group: In formula (3), A is Ar in formula (2). 11 or the following general formula (4): (In formula (4), A 1 represents a nitro group or an amino group), and R 1 ~R 4 , R 6 is Rr in the formula (2) 11 ~Rr 14 X is the same as Xr 11 where m and n are each 0 or 1. When the polarizing film contains the first dye, the second dye, and the third dye, the polarizing properties of the polarizing film can be further improved and the thermal shrinkage of the polarizing film can be more stably suppressed.

[0020] The PVA resin and the organic dye will be described in detail below.

[0021] B. Details of PVA-Based Resin A PVA-based resin is an alignment substrate that incorporates a dichroic substance by adsorption or the like and aligns the substance to form a polarizing film. Examples of PVA-based resins include polyvinyl alcohol, acetal-modified polyvinyl alcohol, acetoacetyl-modified polyvinyl alcohol, and ethylene-vinyl alcohol copolymer. These PVA-based resins may be used alone, or two or more PVA-based resins that differ from each other in the type of modification, modification rate, degree of polymerization, degree of saponification, etc. may be used in combination.

[0022] As described later in the description of the method for producing a polarizing film, the PVA-based resin usable in the present invention can be suitably used as an alignment substrate to form a PVA-based resin layer by coating a resin substrate with a coating liquid containing the resin. The coating liquid contains various additives, and the resulting PVA-based resin layer contains the additives. The PVA-based resin layer formed on the resin substrate in this manner can minimize the thickness of the polarizing film, i.e., to 10 μm or less, preferably 8 μm or less, and more preferably 6 μm or less, compared to a commercially available film made of a single PVA-based resin. Despite the thin film, the resulting film can be reliably processed.

[0023] The PVA-based resin typically contains polyvinyl alcohol, which is obtained by saponifying polyvinyl acetate. The content of polyvinyl alcohol in the PVA-based resin is, for example, 80% by mass or more, preferably 88% by mass or more, and is, for example, 100% by mass or less, or, for example, 95% by mass or less.

[0024] In one embodiment, the PVA-based resin contains, in addition to polyvinyl alcohol, acetoacetyl-modified polyvinyl alcohol. The content of the acetoacetyl-modified polyvinyl alcohol in the PVA-based resin is, for example, 5% by mass or more, preferably 8% by mass or more, and for example, 20% by mass or less, preferably 12% by mass or less. When the content of the acetoacetyl-modified polyvinyl alcohol in the PVA-based resin is within the above range, the polarizing film can be stably dyed with an organic dye, and the mechanical strength of the polarizing film can be improved.

[0025] The saponification degree of the PVA-based resin is usually 85 mol% to 100 mol%, preferably 95.0 mol% to 99.95 mol%, more preferably 99.0 mol% to 99.93 mol%, and even more preferably 99.0 mol% to 99.5 mol%. The saponification degree can be measured in accordance with JIS K 6726-1994. By using a PVA-based resin with such a saponification degree, a thin polarizing film with excellent durability can be realized.

[0026] The average degree of polymerization of the PVA-based resin can be appropriately selected depending on the purpose. The average degree of polymerization is, for example, 1,000 or more, preferably 1,500 or more, more preferably 2,000 or more, and even more preferably 3,000 or more, and is, for example, 10,000 or less, preferably 6,000 or less, and even more preferably 4,300 or less. The average degree of polymerization can be measured in accordance with JIS K 6726-1994.

[0027] C. Details of Organic Dye C-1. First Dye The first dye is an azo compound having a ureido skeleton represented by the above formula (1) or a salt thereof. Examples of such a first dye include the azo compounds or salts thereof described in WO 2019 / 124161. The entire disclosure of this publication is incorporated herein by reference. In one embodiment, preferably, in the above formula (1), Ay 1 and Ay 2are each independently a phenyl group which may have a substituent selected from the group consisting of an alkoxy group having 1 to 4 carbon atoms and having a sulfo group, an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a carboxy group, a halogen group, a nitro group, a sulfo group, a substituted or unsubstituted amino group, and an amido group; s and t are each independently 0 or 1, and either s or t is 1; Ry 1 , Ry 2 , Ry 7 , and Ry 8 are each independently a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, or an alkoxy group having 1 to 4 carbon atoms, and Ry 3 ~Ry 6 are each independently a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, or an alkoxy group having 1 to 4 carbon atoms and a sulfo group. 1 and Ay 2 are each independently a phenyl group which may have a substituent selected from the group consisting of a carboxy group, a halogen group, and a sulfo group; s and t are each independently 0 or 1, and either s or t is 1; Ry 1 , Ry 2 , Ry 7 , and Ry 8 are each independently a hydrogen atom, a methyl group, or a methoxy group, and Ry 3 ~Ry 6 are each independently a hydrogen atom, a methyl group, a methoxy group, or a 3-sulfopropoxy group. 1 and Ay 2 are each independently a 4-sulfophenyl group, a 4-carboxyphenyl group, a 4-chloro-4-carboxyphenyl group, or a 2,4-disulfophenyl group; s and t are each independently 0 or 1, and either s or t is 1; Ry 1 , Ry 2 , Ry 7 , and Ry 8 are each independently a hydrogen atom, a methyl group, or a methoxy group, and Ry 3 ~Ry 6 are each independently a hydrogen atom, a methyl group, a methoxy group, or a 3-sulfopropoxy group.1 and Ay 2 are each a combination of a 4-sulfophenyl group and a 4-carboxyphenyl group, a combination of a 4-carboxyphenyl group and a 4-chloro-3-carboxyphenyl group, a combination of a 4-sulfophenyl group and a 4-chloro-3-carboxyphenyl group, or a combination of a 4-carboxyphenyl group and a 2,4-disulfophenyl group; s and t each independently represent 0 or 1, and either s or t is 1; Ry 1 , Ry 2 , Ry 7 , and Ry 8 are each independently a hydrogen atom, a methyl group, or a methoxy group, and Ry 3 ~Ry 6 are each independently a hydrogen atom, a methyl group, a methoxy group, or a 3-sulfopropoxy group. 1 and Ay 2 are each independently a naphthyl group which may have a substituent selected from the group consisting of an alkoxy group having 1 to 4 carbon atoms and a sulfo group, or a phenyl group which may have an alkoxy group having 1 to 4 carbon atoms and a sulfo group, an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a carboxy group, a halogen group, a nitro group, a sulfo group, a substituted or unsubstituted amino group, or an amido group; either Ay1 or Ay2 is a naphthyl group which may have a substituent selected from the group consisting of an alkoxy group having 1 to 4 carbon atoms and a sulfo group; s and t are each independently 0 or 1, and either s or t is 1; Ry 1 , Ry 2 , Ry 7 , and Ry 8 are each independently a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, or an alkoxy group having 1 to 4 carbon atoms, and Ry 3 ~Ry 6 are each independently a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, or an alkoxy group having 1 to 4 carbon atoms and a sulfo group. 1 and Ay 2are each independently a naphthyl group which may have a substituent selected from the group consisting of an alkoxy group having 1 to 4 carbon atoms and a sulfo group, or a phenyl group which may have a substituent selected from the group consisting of a carboxy group, a halogen group, and a sulfo group; Ay 1 and / or Ay 2 is a naphthyl group which may have a substituent selected from the group consisting of an alkoxy group having 1 to 4 carbon atoms and a sulfo group, s and t each independently represent 0 or 1, and either s or t represents 1; Ry 1 , Ry 2 , Ry 7 , and Ry 8 are each independently a hydrogen atom, a methyl group, or a methoxy group, and Ry 3 ~Ry 6 are each independently a hydrogen atom, a methyl group, a methoxy group, or a 3-sulfopropoxy group. 1 and Ay 2 are each independently a naphthyl group which may have a substituent selected from the group consisting of a 3-sulfopropoxy group and a sulfo group, s and t are each independently 0 or 1, and either s or t is 1, Ry 1 , Ry 2 , Ry 7 , and Ry 8 are each independently a hydrogen atom, a methyl group, or a methoxy group, and Ry 3 ~Ry 6 are each independently a hydrogen atom, a methyl group, a methoxy group, or a 3-sulfopropoxy group. 1 and Ay 2 are each 6,8-disulfonaphthalene or 6-sulfo-8-(3-sulfopropoxy)naphthalene, s and t are each independently 0 or 1, and either s or t is 1; Ry 1 , Ry 2 , Ry 7 , and Ry 8 are each independently a hydrogen atom, a methyl group, or a methoxy group, and Ry 3 ~Ry 6are each independently a hydrogen atom, a methyl group, a methoxy group, or a 3-sulfopropoxy group. 1 and Ay 2 are each 6,8-disulfonaphthalene or 6-sulfo-8-(3-sulfopropoxy)naphthalene, s and t are each 1, and Ry 1 , Ry 2 , Ry 7 , and Ry 8 are each independently a hydrogen atom, a methyl group, or a methoxy group, and Ry 3 ~Ry 6 are each independently a hydrogen atom, a methyl group, a methoxy group, or a 3-sulfopropoxy group.

[0028] Specific examples of such a first dye include the following Compound Examples 1 to 268. (Compound Example 1) (Compound example 2) (Compound example 3) (Compound example 4) (Compound example 5) (Compound example 6) (Compound Example 7) (Compound example 8) (Compound Example 9) (Compound Example 10) (Compound Example 11) (Compound Example 12) (Compound Example 13) (Compound Example 14) (Compound Example 15) (Compound Example 16) (Compound Example 17) (Compound Example 18) (Compound Example 19) (Compound Example 20) (Compound Example 21) (Compound Example 22) (Compound Example 23) (Compound Example 24) (Compound Example 25) (Compound Example 26) (Compound Example 27) (Compound Example 28) (Compound Example 29) (Compound Example 30) (Compound Example 31) (Compound Example 32) (Compound Example 33) (Compound Example 34) (Compound Example 35) (Compound Example 36) (Compound Example 37) (Compound Example 38) (Compound Example 39) (Compound Example 40) (Compound Example 41) (Compound Example 42) (Compound Example 43) (Compound Example 44) (Compound Example 45) (Compound Example 46) (Compound Example 47) (Compound Example 48) (Compound Example 49) (Compound Example 50) (Compound Example 51) (Compound Example 52) (Compound Example 53) (Compound Example 54) (Compound Example 55) (Compound Example 56) (Compound Example 57) (Compound Example 58) (Compound Example 59) (Compound Example 60) (Compound Example 61) (Compound Example 62) (Compound Example 63) (Compound Example 64) (Compound Example 65) (Compound Example 66) (Compound Example 67) (Compound Example 68) (Compound Example 69) (Compound Example 70) (Compound Example 71) (Compound Example 72) (Compound Example 73) (Compound Example 74) (Compound Example 75) (Compound Example 76) (Compound Example 77) (Compound Example 78) (Compound Example 79) (Compound Example 80) (Compound Example 81) (Compound Example 82) (Compound Example 83) (Compound Example 84) (Compound Example 85) (Compound Example 86) (Compound Example 87) (Compound Example 88) (Compound Example 89) (Compound Example 90) (Compound Example 91) (Compound Example 92) (Compound Example 93) (Compound Example 94) (Compound Example 95) (Compound Example 96) (Compound Example 97) (Compound Example 98) (Compound Example 99) (Compound Example 100) (Compound Example 101) (Compound Example 102) (Compound Example 103) (Compound Example 104) (Compound Example 105) (Compound Example 106) (Compound Example 107) (Compound Example 108) (Compound Example 109) (Compound Example 110) (Compound Example 111) (Compound Example 112) (Compound Example 113) (Compound Example 114) (Compound Example 115) (Compound Example 116) (Compound Example 117) (Compound Example 118) (Compound Example 119) (Compound Example 120) (Compound Example 121) (Compound Example 122) (Compound Example 123) (Compound Example 124) (Compound Example 125) (Compound Example 126) (Compound Example 127) (Compound Example 128) (Compound Example 129) (Compound Example 130) (Compound Example 131) (Compound Example 132) (Compound Example 133) (Compound Example 134) (Compound Example 135) (Compound Example 136) (Compound Example 137) (Compound Example 138) (Compound Example 139) (Compound Example 140) (Compound Example 141) (Compound Example 142) (Compound Example 143) (Compound Example 144) (Compound Example 145) (Compound Example 146) (Compound Example 147) (Compound Example 148) (Compound Example 149) (Compound Example 150) (Compound Example 151) (Compound Example 152) (Compound Example 153) (Compound Example 154) (Compound Example 155) (Compound Example 156) (Compound Example 157) (Compound Example 158) (Compound Example 159) (Compound Example 160) (Compound Example 161) (Compound Example 162) (Compound Example 163) (Compound Example 164) (Compound Example 165) (Compound Example 166) (Compound Example 167) (Compound Example 168) (Compound Example 169) (Compound Example 170) (Compound Example 171) (Compound Example 172) (Compound Example 173) (Compound Example 174) (Compound Example 175) (Compound Example 176) (Compound Example 177) (Compound Example 178) (Compound Example 179) (Compound Example 180) (Compound Example 181) (Compound Example 182) (Compound Example 183) (Compound Example 184) (Compound Example 185) (Compound Example 186) (Compound Example 187) (Compound Example 188) (Compound Example 189) (Compound Example 190) (Compound Example 191) (Compound Example 192) (Compound Example 193) (Compound Example 194) (Compound Example 195) (Compound Example 196) (Compound Example 197) (Compound Example 198) (Compound Example 199) (Compound Example 200) (Compound Example 201) (Compound Example 202) (Compound Example 203) (Compound Example 204) (Compound Example 205) (Compound Example 206) (Compound Example 207) (Compound Example 208) (Compound Example 209) (Compound Example 210) (Compound Example 211) (Compound Example 212) (Compound Example 213) (Compound Example 214) (Compound Example 215) (Compound Example 216) (Compound Example 217) (Compound Example 218) (Compound Example 219) (Compound Example 220) (Compound Example 221) (Compound Example 222) (Compound Example 223) (Compound Example 224) (Compound Example 225) (Compound Example 226) (Compound Example 227) (Compound Example 228) (Compound Example 229) (Compound Example 230) (Compound Example 231) (Compound Example 232) (Compound Example 233) (Compound Example 234) (Compound Example 235) (Compound Example 236) (Compound Example 237) (Compound Example 238) (Compound Example 239) (Compound Example 240) (Compound Example 241) (Compound Example 242) (Compound Example 243) (Compound Example 244) (Compound Example 245) (Compound Example 246) (Compound Example 247) (Compound Example 248) (Compound Example 249) (Compound Example 250) (Compound Example 251) (Compound Example 252) (Compound Example 253) (Compound Example 254) (Compound Example 255) (Compound Example 256) (Compound Example 257) (Compound Example 258) (Compound Example 259) (Compound Example 260) (Compound Example 261) (Compound Example 262) (Compound Example 263) (Compound Example 264) (Compound Example 265) (Compound Example 266) (Compound Example 267) (Compound Example 268)

[0029] These first dyes can be used alone or in combination. Among the first dyes, preferred examples include the compounds shown in Compound Example 25, Compound Example 140, Compound Example 167, Compound Example 177, Compound Example 180, and Compound Example 241.

[0030] C-2. Second dye The second dye is typically an azo compound represented by the above formula (2) or a salt thereof. 11 represents a phenyl group having a substituent or a naphthyl group having a substituent, Rr 11 ~Rr 16each independently represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, or an alkoxy group having 1 to 4 carbon atoms and having a sulfo group, and Xr11 represents an amino group which may have a substituent selected from the group consisting of an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a sulfo group, an amino group, and a substituted amino group, a benzoyl group which may have a substituent selected from the group consisting of an alkoxy group having 1 to 4 carbon atoms, a sulfo group, an amino group, and a substituted amino group, and a phenylamino group, a benzoylamino group which may have a substituent selected from the group consisting of an alkoxy group having 1 to 4 carbon atoms, a sulfo group, an amino group, and a substituted amino group; a phenylazo group which may have a substituent selected from the group consisting of an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a sulfo group, a hydroxy group, an amino group, or a substituted amino group; or a naphthotriazole group which may have a substituent selected from the group consisting of an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a sulfo group, an amino group, and a substituted amino group; m1 and n1 each independently represent 0 or 1; 15 and Rr 16 each independently represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, or an alkoxy group having 1 to 4 carbon atoms and a sulfo group. 11 represents a phenyl group having a substituent or a naphthyl group having a substituent, and Ar 11When is a substituted phenyl group, the phenyl group preferably has at least one sulfo group or carboxy group as a substituent; when the phenyl group has two or more substituents, at least one of the substituents is a sulfo group or a carboxy group, and the other substituents are preferably a sulfo group, a carboxy group, an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms and having a sulfo group, a hydroxyl group, a nitro group, an amino group, or a substituted amino group (particularly, an acetylamino group or an alkylamino group having 1 to 4 carbon atoms); the other substituents are more preferably a sulfo group, a carboxy group, a methyl group, an ethyl group, a methoxy group, an ethoxy group, a hydroxyl group, a nitro group, or an amino group, and particularly preferably a sulfo group, a carboxy group, a methyl group, a methoxy group, or an ethoxy group. Furthermore, the alkoxy group having 1 to 4 carbon atoms and having a sulfo group is preferably a linear alkoxy group, and the substitution position of the sulfo group is preferably the terminal of the alkoxy group. The alkoxy group having 1 to 4 carbon atoms and a sulfo group is preferably a 3-sulfopropoxy group or a 4-sulfobutoxy group, and particularly preferably a 3-sulfopropoxy group. The number of substituents on the phenyl group is preferably 1 or 2, and the positions of the substituents on the phenyl group are not particularly limited, but are preferably only the 4-position, or a combination of the 2- and 4-positions, or a combination of the 3- and 5-positions. Ar 11When is a naphthyl group having a substituent, it is preferable that the naphthyl group has at least one sulfo group as a substituent. When the naphthyl group has two or more substituents, it is preferable that at least one of the substituents is a sulfo group and the other substituents are a sulfo group, a hydroxy group, a carboxy group, or an alkoxy group having 1 to 4 carbon atoms and having a sulfo group. Furthermore, the alkoxy group having 1 to 4 carbon atoms and having a sulfo group is preferably a linear alkoxy group, and the substitution position of the sulfo group is preferably the terminal of the alkoxy group. As the alkoxy group having 1 to 4 carbon atoms and having a sulfo group, a 3-sulfopropoxy group or a 4-sulfobutoxy group is more preferable, and a 3-sulfopropoxy group is particularly preferable. When the number of sulfo groups on the naphthyl group is two, the substitution positions of the sulfo groups are preferably a combination of the 4- and 8-positions or a combination of the 6- and 8-positions, and a combination of the 6- and 8-positions is particularly preferable. When the number of sulfo groups on the naphthyl group is 3, the substitution positions of the sulfo groups are particularly preferably a combination of 1-position, 3-position and 6-position. 11 represents an amino group optionally having a substituent selected from the group consisting of an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a sulfo group, an amino group, and a substituted amino group, a benzoyl group optionally having a substituent selected from the group consisting of an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a sulfo group, an amino group, and a substituted amino group, a phenylamino group optionally having a substituent selected from the group consisting of an alkoxy group having 1 to 4 carbon atoms, a sulfo group, an amino group, and a substituted amino group, a benzoylamino group optionally having a substituent selected from the group consisting of an alkoxy group having 1 to 4 carbon atoms, a sulfo group, an amino group, and a substituted amino group, a phenylazo group optionally having a substituent selected from the group consisting of an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a sulfo group, a hydroxy group, an amino group, and a substituted amino group, or a naphthotriazole group optionally having a substituent selected from the group consisting of an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a sulfo group, an amino group, and a substituted amino group. 11is preferably an amino group which may have one or two substituents selected from the group consisting of a methyl group, a methoxy group, a sulfo group, an amino group, and an alkylamino group having 1 to 4 carbon atoms, a phenylamino group which may have one or two substituents selected from the group consisting of a methyl group, a methoxy group, a sulfo group, an amino group, and an alkylamino group having 1 to 4 carbon atoms, a benzoyl group which may have one substituent selected from the group consisting of an amino group and a carboxyethylamino group, a benzoylamino group which may have one substituent selected from the group consisting of an amino group and a carboxyethylamino group, or a phenylazo group which may have one to three substituents selected from the group consisting of a hydroxy group, an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, an amino group, and a carboxyethylamino group. 11 is preferably a phenylamino group which may have a substituent selected from the group consisting of an alkoxy group having 1 to 4 carbon atoms, a sulfo group, an amino group, and a substituted amino group, a benzoyl group which may have a substituent selected from the group consisting of an alkoxy group having 1 to 4 carbon atoms, a sulfo group, an amino group, and a substituted amino group, or a benzoylamino group which may have a substituent selected from the group consisting of an alkoxy group having 1 to 4 carbon atoms, a sulfo group, an amino group, and a substituted amino group, and is particularly preferably a phenylamino group which may have a substituent. Furthermore, it is even more preferable that Xr is a benzoyl group which may have a substituent selected from the group consisting of an amino group and a substituted amino group, or a benzoylamino group which may have a substituent selected from the group consisting of an amino group and a substituted amino group. 11is a benzoyl group having a substituent selected from the group consisting of an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a sulfo group, an amino group, and a substituted amino group; a phenylamino group having a substituent selected from the group consisting of an alkoxy group having 1 to 4 carbon atoms, a sulfo group, an amino group, and a substituted amino group; a benzoylamino group having a substituent selected from the group consisting of an alkoxy group having 1 to 4 carbon atoms, a sulfo group, an amino group, and a substituted amino group; or a phenylazo group having a substituent selected from the group consisting of an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a sulfo group, a hydroxy group, an amino group, and a substituted amino group, and when there is one substituent on the phenyl group, the position of the substituent on the phenyl group is not particularly limited, but it is particularly preferably the p-position of the phenyl group relative to the amino group. 11 ~Rr 16 each independently represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, or an alkoxy group having 1 to 4 carbon atoms and a sulfo group; preferably a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, or an alkoxy group having 1 to 4 carbon atoms, and more preferably a hydrogen atom, a methyl group, or a methoxy group. The alkoxy group having 1 to 4 carbon atoms and a sulfo group is preferably a linear alkoxy group, and the substitution position of the sulfo group is preferably the terminal of the alkoxy group. The alkoxy group having 1 to 4 carbon atoms and a sulfo group is more preferably a 3-sulfopropoxy group or a 4-sulfobutoxy group, and particularly preferably a 3-sulfopropoxy group. m1 and n1 may each independently be 0 or 1; however, in order to obtain good polarization performance in the polarizing film (polarizing element) of this embodiment, it is preferable that when either m1 or n1 is 0, the other is 1. Note that when m1 and n1 are 1, in order for the polarizing film (polarizing element) of this embodiment to exhibit the desired performance, Rr 15 and Rr 16are each independently a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, or an alkoxy group having 1 to 4 carbon atoms and having a sulfo group, and are preferably a hydrogen atom or a methyl group. As the alkyl group having 1 to 4 carbon atoms, the alkoxy group having 1 to 4 carbon atoms, and the alkoxy group having 1 to 4 carbon atoms and having a sulfo group, an alkyl group having 1 to 3 carbon atoms, an alkoxy group having 1 to 3 carbon atoms, and an alkoxy group having 3 or 4 carbon atoms and having a sulfo group are preferred. In addition, the substituted amino group is not particularly limited, and examples thereof include an amino group substituted with an alkyl group having 1 to 4 carbon atoms, and an amino group substituted with an acyl group. Examples of methods for synthesizing azo compounds in which the free acid form is represented by the general formula (2) include, but are not limited to, methods described in JP-A-9-302250, Japanese Patent No. 2622748, Japanese Patent No. 4662853, WO 2012 / 108169, and WO 2012 / 108173. Examples of azo compounds in which the free acid form is represented by the general formula (2) include, for example, C.I. Direct Red 117, C.I. Direct Red 127, azo compounds described in Japanese Patent No. 2622748, azo compounds described in Japanese Patent No. 4662853, and azo compounds described in WO 2012 / 108169. Next, specific examples of azo compounds in which the free acid form is represented by the general formula (2) are listed below. In the following compound examples, the sulfo group and hydroxy group are shown in the form of free acid, but the sulfo group and hydroxy group may be in the form of a salt.

[0031] (Compound Example 269) (Compound Example 270) (Compound Example 271) (Compound Example 272) (Compound Example 273) (Compound Example 274) (Compound Example 275) (Compound Example 276) (Compound Example 277) (Compound Example 278) (Compound Example 279) (Compound Example 280) (Compound Example 281) (Compound Example 282) (Compound Example 283) (Compound Example 284) (Compound Example 285) (Compound Example 286) (Compound Example 287) (Compound Example 288) (Compound Example 289) (Compound Example 290) (Compound Example 291) (Compound Example 292) (Compound Example 293) (Compound Example 294) (Compound Example 295) (Compound Example 296) (Compound Example 297) (Compound Example 298) (Compound Example 299) (Compound Example 300) (Compound Example 301) (Compound Example 302) (Compound Example 303) (Compound Example 304) (Compound Example 305) (Compound Example 306) (Compound Example 307) (Compound Example 308) (Compound Example 309) (Compound Example 310) (Compound Example 311) (Compound Example 312) (Compound Example 313) (Compound Example 314) (Compound Example 315) (Compound Example 316) (Compound Example 317) (Compound Example 318) (Compound Example 319) (Compound Example 320) (Compound Example 321) (Compound Example 322) (Compound Example 323) (Compound Example 324) (Compound Example 325) (Compound Example 326) (Compound Example 327) (Compound Example 328) (Compound Example 329) (Compound Example 330) (Compound Example 331) (Compound Example 332) (Compound Example 333) (Compound Example 334) (Compound Example 335) (Compound Example 336) (Compound Example 337) (Compound Example 338) (Compound Example 339) (Compound Example 340) (Compound Example 341) (Compound Example 342) (Compound Example 343) (Compound Example 344) (Compound Example 345) (Compound Example 346) (Compound Example 347) (Compound Example 348) (Compound Example 349) (Compound Example 350) (Compound Example 351) (Compound Example 352) (Compound Example 353) (Compound Example 354) (Compound Example 355) (Compound Example 356) (Compound Example 357) (Compound Example 358) (Compound Example 359) (Compound Example 360) (Compound Example 361) (Compound Example 362) (Compound Example 363) (Compound Example 364) (Compound Example 365) (Compound Example 366) (Compound Example 367) (Compound Example 368) (Compound Example 369) (Compound Example 370) (Compound Example 371) (Compound Example 372) (Compound Example 373) (Compound Example 374) (Compound Example 375) (Compound Example 376) (Compound Example 377) (Compound Example 378) (Compound Example 379) (Compound Example 380) (Compound Example 381) (Compound Example 382) (Compound Example 383) (Compound Example 384) (Compound Example 385) (Compound Example 386) (Compound Example 387) (Compound Example 388) (Compound Example 389) (Compound Example 390) (Compound Example 391) (Compound Example 392) (Compound Example 393) (Compound Example 394) (Compound Example 395) (Compound Example 396) (Compound Example 397) (Compound Example 398) (Compound Example 399) (Compound Example 400) (Compound Example 401) (Compound Example 402) (Compound Example 403) (Compound Example 404) (Compound Example 405) (Compound Example 406) (Compound Example 407) (Compound Example 408) (Compound Example 409) (Compound Example 410) (Compound Example 411) (Compound Example 412) (Compound Example 413) (Compound Example 414) (Compound Example 415) (Compound Example 416) (Compound Example 417) (Compound Example 418) (Compound Example 419) (Compound Example 420) (Compound Example 421) (Compound Example 422) (Compound Example 423) (Compound Example 424) (Compound Example 425) (Compound Example 426) (Compound Example 427) (Compound Example 428) (Compound Example 429) (Compound Example 430) (Compound Example 431) (Compound Example 432) (Compound Example 433) (Compound Example 434) (Compound Example 435) (Compound Example 436) (Compound Example 437)

[0032] These second dyes can be used alone or in combination. Among the second dyes, preferred examples include Compound Example 269, Compound Example 270, Compound Example 303, Compound Example 311, Compound Example 384, and Compound Example 396.

[0033] C-3. Third dye The third dye is typically an azo compound represented by the above formula (3) or a salt thereof. In formula (3), A is the same as Ar in formula (2). 11 or the above formula (4), and R 1 ~R 4 , R 6 is Rr in the above formula (2) 11 ~Rr 14 X is the same as Xr in the above formula (2). 11where m and n are each 0 or 1. Specific examples of such third dyes are listed below.

[0034] (Compound Example 438) (Compound Example 439) (Compound Example 440) (Compound Example 441) (Compound Example 442) (Compound Example 443) (Compound Example 444) (Compound Example 445) (Compound Example 446) (Compound Example 447) (Compound Example 448) (Compound Example 449) (Compound example 450) (Compound Example 451) (Compound Example 452) (Compound Example 453) (Compound Example 454) (Compound Example 455) (Compound Example 456) (Compound Example 457) (Compound Example 458) (Compound Example 459) (Compound Example 460) (Compound Example 461) (Compound Example 462) (Compound Example 463) (Compound Example 464) (Compound Example 465) (Compound Example 466) (Compound Example 467) (Compound Example 468) (Compound Example 469) (Compound Example 470)

[0035] These third dyes can be used alone or in combination. Among the third dyes, preferred are Compound Example 454, Compound Example 455, Compound Example 441, and Compound Example 465.

[0036] The azo compounds shown in the compound examples of the first to third dyes described above may be in the form of free acids or salts. Examples of such salts include alkali metal salts such as lithium salts, sodium salts, and potassium salts, and organic salts such as ammonium salts and amine salts, with sodium salts being preferred. In one embodiment, the polarizing film 11 contains one type of first dye, two or more types of second dyes (preferably two types of second dyes), and one type of third dye. A polarizing film containing such multiple dyes allows adjustment of the hue, and the hue value (CIE 1976 L * a * b * (based on the color space) is calculated from the single transmittance Ts of one polarizing film 11. * s and b * s is −3 to 3, and a is calculated from the parallel transmittance Tp of the two polarizing films 11. * p and b * By adjusting p to be in the range of −5 to 5, it is possible to obtain a neutral gray, which makes it possible to improve image visibility (especially color clarity) when used in an image display device.

[0037] D. Characteristics of Polarizing Film The polarizing film 11 has a single transmittance Ts for light with wavelengths of 380 nm to 780 nm of, for example, 38.0% or more, preferably 40.0% or more, and more preferably 40.5% or more. The polarizing film 11 has a polarization degree P of, for example, 97.5% or more, preferably 98.0% or more, more preferably 98.5% or more, and even more preferably 99.0% or more. The polarizing film described above can suppress discoloration in a humid environment, and therefore can stably maintain the single transmittance and / or polarization degree within the above ranges even when exposed to a humid environment.

[0038] E. Method for Producing Polarizing Film Next, a method for producing a polarizing film according to one embodiment will be described. The method for producing a polarizing film according to one embodiment includes, in this order, a laminate production step, a dry stretching step, a dyeing step, a wet stretching step, and a drying shrinkage step. The method for producing a polarizing film described above may also include a swelling step and / or a crosslinking step. The swelling step is typically carried out after the dry stretching step and before the dyeing step. The crosslinking step is typically carried out after the dyeing step and before the wet stretching step. The method for producing a polarizing film described above may further include a cleaning step. The cleaning step is typically carried out after the wet stretching step and before the drying shrinkage step.

[0039] E-1. Laminate Preparation Step In the laminate preparation step, the coating liquid containing the PVA-based resin described above is applied onto a long resin substrate by any appropriate method.

[0040] The coating liquid is typically a solution in which the PVA resin described above is dissolved in a solvent. Examples of the solvent include water, dimethyl sulfoxide, dimethylformamide, dimethylacetamide, N-methylpyrrolidone, various glycols, polyhydric alcohols such as trimethylolpropane, and amines such as ethylenediamine and diethylenetriamine. These can be used alone or in combination. Of the solvents, water is preferred.

[0041] The content of the PVA resin in the coating solution is, for example, 3 to 20 parts by mass relative to 100 parts by mass of the solvent. With such a resin concentration, a uniform coating film that adheres tightly to the resin substrate can be formed.

[0042] The coating solution may preferably contain the above-mentioned halide in the above-mentioned ratio. Furthermore, the coating solution may contain additives. Examples of additives include plasticizers and surfactants. Examples of plasticizers include polyhydric alcohols such as ethylene glycol and glycerin. Examples of surfactants include nonionic surfactants.

[0043] The resin substrate may be made of any suitable material. A typical example of the material for the resin substrate is an amorphous (uncrystallized) polyethylene terephthalate resin, preferably an amorphous (hardly crystallized) polyethylene terephthalate resin. Specific examples of amorphous polyethylene terephthalate resins include copolymers further containing isophthalic acid as a dicarboxylic acid and copolymers further containing cyclohexanedimethanol as a glycol. Among the resin substrates, an amorphous isophthalic copolymerized polyethylene terephthalate film resin substrate is preferred.

[0044] The glass transition temperature (Tg) of the resin substrate is, for example, 170°C or lower, preferably 120°C or lower. When the Tg of the resin substrate is equal to or lower than the upper limit, the stretchability of the laminate can be sufficiently ensured while suppressing excessive crystallization of the PVA-based resin layer. Furthermore, the glass transition temperature (Tg) of the resin substrate is typically 60°C or higher. This can suppress problems such as deformation of the resin substrate (for example, the occurrence of unevenness, sagging, or wrinkles) when a coating liquid is applied to the resin substrate and dried. The glass transition temperature (Tg) is measured in accordance with JIS K 7121.

[0045] The thickness of the resin substrate before stretching is, for example, 20 μm or more, preferably 50 μm or more, and for example, 300 μm or less, preferably 200 μm or less. The surface of the resin substrate may be subjected to any appropriate surface treatment (e.g., corona treatment), or an easy-adhesion layer may be formed. This can improve the adhesion between the resin substrate and the PVA-based resin layer. The surface of the resin substrate is preferably subjected to corona treatment.

[0046] The coating film (coating liquid) formed on the resin substrate is dried at any appropriate drying temperature, for example, 50°C or higher and 100°C or lower, as needed.

[0047] This produces a laminate including the PVA-based resin layer and the resin substrate. The thickness of the PVA-based resin layer before dry stretching is, for example, 3 μm or more, preferably 5 μm or more, and for example, 40 μm or less, preferably 30 μm or less.

[0048] E-2. Dry Stretching Step In the dry stretching step, a laminate including a PVA-based resin layer and a resin substrate is stretched in the air in the longitudinal direction. In other words, the dry stretching step is an in-air stretching step.

[0049] The stretching method in the dry stretching step may be fixed-end stretching (e.g., a method of stretching using a tenter stretching machine) or free-end stretching (e.g., a method of uniaxially stretching the laminate by passing it between rolls having different peripheral speeds).

[0050] The stretching temperature in the dry stretching step is typically equal to or higher than the glass transition temperature (Tg) of the PVA-based resin, for example, 95°C or higher, and preferably 120°C or higher. The stretching temperature in the dry stretching step is typically 150°C or lower. The stretching ratio of the laminate in the dry stretching step is, for example, 2.1 times or higher, preferably 2.3 times or higher, and for example, 4.0 times or lower, preferably 3.0 times or lower. When the stretching ratio of the laminate is within this range, the orientation of the PVA-based resin layer contained in the laminate can be suitably adjusted.

[0051] The crystallization index of the PVA-based resin layer after the dry stretching step and before the dyeing step is, for example, 0.50 or less, preferably 0.48 or less, more preferably 0.40 or less, and even more preferably 0.38 or less. The lower limit of the crystallization index of the PVA-based resin layer is typically 0.20. The orientation function of the PVA-based resin layer after the dry stretching step and before the dyeing step is typically smaller than the orientation function of the polarizing film. The orientation function of the PVA-based resin layer after the dry stretching step and before the dyeing step is, for example, 0.35 or less, preferably 0.28 or less, more preferably 0.24 or less, and for example, 0.15 or more. When the crystallization index and / or orientation function of the PVA-based resin layer after the dry stretching step and before the dyeing step are not more than the above-mentioned upper limit, the PVA-based resin layer can be smoothly dyed with an organic dye in the dyeing step.

[0052] E-3. Swelling Step In the swelling step, the laminate is typically immersed in a swelling liquid (swelling bath). The swelling liquid is typically water. The temperature of the swelling bath is, for example, 10°C or higher, preferably 20°C or higher, and, for example, 60°C or lower, preferably 50°C or lower. The immersion time in the swelling step is, for example, 10 seconds or higher, preferably 20 seconds or higher, and, for example, 200 seconds or lower, preferably 60 seconds or lower. Note that an insolubilization step can also be performed instead of the swelling step. In the insolubilization step, the laminate is typically immersed in an insolubilizing liquid (insolubilizing bath). The insolubilizing liquid is typically an aqueous boric acid solution. The content of boric acid in the insolubilizing liquid is, for example, 1 part by mass or more and 10 parts by mass or less per 100 parts by mass of water. The temperature range of the insolubilizing bath is, for example, the same as the temperature range of the swelling bath described above. The range of the immersion time in the insolubilization step is, for example, the same as the range of the immersion time in the swelling step described above.

[0053] In the dyeing step, the PVA-based resin layer after the dry stretching step (preferably after the swelling step) is dyed with the organic dye. Specifically, the PVA-based resin layer is brought into contact with a dyeing solution containing the organic dye, thereby allowing the organic dye to be adsorbed onto the PVA-based resin layer.

[0054] The dye solution is typically an aqueous solution of the organic dye in which the organic dye is dissolved in water. The content of the organic dye in the dye solution is, for example, 0.01% by mass or more, preferably 0.05% by mass or more, and for example, 4% by mass or less, preferably 2% by mass or less.

[0055] In one embodiment, the dyeing solution contains at least the first dye. Preferably, the dyeing solution further contains the second dye and the third dye in addition to the first dye. The content of each dye can be adjusted appropriately depending on the desired transmittance and hue of the polarizing film. The content of the first dye in the dyeing solution is, for example, 0.01% by mass or more, preferably 0.05% by mass or more, and, for example, 4% by mass or less, preferably 2% by mass or less. The content of the second dye is, for example, 0.1 parts by mass or more, preferably 0.2 parts by mass or more, and, for example, 10 parts by mass or less, preferably 5 parts by mass or less, per part by mass of the first dye. The content of the third dye is, for example, 0.1 parts by mass or more, preferably 0.2 parts by mass or more, and, for example, 10 parts by mass or less, preferably 5 parts by mass or less, per part by mass of the first dye.

[0056] In a polarizing film (polarizing element) according to one embodiment, the blending ratio of the azo compounds used is preferably adjusted so that the transmittance falls within the above-described range. The polarizing performance of the polarizing film varies depending not only on the blending ratio of the azo compounds in the polarizing film but also on various factors such as the swelling degree of the substrate to which the azo compounds are adsorbed, the stretching ratio, the dyeing time, the dyeing temperature, the pH during dyeing, and the influence of salt. The blending ratio of the azo compounds can be determined depending on the swelling degree of the substrate, the dyeing temperature, the dyeing time, the pH, the type and concentration of salt, and the stretching ratio. The first dye, the second dye, and the third dye can each be used alone or in combination of two or more.

[0057] In one embodiment, the dyeing solution contains one first dye, two or more second dyes (preferably two second dyes), and one third dye. Suitable combinations of one first dye, two second dyes, and one third dye are shown in Table 1 below.

[0058] In the dyeing step, for example, the laminate is immersed in the dye bath described above. The temperature of the dye bath is, for example, 10°C or higher, preferably 20°C or higher, and, for example, 80°C or lower, preferably 60°C or lower. The immersion time (dyeing time) in the dyeing step is, for example, 5 seconds or higher, preferably 30 seconds or higher, and, for example, 300 seconds or lower, preferably 90 seconds or lower. The method for adsorbing the dye in the dyeing step is not limited to the immersion described above. For example, the dye solution may be applied to the PVA-based resin layer, or the dye solution may be sprayed onto the PVA-based resin layer.

[0059] E-5. Crosslinking Step In the crosslinking step, the laminate after the dyeing step is typically immersed in a crosslinking liquid (crosslinking bath). The crosslinking liquid is typically an aqueous boric acid solution. The content of boric acid in the crosslinking liquid is, for example, 1 part by mass or more and 10 parts by mass or less per 100 parts by mass of water. The temperature of the crosslinking bath is, for example, 10°C or more, preferably 20°C or more, and, for example, 60°C or less, preferably 50°C or less. The immersion time in the crosslinking step is, for example, 10 seconds or more, preferably 20 seconds or more, and, for example, 200 seconds or less, preferably 60 seconds or less.

[0060] E-6. Wet Stretching Step In the wet stretching step, the dyed PVA-based resin layer (preferably the PVA-based resin layer after the crosslinking step) is stretched in the longitudinal direction in a boric acid aqueous solution as a stretching bath. In other words, the wet stretching step is an underwater stretching step. Stretching the PVA-based resin layer in the boric acid aqueous solution can prevent the PVA-based resin layer from dissolving in the boric acid aqueous solution.

[0061] The stretching ratio in the wet stretching step is typically smaller than the stretching ratio in the dry stretching step. The stretching ratio in the wet stretching step is, for example, 3.0 times or less, preferably 2.5 times or less, more preferably 2.0 times or less, and for example, 1.3 times or more. The product of the stretching ratio in the dry stretching step and the stretching ratio in the wet stretching step is, for example, 7.0 times or less, preferably 6.5 times or less, more preferably 5.5 times or less, and even more preferably 4.5 times or less, and for example, 3.5 times or more, preferably 4.0 times or more. Stretching at such a stretching ratio allows the thickness of the polarizing film to be stably adjusted within the above-mentioned range, and the orientation function of the PVA-based resin in the polarizing film to be stably adjusted within the above-mentioned range.

[0062] The content of boric acid in the stretching solution (boric acid aqueous solution) is, for example, 0.5 parts by mass or more, preferably 0.7 parts by mass or more, and for example, 5 parts by mass or less, preferably 3 parts by mass or less, relative to 100 parts by mass of water. The temperature of the stretching bath is, for example, 40°C or more, preferably 50°C or more, and for example, 85°C or less, preferably 80°C or less, more preferably 65°C or less. When the temperature of the stretching bath is not more than the above-mentioned upper limit, dissolution of the PVA-based resin layer in the stretching bath can be stably prevented even if the concentration of boric acid in the stretching bath is not more than the above-mentioned upper limit. The immersion time in the stretching step is, for example, 15 seconds or more and 300 seconds or less.

[0063] E-7. Washing Step In the washing step, the laminate after the wet stretching step is typically immersed in a washing bath. The washing bath is typically water. The temperature of the washing bath is, for example, 0°C or higher, preferably 10°C or higher, and for example, 40°C or lower, preferably 30°C or lower. The immersion time in the washing step is, for example, 5 seconds or higher, preferably 10 seconds or higher, and for example, 200 seconds or lower, preferably 60 seconds or lower.

[0064] E-8. Drying and Shrinking Step In the drying and shrinking step, the PVA-based resin layer after the wet stretching step (preferably after the washing step) is heated while being transported in the longitudinal direction. The drying and shrinking step is carried out in a heating and drying section. The heating and drying section may be a zone heating type in which the entire interior of the heating and drying section is heated, or a heating roll drying type in which the transport rolls are heated. Preferably, both types of heating and drying sections are used.

[0065] The internal temperature of the heat drying section is, for example, 70° C. or higher, preferably 80° C. or higher, and for example, 120° C. or lower, preferably 100° C. or lower. The surface temperature of the heating roll is, for example, 60° C. or higher, preferably 70° C. or higher, and for example, 100° C. or lower, preferably 80° C. or lower. Drying using a heating roll efficiently prevents heat curling of the PVA-based resin layer (laminate), allowing for efficient production of a polarizing film with excellent appearance.

[0066] In the drying shrinkage step, the PVA-based resin layer shrinks in the width direction perpendicular to the longitudinal direction. This allows the thickness of the polarizing film to be stably adjusted within the above-mentioned range. The shrinkage percentage of the PVA-based resin layer in the width direction in the drying shrinkage step is, for example, 2% or more, preferably 4% or more. If the shrinkage percentage in the width direction is equal to or higher than this lower limit, the orientation of the PVA and the PVA / each dye can be improved, and the polarization properties of the polarizing film can be improved. The shrinkage percentage of the PVA-based resin layer in the width direction is typically 10% or less, preferably 8% or less, and more preferably 6% or less. If the shrinkage percentage in the width direction is equal to or lower than this upper limit, the polarizing film can be prevented from suffering from defects in appearance such as wrinkles.

[0067] In this way, polarizing film 11 is produced. The polarizing films described in the above items A to E can be suitably applied to polarizing plates, as shown in Figures 1 and 2. A polarizing plate including the above polarizing film can suppress discoloration in a humid environment and can suppress thermal shrinkage, similar to polarizing films.

[0068] F. Polarizing Plate The polarizing plate 10 in the illustrated example includes the above-described polarizing film 11 and protective layers 12 and 13 provided on at least one surface of the polarizing film 11 .

[0069] A protective layer is provided on at least one surface of the polarizing film. In the polarizing plate 10 shown in Fig. 1, a protective layer 12 is provided on only one surface of the polarizing film 11. In the polarizing plate 10 shown in Fig. 2, protective layers 12 and 13 are provided on both surfaces of the polarizing film 11. The protective layer may be attached to the polarizing film via a pressure-sensitive adhesive layer or an adhesive layer.

[0070] The protective layer is formed of any appropriate film that can be used as a protective layer for a polarizing film. Specific examples of materials that can serve as the main component of the film include cellulose-based resins such as triacetyl cellulose (TAC), and transparent resins such as polyesters, polyvinyl alcohols, polycarbonates, polyamides, polyimides, polyethersulfones, polysulfones, polystyrenes, polynorbornenes, polyolefins, cycloolefin (COP), (meth)acrylic, and acetates. Other examples include thermosetting or ultraviolet-curing resins such as (meth)acrylic, urethane, (meth)acrylic urethane, epoxy, and silicone. Other examples include glassy polymers such as siloxane polymers. The polymer films described in JP 2001-343529 A (WO 01 / 37007) can also be used. Note that "(meth)acrylic" refers to acrylic and / or methacrylic.

[0071] In one embodiment, the protective layer is a retardation film having an in-plane retardation. The in-plane retardation Re(550) of the retardation film is, for example, 100 nm to 200 nm, preferably 110 nm to 180 nm, more preferably 120 nm to 160 nm, and even more preferably 130 nm to 150 nm. That is, the retardation film can function as a so-called λ / 4 plate. The Nz coefficient of the retardation film is, for example, 0.9 to 2.0, preferably 0.9 to 1.5, and more preferably 0.9 to 1.2.

[0072] The retardation film may exhibit an inverse dispersion wavelength characteristic in which the retardation value increases according to the wavelength of the measurement light, a positive wavelength dispersion characteristic in which the retardation value decreases according to the wavelength of the measurement light, or a flat wavelength dispersion characteristic in which the retardation value changes little depending on the wavelength of the measurement light.

[0073] The protective layer made of a retardation film is typically disposed on the viewing side of the polarizing film 11. As the protective layer made of a retardation film, a COP film is preferably used.

[0074] The thickness of the protective layer is, for example, 5 mm or less, preferably 1 mm or less, more preferably 500 μm or less, even more preferably 150 μm or less, particularly preferably 40 μm or less, and is, for example, 1 μm or more, preferably 5 μm or more.

[0075] A surface treatment layer may be provided on the surface of the protective layer (the surface opposite to the polarizing film). Examples of the surface treatment layer include a hard coat treatment layer, an anti-reflection treatment layer, an anti-sticking treatment layer, and an anti-glare treatment layer. The thickness of the surface treatment layer may be set arbitrarily and appropriately. The thickness of the surface treatment layer is, for example, 1 μm or more and 10 μm or less.

[0076] The protective layer having in-plane retardation may also be a layer of a liquid crystal compound with a fixed orientation. Because the polarizing film is dyed with an organic dye containing a first dye, even if the protective layer is a layer of a liquid crystal compound with a fixed orientation, discoloration can be sufficiently suppressed in a humidified environment (typically, a relative humidity of 80% or higher). Furthermore, by using a liquid crystal compound, the difference between nx and ny of the protective layer having in-plane retardation can be significantly increased compared to non-liquid crystal materials, thereby significantly reducing the thickness of the protective layer to obtain a desired in-plane retardation. As a result, a significantly thinner polarizing plate can be achieved. In this specification, the term "fixed orientation layer" refers to a layer in which the liquid crystal compound is oriented in a predetermined direction within the layer and the orientation state is fixed. The term "fixed orientation layer" encompasses a concept including a hardened orientation layer obtained by hardening a liquid crystal monomer, as described below. In a protective layer having in-plane retardation, typically, rod-shaped liquid crystal compounds are oriented in the slow axis direction of the protective layer (homogeneous orientation).

[0077] Examples of liquid crystal compounds include liquid crystal compounds whose liquid crystal phase is a nematic phase (nematic liquid crystals). Examples of such liquid crystal compounds include liquid crystal polymers and liquid crystal monomers. The mechanism by which the liquid crystallinity of liquid crystal compounds is expressed may be either lyotropic or thermotropic. Liquid crystal polymers and liquid crystal monomers may be used alone or in combination.

[0078] When the liquid crystal compound is a liquid crystal monomer, the liquid crystal monomer is preferably a polymerizable monomer and a crosslinkable monomer. The alignment state of the liquid crystal monomer can be fixed by polymerizing or crosslinking (i.e., curing) the liquid crystal monomer. After aligning the liquid crystal monomer, for example, the alignment state can be fixed by polymerizing or crosslinking the liquid crystal monomers with each other. Here, a polymer is formed by polymerization, and a three-dimensional network structure is formed by crosslinking, but these are non-liquid crystals. Therefore, the formed protective layer with in-plane retardation does not undergo, for example, a transition to a liquid crystal phase, glass phase, or crystalline phase due to temperature changes, which is specific to liquid crystal compounds. As a result, the protective layer with in-plane retardation has extremely excellent stability and is not affected by temperature changes.

[0079] The temperature range in which the liquid crystal monomer exhibits liquid crystallinity varies depending on the type of the liquid crystal monomer. Specifically, the temperature range is preferably 40°C to 120°C, more preferably 50°C to 100°C, and most preferably 60°C to 90°C.

[0080] Any appropriate liquid crystal monomer can be used as the liquid crystal monomer. For example, polymerizable mesogen compounds described in JP-A-2002-533742 (WO 00 / 37585), EP 358208 (US 5,211,877), EP 66137 (US 4,388,453), WO 93 / 22397, EP 0,261,712, DE 19,504,224, DE 4,408,171, and GB 2,280,445 can be used. Specific examples of such polymerizable mesogen compounds include LC242 (product name) from BASF, E7 (product name) from Merck, and LC-Silicon-CC3767 (product name) from Wacker-Chem. As the liquid crystal monomer, for example, a nematic liquid crystal monomer is preferred.

[0081] The alignment and solidification layer of the liquid crystal compound can be formed by performing an alignment treatment on the surface of a predetermined substrate, applying a coating liquid containing a liquid crystal compound to the surface to align the liquid crystal compound in a direction corresponding to the alignment treatment, and fixing the alignment state. In one embodiment, the substrate is any appropriate resin film, and the alignment and solidification layer of the liquid crystal compound (protective layer) formed on the substrate can be transferred to the surface of the polarizing film 11 via a pressure-sensitive adhesive layer or an adhesive layer.

[0082] Any appropriate alignment treatment can be adopted as the alignment treatment. Specific examples include mechanical alignment treatment, physical alignment treatment, and chemical alignment treatment. Specific examples of mechanical alignment treatment include rubbing treatment and stretching treatment. Specific examples of physical alignment treatment include magnetic field alignment treatment and electric field alignment treatment. Specific examples of chemical alignment treatment include oblique deposition and photoalignment treatment. Any appropriate treatment conditions can be adopted for the various alignment treatments depending on the purpose.

[0083] The alignment of liquid crystal compounds is achieved by treating them at a temperature at which they exhibit a liquid crystal phase depending on the type of liquid crystal compound. By performing such temperature treatment, the liquid crystal compounds assume a liquid crystal state and are aligned in accordance with the alignment treatment direction on the substrate surface.

[0084] In one embodiment, the alignment state is fixed by cooling the liquid crystal compound aligned as described above. When the liquid crystal compound is a polymerizable monomer or a crosslinkable monomer, the alignment state is fixed by subjecting the liquid crystal compound aligned as described above to a polymerization treatment or a crosslinking treatment.

[0085] Specific examples of liquid crystal compounds and details of the method for forming the alignment solidified layer are described in JP-A-2006-163343, the disclosure of which is incorporated herein by reference.

[0086] Furthermore, the layer of solidified alignment of the liquid crystal compound may be a single layer, or two or more layers may be laminated. When two or more layers of solidified alignment of the liquid crystal compound are laminated, the retardation values ​​of the respective layers of solidified alignment of the liquid crystal compound may be different. When the protective layer is composed of a layer of solidified alignment of the liquid crystal compound, the thickness thereof is, for example, 0.5 μm to 5.0 μm, preferably 0.5 μm to 3.0 μm, and more preferably 0.5 μm to 1.5 μm.

[0087] The range of the single transmittance Ts of the polarizing plate 10 is, for example, the same as the range of the single transmittance Ts of the polarizing film 11 described above. In addition, the range of the polarization degree P of the polarizing plate 10 is, for example, the same as the range of the polarization degree P of the polarizing film 11 described above.

[0088] G. Optical Laminate The polarizing films described in sections A to E above and the polarizing plate described in section F above can be applied to optical laminates. Optical laminates including the above-described polarizing films can suppress discoloration in humid environments and thermal shrinkage, similar to polarizing films. The retardation layer-attached polarizing plate 100 shown in the figure includes the above-described polarizing plate 10; a retardation layer 20 attached to the polarizing plate 10 via a pressure-sensitive adhesive layer 30; and a pressure-sensitive adhesive layer 40 located on the opposite side of the retardation layer 20 from the polarizing plate 10.

[0089] The retardation layer 20 is a layer having birefringence in which any one of nx, ny, and nz is not equal to the others. In one embodiment, the retardation layer 20 functions as a λ / 4 plate. The retardation layer 20 may be composed of one layer or two or more layers. The retardation layer 20 preferably includes a first retardation film whose refractive index characteristics exhibit the relationship nx>ny≧nz and a second retardation film whose refractive index characteristics exhibit the relationship nz>nx=ny. The first retardation film is typically composed of a stretched film of a polyester carbonate-based resin film. The second retardation film is typically composed of a film containing a liquid crystal material fixed in a homeotropic orientation.

[0090] The angle between the absorption axis direction of the polarizing film 11 and the slow axis direction of the retardation layer 20 is typically 40° to 50°, preferably 42° to 48°, more preferably 44° to 46°, and particularly preferably 45°. Such an angle allows the optical laminate to function as a circular polarizer. When there are multiple retardation plates (layers), the relative angles of their slow axes and the relative angles of their polarization axes (absorption axes) with the polarizing elements (films) can be appropriately set to obtain desired optical performance. Furthermore, when the optical laminate is used in an IPS (in-plane switching) mode liquid crystal display device, a first retardation film having a refractive index characteristic of nx > ny = nz and a second retardation film having a refractive index characteristic of nz > nx = ny may be used, and the absorption axis direction of the polarizing film and the slow axis direction of the first retardation film may be arranged substantially parallel to each other.

[0091] Each of the pressure-sensitive adhesive layer 30 and the pressure-sensitive adhesive layer 40 is typically made of a (meth)acrylic pressure-sensitive adhesive. The thickness of each of the pressure-sensitive adhesive layer 30 and the pressure-sensitive adhesive layer 40 is, for example, 3.5 μm or more and 35 μm or less.

[0092] As shown in Fig. 3, the retardation layer 20 may be attached to the polarizing plate 10 via an adhesive layer 31. The adhesive layer 31 is made of any appropriate adhesive. Typical examples of the adhesive include an ultraviolet-curable adhesive and a thermosetting adhesive, and more preferably, a (meth)acrylic ultraviolet-curable adhesive. The thickness of the adhesive layer 31 is, for example, 0.4 µm or more and 3.0 µm or less.

[0093] H. Image Display Device The polarizing film described in Sections A to E above, the polarizing plate described in Section F above, and the optical laminate described in Section G above can be applied to an image display device. Therefore, one embodiment of the present invention also encompasses such an image display device. Representative examples of image display devices include liquid crystal display devices such as in-vehicle liquid crystal display devices and organic EL display devices, and preferably in-vehicle liquid crystal display devices and organic EL display devices. In-vehicle liquid crystal display devices include in-vehicle center information displays, in-vehicle meter displays, mirror displays, and head-up displays. An image display device according to an embodiment of the present invention comprises an image display panel including an image display cell and the polarizing film described in Sections A to E above. Another embodiment of the image display device comprises an image display panel including an image display cell and the polarizing plate described in Section F above or the optical laminate described in Section G above. Note that an image display device may also be referred to as an optical display device, an image display panel may also be referred to as an optical display panel, and an image display cell may also be referred to as an optical display cell. Furthermore, polarizing plates and optical laminates including a protective layer made of a liquid crystal compound alignment solidified layer can be thinner than those in which the protective layer is made of a resin film. The thickness of the optical laminate including a protective layer made of a liquid crystal compound alignment solidified layer is, for example, 30 μm or less, preferably 20 μm. Therefore, polarizing plates and optical laminates including a protective layer made of a liquid crystal compound alignment solidified layer can be applied to foldable image display devices (e.g., liquid crystal display devices, organic EL display devices, inorganic EL display devices), and are particularly suitable for foldable organic EL display devices.

[0094] I. Polarized Sunglasses The polarizing film described in Sections A to E above and the polarizing plate described in Section F above can be applied to polarized sunglasses. Accordingly, one embodiment of the present invention also encompasses such polarized sunglasses. Typical examples of polarized sunglasses include those for driving, sports, and leisure, depending on the transmittance, hue, and polarization level, and also include overglasses and prescription lenses. Polarized sunglasses according to an embodiment of the present invention comprise lenses including the polarizing film described in Sections A to E above and a frame made of resin or metal. Polarized sunglasses according to another embodiment comprise lenses including the polarizing plate described in Section F above and a frame made of resin or metal. Lenses are typically made of glass, polycarbonate, or polyamide resin. A polarizing film or polarizing plate is generally laminated to a lens material by fusing an adhesive layer or a protective layer for the polarizing film to the lens material to form a polarized lens. A hard coat, an anti-reflection film, or the like is formed on the surface of the polarized lens, and then the polarized lens is secured to the frame by beading, drilling, screwing, or the like to form polarized sunglasses. Polarized sunglasses may also be called polarized glasses, sunglasses with a polarizing function, or glasses with a polarizing function.

[0095] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. The methods for measuring each property are as follows.

[0096] (1) Thickness Measurement The thickness of the polarizing films obtained in the examples and comparative examples was measured using a film tester thickness measuring instrument (HKT-1202 manufactured by Fujiwork Co., Ltd.) The results are shown in Tables 2 and 3.

[0097] (2) Measurement of Crystallization Index In the examples and comparative examples, the crystallization index of the PVA-based resin layer (before wet stretching) was measured by attenuated total reflection spectroscopy (ATR) using a Fourier transform infrared spectrophotometer. Specifically, polarized light was used as the measurement light, and based on the obtained spectrum, the crystallization index was measured at 1092 cm -1 1142 cm for the first peak having a peak wavelength -1The area ratio of the second peak (second peak / first peak) with the peak wavelength of 1000 nm was calculated as the crystallization index of the PVA-based resin. The results are shown in Tables 2 and 3.

[0098] (3) Measurement of Orientation Function In the Examples and Comparative Examples, the PVA-based resin layer (before wet stretching) and the polarizing film were each subjected to ATR measurement of their surfaces (specifically, the surface of the PVA-based resin layer opposite the resin substrate, or the peeled surface of the resin substrate in the polarizing film) using a Fourier transform infrared spectrophotometer (FT-IR) (manufactured by Perkin-Elmer, product name: "Frontier") with polarized infrared light as the measurement light. Germanium crystallites were used, and the angle of incidence of the measurement light was 45°. The orientation function was calculated using the following procedure. The incident polarized infrared light (measurement light) was polarized light (s-polarized light) vibrating parallel to the surface to which the germanium crystal sample was attached, and the absorbance spectrum of each was measured with the stretching direction of the polarizing film aligned perpendicular (⊥) and parallel ( / / ) to the polarization direction of the measurement light. From the obtained absorbance spectrum, the absorbance at (3330 cm -1 Intensity) was used as a reference (2941 cm -1 The intensity (I) was calculated. I⊥ was obtained from the absorbance spectrum obtained when the stretching direction of the polarizing film was placed perpendicular (⊥) to the polarization direction of the measurement light (2941 cm -1 strength) / (3330cm -1 In addition, I / / is obtained from the absorbance spectrum obtained when the stretching direction is arranged parallel ( / / ) to the polarization direction of the measurement light (2941 cm -1 strength) / (3330cm -1 Intensity), where (2941 cm -1 Intensity) is the bottom of the absorbance spectrum, 2770 cm -1 and 2990 cm -1 2941 cm when the baseline is -1 and the absorbance of (3330 cm -1 Strength) is 2990 cm -1 and 3650 cm -1 3330 cm when the baseline is -1The orientation function f was calculated using the obtained I⊥ and I / / according to the following formula (1). The results are shown in Tables 2 and 3. f = (3 < cos 2 θ>-1) / 2=(1-D) / [c(2D+1)]...(1) However, c=(3cos 2 β-1) / 2, as mentioned above, 2941 cm -1 When using the above formula, β = 90° ⇒ f = -2 × (1 - D) / (2D + 1). θ: Angle of molecular chain with respect to stretching direction β: Angle of transition dipole moment with respect to molecular chain axis D = (I⊥) / (I / / ) I⊥: Absorption intensity when the polarization direction of measurement light and stretching direction are perpendicular I / / : Absorption intensity when the polarization direction of measurement light and stretching direction are parallel Note that f = 1 indicates complete alignment, and f = 0 indicates random. Also, 2941 cm -1 The peak is due to the main chain (-CH 2 -) vibration-induced absorption. -1 The peak is said to be due to the absorption caused by the vibration of the hydroxyl group of the PVA-based resin.

[0099] (4) Puncture Strength Test The polarizing films obtained in the Examples and Comparative Examples were peeled from the resin substrate and placed in a compression tester (manufactured by Kato Tech Co., Ltd., product name "NDG5" needle penetration force measurement specifications) equipped with a needle. The needle was pierced at a piercing speed of 0.33 cm / sec at room temperature (23°C ± 3°C). The strength at which the polarizing film broke was taken as the piercing strength (breaking strength). The piercing strength (breaking strength) of 10 sample pieces was measured, and the average value was used as the evaluation value. The needle had a tip diameter of 1 mm and a radius of 0.5 mm. The polarizing film to be measured was clamped on both sides of the polarizing film using a jig with a circular opening approximately 11 mm in diameter, and the needle was pierced into the center of the opening. The results are shown in Tables 2 and 3.

[0100] (5) Measurement of Single-Plate Transmittance and Degree of Polarization The single-plate transmittance (Ts: initial transmittance), parallel transmittance (Tp), and crossed transmittance (Tc) of the polarizing plates obtained in the Examples and Comparative Examples were measured using an ultraviolet-visible spectrophotometer (manufactured by JASCO Corporation, product name "V7100"). Furthermore, the degree of polarization (P) of the polarizing plate was calculated using the following formula (1): Degree of Polarization (P) (%) = {(Tp - Tc) / (Tp + Tc)} 1 / 2 × 100 ... (1) Note that the above Ts, Tp, and Tc are Y values ​​measured using a 2-degree visual field (C light source) according to JIS Z8701 and corrected for luminosity.

[0101] (6) Measurement of reflectance The optical laminates obtained in the examples and comparative examples were placed on an aluminum reflector. Then, using a spectrophotometer (Konica Minolta "CM-2600d"), light was irradiated from the polarizing plate side, and the reflectance (initial reflectance) of the optical laminate was measured using the SCI method. The results are shown in Tables 2 and 3.

[0102] (7) High-humidity durability test (edge ​​discoloration) The optical laminates obtained in the examples and comparative examples were laminated to glass and then left to stand for 120 hours in an environment of 65°C and 90% RH (relative humidity). Then, both ends of the polarizing film in the absorption axis direction were observed using an optical microscope to see if discoloration had occurred at the edges of the polarizing film. The results are shown in Tables 2 and 3. Furthermore, the dimensional shrinkage rate in the stretching direction (MD direction) of the polarizing film in the high-humidity durability test was measured by the following method. The obtained optical laminates were cut into squares measuring 10 cm in the absorption axis direction x 10 cm in the transmission axis direction to prepare test samples. The precise dimensions of the test samples in the absorption axis direction and transmission axis direction were measured using a "CNC image measuring instrument" manufactured by Mitutoyo Corporation, and the dimension in the absorption axis direction (MD direction) was measured by S. MD0 After measuring the dimensions, the test sample was left standing at 65°C and 90% RH for 120 hours, and then the dimensions after the test were measured in the same manner. The dimensions in the MD direction after the test were S MD1 The shrinkage rate in the absorption axis direction S MD is (S MD1 -S MD0 ) / S MD0× 100. The results are shown in Table 2. In addition, the single transmittance (Ts) of the polarizing plate after the high-humidity durability test was measured in the same manner as in "(5) Measurement of single transmittance and degree of polarization" above, and ΔTs of the polarizing plate ((transmittance after high-humidity durability test) - (transmittance before high-humidity durability test)) was calculated. The results are shown in Tables 2 and 3.

[0103] (8) Heat Shrinkage Test The optical laminates obtained in the Examples and Comparative Examples were attached to glass and then allowed to stand in an environment of 80°C for 120 hours. At this time, the optical laminates were observed for the presence or absence of cracks. The results are shown in Table 2. Thereafter, the dimensional shrinkage rate in the stretching direction (MD direction) of the polarizing film in the heat shrinkage test was measured in the same manner as in the measurement of dimensional shrinkage in (7) High Humidity Durability Test. The results are shown in Tables 2 and 3.

[0104] (9) Humidity and Heat Durability Test The optical laminates obtained in the Examples and Comparative Examples were attached to glass and then allowed to stand for 500 hours in an environment of 85°C and 85% RH (relative humidity). Thereafter, the single transmittance (Ts) of the polarizing plate after the humidity and heat durability test was measured in the same manner as in "(5) Measurement of Single Transmittance and Degree of Polarization" above, and ΔTs of the polarizing plate ((transmittance after durability test) - (transmittance before durability test)) was calculated. The results are shown in Table 2.

[0105] (10) High-Temperature Durability Test The optical laminates obtained in the Examples and Comparative Examples were attached to glass and then left to stand for 1,000 hours in an environment at 105°C. Thereafter, the single-piece transmittance (Ts) of the polarizing plate after the high-temperature durability test was measured in the same manner as in "(5) Measurement of Single-Piece Transmittance and Degree of Polarization" above, and the ΔTs of the polarizing plate was calculated. The results are shown in Table 2.

[0106] <<Production Example 1>> <First Retardation Film> A batch polymerization apparatus consisting of two vertical reactors equipped with a stirring blade and a reflux condenser controlled to 100°C was charged with 29.60 parts by mass (0.046 mol) of bis[9-(2-phenoxycarbonylethyl)fluoren-9-yl]methane, 29.21 parts by mass (0.200 mol) of isosorbide (ISB), 42.28 parts by mass (0.139 mol) of spiroglycol (SPG), 63.77 parts by mass (0.298 mol) of diphenyl carbonate (DPC), and 1.19 × 10 mol of calcium acetate monohydrate as a catalyst. -2 Parts by mass (6.78×10 -5 mol) was charged. After purging the reactor with nitrogen under reduced pressure, heating was performed with a heat medium, and stirring was initiated when the internal temperature reached 100°C. 40 minutes after the start of the temperature increase, the internal temperature reached 220°C, and while controlling to maintain this temperature, pressure reduction was initiated. 90 minutes after reaching 220°C, the pressure was reduced to 13.3 kPa. Phenol vapor by-produced during the polymerization reaction was introduced into a reflux condenser at 100°C, and a small amount of monomer components contained in the phenol vapor were returned to the reactor, while uncondensed phenol vapor was introduced into a condenser at 45°C and recovered. Nitrogen was introduced into the first reactor, and the pressure was temporarily restored to atmospheric pressure. The oligomerized reaction liquid in the first reactor was then transferred to the second reactor. Next, heating and pressure reduction in the second reactor were initiated, and the internal temperature reached 240°C and the pressure reached 0.2 kPa in 50 minutes. Polymerization was then allowed to proceed until the predetermined stirring power was achieved. When the predetermined power was reached, nitrogen was introduced into the reactor to restore the pressure, and the resulting polyester carbonate resin was extruded into water and cut into strands to obtain pellets. The obtained polyester carbonate resin (pellets) was vacuum-dried at 80 ° C. for 5 hours, and then a single-screw extruder (manufactured by Toshiba Machine Co., Ltd., cylinder setting temperature: 250 ° C.), a T-die (width 200 mm, setting temperature: 250 ° C.), a chill roll (setting temperature: 120-130 ° C.) and a film-forming device equipped with a winder were used to produce a long resin film with a thickness of 125 μm. The obtained long resin film was stretched 2.5 times at 140 ° C. at the free end longitudinally to obtain a first retardation film (positive A plate) with a thickness of 50 μm. The refractive index characteristics of the second retardation film showed a relationship of nx>ny=nz.

[0107] <Second Retardation Film> A liquid crystal coating solution was prepared by dissolving 20 parts by mass of a side-chain liquid crystal polymer represented by the following chemical formula (I) (in the formula, the numbers 65 and 35 indicate the mol % of the monomer unit and are conveniently represented as a block polymer; weight-average molecular weight 5000), 80 parts by mass of a polymerizable liquid crystal exhibiting a nematic liquid crystal phase (manufactured by BASF: trade name Paliocolor LC242), and 5 parts by mass of a photopolymerization initiator (manufactured by IGM Resins B.V.: trade name Omnirad 907) in 200 parts by mass of cyclopentanone. The coating solution was then applied to a substrate film (norbornene-based resin film: manufactured by Zeon Corporation, trade name "Zeonex") using a bar coater, and the liquid crystal was aligned by heating and drying at 80°C for 4 minutes. The liquid crystal layer was irradiated with ultraviolet light to harden it, thereby forming a second retardation film (positive C plate) with a thickness of 2 μm on the substrate. The refractive index characteristics of the second retardation film showed the relationship nz > nx = ny.

[0108] <λ / 4 Plate> Next, the first retardation film (positive A plate) and the second retardation film (positive C plate) were bonded together with a UV-curable adhesive (thickness 1 μm) to obtain a λ / 4 plate.

[0109] <<Production Example 2>> A liquid crystal composition (coating liquid) was prepared by dissolving 10 parts by mass of a polymerizable liquid crystal exhibiting a nematic liquid crystal phase (manufactured by BASF: trade name "Paliocolor LC242") and 3 parts by mass of a photopolymerization initiator for the polymerizable liquid crystal compound (manufactured by IGM Resins B.V.: trade name Omnirad 907) in 40 parts by mass of toluene. The surface of a polyethylene terephthalate (PET) film (thickness 38 μm) was rubbed with a rubbing cloth to perform an alignment treatment. The direction of the alignment treatment was such that, when laminated to a polarizing plate, it was at a 45° angle from the viewing side with respect to the direction of the absorption axis of the polarizer. The liquid crystal coating liquid was applied to this alignment-treated surface using a bar coater and then heated and dried at 90°C for 2 minutes to align the liquid crystal compound. The liquid crystal layer thus formed was then irradiated with 1 mJ / cm using a metal halide lamp. 2The liquid crystal layer was cured by irradiating the PET film with light of 1000 W at 1000 W. The thickness of the liquid crystal layer was 1 μm. The liquid crystal layer had a refractive index characteristic of nx > ny = nz, and its in-plane retardation Re(550) was 140 nm.

[0110] Examples 1 to 3: A long, amorphous, isophthalic copolymerized polyethylene terephthalate film (thickness: 100 μm) with a Tg of approximately 75°C was used as the thermoplastic resin substrate, and one side of the resin substrate was subjected to a corona treatment. A PVA-based resin was prepared by mixing polyvinyl alcohol (degree of polymerization: 4200, degree of saponification: 99.2 mol%) and acetoacetyl-modified PVA (manufactured by Nippon Synthetic Chemical Industry Co., Ltd., trade name "GOHSEFIMER") in a 9:1 ratio. 12 parts by mass of potassium iodide was added to 100 parts by mass of the resulting mixture, and the mixture was dissolved in water to prepare an aqueous PVA solution (coating solution). The PVA aqueous solution was applied to the corona-treated surface of the resin substrate and dried at 60°C to form a 13 μm-thick PVA-based resin layer, producing a laminate. The laminate was then uniaxially stretched in the machine direction (longitudinal direction) at the dry stretching ratios shown in Table 2 in an oven at 130°C (dry stretching step). The PVA-based resin layer after uniaxial stretching was subjected to the above-mentioned "(2) Measurement of Crystallization Index" and "(3) Measurement of Orientation Function." The laminate was then immersed in a swelling bath (pure water) at a liquid temperature of 40°C for 60 seconds (swelling step). Subsequently, the laminate was immersed in a dye bath at a liquid temperature of 52°C for 60 seconds (dyeing step). The dye bath was prepared by dissolving Combination Example 1, i.e., a first dye (Example Compound 140), a second dye A (Example Compound 269), a second dye B (Example Compound 396), and a third dye (Example Compound 454) in water. In the dye bath, the concentrations of the first dye, second dye A, second dye B, and third dye were 0.18% by mass, 0.09% by mass, 0.11% by mass, and 0.11% by mass, respectively. The laminate was then immersed in a stretching bath (a boric acid aqueous solution prepared by blending 4 parts by mass of boric acid with 100 parts by mass of water) at a liquid temperature of 60°C and uniaxially stretched in the machine direction (longitudinal direction) between rolls operating at different peripheral speeds at the wet stretching ratios shown in Table 2 (wet stretching step). The total stretching ratios in the dry stretching step and the wet stretching step are also shown in Table 2. The laminate was then immersed in a washing bath (water) at a liquid temperature of 20°C (washing treatment). The laminate was then dried in an oven maintained at approximately 90°C and brought into contact with a heated SUS roll maintained at a surface temperature of approximately 75°C (drying shrinkage step). This caused the PVA-based resin layer on the resin substrate to shrink in the width direction, forming a polarizing film. The thickness of the polarizing film is shown in Table 2.The obtained polarizing film was subjected to the above-mentioned "(3) Measurement of Orientation Function" and "(4) Puncture Strength Test".

[0111] Next, a cycloolefin (COP) film (ZD+, manufactured by Zeon Corporation, thickness 27 μm) was attached as a protective layer to the polarizing film surface (the surface opposite to the resin substrate) via a UV-curable adhesive layer (thickness 1 μm). The COP film had an in-plane retardation, and its Re(550) was 137.5 nm. In other words, the COP film was a retardation film that could function as a λ / 4 plate. In addition, a hard coat layer with a thickness of 2 μm was provided on the surface of the COP film opposite to the polarizing film. Next, the resin substrate was peeled off to obtain a polarizing plate having a protective layer / polarizing film configuration. The obtained polarizing plate was subjected to the above-mentioned "(5) Measurement of single transmittance and polarization degree."

[0112] Next, the λ / 4 plate of Production Example 1 was attached to the release surface (the surface opposite the protective layer) of the resin substrate of the polarizing film via a (meth)acrylic pressure-sensitive adhesive layer (thickness: 5 μm). Then, a (meth)acrylic pressure-sensitive adhesive layer (thickness: 15 μm) was formed on the λ / 4 plate. This resulted in an optical laminate having a configuration of protective layer / polarizing film / (meth)acrylic pressure-sensitive adhesive layer / first retardation film / second retardation film / (meth)acrylic pressure-sensitive adhesive layer. The obtained optical laminate was subjected to the above-mentioned "(6) Reflectance Measurement," "(7) High-Humidity Durability Test (Edge Discoloration)," "(8) Heat Shrinkage Test," "(9) Humidity and Heat Durability Test," and "(10) High-Temperature Durability Test."

[0113] Example 4 A polarizing film was prepared in the same manner as in Example 3. Next, the above-described COP film (ZD+, manufactured by Zeon Corporation, thickness 27 μm) was attached as a protective layer to the surface of the polarizing film (the surface opposite to the resin substrate) via a UV-curable adhesive layer (thickness 1 μm). The resin substrate was then peeled off, and a triacetyl cellulose (TAC) film (KC-2CT, manufactured by Konica Minolta, Inc., thickness 20 μm) was attached as a protective layer to the surface of the polarizing film from which the resin substrate had been removed via a UV-curable adhesive layer (thickness 1 μm). This resulted in a polarizing plate having a protective layer (COP film) / polarizing film / protective layer (TAC film) configuration. Next, the λ / 4 plate of Production Example 1 was attached to the surface of the TAC film via a (meth)acrylic adhesive layer (thickness 15 μm). A (meth)acrylic adhesive layer (thickness 23 μm) was then formed on the λ / 4 plate. This resulted in an optical laminate having a structure of protective layer / polarizing film / protective layer / (meth)acrylic pressure-sensitive adhesive layer / first retardation film / second retardation film / (meth)acrylic pressure-sensitive adhesive layer. The obtained polarizing plate and optical laminate were subjected to the respective measurements and tests in the same manner as in Example 1.

[0114] Example 5 A polarizing film was prepared in the same manner as in Example 2. Next, the liquid crystal compound alignment layer prepared in Production Example 2 was attached as a protective layer to the surface of the polarizing film (the surface opposite to the resin substrate) via a UV-curable adhesive layer (thickness: 1 μm). Next, the resin substrate was peeled off to obtain a polarizing plate having a configuration of the liquid crystal compound alignment layer / polarizing film. The obtained polarizing plate was subjected to the above-mentioned "(5) Measurement of single transmittance and polarization degree."

[0115] Next, the λ / 4 plate of Production Example 1 was attached to the release surface (the surface opposite the protective layer) of the resin substrate of the polarizing film via a UV-curable adhesive layer (thickness 1 μm). Then, a (meth)acrylic pressure-sensitive adhesive layer (thickness 5 μm) was formed on the λ / 4 plate. This resulted in an optical laminate having a configuration of liquid crystal compound alignment solidified layer / polarizing film / first retardation film / second retardation film / (meth)acrylic pressure-sensitive adhesive layer. The obtained optical laminate was subjected to the above-mentioned "(6) Reflectance Measurement," "(7) High-Humidity Durability Test (Edge Discoloration)," and "(8) Heat Shrinkage Test."

[0116] <<Comparative Example 1>> An optical laminate was obtained in the same manner as in Example 4, except that the first dye was changed to the azo compound of formula (4) described in Japanese Patent No. 5296536. The obtained optical laminate was subjected to the respective measurements and tests in the same manner as in Example 1.

[0117] <<Comparative Example 2>> An optical laminate was obtained in the same manner as in Comparative Example 1, except that a dye bath was prepared by dissolving iodine and potassium iodide in water instead of the organic dyes (first dye, second dye, and third dye). The mass ratio of iodine to potassium iodide in the dye bath was 1:7, and the iodine concentration in the dye bath was 0.2 mass%. The obtained optical laminate was subjected to the respective measurements and tests in the same manner as in Example 1.

[0118] <<Comparative Example 3>> A 30 μm thick polyvinyl alcohol (PVA) film (PE3000, manufactured by Kuraray Co., Ltd.) was stretched twice while being treated with pure water at 20°C (swelling step). The PVA film was then dyed while being uniaxially stretched to a total stretch ratio of 2.4 times its original length while being immersed in a dye bath at 30°C for 60 seconds (dyeing step). An iodine dyeing solution with a concentration of 0.7% by mass of iodine:potassium iodide (mass ratio = 1:7) was used as the dye bath. The PVA resin film after the dyeing step was then immersed in a crosslinking bath at 40°C (a boric acid aqueous solution obtained by blending 5 parts by mass of boric acid and 3 parts by mass of potassium iodide with 100 parts by mass of water) for 45 seconds while being uniaxially stretched to a total stretch ratio of 3 times its original length while being crosslinked with boric acid (crosslinking step). Next, the PVA-based resin film after the crosslinking step was immersed in a stretching bath (a boric acid aqueous solution obtained by blending 4 parts by mass of boric acid and 5 parts by mass of potassium iodide with 100 parts by mass of water) at a liquid temperature of 60°C for 30 seconds, while being uniaxially stretched to a total stretch ratio of 6 times the original length (stretching step). Next, the PVA-based resin film after the stretching step was immersed in a cleaning bath (a potassium iodide aqueous solution) at a liquid temperature of 20°C (washing treatment). The PVA-based resin film after the washing step was then dried in an oven at 60°C for 4 minutes to obtain a polarizing film with a thickness of 12 μm. The obtained polarizing film was subjected to various measurements and tests in the same manner as in Example 1. Next, the above-mentioned COP-based film (ZD+, manufactured by Zeon Corporation, thickness 27 μm) was attached as a protective layer to one side of the obtained polarizing film via an aqueous adhesive layer. Next, the above-described TAC film (KC-2CT, manufactured by Konica Minolta, Inc., thickness 20 μm) was attached to the other side of the polarizing film as a protective layer via an aqueous adhesive layer. This resulted in a polarizing plate having a configuration of protective layer (COP film) / polarizing film / protective layer (TAC film). Next, the λ / 4 plate of Production Example 1 was attached to the surface of the TAC film via a (meth)acrylic pressure-sensitive adhesive layer (thickness 15 μm). Thereafter, a (meth)acrylic pressure-sensitive adhesive layer (thickness 23 μm) was formed on the λ / 4 plate. This resulted in an optical laminate having a configuration of protective layer / polarizing film / protective layer / (meth)acrylic pressure-sensitive adhesive layer / first retardation film / second retardation film / (meth)acrylic pressure-sensitive adhesive layer.The obtained polarizing plate and optical laminate were subjected to the respective measurements and tests in the same manner as in Example 1.

[0119] <<Comparative Example 4>> A polarizing film was prepared in the same manner as in Comparative Example 2, and an optical laminate was obtained using the polarizing film in the same manner as in Example 3. The obtained polarizing plate and optical laminate were subjected to the respective measurements and tests in the same manner as in Example 1.

[0120] <<Comparative Example 5>> An optical laminate was obtained in the same manner as in Example 5, except that a dye bath was prepared by dissolving iodine and potassium iodide in water instead of the organic dyes (first dye, second dye, and third dye). The mass ratio of iodine to potassium iodide in the dye bath was 1:7, and the iodine concentration in the dye bath was 0.2 mass%. The obtained optical laminate was subjected to the respective measurements and tests in the same manner as in Example 5.

[0121] Comparative Example 6 A polarizing film was prepared in the same manner as in Example 3, except that a dye bath was prepared by dissolving iodine and potassium iodide in water instead of the organic dyes (first dye, second dye, and third dye). Next, the liquid crystal compound alignment layer prepared in Production Example 2 was attached as a protective layer to the surface of the polarizing film (the surface opposite the resin substrate) via a UV-curable adhesive layer (thickness: 1 μm). The resin substrate was then peeled off to obtain a polarizing plate having a configuration of liquid crystal compound alignment layer / polarizing film. The obtained polarizing plate was subjected to the above-mentioned "(5) Measurement of single transmittance and polarization degree."

[0122] Next, the λ / 4 plate of Production Example 1 was attached to the release surface (the surface opposite the protective layer) of the resin substrate of the polarizing film via a UV-curable adhesive layer (thickness 1 μm). Then, a (meth)acrylic pressure-sensitive adhesive layer (thickness 5 μm) was formed on the λ / 4 plate. This resulted in an optical laminate having a configuration of liquid crystal compound alignment solidified layer / polarizing film / first retardation film / second retardation film / (meth)acrylic pressure-sensitive adhesive layer. The obtained optical laminate was subjected to the above-mentioned "(6) Reflectance Measurement," "(7) High-Humidity Durability Test (Edge Discoloration)," and "(8) Heat Shrinkage Test."

[0123]

[0124]

[0125] [Evaluation] As is clear from Tables 2 and 3, the optical laminates (Examples 1 to 5) including a polarizing film containing the first dye represented by formula (1) and having a thickness of 10 μm or less suppressed discoloration and thermal shrinkage in a humid environment, and were able to ensure excellent optical properties. In particular, when the orientation function of the PVA-based resin contained in the polarizing film was 0.30 or less (Examples 1 and 2), thermal shrinkage was significantly suppressed in the polarizing film containing an organic dye. Furthermore, the optical laminates (Examples 1 to 5) including a polarizing film containing the first dye were found to be superior in various durability properties compared to the optical laminates (Comparative Examples 2 to 6) including a polarizing film containing iodine.

[0126] The polarizing film of the present invention can be suitably used in image display devices (typically, liquid crystal display devices and organic EL display devices) and polarized sunglasses. Among image display devices, the polarizing film of the present invention can be more suitably used in in-vehicle liquid crystal display devices such as in-vehicle center information displays, in-vehicle meter displays, mirror displays, and head-up displays, which require stable display even in harsh environments.

[0127] REFERENCE SIGNS LIST 10 Polarizing plate 11 Polarizing film 12 Protective layer 100 Optical laminate

Claims

1. A polarizing film having a thickness of 10 μm or less and containing a polyvinyl alcohol resin, the polarizing film containing at least a first dye which is an azo compound having a ureido skeleton represented by the following formula (1) or a salt thereof: In formula (1), Ay 1 and Ay 2 each independently represents a naphthyl group which may have a substituent, or a phenyl group which may have a substituent; each of s and t is independently 0 or 1, and either s or t is 1; 1 ~Ry 8 each independently represents a hydrogen atom or a substituent; the phenyl group which may have a substituent is a phenyl group which has at least one or more substituents selected from the group consisting of a sulfo group, a carboxy group, an alkoxy group having 1 to 4 carbon atoms and a sulfo group, an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a halogen atom, a nitro group, an amino group, an alkyl-substituted amino group having 1 to 4 carbon atoms, and an alkyl-substituted acylamino group having 1 to 4 carbon atoms; and the naphthyl group which may have a substituent is a naphthyl group which may have a substituent selected from the group consisting of a hydroxy group, an alkoxy group having 1 to 4 carbon atoms and a sulfo group, and a sulfo group. 1 , Ry 2 , Ry 7 , Ry 8 are each independently a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, or an alkoxy group having 1 to 4 carbon atoms; R 3 ~Ry 6 each independently represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, or an alkoxy group having 1 to 4 carbon atoms and a sulfo group.

2. The polarizing film according to claim 1, wherein the orientation function of the polyvinyl alcohol resin is 0.30 or less.

3. The polarizing film according to claim 1, further comprising a second dye which is an azo compound represented by the following formula (2) or a salt thereof, and a third dye which is an azo compound represented by the following formula (3) or a salt thereof: In formula (2), Ar 11 represents a phenyl group having a substituent or a naphthyl group having a substituent; Rr 11 ~Rr 16each independently represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, or an alkoxy group having 1 to 4 carbon atoms and a sulfo group; 11 represents an amino group which may have a substituent selected from the group consisting of an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a sulfo group, an amino group, and a substituted amino group; a benzoyl group which may have a substituent selected from the group consisting of an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a sulfo group, an amino group, and a substituted amino group; a phenylamino group which may have a substituent selected from the group consisting of an alkoxy group having 1 to 4 carbon atoms, a sulfo group, an amino group, and a substituted amino group; a benzoylamino group which may have a substituent selected from the group consisting of an alkoxy group having 1 to 4 carbon atoms, a sulfo group, an amino group, and a substituted amino group; a phenylazo group which may have a substituent selected from the group consisting of an alkoxy group having 1 to 4 carbon atoms, a sulfo group, a hydroxy group, an amino group, and a substituted amino group; or a naphthotriazole group which may have a substituent selected from the group consisting of an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a sulfo group, an amino group, and a substituted amino group; 15 and Rr 16 each independently represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, or an alkoxy group having 1 to 4 carbon atoms; when m1 and n1 are 0, Rr 11 and Rr 12 each independently represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, or an alkoxy group having 1 to 4 carbon atoms and a sulfo group: In formula (3), A is Ar in formula (2). 11 or the following general formula (4): (In formula (4), A 1 represents a nitro group or an amino group, 1 ~R 4 , R 6 is Rr in the formula (2) 11 ~Rr 14 X is the same as Xr 11 where m and n are each 0 or 1.

4. An in-vehicle liquid crystal display device comprising the polarizing film according to any one of claims 1 to 3.

5. An image display device comprising the polarizing film according to any one of claims 1 to 3.

6. Polarized sunglasses comprising the polarizing film according to any one of claims 1 to 3.

7. A method for producing a polarizing film, comprising the steps of: a laminate preparation step of applying a coating liquid containing a polyvinyl alcohol-based resin onto a long thermoplastic resin substrate to prepare a laminate comprising a polyvinyl alcohol-based resin layer and the thermoplastic resin substrate; a dry stretching step of stretching the laminate in air; a dyeing step of dyeing the polyvinyl alcohol-based resin layer after the dry stretching step with a first dye which is an azo compound having a ureido skeleton represented by the following formula (1) or a salt thereof; a wet stretching step of stretching the polyvinyl alcohol-based resin layer after the dyeing step in a stretching bath; and a dry shrinking step of shrinking the polyvinyl alcohol-based resin layer after the wet stretching step in a width direction perpendicular to the long direction while transporting the polyvinyl alcohol-based resin layer in the long direction to adjust the thickness to 10 μm or less: In formula (1), Ay 1 and Ay 2 each independently represents a naphthyl group which may have a substituent, or a phenyl group which may have a substituent; each of s and t is independently 0 or 1, and either s or t is 1; 1 ~Ry 8 each independently represents a hydrogen atom or a substituent; the phenyl group which may have a substituent is a phenyl group which has at least one or more substituents selected from the group consisting of a sulfo group, a carboxy group, an alkoxy group having 1 to 4 carbon atoms and a sulfo group, an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a halogen atom, a nitro group, an amino group, an alkyl-substituted amino group having 1 to 4 carbon atoms, and an alkyl-substituted acylamino group having 1 to 4 carbon atoms; and the naphthyl group which may have a substituent is a naphthyl group which may have a substituent selected from the group consisting of a hydroxy group, an alkoxy group having 1 to 4 carbon atoms and a sulfo group, and a sulfo group. 1 , Ry 2 , Ry 7 , Ry 8are each independently a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, or an alkoxy group having 1 to 4 carbon atoms; R 3 ~Ry 6 each independently represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, or an alkoxy group having 1 to 4 carbon atoms and a sulfo group.

8. The method for producing a polarizing film according to claim 7, wherein the stretching ratio in the dry stretching is 2.1 times or more, and the stretching ratio in the wet stretching is 2.0 times or less.

Citation Information

Patent Citations

  • Manufacturing method of polarization film

    CN1831571A

  • Polarizing film, optical film laminate including polarizing film, extended laminate to be used for manufacturing optical film laminate including polarizing film, method for manufacturing these laminates, and organic el display device having polarizing film

    JP2017068282A

  • Polarizer, polarizing plate using the same and display device

    JP2021152672A

  • Azo compound or salt thereof, and polarizing element, polarizing plate, and display device comprising same

    WO2019124161A1

  • Polarizing film, polarizing plate and method for manufacturing said polarizing film

    WO2020162531A1