Metallic diatomic material, and preparation method therefor and use thereof
The synthesis of metal diatomic materials through peroxide etching method solves the problems of insufficient density and stability of metal diatomic materials in the existing technology, and achieves efficient oxygen reduction catalytic performance and cycle stability.
Patent Information
- Application Number
- PCT/CN2023/089387
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-17
- Filing Date
- 2023-04-20
- Publication Date
- 2024-10-24
AI Technical Summary
It is difficult to effectively synthesize high-density metal diatomic materials with existing technology, resulting in poor oxygen reduction activity, four-electron selectivity and cycle stability, making it difficult to meet the needs of applications such as fuel cells.
The peroxide etching method is used to synthesize metal diatomic materials. By regulating the spacing and proportion of metal atoms and increasing the density and synergy of diatomic pairs, metal diatomic materials with excellent catalytic properties are prepared.
The controllable synthesis of high-density metal diatomic materials has been achieved, significantly improving oxygen reduction activity, four-electron selectivity and cycle stability, and improving catalytic performance.
Smart Images

Figure CN2023089387_24102024_PF_FP_ABST
Abstract
Description
A metal diatomic material and its preparation method and use Technical Field
[0001] The present invention belongs to the technical field of electrocatalysis, and in particular relates to a metal diatomic material and a preparation method and application thereof. Background Art
[0002] In hydrogen-oxygen fuel cells, the oxygen reduction reaction (ORR) at the cathode is slower than the hydrogen oxidation reaction at the anode due to its four-electron process, making it the rate-determining step in the cell reaction. Therefore, efficient catalysts are needed to boost the ORR rate. Among numerous catalysts, precious metal catalysts, due to their unique catalytic properties, have been the subject of active research. While these precious metal catalysts offer excellent catalytic performance, the limited reserves and high costs of precious metals such as Pt, Pd, Ru, and Ir, as well as their non-renewable nature, severely limit their large-scale use. Therefore, the gradual adoption of alternatives is needed to reduce the use of precious metals. Non-precious metals, on the other hand, are more abundant in nature and more affordable in the market, making them more suitable for long-term sustainable development.
[0003] Among the numerous oxygen reduction electrocatalysts, diatomic metal catalysts with higher metal atom loadings and more flexible active sites are a key area of future research. While offering advantages such as fully exposed active sites, high selectivity, and up to 100% atomic utilization, diatomic catalysts further promote the cleavage of O-O bonds through synergistic interactions between adjacent dissimilar metals. This also breaks the linear relationship between the adsorption energies of reaction intermediates, increasing both metal loading and oxygen reduction rates. These catalysts possess significant potential for applications in fuel cells and zinc-air batteries.
[0004] However, the metal diatomic materials currently synthesized usually use one-pot hydrothermal methods, pre-constrained metal atom pair strategies, heteroatom doping strategies, etc. to anchor different metal atoms in order to synthesize metal diatomic materials. However, the metal diatomic materials synthesized by these methods have fewer metal atom pairs; and the strategy used to synthesize diatoms is usually one-pot synthesis, and the synthesis of diatoms is random and uncertain. At the same time, it is difficult to synthesize diatoms for some specified combinations of metal elements, and therefore there is a lack of effective and controllable synthesis of specified diatoms. The reason why it is difficult to synthesize diatoms for some specified combinations of metal elements is that some metals such as Ni, Pt, Ru, Mn, and Ir easily agglomerate to form nanoparticles or clusters during the reaction process. It is difficult to stably anchor the metal atoms by directly using one-pot synthesis, so it is difficult to effectively synthesize specified diatoms.
[0005] For example, in reference 1, "Wang Y, Li Z, Zhang P, et al. Flexible carbon nanofiber film with diatomic Fe-Co sites for efficient oxygen reduction and evolution reactions in wearable zinc-air batteries[J]. Nano Energy, 2021, 87.", Figure 1 shows that at a scale of 2 nanometers, or 156.11 square nanometers, there are 9 pairs of metal diatomic materials, and the number of atomic pairs is relatively small. At the same time, the smaller number of diatoms also affects the electrocatalytic oxygen reduction activity, four-electron selectivity, and cycle stability of the metal diatomic material. For example, in reference Figure 2, the half-wave potential of the Fe1Co1-CNF metal diatomic material is only 0.87V (Note: the larger the half-wave potential value, the greater the activity).
[0006] For example, reference 2 "Zhong X, Ye S, Tang J, et al. Engineering Pt and Fe dual-metal single atoms anchored on nitrogen-doped carbon with high activity and durability towards oxygen reduction reaction for zinc-air battery [J]. Applied Catalysis B: Environmental, 2021, 286: 119891" uses a bimetallic atom catalyst synthesized by high-temperature calcination. As can be seen from Figure 1d of reference 2, there are 15 pairs of bimetallic atoms at a scale of 2 nanometers, that is, 1126.388 square nanometers, and the number of atomic pairs is relatively small. At the same time, the smaller number of diatoms also affects the electrocatalytic oxygen reduction activity and four-electron selectivity of the bimetallic atom catalyst, as well as the cyclic stability, etc. As shown in the figure in reference 2, the half-wave potential of its PtFe-NC bimetallic catalyst is 0.895V (Note: the larger the half-wave potential value, the greater the activity). Meanwhile, the hydrogen peroxide yield of the PtFe-NC diatomic catalyst is less than 5% within the potential range of 0.1–0.8 V (Note: The lower the hydrogen peroxide yield, the wider the potential range, and the higher the four-electron selectivity). Furthermore, the cyclic stability of the PtFe-NC diatomic catalyst is poor (Note: The smaller the negative shift of the half-wave potential, the longer the cycle time, and the higher the cyclic stability). As shown in Figure S26b of Reference 2, after 5000 cycles of CV, the half-wave potential of the PtFe-NC diatomic catalyst has shifted negatively by 13 mV, indicating poor stability. The low number of diatoms results in poor oxygen reduction activity, four-electron selectivity, and cyclic stability of the dimetallic atom catalyst.
[0007] Therefore, there is an urgent need for a method to synthesize metal diatomic materials containing high-density metal atom pairs to further improve the oxygen reduction activity of metal diatomic materials.
[0008] Summary of the Invention
[0009] To this end, this paper has developed a method for the controllable synthesis of metal diatomic materials using a peroxide etching method to synthesize high-density metal diatomic materials. This synthesis method can effectively and controllably synthesize diatoms of a specified combination. In addition, the metal diatomic materials prepared by this synthesis method have excellent oxygen reduction activity, four-electron selectivity and cyclic stability. For example, the metal diatomic material ZnFeNC prepared by hydrogen peroxide etching also has 56 pairs of dimetallic atomic pairs at a scale of 2 nanometers, and the density of atomic pairs is higher, indicating that this synthesis method has unique advantages and a higher success rate for synthesizing dimetallic atomic pairs. In addition, the half-wave potential of the metal diatomic material CoFeNC is 0.86V. This shows that the metal diatomic material prepared by the peroxide etching method has excellent catalytic oxygen reduction activity, selectivity and cyclic stability.
[0010] A first aspect of the present invention provides a metal diatomic material, which comprises: a conductive substrate and a first metal single atom and a second metal single atom loaded on the conductive substrate, wherein the distance between the first metal single atom and the second metal single atom is less than or equal to 0.5 nanometers.
[0011] Preferably, on the conductive substrate, a first metal single atom and an adjacent second metal single atom form a diatomic pair, and the density of the diatomic pairs is not less than 0.06 pairs / square nanometer.
[0012] More preferably, the density of diatomic pairs is not less than 0.08 pairs / nm², for example, the density of diatomic pairs is 0.09 pairs / nm² (26 pairs / 275 nm) to 0.21 pairs / nm² (56 pairs / 265 nm).
[0013] More preferably, the density of diatomic pairs is 0.10 pairs / square nanometer (57 pairs / 555 nanometers) to 0.21 pairs / square nanometer (56 pairs / 265 nanometers).
[0014] Preferably, the distance between the first metal single atom and the second metal single atom is 0.1 to 0.5 nanometers.
[0015] More preferably, the distance between the first metal atom and the second metal atom is 0.11 to 0.5 nanometers.
[0016] Preferably, the first metal in the first metal single atom is selected from: one or more of cobalt, iron, zinc, nickel, manganese, platinum, ruthenium, iridium, gold, and silver;
[0017] The second metal in the second metal single atom is selected from: one or more of cobalt, iron, zinc, nickel, manganese, platinum, ruthenium, iridium, gold, and silver.
[0018] When the first metal in the first metal single atom is selected from the group consisting of cobalt, iron, zinc, nickel, manganese, platinum, ruthenium, iridium, gold, and silver, or the second metal in the second metal single atom is selected from the group consisting of cobalt, iron, zinc, nickel, manganese, platinum, ruthenium, iridium, gold, and silver, a variety of diatomic pairs of different metal types may exist on the conductive substrate.
[0019] For example, if the first metal in the first metal atom is selected from cobalt and iron, and the second metal in the second metal atom is selected from nickel, then the diatomic pairs present on the conductive substrate are cobalt-nickel diatomic pairs and iron-nickel diatomic pairs.
[0020] For another example: the first metal in the first metal single atom is selected from cobalt and iron, and the second metal in the second metal single atom is selected from nickel and manganese, then the diatomic pairs present on the conductive substrate are: cobalt-nickel diatomic pairs, iron-nickel diatomic pairs, cobalt-manganese diatomic pairs and iron-manganese diatomic pairs.
[0021] The first metal single atom and the second metal single atom are the same as or different from each other.
[0022] Preferably, the conductive substrate is selected from: nitrogen-carbon material or sulfur-nitrogen-carbon material. During the etching step, the sites of the nitrogen-carbon material or sulfur-nitrogen-carbon material etched by the peroxide are carbon atoms, thereby exposing more nitrogen atoms and increasing the nitrogen / carbon ratio, thereby effectively adsorbing the second metal single atom.
[0023] Preferably, the first metal single atom is an iron single atom, the second metal single atom is a platinum single atom, and the distance between the iron single atom and the platinum single atom is 0.14 to 0.5 nanometers.
[0024] Preferably, on the conductive substrate, the density of diatomic pairs is not less than 0.06 pairs / square nanometer.
[0025] More preferably, on the conductive substrate, the density of diatomic pairs is 0.09 pairs / nm² (15 pairs / 158.24 nm²) to 0.18 pairs / nm² (21 pairs / 112 nm²).
[0026] Preferably, the first metal single atom is a cobalt single atom, and the second metal single atom is an iron single atom.
[0027] The distance between a single cobalt atom and a single iron atom is 0.1 to 0.5 nanometers.
[0028] More preferably, the distance between a cobalt atom and an iron atom is 0.15 to 0.5 nanometers.
[0029] Preferably, on the conductive substrate, a cobalt single atom and its adjacent iron single atom form a diatomic pair.
[0030] Preferably, on the conductive substrate, the density of diatomic pairs is not less than 0.06 pairs / square nanometer.
[0031] More preferably, on the conductive substrate, the density of diatomic pairs is 0.10 pairs / nm² (29 pairs / 280 nm²) to 0.16 pairs / nm² (44 pairs / 280 nm²).
[0032] A second aspect of the present invention provides a method for preparing the metal diatomic material according to the first aspect, the method comprising the following steps:
[0033] Etching: placing the conductive substrate loaded with the first metal single atom in a peroxide aqueous solution for etching to obtain an etched first metal single atom material;
[0034] Preparation of metal diatomic material: The first metal single-atom material obtained after etching is loaded with a second metal single atom to obtain a metal diatomic material.
[0035] Preferably, the specific method of etching is as follows:
[0036] Step A, mixing alcohol and water into a solution, placing a conductive substrate loaded with a first metal atom in the mixed solution, and sonicating;
[0037] Step B, stirring the mixed solution obtained in step A and uniformly adding a peroxide aqueous solution dropwise to obtain a uniformly mixed reaction solution;
[0038] Step C, transferring the reaction solution obtained in step B to a high-pressure reactor, placing it in an oven, setting the reaction temperature to 100°C to 200°C, and reacting for 3-10 hours; after the reaction is completed, filtering and washing the solid material obtained in the high-pressure reactor, and vacuum freeze-drying it to obtain the etched first metal single atom material.
[0039] In the reaction solution obtained in the above step B, the concentration of the conductive substrate loaded with the first metal single atom is 1 mg / mL-5 mg / mL, and the concentration of the peroxide is 0.1 mol / L-1.0 mol / L.
[0040] Preferably, the specific method for preparing the metal diatomic material is as follows:
[0041] The etched first metal single atom material is dissolved in a mixed solution of alcohol and water, and ultrasonicated until a uniformly dispersed turbid solution is obtained. An appropriate amount of the second metal precursor is weighed and added to the turbid solution to obtain a mixed solution, which is mixed evenly, and the solid-liquid separation is performed. The obtained solid material is then freeze-dried in a vacuum;
[0042] The solid material obtained after freeze-drying is placed in a porcelain boat, carbonized under the protection of inert gas, and then naturally cooled to room temperature to finally obtain a metal diatomic material.
[0043] An appropriate amount of the second metal precursor is weighed and added to the mixed solution after the turbid solution. The concentration of the first metal single atom material after etching is 1 mg / mL-5 mg / mL, and the concentration of the second metal precursor is 0.001 mol / L~0.024 mol / L.
[0044] Preferably, the peroxide in the aqueous peroxide solution is one or more selected from hydrogen peroxide, peroxodisulfate, persulfate, peracetate, peroxyphosphate or peroxycarbonate.
[0045] Preferably, when the conductive substrate is a nitrogen-carbon substrate, the preparation method of the conductive substrate loaded with the first metal single atom is as follows:
[0046] (a) dissolving a first metal salt and a zinc salt in formamide as a solvent, and sonicating to ensure that the two salts are fully dissolved in the formamide to obtain a hydrothermal reaction mother solution A, wherein the molar ratio of the first metal salt to the zinc salt is 1:4 to 1:20;
[0047] (b) pouring the hydrothermal reaction mother liquor A into a sealed reactor and conducting a hydrothermal reaction at 160° C. to 220° C. under autogenous pressure. After completion, the sealed reactor is naturally cooled to room temperature, solid-liquid separation is performed, and the solid is washed to obtain a solid material B free of formamide residue, and the solid material B is dried to obtain a solid material C;
[0048] (c) Grinding the solid material C and placing it in a porcelain boat, heating it under the protection of an inert gas, and then maintaining the temperature at 800° C.-1100° C. for 2-6 hours. After the reaction is completed, naturally cooling it to room temperature to obtain the conductive substrate loaded with the first metal single atom.
[0049] When the conductive substrate is a sulfur-nitrogen-carbon substrate, the preparation method of the conductive substrate loaded with the first metal single atom is as follows:
[0050] (a) dissolving a first metal salt, a zinc salt, and a sulfur source in formamide as a solvent, and sonicating to ensure that the two salts are fully dissolved in the formamide to obtain a hydrothermal reaction mother solution A, wherein the molar ratio of the first metal salt to the zinc salt is 1:4 to 1:20, and the molar amount of the sulfur source is consistent with that of the first metal salt;
[0051] (b) pouring the hydrothermal reaction mother liquor A into a sealed reactor and conducting a hydrothermal reaction at 160° C. to 220° C. under autogenous pressure. After completion, the sealed reactor is naturally cooled to room temperature, solid-liquid separation is performed, and the solid is washed to obtain a solid material B free of formamide residue, and the solid material B is dried to obtain a solid material C;
[0052] (c) Grinding the solid material C and placing it in a porcelain boat, heating it under the protection of an inert gas, and then maintaining the temperature at 600° C. to 1100° C. for 1 to 4 hours. After the reaction is completed, naturally cooling it to room temperature to obtain the conductive substrate loaded with the first metal single atom.
[0053] Preferably, the first metal in the first metal salt is selected from one or more of cobalt, iron, zinc, nickel, manganese, platinum, ruthenium, iridium, gold, and silver. The first metal salt can be a first metal nitrate, a first metal sulfate, or a first metal chloride.
[0054] Preferably, the precursor of the second metal is a second metal salt, and the second metal is selected from one or more of cobalt, iron, zinc, nickel, manganese, platinum, ruthenium, iridium, gold, and silver. The second metal salt can be a second metal nitrate, a second metal sulfate, or a second metal chloride.
[0055] The third aspect of the present invention provides use of the metal diatomic material described in the first aspect for catalyzing an oxygen reduction reaction.
[0056] The above technical solutions can be freely combined under the premise of no contradiction.
[0057] Compared with the prior art, the present invention has the following beneficial effects:
[0058] 1. The present invention uses a single-atom metal material as a substrate (including but not limited to a single-atom metal nitrogen-carbon material), etches the single-atom metal material with peroxide to form a porous and defect-rich metal nitrogen-carbon material, and then impregnates the material with a second metal precursor to form a diatomic metal nitrogen-carbon catalytic material with an atomic spacing of 0 to 0.5 nanometers. By regulating the ratio and type of different metal species, the type of etchant (hydrogen peroxide, peroxodisulfate, persulfate, peroxyacetate, peroxyphosphate, peroxycarbonate), the amount of etchant added, and the etching temperature, different types of diatomic metal nitrogen-carbon catalytic materials can be produced to meet the requirements of different catalytic systems.
[0059] 2. Compared with existing diatomic preparation methods, such as the one-pot hydrothermal method for preparing metal diatomic materials, the metal diatomic materials prepared by the peroxide etching method of the present invention have a higher diatomic density, are more controllable, and have a high probability of successful diatomic sites.
[0060] 3. The present invention utilizes a peroxide-oxidative etching method for metallic monoatomic materials to effectively create defects and vacancies to synthesize atomically dispersed heterodiatomic metal nitrogen-carbon catalysts. This synthesis method is universal and can be used to synthesize both heterodiatomic and homodiatomic metal catalysts.
[0061] 4. Compared with existing non-precious metal diatomic catalysts, the hetero-diatomic metal catalyst of the present invention has excellent oxygen reduction performance under alkaline conditions. For example, the half-wave potential of oxygen reduction of ZnFeNC metal diatomic material is 0.876V.
[0062] 5. In the present invention, if the first metal atom and the second metal atom are different, the material is a heterodiatomic metal catalyst. In heterodiatomic metal catalysts, the synergistic effect between the two different atoms enhances the catalyst's oxygen reduction activity and also increases the oxygen reduction reaction rate.
[0063] 6. In particular, in the iron-platinum metal diatomic material of the present invention, the distance between a single iron atom and a single platinum atom is less than or equal to 0.5 nanometers, and on the conductive substrate, the density of diatomic pairs is 0.09 pairs / square nanometer (15 pairs / 158.24 square nanometers) to 0.18 pairs / square nanometer (21 pairs / 112 square nanometers). This shows that the synthesis method herein has unique advantages and a higher success rate for synthesizing dimetallic atom pairs. Therefore, the iron-platinum metal diatomic material of the present invention has more diatomic sites, and there is a synergistic effect between the two different atoms, which improves the activity of the catalyst in catalyzing oxygen reduction, and also improves the rate of the oxygen reduction reaction. At the same time, the selectivity and stability of the material are also greatly improved.
[0064] 7. In particular, in the cobalt-iron metal diatomic material of the present invention, the distance between the cobalt single atom and the iron single atom is less than or equal to 0.5 nanometers. On the conductive substrate, the density of diatomic pairs is 0.10 pairs / square nanometer (29 pairs / 280 square nanometers) to 0.16 pairs / square nanometer (44 pairs / 280 square nanometers), and the density of atomic pairs is higher. This shows that the synthesis method herein has unique advantages and a higher success rate for synthesizing dimetallic atom pairs. Therefore, there are more diatomic sites in the cobalt-iron metal diatomic material of the present invention, and there is a synergistic effect between the two different atoms, which improves the activity of the catalyst in catalyzing oxygen reduction, and also improves the rate of the oxygen reduction reaction. At the same time, the selectivity and stability of the material are also greatly improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0065] Figure 1 is a high-angle annular dark field scanning transmission image of the Fe1Co1-CNF metal diatomic material in reference 1.
[0066] Figure 2 shows the oxygen reduction polarization curve of the Fe1Co1-CNF metal diatomic material in reference 1 before and after working at a potential of 0.5V for 10000s.
[0067] FIG3 is a scanning electron microscope (SEM) image of the ZnFeNC metal diatomic material in Example 1.
[0068] Figure 4 is a transmission electron microscopy (TEM) image of the ZnFeNC metal diatomic material in Example 1.
[0069] FIG5 is an X-ray diffraction pattern (XRD) of the ZnFeNC metal diatomic material in Example 1.
[0070] FIG6 is a high-angle annular dark field scanning transmission image (HADDF-STEM) of the ZnFeNC metal diatomic material in Example 1.
[0071] FIG7 is a peak fitting diagram of the XPS Zn2p spectra of ZnNC, etched ZnNC, and ZnFeNC in Example 1.
[0072] FIG8 is a peak fitting diagram of the Fe2p spectrum of XPS of ZnFeNC in Example 1.
[0073] FIG9 is a comparison of the linear scan curves of the ZnFeNC metal diatomic material and various single metal catalysts under the alkaline condition of 0.1 M KOH in Example 1.
[0074] FIG. 10 is a graph showing the cycling stability of the ZnFeNC metal diatomic material and 20% Pt / C under alkaline conditions of 0.1 M KOH in Example 1.
[0075] FIG11 is a scanning electron microscope (SEM) image of the f-CoNiNC-1 metal diatomic material in Example 2.
[0076] FIG12 is a transmission electron microscope (TEM) image of the f-CoNiNC-1 metal diatomic material in Example 2.
[0077] 13 is an X-ray diffraction pattern (XRD) of f-CoNiNC-1 metal diatomic material, f-CoNiNC-2 metal diatomic material, f-CoNC obtained in step 5, and etched f-CoNC obtained in step 9 in Example 2.
[0078] FIG14 is a high-angle annular dark field scanning transmission image (HAADF-STEM) of the f-CoNiNC metal diatomic material in Example 2.
[0079] FIG15 is a comparison of the linear scan curves of f-CoNiNC-1 and f-CoNiNC-2 metal diatomic materials and various single metal catalysts under the alkaline condition of 0.1 M KOH in Example 2.
[0080] FIG. 16 is a scanning electron microscope (SEM) image of the f-CoCoNC metal diatomic material in Example 3.
[0081] FIG. 17 is a transmission electron microscopy (TEM) image of the f-CoCoNC metal diatomic material in Example 3.
[0082] FIG18 is an X-ray diffraction pattern (XRD) of the f-CoCoNC metal diatomic material in Example 3.
[0083] FIG19 is a high-angle annular dark field scanning transmission image (HAADF-STEM) of the f-CoCoNC metal diatomic material in Example 3.
[0084] FIG20 is a comparison of the linear scan curves of the f-CoCoNC metal diatomic material and various single metal catalysts under the alkaline condition of 0.1 M KOH in Example 3.
[0085] FIG21 is a scanning electron microscope (SEM) image of the FeRuNC metal diatomic material in Example 4.
[0086] FIG22 is a transmission electron microscope (TEM) image of the FeRuNC metal diatomic material in Example 4.
[0087] FIG. 23 is an X-ray diffraction pattern (XRD) of f-FeRuNC metal diatomic material, FeNC, and etched FeNC in Example 4.
[0088] Figure 24 Comparison of the linear scan curves of FeRuNC metal diatomic materials and various single metal catalysts under alkaline conditions of 0.1 M KOH.
[0089] FIG25 is a scanning electron microscope (SEM) image of the NiPtNC metal diatomic material in Example 5.
[0090] FIG26 is a transmission electron microscopy (TEM) image of the NiPtNC metal diatomic material in Example 5.
[0091] FIG27 is an X-ray diffraction pattern (XRD) of the NiPtNC metal diatomic material, the NiNC material obtained in step 5, and the etched NiPNC material obtained in step 9 in Example 5.
[0092] FIG28 is a comparison of the linear scanning curves of NiPtNC metal diatomic materials and various single metal catalysts under alkaline conditions of 0.1 M KOH.
[0093] FIG29 is a scanning electron microscope (SEM) image of the CoIrNC metal diatomic material in Example 6.
[0094] FIG30 is a transmission electron microscope (TEM) image of the CoIrNC metal diatomic material in Example 6.
[0095] FIG31 is an X-ray diffraction pattern (XRD) of the CoIrNC metal diatomic material in Example 6.
[0096] FIG32 is a comparison of the linear scan curves of the CoIrNC metal diatomic material and various single metal catalysts under alkaline conditions of 0.1 M KOH.
[0097] FIG33 is a scanning electron microscope (SEM) image of the MnRuNC metal diatomic material in Example 7.
[0098] FIG34 is a comparison of the linear scan curves of the MnRuNC metal diatomic material and various single metal catalysts under alkaline conditions of 0.1 M KOH.
[0099] FIG35 is a scanning electron microscope (SEM) image of the MnPtNC metal diatomic material in Example 8.
[0100] FIG36 is a comparison of the linear scanning curves of the MnPtNC metal diatomic material and various single metal catalysts under alkaline conditions of 0.1 M KOH.
[0101] FIG37 is a scanning electron microscope (SEM) image of the NiAuNC metal diatomic material in Example 9.
[0102] FIG38 is a comparison of the linear scan curves of the NiAuNC metal diatomic material and various single metal catalysts under alkaline conditions of 0.1 M KOH.
[0103] FIG39 is a scanning electron microscope (SEM) image of the NiAgNC metal diatomic material in Example 10.
[0104] FIG40 is a comparison of the linear scanning curves of the NiAgNC metal diatomic material and various single metal catalysts under alkaline conditions of 0.1 M KOH.
[0105] FIG41 is a scanning electron microscope (SEM) image of the FeRuSNC metal diatomic material in Example 11.
[0106] FIG42 is a transmission electron microscope (TEM) image of the FeRuSNC metal diatomic material in Example 11.
[0107] FIG43 is an X-ray diffraction pattern (XRD) of FeRuSNC metal diatomic material, FeSNC, and etched FeSNC in Example 11.
[0108] FIG44 is a comparison of the linear scan curves of the FeRuSNC metal diatomic material and various single metal catalysts under the alkaline condition of 0.1 M KOH in Example 11.
[0109] FIG45 is a comparison of the XPS full spectrum data of f-CoNC and etched f-CoNC materials in Example 2.
[0110] FIG46 is a scanning electron microscope (SEM) image of FePtNC-1 of Example 12.
[0111] FIG47 is a transmission electron micrograph (TEM) of FePtNC-1 of Example 12.
[0112] Figure 48 is a high-angle annular dark field scanning transmission electron microscopy (HAADF-STEM) image of FePtNC-1 of Example 12.
[0113] FIG49 is an X-ray diffraction (XRD) pattern of FePtNC-1, FeNC-1, and etched FeNC-1 of Example 12.
[0114] FIG50 is a linear sweep polarization curve of oxygen reduction of the FePtNC-1 bimetallic atom catalyst, FeNC-1, etched FeNC-1, and 20 wt % Pt / C materials of Example 12 at 1600 rpm.
[0115] FIG51 shows the four-electron transfer number and hydrogen peroxide yield of the FePtNC-1 bimetallic atom catalyst and 20 wt% Pt / C material of Example 12.
[0116] FIG52 shows the oxygen reduction polarization curves of the FePtNC-1 diatomic material and the 20 wt % Pt / C material of Example 12 before and after 10,000 cycles.
[0117] FIG53 is a scanning electron microscope (SEM) image of the FePtNC-2 diatomic material of Example 13.
[0118] FIG54 shows X-ray diffraction (XRD) patterns of the FePtNC-2 diatomic material obtained in step 13 of Example 13, the FeNC-2 obtained in step 5, and the etched FeNC-2 obtained in step 9.
[0119] FIG55 is a high-angle annular dark field scanning transmission electron microscopy (HAADF-STEM) image of the FePtNC-2 diatomic material of Example 13.
[0120] 56 shows linear sweep polarization curves of oxygen reduction of the FePtNC-2 diatomic material of Example 13, the FeNC-2 obtained in step 5, and the etched FeNC-2 obtained in step 9 under the alkaline condition of O2-saturated 0.1 M KOH at a rotation speed of 1600 rpm.
[0121] FIG57 is a scanning electron microscope (SEM) image of the FePtNC-3 diatomic material of Example 14.
[0122] 58 is an X-ray diffraction (XRD) pattern of the FePtNC-3 diatomic material obtained in step 13 of Example 14, the FeNC-3 obtained in step 5, and the etched FeNC-3 obtained in step 9.
[0123] FIG59 is a linear sweep polarization curve of oxygen reduction of the FePtNC-3 diatomic material of Example 14, the FeNC-3 obtained in Step 5, and the etched FeNC-3 obtained in Step 9 at 1600 rpm.
[0124] FIG60 is a scanning electron microscope (SEM) image of FePtSNC-1 of Example 15.
[0125] 61 is an X-ray diffraction (XRD) pattern of FePtSNC-1 obtained in step 13 of Example 15, FeSNC-1 obtained in step 5, and etched FeSNC-1 obtained in step 9.
[0126] FIG62 is a linear sweep polarization curve of oxygen reduction of the FePtSNC-1 bimetallic atomic material of Example 15, the FeSNC-1 obtained in step 5, and the etched FeSNC-1 obtained in step 9 at 1600 rpm.
[0127] Figure 63 is a scanning electron microscope (SEM) image of FePtSNC-2 of Example 16.
[0128] Figure 64 is the X-ray diffraction (XRD) patterns of FePtSNC-2 obtained in step 13 of Example 16, FeSNC-2 obtained in step 5, and etched FeSNC-2 obtained in step 9.
[0129] FIG65 is a linear sweep polarization curve of oxygen reduction of the FePtSNC-2 bimetallic atomic material of Example 16, the FeSNC-2 obtained in step 5, and the etched FeSNC-2 obtained in step 9 at 1600 rpm.
[0130] Figure 66 is a scanning electron microscope (SEM) image of FePtSNC-3 of Example 17.
[0131] Figure 67 is the X-ray diffraction (XRD) pattern of FePtSNC-3 obtained in step 13 of Example 17, FeSNC-3 obtained in step 5, and etched FeSNC-3 obtained in step 9.
[0132] FIG68 is a linear sweep polarization curve of oxygen reduction of the FePtSNC-3 bimetallic atomic material of Example 17, the FeSNC-3 obtained in step 5, and the etched FeSNC-3 obtained in step 9 at 1600 rpm.
[0133] FIG69 is a scanning electron microscope (SEM) image of the CoFeNC-1 diatomic material of Example 18.
[0134] FIG70 is a transmission electron micrograph (TEM) of the CoFeNC-1 diatomic material of Example 18.
[0135] FIG71 is a high-angle annular dark field scanning transmission electron microscopy (HAADF-STEM) image of the CoFeNC-1 diatomic material of Example 18.
[0136] FIG72 is an X-ray diffraction (XRD) pattern of the CoFeNC-1 diatomic material, CoNC-1, and etched CoNC-1 of Example 18.
[0137] 73 is a linear sweep polarization curve of oxygen reduction of the CoFeNC-1 diatomic material, etched CoNC-1, FeNC, CoNC-1, and 20 wt % Pt / C material of Example 18 at 1600 rpm.
[0138] FIG74 shows the four-electron transfer number and hydrogen peroxide yield of the CoFeNC-1 diatomic material and the 20 wt % Pt / C material of Example 18.
[0139] FIG75 shows the oxygen reduction polarization curves of the CoFeNC-1 diatomic material and the 20 wt % Pt / C material of Example 18 before and after working for 40,000 seconds.
[0140] FIG76 is a scanning electron microscope (SEM) image of the CoFeNC-2 diatomic material of Example 19.
[0141] 77 is an X-ray diffraction (XRD) pattern of the CoFeNC-2 diatomic material obtained in step 14 of Example 19, the CoNC-2 obtained in step 5, and the etched CoNC-2 obtained in step 9.
[0142] FIG78 is a high-angle annular dark field scanning transmission electron microscopy (HAADF-STEM) image of the CoFeNC-2 diatomic material of Example 19.
[0143] Figure 79 shows the linear sweep polarization curves of oxygen reduction of the CoFeNC-2 diatomic material obtained in step 14 of Example 19, the CoNC-2 obtained in step 5, the etched CoNC-2 and FeNC-2 obtained in step 9, and the 20 wt% Pt / C material under the alkaline conditions of O2-saturated 0.1 M KOH at a rotation speed of 1600 rpm.
[0144] FIG80 is a scanning electron microscope (SEM) image of the CoFeNC-3 diatomic material of Example 20.
[0145] Figure 81 is an X-ray diffraction (XRD) pattern of the CoFeNC-3 diatomic material of Example 20.
[0146] FIG82 is a linear sweep polarization curve of oxygen reduction of the CoFeNC-3 diatomic material of Example 20, the CoNC-3 obtained in step 5, and the etched CoNC-3 obtained in step 9 at 1600 rpm. DETAILED DESCRIPTION
[0147] The present invention is further illustrated below by way of examples, but is not intended to be limiting. Experimental procedures not specifically specified in the examples generally followed conventional conditions, those described in manuals, or those recommended by the manufacturer. The general equipment, materials, and reagents used were commercially available unless otherwise noted. The raw materials required in the following examples and comparative examples were all commercially available.
[0148] Example 1
[0149] Preparation method of ZnFeNC metal diatomic material:
[0150] 1. Dissolve anhydrous zinc chloride in 30 mL of formamide as a solvent and ultrasonicate for 30 minutes to ensure that the anhydrous zinc chloride is fully dissolved in the formamide. The resulting clear solution is the hydrothermal reaction mother liquor A. The concentration of anhydrous zinc chloride in the hydrothermal reaction mother liquor A is 0.01 mol L -1 .
[0151] 2. Pour the above mother liquor A into a clean, dry, closed reactor and carry out hydrothermal reaction at 180°C for 12 hours.
[0152] 3. After the hydrothermal reaction is completed, the sealed reactor is cooled naturally to room temperature, the reactor is opened, and the reaction liquid is filtered, and washed twice with deionized water and anhydrous ethanol to obtain a solid material B without formamide residue.
[0153] 4. Place solid material B in a 60°C forced air drying oven and dry for 2 hours to obtain dry solid material C.
[0154] 5. Grind the obtained solid material C into fine powder, and place the fine powder in a porcelain boat. Start from room temperature under the protection of inert gas N2, and heat at 5℃min. -1 The temperature was raised at a heating rate of 1000 ℃, and then carbonized at a constant temperature of 800 ℃ for 2 hours. After the constant temperature was completed, it was naturally cooled to room temperature to obtain zinc single-atom nitrogen-carbon material (ZnNC).
[0155] 6. Measure 12.5 mL of ethanol and deionized water of equal volume, mix them to obtain a mixed solution, dissolve 50 mg of the zinc single-atom nitrogen-carbon material synthesized above in the mixed solution, and sonicate for 30 minutes until it is evenly dispersed to obtain a mixed solution D.
[0156] 7. The mixed solution D obtained in step 6 was placed on a stirring platform at room temperature and stirred for 10 minutes. During the stirring period, 0.25 mL of 30% (10 mol / L) hydrogen peroxide solution was evenly added dropwise to obtain a uniformly mixed reaction solution E. The concentration of hydrogen peroxide in the reaction solution E was 0.1 mol / L, and the concentration of the zinc single-atom nitrogen-carbon material ZnNC was 2 mg / mL.
[0157] 8. Transfer the reaction solution E to a high-pressure reactor, place it in an oven at 200°C, and react for 6 hours.
[0158] 9. After the reaction is completed, the solid material obtained in the high-pressure reactor is filtered, washed three times with deionized water, and placed in a vacuum freeze drying box for overnight freeze drying to obtain the etched zinc single-atom nitrogen-carbon material (etched ZnNC).
[0159] 10. Weigh 50 mg of the dry solid of the etched ZnNC material and dissolve it in a mixed solution of equal volumes of 12.5 mL of anhydrous ethanol and 12.5 mL of deionized water. After ultrasonication for 1 hour, transfer it to a stirring platform at room temperature to obtain a hydroalcoholic solution of etched ZnNC.
[0160] 11. Weigh 0.00025 mol of ferric chloride powder and dissolve it in a mixture of 12.5 mL of anhydrous ethanol and 12.5 mL of deionized water, and ultrasonicate until dissolved to obtain 0.01 mol L -1 of ferric chloride solution.
[0161] 12. The hydroalcoholic solution for etching ZnNC obtained in step 10 was evenly added dropwise to the ferric chloride solution obtained in step 11 under vigorous stirring for 2 hours, and the iron ions were adsorbed on the surface of the etched ZnNC material by an immersion method.
[0162] 13. After 2 hours of stirring, the mixture was filtered and washed, and the obtained solid material was vacuum freeze-dried.
[0163] 14. Place the solid material obtained after freeze drying in a porcelain boat. Under the protection of inert gas Ar / N2, heat it from room temperature at a rate of 5°C min -1 The temperature was raised to 800°C and carbonized at this temperature for 1 hour, followed by natural cooling to room temperature. Finally, the ZnFeNC heteronuclear diatomic metal nitrogen-carbon catalyst was obtained.
[0164] The ZnNC obtained in step (5), the etched ZnNC obtained in step (9), and the ZnFeNC obtained in step (14) were characterized:
[0165] FIG3 is a scanning electron microscope (SEM) image of the ZnFeNC metal diatomic material in Example 1.
[0166] Figure 4 is a transmission electron microscopy (TEM) image of the ZnFeNC metal diatomic material in Example 1. At a scale of 50 nanometers, no nanoparticles of metal zinc or iron are visible.
[0167] FIG5 is an X-ray diffraction pattern (XRD) of the ZnFeNC metal diatomic material in Example 1.
[0168] Figures 4 and 5 demonstrate that the diatoms did not form metal nanoparticles or alloys.
[0169] Figure 6 is a high-angle annular dark field scanning transmission image (HADDF-STEM) of the ZnFeNC metal diatomic material in Example 1. Figure 6 shows that the distance between the first Zn single atom and the second Fe single atom is less than 0.5 nm.
[0170] Table 1 shows the spacing statistics for the 56 pairs of atoms in the ZnFeNC metal diatomic material from Example 1. The statistical results show that the spacing between all pairs is less than 0.5 nanometers. Specifically, the distance between the first Zn atom and the second Fe atom is 0.11 to 0.5 nm.
[0171] At a scale of 2 nanometers, or 265 square nanometers, there are numerous diatomic sites, totaling 56 pairs of dimetallic atoms, with a diatomic pair density of 0.21 pairs per square nanometer. This indicates a high probability of diatomic success. In this application, the area of the high-angle annular dark field scanning transmission image (HAADF-STEM) image was calculated by the inventors based on the scale and actual size of the image.
[0172] Table 1
[0173] Figure 7 is the peak fitting diagram of the XPS Zn2p spectrum of ZnNC, etched ZnNC and ZnFeNC. 2+ .
[0174] Figure 8 is the peak fitting diagram of the XPS Fe2p spectrum of ZnFeNC. According to the peak results, the material contains Fe 2+ and Fe 3+ of iron in different oxidation states.
[0175] FIG9 is a comparison of the linear scanning curves of ZnFeNC metal diatomic materials and various single metal catalysts under 0.1 M KOH.
[0176] The FeNC preparation method is as follows: The preparation of FeNC is the same as the preparation of ZnNC in steps 1-5 of Example 1, except that the zinc salt is replaced with an iron salt, namely, ferric acetylacetonate, at a molar concentration of 0.005 mol / L. The resulting material is FeNC.
[0177] The ZnNC source was prepared according to the preparation process in Example 1, and the product obtained in step 5.
[0178] The one-pot preparation method of ZnFeNC is as follows:
[0179] Dissolve 0.1 mol / L anhydrous zinc chloride and 0.01 mol / L anhydrous ferric chloride in 30 mL of formamide and sonicate until uniformly dispersed. Place the reaction mixture in an oven at 180°C for 12 hours. After cooling naturally, filter and dry in an oven at 60°C. The dried powder is then carbonized in a tube furnace at 800°C for 2 hours, with a heating rate of 5°C / min and argon as the shielding gas.
[0180] The etched ZnNC source was prepared according to the preparation process in Example 1, and the product obtained in step 9.
[0181] The 20% Pt / C material is a Pt / C material with a Pt content of 20% by mass, that is, 20 wt % Pt / C, which can be purchased on the market.
[0182] As shown in Figure 9, the onset potential of the ZnFeNC metal diatomic material is 1.00 V, and its half-wave potential is 0.876 V. The onset potential of FeNC is 0.98 V, and its half-wave potential is 0.63 V. The onset potential of ZnNC is 0.93 V, and its half-wave potential is 0.693 V. The onset potential of the one-pot ZnFeNC method is 0.98 V, and its half-wave potential is 0.68 V. The onset potential of 20% Pt / C is 0.99 V, and its half-wave potential is 0.84 V. Figure 9 demonstrates that the ZnFeNC metal diatomic material exhibits superior electrocatalytic oxygen reduction activity compared to the other materials shown in Figure 9.
[0183] Figure 10 shows the cycling stability of the ZnFeNC metal diatomic material and 20% Pt / C under alkaline conditions (0.1 M KOH). After 5000 CV cycles, the half-wave potential of the ZnFeNC metal diatomic material only decayed by 16 mV, while the half-wave potential of the 20% Pt / C material decayed by 51 mV. This demonstrates the superior cycling stability of the ZnFeNC metal diatomic material.
[0184] Example 2
[0185] The preparation method of CoNiNC metal diatomic material is as follows:
[0186] 1. Dissolve the cobalt and zinc salts in 30 mL of formamide. Ultrasonicate for 30 minutes to ensure full dissolution of the salts. The resulting clear pink solution is hydrothermal reaction mother liquor A. The molar ratio of the cobalt and zinc salts is 1:10. The cobalt salt is anhydrous cobalt chloride, and the zinc salt is anhydrous zinc chloride. The concentration of anhydrous cobalt chloride in hydrothermal reaction mother liquor A is 0.025 mol / L, and the concentration of anhydrous zinc chloride is 0.1 mol / L.
[0187] 2. Pour the above mother liquor A into a clean and dry closed reactor and carry out hydrothermal reaction at 220°C for 10 hours.
[0188] 3. After the hydrothermal reaction is completed, the sealed reactor is cooled naturally to room temperature, the reactor is opened, and the reaction liquid is filtered, and washed twice with deionized water and anhydrous ethanol to obtain a solid material B without formamide residue.
[0189] 4. Place solid material B in a 60°C forced air drying oven and dry for 2 hours to obtain dry solid material C.
[0190] 5. Grind the obtained solid material C into fine powder, and place the fine powder in a porcelain boat. Start from room temperature under the protection of inert gas N2, and heat at 5℃min. -1 The temperature was raised at a heating rate of 100 ℃, and then carbonized at a constant temperature of 1100 ℃ for 2 hours. After the constant temperature was completed, it was naturally cooled to room temperature to obtain cobalt single-atom nitrogen-carbon material (f-CoNC).
[0191] 6. Measure 12.5 mL of ethanol and deionized water of equal volume, mix them to obtain a mixed solution, dissolve 125 mg of the cobalt nitrogen carbon material synthesized above in the mixed solution, and sonicate for 1 hour to uniformly disperse it to obtain a mixed solution D.
[0192] 7. Place mixed solution D on a thermostatic stirring platform and stir for 10 minutes. During stirring, 2.53 mL of 10 mol / L hydrogen peroxide was evenly added dropwise to obtain a uniformly mixed reaction solution E. In reaction solution E, the concentration of the conductive substrate loaded with the first metal atom was 5 mg / mL, and the concentration of the peroxide was 1.0 mol / L.
[0193] 8. Transfer the reaction solution E to a high-pressure reactor, place it in an oven at 200°C, and react for 10 hours.
[0194] 9. After the reaction is completed, the solid material obtained in the high-pressure reactor is filtered, washed three times with deionized water, and placed in a vacuum freeze drying oven for overnight freeze drying to obtain the etched cobalt single-atom nitrogen-carbon material (etched f-CoNC).
[0195] 10. Weigh 250 mg of the dried solid of the etched f-CoNC material and dissolve it in a mixture of equal volumes of 12.5 mL of anhydrous ethanol and 12.5 mL of deionized water. After sonication for 1 hour, transfer the mixture to a thermostatic stirring platform to obtain a hydroalcoholic solution of the etched f-CoNC.
[0196] 11. Weigh an appropriate amount of nickel chloride powder and dissolve it in a mixture of equal volumes of 12.5 mL of anhydrous ethanol and 12.5 mL of deionized water. Ultrasonicate until dissolved to obtain a nickel chloride solution of 0.75 mg / mL (i.e., 0.006 mol / L) or 1.27 mg / mL (i.e., 0.01 mol / L).
[0197] 12. The aqueous alcohol solution of f-CoNC obtained in step 10 was stirred vigorously for 2 hours, and 25 mL of 0.75 mg of the aqueous alcohol solution obtained in step 11 was evenly added dropwise. Ni / mL or 1.27mg Ni / mL nickel chloride solution to obtain a mixed solution, and the nickel ions are adsorbed on the surface of the etched f-CoNC material by an immersion method. In this step 12, the concentration of the etched f-CoNC material in the mixed solution is 5mg / mL.
[0198] 13. After stirring the mixture obtained in step 12 for 2 hours, the mixture is filtered and washed, and the obtained solid material is freeze-dried in vacuum overnight.
[0199] 14. Place the solid material obtained after freeze drying in a porcelain boat. Under the protection of inert gas Ar / N2, heat it from room temperature at a rate of 5°C min -1 The temperature was raised to 900°C and carbonized at this temperature for 1 hour, followed by natural cooling to room temperature. Finally, a CoNiNC heteronuclear diatomic metal nitrogen-carbon catalyst (f-CoNiNC-1 or f-CoNiNC-2) was obtained.
[0200] FIG11 is a scanning electron microscope (SEM) image of the f-CoNiNC-1 metal diatomic material in Example 2.
[0201] Figure 12 is a transmission electron microscopy (TEM) image of the f-CoNiNC metal diatomic material in Example 2. At a scale of 5 nanometers, no nanoparticles of metal cobalt or nickel are visible.
[0202] In step 12, the concentration of nickel chloride solution is 0.75 mg Ni / mL, the product is f-CoNiNC-1.
[0203] In step 12, the concentration of nickel chloride solution is 1.27 mg Ni / mL, the product is f-CoNiNC-2.
[0204] FIG13 is an X-ray diffraction pattern (XRD) of f-CoNiNC-1 metal diatomic material and f-CoNiNC-2 metal diatomic material in Example 2.
[0205] FIG12 and FIG13 demonstrate that there are no nanoparticles of metal cobalt and metal nickel in the f-CoNiNC-1 metal diatomic material and the f-CoNiNC-2 metal diatomic material.
[0206] FIG14 is a high-angle annular dark field scanning transmission image (HAADF-STEM) of the f-CoNiNC-1 metal diatomic material in Example 2.
[0207] As shown in Figure 14, at a scale of 5 nanometers, or 555 square nanometers, there are many diatomic sites, with a total of 57 pairs of dimetallic atoms and a density of 0.10 pairs per square nanometer. This indicates a high probability of diatomic success.
[0208] Figure 15 compares the linear scan curves of f-CoNiNC-1 and f-CoNiNC-2 metal diatomic materials and various monometallic catalysts under alkaline conditions of 0.1 M KOH. The monometallic catalysts are f-CoNC obtained in step 5 and etched f-CoNC obtained in step 9.
[0209] The half-wave potentials of the f-CoNiNC-1 and f-CoNiNC-2 metal diatomic materials are 0.808 V and 0.810 V, respectively. The half-wave potential of the f-CoNC obtained in step 5 is 0.801 V, and the half-wave potential of the etched f-CoNC obtained in step 9 is 0.793 V. Figure 15 demonstrates that the catalytic performance of f-CoNiNC-1 and f-CoNiNC-2 is superior to that of the f-CoNC obtained in step 5 and the etched f-CoNC obtained in step 9.
[0210] Figure 45 shows a comparison of the full XPS spectra of f-CoNC and etched f-CoNC materials in Example 2. Comparing the full XPS spectra of f-CoNC obtained in step 5 and the etched f-CoNC obtained in step 9 in Figure 45 reveals that the C 1s peak intensity of the etched f-CoNC is significantly lower than that of f-CoNC, indicating that the etching primarily targets carbon atom sites. Furthermore, the N 1s peak intensity of the etched f-CoNC is significantly higher than that of f-CoNC, indicating that more nitrogen atoms are exposed after etching. Exposing more nitrogen atoms on the material surface can more effectively anchor more secondary metal atoms. This also lays a good foundation for the synthesis of high-density diatomic pads.
[0211] Example 3:
[0212] The preparation method of f-CoCoNC metal diatomic material is as follows:
[0213] 1. Dissolve the cobalt and zinc salts in 30 mL of formamide. Ultrasonicate for 30 minutes to ensure full dissolution of the salts. The resulting clear pink solution is hydrothermal reaction mother liquor A. The molar ratio of the cobalt and zinc salts is 1:10. The cobalt salt is anhydrous cobalt chloride, and the zinc salt is anhydrous zinc chloride. The concentration of anhydrous cobalt chloride in hydrothermal reaction mother liquor A is 0.025 mol / L, and the concentration of anhydrous zinc chloride is 0.1 mol / L.
[0214] 2. Pour the above mother liquor A into a clean, dry, closed reactor and carry out hydrothermal reaction at 160°C and autogenous pressure for 18 hours.
[0215] 3. After the hydrothermal reaction is completed, the sealed reactor is cooled naturally to room temperature, the reactor is opened, and the reaction liquid is filtered, and washed twice with deionized water and anhydrous ethanol to obtain a solid material B without formamide residue.
[0216] 4. Place solid material B in a 60°C forced air drying oven and dry for 2 hours to obtain dry solid material C.
[0217] 5. Grind the obtained solid material C into fine powder, and place the fine powder in a porcelain boat. Start from room temperature under the protection of inert gas N2, and heat at 5℃min. -1 The temperature was raised at a heating rate of 100 ℃, and then carbonized at a constant temperature of 900 ℃ for 6 hours. After the constant temperature was completed, it was naturally cooled to room temperature to obtain cobalt single-atom nitrogen-carbon material (f-CoNC).
[0218] 6. Measure 12.5 mL of ethanol and deionized water of equal volume, mix them into a solution, dissolve 25 mg of the cobalt nitrogen carbon material synthesized above in the mixed solution D, and sonicate for 1 hour until it is evenly dispersed.
[0219] 7. Place D on a thermostatic stirring platform and stir for 10 minutes. During the stirring period, 0.25 mL of 10 mol / L peracetate was evenly added dropwise to obtain a uniformly mixed reaction solution E. The concentration of the cobalt single-atom nitrogen-carbon material obtained in the reaction solution was 1 mg / mL, and the concentration of the peracetate was 0.1 mol / L.
[0220] 8. Transfer the reaction solution E to a high-pressure reactor, place it in an oven at 100°C, and react for 3 hours.
[0221] 9. After the reaction is completed, the solid material obtained in the high-pressure reactor is filtered, washed three times with deionized water, and placed in a vacuum freeze drying oven for overnight freeze drying to obtain the etched cobalt single-atom nitrogen-carbon material, which is the etched f-CoNC.
[0222] 10. Weigh 50 mg of the dry solid of the etched f-CoNC material and dissolve it in a mixed solution of equal volumes of 12.5 mL of anhydrous ethanol and 12.5 mL of deionized water. After sonication for 1 hour, transfer the solution to a stirring platform at room temperature to obtain a hydroalcoholic solution of the etched f-CoNC.
[0223] 11. Weigh 0.0324 mg of cobalt chloride powder and dissolve it in a mixture of equal volumes of 12.5 mL of anhydrous ethanol and 12.5 mL of deionized water. Ultrasonicate until dissolved to obtain a 1.30 mg / mL (i.e., 0.01 mol / L) cobalt chloride solution.
[0224] 12. The aqueous alcohol solution for etching f-CoNC obtained in step 10 was evenly added dropwise to the cobalt chloride solution obtained in step 11 under vigorous stirring for 2 hours, and nickel ions were adsorbed on the surface of the etched f-CoNC material by an immersion method.
[0225] 13. After stirring the mixture obtained in step 12 for 2 hours, the mixture was filtered and washed, and the obtained solid material was vacuum freeze-dried.
[0226] 14. Place the solid material obtained after freeze drying in a porcelain boat. Under the protection of inert gas Ar / N2, heat it from room temperature at a rate of 5°C min -1 The temperature was raised to 600°C and carbonized for 4 hours, followed by natural cooling to room temperature. Finally, the f-CoCoNC homonuclear metal diatomic material was obtained.
[0227] FIG. 16 is a scanning electron microscope (SEM) image of the f-CoCoNC metal diatomic material in Example 3.
[0228] 17 is a transmission electron microscopy (TEM) image of the f-CoCoNC metal diatomic material in Example 3. At a scale of 50 nanometers, no metallic cobalt nanoparticles are visible.
[0229] FIG18 is an X-ray diffraction pattern (XRD) of the f-CoCoNC metal diatomic material, the f-CoNC obtained in step 5, and the etched f-CoNC obtained in step 9 in Example 3.
[0230] FIG17 and FIG18 demonstrate that there are no metallic cobalt nanoparticles in the f-CoCoNC metallic diatomic material.
[0231] FIG19 is a high-angle annular dark field scanning transmission image (HAADF-STEM) of the f-CoCoNC metal diatomic material in Example 3.
[0232] As shown in Figure 19, at a scale of 2 nanometers, or within a range of 275 square nanometers, there are many diatomic sites, totaling 26 pairs of dimetallic atoms, with a diatomic pair density of 0.09 pairs / square nanometer, indicating a high probability of diatomic success.
[0233] Figure 20 compares the linear sweep curves of the f-CoCoNC metal diatomic material and various monometallic catalysts (f-CoNC obtained in step 5 and etched f-CoNC obtained in step 9) under alkaline conditions of 0.1 M KOH. The half-wave potential of the f-CoCoNC metal diatomic material is 0.800 V, while the half-wave potential of the f-CoNC obtained in step 5 is 0.795 V and the half-wave potential of the etched f-CoNC obtained in step 9 is 0.794 V. This demonstrates that the f-CoNC metal diatomic material exhibits superior oxygen reduction catalytic performance under alkaline conditions compared to the f-CoNC obtained in step 5 and the etched f-CoNC obtained in step 9.
[0234] Example 4:
[0235] The preparation method of FeRuNC metal diatomic material is as follows:
[0236] 1. Dissolve the iron and zinc salts in 30 mL of formamide as the solvent. Ultrasonicate for 30 minutes until both salts are fully dissolved in the formamide. The resulting homogeneous reddish-brown solution is hydrothermal reaction mother liquor A. The molar ratio of the iron and zinc salts is 1:20. The iron salt is ferric acetylacetonate, and the zinc salt is anhydrous zinc chloride. In hydrothermal reaction mother liquor A, the concentration of ferric acetylacetonate is 0.005 mol / L, and the concentration of anhydrous zinc chloride is 0.2 mol / L.
[0237] 2. Pour the above mother liquor A into a clean, dry, closed reactor and carry out hydrothermal reaction at 180°C for 12 hours.
[0238] 3. After the hydrothermal reaction is completed, the sealed reactor is cooled naturally to room temperature, the reactor is opened, and the reaction liquid is filtered, and washed twice with deionized water and anhydrous ethanol to obtain a solid material B without formamide residue.
[0239] 4. Place solid material B in a 60°C forced air drying oven and dry for 2 hours to obtain dry solid material C.
[0240] 5. Grind the obtained solid material C into fine powder, and place the fine powder in a porcelain boat. Start from room temperature under the protection of inert gas N2, and heat at 5℃min. -1 The temperature was raised at a heating rate of 1000 ℃, and then carbonized at a constant temperature of 900 ℃ for 2 hours. After the constant temperature was completed, it was naturally cooled to room temperature to obtain iron single-atom nitrogen-carbon material (FeNC).
[0241] 6. Measure 12.5 mL of ethanol and deionized water of equal volume, mix them into a solution, dissolve 50 mg of the iron-nitrogen-carbon material synthesized above in the mixed solution D, and sonicate for 1 hour until it is evenly dispersed.
[0242] 7. Place the mixed solution D on a constant temperature stirring table and stir for 10 minutes. During the stirring period, 0.25 mL of 10 mol / L sodium persulfate solution is evenly added dropwise to obtain a uniformly mixed reaction solution E.
[0243] 8. Transfer the reaction solution E to a high-pressure reactor, place it in an oven at 110°C, and react for 3 hours.
[0244] 9. After the reaction is completed, the solid material obtained in the high-pressure reactor is filtered, washed three times with deionized water, and placed in a vacuum freeze drying box for overnight freeze drying to obtain the etched iron single-atom nitrogen-carbon material (etched FeNC).
[0245] 10. Weigh 50 mg of the dry solid of the etched FeNC material and dissolve it in a mixed solution of equal volumes of 12.5 mL of anhydrous ethanol and 12.5 mL of deionized water. After ultrasonication for 1 hour, transfer it to a constant temperature stirring table to obtain a hydroalcoholic solution of etched FeNC.
[0246] 11. Weigh an appropriate amount of ruthenium chloride powder and dissolve it in a mixed solution of equal volumes of 12.5 mL of anhydrous ethanol and 12.5 mL of deionized water. Ultrasonicate until dissolved to obtain a 10 mg / mL (i.e., 0.0480 mol / L) ruthenium chloride solution.
[0247] 12. The hydroalcoholic FeNC-etched solution obtained in step 10 was evenly added dropwise to the ruthenium chloride solution obtained in step 11 under vigorous stirring for 2 hours to form a mixed solution. Ruthenium ions were adsorbed onto the surface of the FeNC-etched material by impregnation. The concentration of the FeNC-etched material in the mixed solution was 1 mg / mL, and the concentration of ruthenium chloride was 0.0240 mol / L.
[0248] 13. After stirring the mixture obtained in step 12 for 2 hours, the mixture is filtered and washed, and the obtained solid material is vacuum freeze-dried.
[0249] 14. Place the solid material obtained after freeze drying in a porcelain boat. Under the protection of inert gas Ar / N2, heat it from room temperature at a rate of 5°C min -1 The temperature was raised to 950°C and carbonized for 1 hour, followed by natural cooling to room temperature. Finally, the FeRuNC heteronuclear diatomic metal nitrogen-carbon catalyst was obtained.
[0250] FIG21 is a scanning electron microscope (SEM) image of the FeRuNC metal diatomic material in Example 4.
[0251] 22 is a transmission electron microscopy (TEM) image of the FeRuNC metal diatomic material in Example 4. At a scale of 50 nanometers, no nanoparticles of metallic iron or ruthenium are visible.
[0252] FIG. 23 is an X-ray diffraction pattern (XRD) of the FeRuNC metal diatomic material, the FeNC obtained in step 5, and the etched FeNC obtained in step 9 in Example 4.
[0253] 22 and 23 demonstrate that there are no nanoparticles of metallic iron and metallic ruthenium in the FeRuNC metallic diatomic material.
[0254] Figure 24 compares the linear sweep curves of the FeRuNC metal diatomic material and various monometallic catalysts (FeNC obtained in step 5 and etched FeNC obtained in step 9) under alkaline conditions of 0.1 M KOH. The half-wave potential of the FeRuNC metal diatomic material is 0.886 V. The half-wave potential of the FeNC obtained in step 5 is 0.853 V, and the half-wave potential of the etched FeNC obtained in step 9 is 0.842 V. This indicates that the FeRuNC metal diatomic material has superior electrocatalytic oxygen reduction activity compared to the FeNC obtained in step 5 and the etched FeNC obtained in step 9.
[0255] Example 5:
[0256] NiPtNC metallic diatomic materials
[0257] 1. Dissolve the nickel and zinc salts in 30 mL of formamide as the solvent. Ultrasonicate for 30 minutes until both salts are fully dissolved in the formamide, resulting in a homogeneous hydrothermal reaction solution A. The molar ratio of the nickel and zinc salts is 1:20. The iron salt is anhydrous nickel chloride, and the zinc salt is anhydrous zinc chloride. The concentrations of anhydrous nickel chloride and anhydrous zinc chloride in hydrothermal reaction solution A are 0.01 mol / L and 0.1 mol / L, respectively.
[0258] 2. Pour the above mother liquor A into a clean, dry, closed reactor and carry out hydrothermal reaction at 180°C for 12 hours.
[0259] 3. After the hydrothermal reaction is completed, the sealed reactor is cooled naturally to room temperature, the reactor is opened, and the reaction liquid is filtered, and washed twice with deionized water and anhydrous ethanol to obtain a solid material B without formamide residue.
[0260] 4. Place solid material B in a 60°C forced air drying oven and dry for 2 hours to obtain dry solid material C.
[0261] 5. Grind the obtained solid material C into fine powder, and place the fine powder in a porcelain boat. Start from room temperature under the protection of inert gas N2, and heat at 5℃min.-1 The temperature was raised at a heating rate of , and then carbonized at a constant temperature of 900 ° C for 2 hours. After the constant temperature was completed, it was naturally cooled to room temperature to obtain nickel single-atom nitrogen-carbon material (NiNC).
[0262] 6. Measure 12.5 mL of ethanol and deionized water of equal volume, mix them to obtain a mixed solution, dissolve 50 mg of the nickel-nitrogen-carbon material synthesized above in the mixed solution, and sonicate for 1 hour until it is evenly dispersed to obtain a mixed solution D.
[0263] 7. Place the mixed solution D on a constant temperature stirring table and stir for 10 minutes. During the stirring period, 0.25 mL of 10 mol / L peroxyphosphate solution is evenly added dropwise to obtain a uniformly mixed reaction solution E.
[0264] 8. Transfer the reaction solution E to a high-pressure reactor, place it in an oven at 200°C, and react for 3 hours.
[0265] 9. After the reaction is completed, the solid material obtained in the high-pressure reactor is filtered, washed three times with deionized water, and placed in a vacuum freeze drying box for overnight freeze drying to obtain the etched iron single-atom nitrogen-carbon material (etched NiNC).
[0266] 10. Weigh 50 mg of the dry solid of the etched NiNC material and dissolve it in a mixed solution of equal volumes of 12.5 mL of anhydrous ethanol and 12.5 mL of deionized water. After ultrasonication for 1 hour, transfer the solution to a thermostatic stirring platform to obtain a hydroalcoholic solution of the etched NiNC.
[0267] 11. Take an appropriate amount of chloroplatinic acid and dissolve it in a mixed solution of equal volumes of 12.5 mL of anhydrous ethanol and 12.5 mL of deionized water, and sonicate until uniformly dispersed to obtain a 10 mg / mL (0.024 mol / L) chloroplatinic acid solution.
[0268] 12. The NiNC etched aqueous alcohol solution obtained in step 10 was evenly added dropwise to the chloroplatinic acid solution obtained in step 11 under vigorous stirring for 2 hours, and ruthenium ions were adsorbed on the surface of the etched NiNC material by an impregnation method.
[0269] 13. After stirring the mixture obtained in step 12 for 2 hours, the mixture is filtered and washed, and the obtained solid material is vacuum freeze-dried.
[0270] 14. Place the solid material obtained after freeze drying in a porcelain boat. Under the protection of inert gas Ar / N2, heat it from room temperature at a rate of 5°C min -1 The temperature was raised to 950°C and carbonized at this temperature for 1 hour, followed by natural cooling to room temperature. Finally, the NiPtNC heteronuclear diatomic metal nitrogen-carbon catalyst was obtained.
[0271] FIG25 is a scanning electron microscope (SEM) image of the NiPtNC metal diatomic material in Example 5.
[0272] Figure 26 is a transmission electron microscopy (TEM) image of the NiPtNC metal diatomic material in Example 5. At a scale of 50 nanometers, no nickel or platinum nanoparticles are visible.
[0273] FIG27 is an X-ray diffraction pattern (XRD) of the NiPtNC metal diatomic material, the NiNC material obtained in step 5, and the etched NiPNC material obtained in step 9 in Example 5.
[0274] 26 and 27 demonstrate that there are no metallic nickel and metallic platinum nanoparticles in the NiPtNC metallic diatomic material.
[0275] Figure 28 compares the linear sweep curves of the NiPtNC metal diatomic material and various monometallic catalysts (the NiNC material obtained in step 5 and the etched NiPtNC material obtained in step 9) under alkaline conditions of 0.1 M KOH. The half-wave potential of the NiPtNC metal diatomic material is 0.812 V. The half-wave potential of the NiNC material obtained in step 5 is 0.707 V, and the half-wave potential of the etched NiPtNC material obtained in step 9 is 0.717 V. This indicates that the NiPtNC metal diatomic material has superior oxygen reduction catalytic activity under alkaline conditions to the NiNC material obtained in step 5 and the etched NiPtNC material obtained in step 9.
[0276] Example 6:
[0277] The preparation method of CoIrNC metal diatomic material is as follows:
[0278] 1. Dissolve the cobalt salt and zinc salt in 30 mL of formamide as the solvent. Ultrasonicate for 30 minutes until both salts are fully dissolved in the formamide, resulting in a homogeneous hydrothermal reaction solution A. The molar ratio of the cobalt salt to the zinc salt is 1:10. The cobalt salt is anhydrous cobalt chloride, and the zinc salt is anhydrous zinc chloride. The concentration of anhydrous cobalt chloride in hydrothermal reaction solution A is 0.005 mol / L, and the concentration of anhydrous zinc chloride is 0.1 mol / L.
[0279] 2. Pour the above mother liquor A into a clean, dry, closed reactor and carry out hydrothermal reaction at 180°C for 12 hours.
[0280] 3. After the hydrothermal reaction is completed, the sealed reactor is cooled naturally to room temperature, the reactor is opened, and the reaction liquid is filtered, and washed twice with deionized water and anhydrous ethanol to obtain a solid material B without formamide residue.
[0281] 4. Place solid material B in a 60°C forced air drying oven and dry for 2 hours to obtain dry solid material C.
[0282] 5. Grind the obtained solid material C into fine powder, and place the fine powder in a porcelain boat. Start from room temperature under the protection of inert gas N2, and heat at 5℃min. -1 The temperature was raised at a heating rate of 1000 ℃, and then carbonized at a constant temperature of 900 ℃ for 2 hours. After the constant temperature was completed, it was naturally cooled to room temperature to obtain cobalt single-atom nitrogen-carbon material (CoNC).
[0283] 6. Measure 12.5 mL of ethanol and deionized water of equal volume, mix them to obtain a mixed solution, dissolve 50 mg of the cobalt nitrogen carbon material synthesized above in the mixed solution, and sonicate for 1 hour until it is evenly dispersed to obtain a mixed solution D.
[0284] 7. Place the mixed solution D on a constant temperature stirring table and stir for 10 minutes. During the stirring period, 0.25 mL of 10 mol / L peroxycarbonate solution is evenly added dropwise to obtain a uniformly mixed reaction solution E.
[0285] 8. Transfer the reaction solution E to a high-pressure reactor, place it in an oven at 150°C, and react for 3 hours.
[0286] 9. After the reaction is completed, the solid material obtained in the high-pressure reactor is filtered, washed three times with deionized water, and placed in a vacuum freeze drying oven for overnight freeze drying to obtain the etched cobalt single-atom nitrogen-carbon material (etched CoNC).
[0287] 10. Weigh 50 mg of the dry solid of the etched CoNC material and dissolve it in a mixed solution of equal volumes of 12.5 mL of anhydrous ethanol and 12.5 mL of deionized water. After ultrasonication for 1 hour, transfer the solution to a thermostatic stirring platform to obtain a hydroalcoholic solution of etched CoNC.
[0288] 11. Take an appropriate amount of chloroiridic acid and dissolve it in a mixed solution of equal volumes of 12.5 mL of anhydrous ethanol and 12.5 mL of deionized water, and sonicate until uniformly dispersed to obtain a 10 mg / mL (0.0194 mol / L) chloroiridic acid solution.
[0289] 12. The aqueous alcohol solution for etching CoNC obtained in step 10 was evenly added dropwise to the chloroiridic acid solution obtained in step 11 under vigorous stirring for 2 hours, and ruthenium ions were adsorbed on the surface of the etched CoNC material by an impregnation method.
[0290] 13. After stirring the mixture obtained in step 12 for 2 hours, the mixture is filtered and washed, and the obtained solid material is vacuum freeze-dried.
[0291] 14. Place the solid material obtained after freeze drying in a porcelain boat. Under the protection of inert gas Ar / N2, heat it from room temperature at a rate of 5°C min -1 The temperature was raised to 950°C and carbonized at this temperature for 1 hour, followed by natural cooling to room temperature. Finally, the CoIrNC heteronuclear diatomic metal nitrogen-carbon catalyst was obtained.
[0292] FIG29 is a scanning electron microscope (SEM) image of the CoIrNC metal diatomic material in Example 6.
[0293] Figure 30 is a transmission electron microscopy (TEM) image of the CoIrNC metal diatomic material in Example 6. At a scale of 50 nanometers, no nanoparticles of metal cobalt or iridium appear.
[0294] FIG31 is an X-ray diffraction pattern (XRD) of the CoIrNC metal diatomic material, the CoNC material obtained in step 5, and the etched CoNC material obtained in step 9 in Example 6.
[0295] 30 and 31 demonstrate that the CoIrNC metal diatomic material does not contain nanoparticles of metallic cobalt and metallic iridium.
[0296] Figure 32 compares the linear scan curves of the CoIrNC metal diatomic material and various monometallic catalysts (the CoNC material obtained in step 5 and the etched CoNC material obtained in step 9) under alkaline conditions of 0.1 M KOH. The half-wave potential of the CoIrNC metal diatomic material is 0.885 V, significantly higher than that of the CoNC material (half-wave potential of 0.801 V) and the etched CoNC material (half-wave potential of 0.793 V). This indicates that the electrocatalytic oxygen reduction activity of the CoIrNC metal diatomic material is superior to that of the CoNC material obtained in step 5 and the etched CoNC material obtained in step 9.
[0297] Example 7:
[0298] The preparation method of MnRuNC metal diatomic material is as follows:
[0299] The method of Example 3 is the same as that of Example 3, except that the metal cobalt in step 1 is replaced by manganese, and the cobalt in step 11 is replaced by ruthenium. The MnRuNC metal diatomic material can be obtained in step 14.
[0300] In step 5, a manganese single atom nitrogen carbon material, namely, MnNC, can be obtained, and in step 9, an etched MnNC material can be obtained.
[0301] FIG33 is a scanning electron microscope (SEM) image of the MnRuNC metal diatomic material.
[0302] Figure 34 compares the linear sweep curves of the MnRuNC metal diatomic material, MnNC, and etched MnNC under alkaline conditions of 0.1 M KOH. The half-wave potential of the MnRuNC metal diatomic material is 0.788 V, which is higher than that of the MnNC material (0.757 V) and the etched MnNC material (0.723 V). This indicates that the electrocatalytic oxygen reduction activity of the MnRuNC metal diatomic material is superior to that of the MnNC and etched MnNC materials.
[0303] Example 8:
[0304] The preparation method of MnPtNC metal diatomic materials is as follows:
[0305] According to the method of Example 3, only the metal cobalt in step 1 is replaced by manganese, the peracetate in step 7 is replaced by peroxodisulfate, and the cobalt in step 11 is replaced by platinum. The remaining steps are the same, and the MnPtNC metal diatomic material can be obtained.
[0306] In step 5, a manganese single atom nitrogen carbon material, namely, MnNC, can be obtained, and in step 9, an etched MnNC material can be obtained.
[0307] FIG35 is a scanning electron microscope (SEM) image of MnPtNC metal diatomic material.
[0308] Figure 36 compares the linear sweep curves of the MnPtNC metal diatomic material, MnNC, and etched MnNC under alkaline conditions of 0.1 M KOH. The half-wave potential of the MnPtNC metal diatomic material is 0.844 V, which is higher than that of the MnNC material (half-wave potential of 0.774 V) and the etched MnNC material (half-wave potential of 0.734 V). This indicates that the electrocatalytic oxygen reduction activity of the MnPtNC metal diatomic material is superior to that of the MnNC and etched MnNC materials.
[0309] Example 9:
[0310] The preparation method of NiAuNC metal diatomic material is as follows:
[0311] According to the method of Example 3, only the metal cobalt in step 1 is replaced by nickel, and the cobalt in step 11 is replaced by gold. The remaining steps are the same, and the NiAuNC metal diatomic material can be obtained.
[0312] In step 5, nickel single-atom nitrogen-carbon material, namely NiNC, can be obtained, and in step 9, etched NiNC material can be obtained.
[0313] FIG37 is a scanning electron microscope (SEM) image of NiAuNC metal diatomic material.
[0314] Figure 38 compares the linear scan curves of the NiAuNC metal diatomic material, NiNC, and etched NiNC under alkaline conditions of 0.1 M KOH. The half-wave potential of the NiAuNC metal diatomic material is 0.786 V, which is higher than that of the NiNC material (0.707 V) and the etched NiNC material (0.717 V). This indicates that the electrocatalytic oxygen reduction activity of the NiAuNC metal diatomic material is superior to that of the NiNC and etched NiNC materials.
[0315] Example 10:
[0316] The preparation method of NiAgNC metal diatomic material is as follows:
[0317] According to the method of Example 3, only the metal cobalt in step 1 is replaced by nickel, and the cobalt in step 11 is replaced by silver. The remaining steps are the same, thereby obtaining the NiAgNC metal diatomic material.
[0318] In step 5, nickel single-atom nitrogen-carbon material, namely NiNC, can be obtained, and in step 9, etched NiNC material can be obtained.
[0319] FIG39 is a scanning electron microscope (SEM) image of NiAgNC metal diatomic material.
[0320] Figure 40 compares the linear sweep curves of the NiAuNC metal diatomic material, NiNC, and etched NiNC under alkaline conditions of 0.1 M KOH. The half-wave potential of the NiAgNC metal diatomic material is 0.807 V, which is higher than that of the NiNC material (0.707 V) and the etched NiNC material (0.717 V). This indicates that the electrocatalytic oxygen reduction activity of the NiAgNC metal diatomic material is superior to that of the NiNC and etched NiNC materials.
[0321] Example 11:
[0322] The preparation method of FeRuSNC metal diatomic material is as follows:
[0323] 1. Dissolve the iron salt, zinc salt, and thiourea in 30 mL of formamide as the solvent. Ultrasonicate for 30 minutes until both salts are fully dissolved in the formamide. The resulting homogeneous reddish-brown solution is hydrothermal reaction mother liquor A. The molar ratio of the iron salt to the zinc salt is 1:20. The iron salt is ferric acetylacetonate, and the zinc salt is anhydrous zinc chloride. In hydrothermal reaction mother liquor A, the concentration of ferric acetylacetonate is 0.005 mol / L, and the concentration of anhydrous zinc chloride is 0.2 mol / L.
[0324] 2. Pour the above mother liquor A into a clean, dry, closed reactor and carry out hydrothermal reaction at 180°C for 12 hours.
[0325] 3. After the hydrothermal reaction is completed, the sealed reactor is cooled naturally to room temperature, the reactor is opened, and the reaction liquid is filtered, and washed twice with deionized water and anhydrous ethanol to obtain a solid material B without formamide residue.
[0326] 4. Place solid material B in a 60°C forced air drying oven and dry for 2 hours to obtain dry solid material C.
[0327] 5. Grind the obtained solid material C into fine powder, and place the fine powder in a porcelain boat. Start from room temperature under the protection of inert gas N2, and heat at 5℃min. -1 The temperature was raised at a heating rate of 1000 ℃, and then carbonized at a constant temperature of 900 ℃ for 2 hours. After the constant temperature was completed, it was naturally cooled to room temperature to obtain iron single-atom sulfur-nitrogen-carbon material (FeSNC).
[0328] 6. Measure 12.5 mL of ethanol and deionized water of equal volume, mix them into a solution, dissolve 50 mg of the iron-sulfur-nitrogen-carbon material synthesized above in the mixed solution D, and sonicate for 1 hour until it is evenly dispersed.
[0329] 7. Place the mixed solution D on a constant temperature stirring table and stir for 10 minutes. During the stirring period, evenly add 0.25 mL of a 30% (10 mol / L) hydrogen peroxide solution to obtain a uniformly mixed reaction solution E.
[0330] 8. Transfer the reaction solution E to a high-pressure reactor, place it in an oven at 110°C, and react for 3 hours.
[0331] 9. After the reaction is completed, the solid material obtained in the high-pressure reactor is filtered, washed three times with deionized water, and placed in a vacuum freeze drying box for overnight freeze drying to obtain the etched iron single-atom nitrogen carbon material (etched FeSNC).
[0332] 10. Weigh 50 mg of the dry solid of the etched FeSNC material and dissolve it in a mixed solution of equal volumes of 12.5 mL of anhydrous ethanol and 12.5 mL of deionized water. After ultrasonication for 1 hour, transfer it to a constant temperature stirring table to obtain a hydroalcoholic solution of etched FeSNC.
[0333] 11. Weigh an appropriate amount of ruthenium chloride powder and dissolve it in a mixed solution of equal volumes of 12.5 mL of anhydrous ethanol and 12.5 mL of deionized water. Ultrasonicate until dissolved to obtain a 10 mg / mL (i.e., 0.048 mol / L) ruthenium chloride solution.
[0334] 12. The hydroalcoholic FeSNC-etched solution obtained in step 10 was evenly added dropwise to the ruthenium chloride solution obtained in step 11 under vigorous stirring for 2 hours to form a mixed solution. Ruthenium ions were adsorbed onto the surface of the etched FeSNC material by impregnation. The concentration of the FeSNC-etched material in the mixed solution was 1 mg / mL, and the concentration of the ruthenium chloride solution was 0.024 mol / L.
[0335] 13. After stirring the mixture obtained in step 12 for 2 hours, the mixture is filtered and washed, and the obtained solid material is vacuum freeze-dried.
[0336] 14. Place the solid material obtained after freeze drying in a porcelain boat. Under the protection of inert gas Ar / N2, heat it from room temperature at a rate of 5°C min -1 The temperature was raised to 950°C and carbonized at this temperature for 1 hour, and then naturally cooled to room temperature. Finally, the FeRuSNC heteronuclear diatomic metal sulfur-nitrogen-carbon catalyst was obtained.
[0337] FIG41 is a scanning electron microscope (SEM) image of the FeRuSNC metal diatomic material in Example 11.
[0338] Figure 42 is a transmission electron microscopy (TEM) image of the FeRuSNC metal diatomic material in Example 11. At a scale of 50 nanometers, no metallic iron or ruthenium nanoparticles are visible.
[0339] FIG43 is an X-ray diffraction pattern (XRD) of the FeRuSNC metal diatomic material, the FeNC obtained in step 5, and the etched FeSNC obtained in step 9 in Example 11.
[0340] 42 and 43 demonstrate that there are no nanoparticles of metallic iron and metallic ruthenium in the FeRuSNC metallic diatomic material.
[0341] Figure 44 compares the linear scan curves of the FeRuSNC metal diatomic material and various monometallic catalysts (FeSNC obtained in step 5 and etched FeSNC obtained in step 9) under alkaline conditions of 0.1 M KOH. The half-wave potential of the FeRuSNC metal diatomic material is 0.878 V. The half-wave potential of the FeSNC obtained in step 5 is 0.833 V, and the half-wave potential of the etched FeSNC obtained in step 9 is 0.813 V. This indicates that the FeRuSNC metal diatomic material has superior electrocatalytic oxygen reduction activity compared to the FeSNC obtained in step 5 and the etched FeSNC obtained in step 9.
[0342] The above embodiments only use several metal elements as examples. It can be expected that other metal elements disclosed in this application will also have the same effect.
[0343] The specific conditions of Examples 12 to 17 are as follows:
[0344] Example 12
[0345] The preparation method of the iron-platinum-nitrogen-carbon material comprises the following steps:
[0346] 1. Dissolve the iron and zinc salts in 30 mL of formamide as the solvent. Ultrasonicate for 30 minutes to ensure that both salts are fully dissolved in the formamide. The resulting homogeneous dark red solution is hydrothermal reaction mother liquor A. The molar ratio of the iron and zinc salts is 1:10. The iron salt is ferric acetylacetonate at a molarity of 0.005 mol / L. The zinc salt is anhydrous zinc chloride at a molarity of 0.1 mol / L.
[0347] 2. Pour the above hydrothermal reaction mother solution A into a clean and dry closed reactor and carry out hydrothermal reaction at 180°C for 12 hours.
[0348] 3. After the hydrothermal reaction is completed, the sealed reactor is cooled naturally to room temperature, the reactor is opened, and the reaction liquid is filtered, and washed twice with deionized water and anhydrous ethanol to obtain a solid material B without formamide residue.
[0349] 4. Place solid material B in a 60°C forced air drying oven and dry for 2 hours until dry solid material C is obtained.
[0350] 5. Grind the obtained solid material C into fine powder, and place the fine powder in a porcelain boat. Start from room temperature under the protection of inert gas N2, and heat at 5℃min. -1 The temperature was raised at a heating rate of 1000 ℃, and then carbonized at a constant temperature of 900 ℃ for 2 hours. After the constant temperature was completed, it was naturally cooled to room temperature to obtain iron single-atom nitrogen-carbon material (FeNC-1).
[0351] 6. Measure equal volumes of ethanol and deionized water (15 mL each) and mix to form a solution. Dissolve 60 mg of the synthesized iron monatomic nitrogen carbon material (FeNC-1) in the mixed solution D. Ultrasonicate for 30 minutes until uniformly dispersed. The resulting concentration of the iron monatomic nitrogen carbon material is 2 mg / mL.
[0352] 7. Mixed solution D was placed on a thermostatic stirring platform and stirred for 10 minutes. During the stirring period, 0.30 mL of a 30% hydrogen peroxide solution was evenly added dropwise to obtain a uniformly mixed reaction solution E. In reaction solution E, the concentration of hydrogen peroxide was 0.1 mol / L, and the concentration of the iron single-atom nitrogen-carbon material was 2 mg / mL.
[0353] 8. Transfer the reaction solution E to a high-pressure reactor, place it in an oven at 110°C, and react for 3 hours.
[0354] 9. After the reaction is completed, the solid material obtained in the high-pressure reactor is filtered, washed three times with deionized water, and placed in a vacuum freeze-drying box for overnight freeze-drying to obtain the etched iron single-atom nitrogen-carbon material (etched FeNC-1).
[0355] 10. Weigh 50 mg of the dry solid of the etched FeNC-1 material and dissolve it in a mixed solution of equal volumes of 25 mL of anhydrous ethanol and 25 mL of deionized water. After ultrasonication for 1 hour, transfer it to a constant temperature stirring table to obtain a hydroalcoholic solution of etched FeNC-1.
[0356] 11. Add 17.5 μL of chloroplatinic acid solution (1.05 g / ml) evenly to the aqueous alcohol solution of etched FeNC-1 obtained in step 10 to obtain a mixed solution. Stir vigorously at room temperature for 2 hours. Adsorb platinum ions onto the surface of the etched FeNC-1 material by immersion. The concentration of etched FeNC-1 in the mixed solution is 1 mg / mL.
[0357] The concentration of chloroplatinic acid is 0.0009 mol / L
[0358] After 12 hours of stirring, the mixture was filtered and washed, and the obtained solid material was vacuum freeze-dried.
[0359] 13. Place the solid material obtained after freeze drying in a porcelain boat. Under the protection of inert gas Ar / N2, heat it from room temperature at a rate of 5°C min -1 The temperature was raised to 950°C and carbonized at this temperature for 1 hour, followed by natural cooling to room temperature. Finally, the heteronuclear diatomic metal nitrogen-carbon catalyst (FePtNC-1) was obtained.
[0360] First, characterize the above materials:
[0361] FIG46 is a scanning electron microscope (SEM) image of FePtNC.
[0362] As shown in FIG46 , scanning electron microscopy (SEM) observations show that the morphology of the FePtNC diatomic particles is amorphous, with some porous structures.
[0363] FIG47 is a transmission electron microscopy (TEM) image of FePtNC.
[0364] As shown in Figure 47: Transmission electron microscopy (TEM) shows that FePtNC diatoms are thin sheets and exhibit a multi-layer stacked sheet structure.
[0365] FIG48 is a high-angle annular dark-field scanning transmission electron microscopy (HAADF-STEM) image of FePtNC.
[0366] Figure 48 confirms the existence of FePtNC diatomic structures. The bright spots in the image represent metal atoms, most of which appear as pairs of iron-platinum atoms, proving that the material is FePtNC diatomic.
[0367] The distance between the two atoms was measured by direct measurement analysis method, and the distance statistics between the two atoms are shown in Table 1 below.
[0368] Table 1
[0369] Table 1 above proves that the distance between all diatoms is less than or equal to 0.5 nm, that is, the distance between a single iron atom and a single platinum atom is less than or equal to 0.5 nanometers, specifically 0.14 to 0.5 nm.
[0370] As shown in Figure 48, there are 15 pairs of bimetallic atomic pairs at a scale of 2 nanometers, that is, 158.24 square nanometers, and the density of atomic pairs is higher, indicating that this FePtNC diatomic material and preparation method have unique advantages, and the success rate of bimetallic atomic pairs prepared by this method is higher.
[0371] Figure 1d of Reference 2 shows a high-angle annular dark-field transmission image of a PtFeNC bimetallic atom catalyst. As shown in Figure 1d of Reference 2, at a 5-nanometer scale, 1126.388 square nanometers, there are 15 pairs of bimetallic atoms, a relatively small number of pairs. Comparing Figure 48 with Figure 1d of Reference 2 demonstrates that the present material exhibits a higher number of diatomic sites. This demonstrates that the success rate of diatomic formation on a conductive nitrogen-carbon substrate is greater than that of bimetallic atoms prepared by a one-pot hydrothermal method.
[0372] In FIG48 and FIG1d of reference 2, the area of the picture was obtained by the inventor through calculation and conversion based on the scale in the picture and the actual size of the picture.
[0373] FIG49 is an X-ray diffraction (XRD) pattern of FePtNC-1, FeNC-1, and etched FeNC-1.
[0374] The X-ray diffraction (XRD) pattern in Figure 49 shows that the FePtNC-1 diatomic material exhibits only two diffraction peaks at 25° and 43°, corresponding to the (002) and (100) planes of graphitic carbon, respectively. No diffraction peaks are observed for metallic iron or platinum nanoparticles, indicating that the synthesized material series contains no metal particles. Both iron and platinum are dispersed in a monoatomic state.
[0375] Second, performance test:
[0376] The performance of the FePtNC-1 obtained above was tested using a CHI three-electrode system, and a linear sweep voltage (LSV) test was performed at an O2-saturated 0.1 M KOH and a rotation speed of 1600 rpm.
[0377] Figure 50 is the linear sweep polarization curve of oxygen reduction of FePtNC-1 bimetallic atom catalyst, FeNC-1 and etched FeNC-1, 20wt% Pt / C material at 1600rmp
[0378] Figure 50 proves that under alkaline conditions of 0.1 M KOH, the half-wave potential of the FePtNC-1 diatomic is 0.905 V, which is much better than that of FeNC-1 at the single-atom level, etched FeNC-1, and FeNC-1 (the half-wave potential of FeNC-1 is 0.853 V, and the half-wave potential of etched FeNC is 0.842 V).
[0379] Meanwhile, the half-wave potential of FePtNC-1 diatoms is 33 mV higher than that of 20 wt% Pt / C (0.872 V).
[0380] Figure 50 proves that adding a second metal species to form a diatomic catalyst can greatly enhance the oxygen reduction performance of the single-atom catalyst and accelerate the oxygen reduction reaction rate.
[0381] The 20 wt % Pt / C material is a Pt / C material with a Pt content of 20% by mass, and can be purchased on the market.
[0382] The etched FeNC-1 source was prepared according to the preparation process in Example 1, and the product was obtained in step 9.
[0383] The FeNC-1 source was prepared according to the preparation process in Example 1, and the product obtained in step 5.
[0384] Figure 51 shows the four-electron transfer number and hydrogen peroxide yield of FePt bimetallic atom catalyst material.
[0385] Figure 51 demonstrates that the electron transfer number of the FePtNC-1 diatoms calculated from experimental data is 4, very close to the 4-electron transfer number. Furthermore, the hydrogen peroxide yield is less than 1% over a wide potential range, indicating the high 4-electron selectivity of the FePtNC-1 diatoms. In Figure 51, a 20 wt% Pt / C material is used as a reference material for comparison with FePtNC-1, demonstrating the excellent electrocatalytic oxygen reduction performance of the FePtNC-1 diatoms.
[0386] FePtNC-1 diatomic catalysts and 20wt% Pt / C materials were tested under oxygen-saturated 0.1M KOH alkaline conditions. Figure 52 shows the oxygen reduction polarization curves of the FePtNC-1 diatomic catalysts and 20wt% Pt / C materials before and after 10,000 cycles. Figure 52 shows that after 10,000 cycles, the half-wave potential of the FePtNC-1 diatomic catalyst only shifted negatively by 8 mV, indicating negligible activity decay. In contrast, the half-wave potential of the 20wt% Pt / C material exhibited a significant decay.
[0387] Example 13
[0388] The preparation method of the iron-platinum-nitrogen-carbon material comprises the following steps:
[0389] 1. Dissolve the iron and zinc salts in 30 mL of formamide as the solvent. Ultrasonicate for 30 minutes to ensure that both salts are fully dissolved in the formamide. The resulting homogeneous dark red solution is hydrothermal reaction mother liquor A. The molar ratio of the iron and zinc salts is 1:4. The iron salt is anhydrous ferric chloride with a molarity of 0.005 mol / L. The zinc salt is anhydrous zinc chloride with a molarity of 0.2 mol / L.
[0390] 2. Pour the above hydrothermal reaction mother solution A into a clean and dry closed reactor and carry out hydrothermal reaction at 160°C for 12 hours.
[0391] 3. After the hydrothermal reaction is completed, the sealed reactor is cooled naturally to room temperature, the reactor is opened, and the reaction liquid is filtered, and washed twice with deionized water and anhydrous ethanol to obtain a solid material B without formamide residue.
[0392] 4. Place solid material B in a 60°C forced air drying oven and dry for 2 hours until dry solid material C is obtained.
[0393] 5. Grind the obtained solid material C into fine powder, and place the fine powder in a porcelain boat. Start from room temperature under the protection of inert gas N2, and heat at 5℃min. -1 The temperature was raised at a heating rate of 1000 ° C., and then carbonized at a constant temperature of 800 ° C. for 4 hours. After the constant temperature was completed, it was naturally cooled to room temperature to obtain iron single-atom nitrogen-carbon material (FeNC-2).
[0394] 6. Measure equal volumes of ethanol and deionized water (12.5 mL each) and mix to form a solution. Dissolve 50 mg of the synthesized iron monatomic nitrogen carbon material (FeNC-2) in the mixed solution D. Ultrasonicate for 30 minutes until uniformly dispersed. The resulting concentration of the iron monatomic nitrogen carbon material is 2 mg / mL.
[0395] 7. Mixed solution D was placed on a thermostatic stirring platform and stirred for 10 minutes. During the stirring period, 0.126 mL of a 10 mol / L peroxodisulfate solution was evenly added dropwise to obtain a uniformly mixed reaction solution E. The concentration of peroxodisulfate in reaction solution E was 0.05 mol / L, and the concentration of the iron monoatomic nitrogen-carbon material was 2 mg / mL.
[0396] 8. Transfer the reaction solution E to a high-pressure reactor, place it in an oven at 150°C, and react for 5 hours.
[0397] 9. After the reaction is completed, the solid material obtained in the high-pressure reactor is filtered, washed three times with deionized water, and placed in a vacuum freeze drying oven for overnight freeze drying to obtain the etched iron single-atom nitrogen-carbon material (etched FeNC-2).
[0398] 10. Weigh 50 mg of the dry solid of the etched FeNC-2 material and dissolve it in a mixed solution of equal volumes of 25 mL of anhydrous ethanol and 25 mL of deionized water.
[0399] 11. After sonicating for 1 hour, transfer the mixture to a thermostatic stirring platform and evenly add 17.5 μL of chloroplatinic acid solution (1.05 g / mL) dropwise to create a mixture. Stir vigorously at room temperature for 2 hours to allow platinum ions to adsorb onto the surface of the etched FeNC-2 material by immersion. The resulting mixture contains 1 mg / mL of FeNC-1 and 0.0009 mol / L of chloroplatinic acid.
[0400] After 12 hours of stirring, the mixture was filtered and washed, and the obtained solid material was vacuum freeze-dried.
[0401] 13. Place the solid material obtained after freeze drying in a porcelain boat. Under the protection of inert gas Ar / N2, heat it from room temperature at a rate of 5°C min -1 The temperature was raised to 950°C and carbonized at this temperature for 1 hour, followed by natural cooling to room temperature. Finally, the heteronuclear diatomic metal nitrogen-carbon catalyst (FePtNC-2) was obtained.
[0402] Material characterization and performance testing are as follows:
[0403] FIG53 is a scanning electron microscope (SEM) image of the FePtNC-2 diatomic material of Example 13.
[0404] Figure 54 shows X-ray diffraction (XRD) patterns of FePtNC-2 obtained in step 13 of Example 13, FeNC-2 obtained in step 9, and etched FeNC-2 obtained in step 5. Figure 54 shows only two carbon peaks, indicating the absence of metal nanoparticles in FeNC-2, etched FeNC-2, and FePtNC-2.
[0405] Figure 55 shows a high-angle annular dark-field scanning transmission electron microscopy (HAADF-STEM) image of the FePtNC-2 diatomic material from Example 13. As shown in Figure 55 , at a scale of 2 nanometers, or 112 square nanometers, there are 21 bimetallic atomic pairs, or 0.18 pairs per square nanometer, indicating a higher atomic pair density. This demonstrates the unique advantages of this FePtNC diatomic material and preparation method, which results in a higher success rate for preparing bimetallic atomic pairs.
[0406] Figure 56 shows the linear sweep polarization curves for oxygen reduction of the FePtNC-2 diatomic material of Example 13, the FeNC-2 obtained in Step 5, and the etched FeNC-2 obtained in Step 9 under the alkaline conditions of 0.1 M KOH saturated with O2 at a rotation speed of 1600 rpm. As shown in Figure 56, the half-wave potential of the FePtNC-2 diatomic material is 0.887 V, while the half-wave potential of FeNC-2 is 0.860 V and the half-wave potential of the etched FeNC-2 is 0.812 V. A comparative analysis reveals that FePtNC-2 has the highest half-wave potential, indicating the best electrocatalytic oxygen reduction activity. This demonstrates that single iron atoms and single platinum atoms have a synergistic effect in the electrocatalytic oxygen reduction reaction, and that the catalytic activity of the iron-platinum diatomic material is higher than that of the iron atoms.
[0407] Example 14
[0408] The preparation method of the iron-platinum-nitrogen-carbon material comprises the following steps:
[0409] 1. Dissolve the iron and zinc salts in 30 mL of formamide as the solvent. Ultrasonicate for 30 minutes to ensure that both salts are fully dissolved in the formamide. The resulting homogeneous dark red solution is hydrothermal reaction mother liquor A. The molar ratio of the iron and zinc salts is 1:20. The iron salt is anhydrous ferric chloride with a molarity of 0.005 mol / L. The zinc salt is anhydrous zinc chloride with a molarity of 0.2 mol / L.
[0410] 2. Pour the above hydrothermal reaction mother solution A into a clean and dry closed reactor and carry out hydrothermal reaction at 220°C for 12 hours.
[0411] 3. After the hydrothermal reaction is completed, the sealed reactor is cooled naturally to room temperature, the reactor is opened, and the reaction liquid is filtered, and washed twice with deionized water and anhydrous ethanol to obtain a solid material B without formamide residue.
[0412] 4. Place solid material B in a 60°C forced air drying oven and dry for 2 hours until dry solid material C is obtained.
[0413] 5. Grind the obtained solid material C into fine powder, and place the fine powder in a porcelain boat. Start from room temperature under the protection of inert gas N2, and heat at 5℃min. -1The temperature was raised at a heating rate of 1000 ° C., and then carbonized at a constant temperature of 1100 ° C. for 6 hours. After the constant temperature was completed, it was naturally cooled to room temperature to obtain iron single-atom nitrogen-carbon material (FeNC-3).
[0414] 6. Measure equal volumes of ethanol and deionized water (12.5 mL each) and mix to form a solution. Dissolve 100 mg of the synthesized FeNC-3 in the mixed solution D. Ultrasonicate for 30 minutes until uniformly dispersed. The resulting concentration of FeNC-3 is 4 mg / mL.
[0415] 7. Place mixed solution D on a thermostatic stirring platform and stir for 10 minutes. During the stirring period, 2.5 mL of 10 mol / L sodium persulfate solution was evenly added dropwise to obtain a uniformly mixed reaction solution E. The concentration of sodium persulfate in reaction solution E was 1.0 mol / L, and the concentration of the iron monoatomic nitrogen-carbon material was 4 mg / mL.
[0416] 8. Transfer the reaction solution E to a high-pressure reactor, place it in an oven at 200°C, and react for 8 hours.
[0417] 9. After the reaction is completed, the solid material obtained in the high-pressure reactor is filtered, washed three times with deionized water, and placed in a vacuum freeze drying oven for overnight freeze drying to obtain the etched iron single-atom nitrogen-carbon material (etched FeNC-3).
[0418] 10. Weigh 100 mg of the dry solid of the etched FeNC-3 material and dissolve it in a mixed solution of equal volumes of 25 mL of anhydrous ethanol and 25 mL of deionized water.
[0419] 11. After sonication for 1 hour, transfer the mixture to a thermostatic stirring platform and evenly add 35 μL of 1.05 g / mL chloroplatinic acid solution dropwise to create a mixture. Stir vigorously at room temperature for 2 hours to allow platinum ions to adsorb onto the surface of the etched FeNC-3 material by impregnation. The resulting mixture contains 2 mg / mL of etched FeNC-1 and 0.0018 mol / L of chloroplatinic acid.
[0420] After 12 hours of stirring, the mixture was filtered and washed, and the obtained solid material was vacuum freeze-dried.
[0421] 13. Place the solid material obtained after freeze drying in a porcelain boat. Under the protection of inert gas Ar / N2, heat it from room temperature at a rate of 5°C min -1 The temperature was raised to 950°C and carbonized at this temperature for 1 hour, followed by natural cooling to room temperature. Finally, the heteronuclear diatomic metal nitrogen-carbon catalyst (FePtNC-3) was obtained.
[0422] Material characterization and performance testing are as follows:
[0423] FIG57 is a scanning electron microscope (SEM) image of the FePtNC-3 diatomic material of Example 14.
[0424] Figure 58 shows X-ray diffraction (XRD) patterns of FePtNC-3 obtained in step 13 of Example 14, FeNC-3 obtained in step 9, and etched FeNC-3 obtained in step 5. Figure 58 shows only two carbon peaks, indicating the absence of metal nanoparticles in FeNC-3, etched FeNC-3, and FePtNC-3.
[0425] Figure 59 shows the linear sweep polarization curves for oxygen reduction of the FePtNC-3 diatomic material from Example 14, the FeNC-3 obtained from Step 5, and the etched FeNC-3 obtained from Step 9 under alkaline conditions of 0.1 M KOH saturated with O2 at a rotation speed of 1600 rpm. As shown in Figure 59, the half-wave potential of the FePtNC-3 diatomic material is 0.884 V, while that of FeNC-3 is 0.855 V and that of the etched FeNC-3 is 0.837 V. A comparative analysis reveals that FePtNC-3 has the highest half-wave potential, indicating the best electrocatalytic oxygen reduction activity. This demonstrates that single iron atoms and single platinum atoms have a synergistic effect in the electrocatalytic oxygen reduction reaction, and that the catalytic activity of the iron-platinum diatomic material is higher than that of the iron atoms.
[0426] Example 15
[0427] The preparation method of platinum iron sulfur nitrogen carbon material comprises the following steps:
[0428] 1. Use 30 mL of formamide as a solvent to dissolve the iron salt, zinc salt, and sulfur source. Ultrasonicate for 30 minutes to ensure that the two salts are fully dissolved in the formamide. The resulting uniform dark red solution is the hydrothermal reaction mother liquor A. The molar ratio of the iron salt, zinc salt, and sulfur source is 1:10:2. The iron salt is anhydrous ferric chloride with a molar number of 0.005 mol / L. The zinc salt is anhydrous zinc chloride with a molar number of 0.1 mol / L. The sulfur source is thiourea with a molar number of 0.01 mol / L.
[0429] 2. Pour the above hydrothermal reaction mother solution A into a clean and dry closed reactor and carry out hydrothermal reaction at 180°C for 12 hours.
[0430] 3. After the hydrothermal reaction is completed, the sealed reactor is cooled naturally to room temperature, the reactor is opened, and the reaction liquid is filtered, and washed twice with deionized water and anhydrous ethanol to obtain a solid material B without formamide residue.
[0431] 4. Place solid material B in a 60°C forced air drying oven and dry for 2 hours until dry solid material C is obtained.
[0432] 5. Grind the obtained solid material C into fine powder, and place the fine powder in a porcelain boat. Start from room temperature under the protection of inert gas N2, and heat at 5℃min. -1 The temperature was raised at a heating rate of 1000 ℃, and then carbonized at a constant temperature of 900 ℃ for 2 hours. After the constant temperature was completed, it was naturally cooled to room temperature to obtain iron single-atom nitrogen-carbon material (FeSNC-1).
[0433] 6. Measure equal volumes of ethanol and deionized water (12.5 mL each) and mix to form a solution. Dissolve 50 mg of the synthesized iron single-atom nitrogen carbon material (FeSNC-1) in the mixed solution D. Ultrasonicate for 30 minutes until uniformly dispersed. The resulting concentration of the iron single-atom nitrogen carbon material is 2 mg / mL.
[0434] 7. Mixed solution D was placed on a thermostatic stirring platform and stirred for 10 minutes. During the stirring period, 0.30 mL of a 30% hydrogen peroxide solution was evenly added dropwise to obtain a uniformly mixed reaction solution E. In reaction solution E, the concentration of hydrogen peroxide was 0.1 mol / L, and the concentration of the iron single-atom nitrogen-carbon material was 2 mg / mL.
[0435] 8. Transfer the reaction solution E to a high-pressure reactor, place it in an oven at 110°C, and react for 3 hours.
[0436] 9. After the reaction is completed, the solid material obtained in the high-pressure reactor is filtered, washed three times with deionized water, and placed in a vacuum freeze drying box for overnight freeze drying to obtain the etched iron single-atom nitrogen-carbon material (etched FeSNC-1).
[0437] 10. Weigh 50 mg of the dry solid of the etched FeSNC-1 material and dissolve it in a mixed solution of equal volumes of 25 mL of anhydrous ethanol and 25 mL of deionized water.
[0438] After 1 hour of sonication, transfer the sample to a thermostatic stirring platform and evenly add 17.5 μL of 1.05 g / mL chloroplatinic acid solution dropwise to create a mixture. Stir vigorously at room temperature for 2 hours to allow platinum ions to adsorb onto the surface of the etched FeSNC-1 material by immersion. The resulting mixture contains 1 mg / mL of etched FeNC-1 and 0.0009 mol / L of chloroplatinic acid.
[0439] After 12 hours of stirring, the mixture was filtered and washed, and the obtained solid material was vacuum freeze-dried.
[0440] 13. Place the solid material obtained after freeze drying in a porcelain boat. Under the protection of inert gas Ar / N2, heat it from room temperature at a rate of 5°C min -1The temperature was raised to 950°C and carbonized at this temperature for 1 hour, followed by natural cooling to room temperature. Finally, the heteronuclear diatomic metal nitrogen-carbon catalyst (FePtSNC-1) was obtained.
[0441] FIG60 is a scanning electron microscope (SEM) image of FePtSNC-1.
[0442] FIG61 is an X-ray diffraction (XRD) pattern of FePtSNC-1, FeSNC-1, and etched FeSNC-1.
[0443] Figure 62 shows the linear sweep polarization curves for oxygen reduction of the FePtSNC-1 bimetallic atom catalyst from Example 2, the FeSNC-1 obtained in Step 5, and the etched FeSNC-1 obtained in Step 9 under alkaline conditions of 0.1 M KOH saturated with O2 at a rotation speed of 1600 rpm. Figure 62 shows that the half-wave potential of FePtSNC-1 is 0.892 V, the half-wave potential of FeSNC-1 is 0.852 V, and the half-wave potential of etched FeSNC-1 is 0.835 V. A comparative analysis reveals that FePtSNC-1 has the highest half-wave potential, indicating the best electrocatalytic oxygen reduction activity. This demonstrates that single iron atoms and single platinum atoms have a synergistic effect in the electrocatalytic oxygen reduction reaction, and that the catalytic activity of the iron-platinum bimetallic atom is higher than that of the iron atom.
[0444] Example 16
[0445] The preparation method of platinum iron sulfur nitrogen carbon material comprises the following steps:
[0446] 1. Use 30 mL of formamide as a solvent to dissolve the iron salt, zinc salt, and sulfur source. Ultrasonicate for 30 minutes to ensure that the two salts are fully dissolved in the formamide. The resulting uniform dark red solution is the hydrothermal reaction mother liquor A. The molar ratio of the iron salt, zinc salt, and sulfur source is 1:4:2. The iron salt is anhydrous ferric chloride with a molar number of 0.005 mol / L. The zinc salt is anhydrous zinc chloride with a molar number of 0.2 mol / L. The sulfur source is thiourea with a molar number of 0.01 mol / L.
[0447] 2. Pour the above hydrothermal reaction mother solution A into a clean and dry closed reactor and carry out hydrothermal reaction at 160°C for 12 hours.
[0448] 3. After the hydrothermal reaction is completed, the sealed reactor is cooled naturally to room temperature, the reactor is opened, and the reaction liquid is filtered, and washed twice with deionized water and anhydrous ethanol to obtain a solid material B without formamide residue.
[0449] 4. Place solid material B in a 60°C forced air drying oven and dry for 2 hours until dry solid material C is obtained.
[0450] 5. Grind the obtained solid material C into fine powder, and place the fine powder in a porcelain boat. Start from room temperature under the protection of inert gas N2, and heat at 5℃min. -1 The temperature was raised at a heating rate of 1000 °C, and then carbonized at a constant temperature of 800 °C for 4 hours. After the constant temperature was completed, it was naturally cooled to room temperature to obtain iron single-atom nitrogen-carbon material (FeSNC-2).
[0451] 6. Measure equal volumes of ethanol and deionized water (12.5 mL each) and mix to form a solution. Dissolve 50 mg of the synthesized iron single-atom nitrogen carbon material (FeSNC-2) in the mixed solution D. Ultrasonicate for 30 minutes until uniformly dispersed. The resulting concentration of the iron single-atom nitrogen carbon material is 2 mg / mL.
[0452] 7. Place mixed solution D on a thermostatic stirring platform and stir for 10 minutes. During the stirring period, 0.126 mL of 10 mol / L peroxodisulfate solution was evenly added dropwise to obtain a uniformly mixed reaction solution E. The peroxodisulfate concentration in reaction solution E was 0.05 mol / L.
[0453] 8. Transfer the reaction solution E to a high-pressure reactor, place it in an oven at 150°C, and react for 5 hours.
[0454] 9. After the reaction is completed, the solid material obtained in the high-pressure reactor is filtered, washed three times with deionized water, and placed in a vacuum freeze drying box for overnight freeze drying to obtain the etched iron single-atom nitrogen-carbon material (etched FeSNC-2).
[0455] 10. Weigh 50 mg of the dry solid of the etched FeSNC-2 material and dissolve it in a mixed solution of equal volumes of 25 mL of anhydrous ethanol and 25 mL of deionized water.
[0456] After 1 hour of sonication, transfer the mixture to a thermostatic stirring platform and evenly add 17.5 μL of chloroplatinic acid solution (1.05 g / mL) dropwise to form a mixture. Stir vigorously at room temperature for 2 hours to allow platinum ions to adsorb onto the surface of the etched FeSNC-2 material by immersion. The resulting mixture contains 1 mg / mL of etched FeNC-1 and 0.0009 mol / L of chloroplatinic acid.
[0457] After 12 hours of stirring, the mixture was filtered and washed, and the obtained solid material was vacuum freeze-dried.
[0458] 13. Place the solid material obtained after freeze drying in a porcelain boat. Under the protection of inert gas Ar / N2, heat it from room temperature at a rate of 5°C min -1The temperature was raised to 950°C and carbonized at this temperature for 1 hour, followed by natural cooling to room temperature. Finally, the heteronuclear diatomic metal nitrogen-carbon catalyst (FePtSNC-2) was obtained.
[0459] Material characterization and performance testing are as follows:
[0460] FIG63 is a scanning electron microscope (SEM) image of the FePtSNC-2 diatomic material of Example 16.
[0461] Figure 64 shows X-ray diffraction (XRD) patterns of FePtNC-2 obtained in step 13 of Example 16, FeSNC-2 obtained in step 9, and etched FeSNC-2 obtained in step 2. Figure 64 shows only two carbon peaks, indicating the absence of metal nanoparticles in FeSNC-5, etched FeNC-2, and FePtNC-2.
[0462] Figure 65 shows the linear sweep polarization curves for oxygen reduction in the FePtSNC-2 bimetallic atomic material of Example 16, the FeSNC-2 obtained in Step 5, and the etched FeSNC-2 obtained in Step 9 under the alkaline conditions of 0.1M KOH saturated with O2 at a rotation speed of 1600 rpm. As shown in Figure 65, the half-wave potential of the FePtSNC-2 bimetallic atomic material is 0.897 V, while the half-wave potential of FeSNC-2 is 0.855 V, and the half-wave potential of the etched FeSNC-2 is 0.844 V. A comparative analysis reveals that FePtSNC-2 has the highest half-wave potential, indicating that it has the best electrocatalytic oxygen reduction activity. This demonstrates that in the electrocatalytic oxygen reduction reaction, iron and platinum atoms have a synergistic effect, and the catalytic activity of the iron-platinum bimetallic atomic material is higher than that of the iron atoms.
[0463] Example 17
[0464] The preparation method of platinum iron sulfur nitrogen carbon material comprises the following steps:
[0465] 1. Use 30 mL of formamide as a solvent to dissolve the iron salt, zinc salt, and sulfur source. Ultrasonicate for 30 minutes to ensure that the two salts are fully dissolved in the formamide. The resulting uniform dark red solution is the hydrothermal reaction mother liquor A. The molar ratio of the iron salt, zinc salt, and sulfur source is 1:20:2. The iron salt is anhydrous ferric chloride with a molar number of 0.005 mol / L. The zinc salt is anhydrous zinc chloride with a molar number of 0.2 mol / L. The sulfur source is thiourea with a molar number of 0.01 mol / L.
[0466] 2. Pour the above hydrothermal reaction mother solution A into a clean and dry closed reactor and carry out hydrothermal reaction at 220°C for 12 hours.
[0467] 3. After the hydrothermal reaction is completed, the sealed reactor is cooled naturally to room temperature, the reactor is opened, and the reaction liquid is filtered, and washed twice with deionized water and anhydrous ethanol to obtain a solid material B without formamide residue.
[0468] 4. Place solid material B in a 60°C forced air drying oven and dry for 2 hours until dry solid material C is obtained.
[0469] 5. Grind the obtained solid material C into fine powder, and place the fine powder in a porcelain boat. Start from room temperature under the protection of inert gas N2, and heat at 5℃min. -1 The temperature was raised at a heating rate of 1000 ° C., and then carbonized at a constant temperature of 1100 ° C. for 6 hours. After the constant temperature was completed, it was naturally cooled to room temperature to obtain iron single-atom nitrogen-carbon material (FeSNC-3).
[0470] 6. Measure equal volumes of ethanol and deionized water (12.5 mL each) and mix to form a solution. Dissolve 50 mg of the synthesized iron single-atom nitrogen carbon material (FeSNC-3) in the mixed solution D. Ultrasonicate for 30 minutes until uniformly dispersed. The resulting concentration of the iron single-atom nitrogen carbon material is 2 mg / mL.
[0471] 7. Place mixed solution D on a constant temperature stirring table and stir for 10 minutes. During the stirring period, 2.5 mL of 10 mol / L sodium persulfate solution was evenly added dropwise to obtain a uniformly mixed reaction solution E. The concentration of sodium persulfate in reaction solution E was 1.0 mol / L.
[0472] 8. Transfer the reaction solution E to a high-pressure reactor, place it in an oven at 200°C, and react for 8 hours.
[0473] 9. After the reaction is completed, the solid material obtained in the high-pressure reactor is filtered, washed three times with deionized water, and placed in a vacuum freeze drying box for overnight freeze drying to obtain the etched iron single-atom nitrogen-carbon material (etched FeSNC-3).
[0474] 10. Weigh 50 mg of the dry solid of the etched FeSNC-3 material and dissolve it in a mixed solution of equal volumes of 25 mL of anhydrous ethanol and 25 mL of deionized water.
[0475] After 1 hour of sonication, transfer the mixture to a thermostatic stirring platform and evenly add 17.5 μL of 1.05 g / mL chloroplatinic acid solution dropwise to create a mixture. Stir vigorously at room temperature for 2 hours to allow platinum ions to adsorb onto the surface of the etched FeSNC-3 material by impregnation. The resulting mixture contains 1 mg / mL of etched FeNC-1 and 0.0009 mol / L of chloroplatinic acid.
[0476] After 12 hours of stirring, the mixture was filtered and washed, and the obtained solid material was vacuum freeze-dried.
[0477] 13. Place the solid material obtained after freeze drying in a porcelain boat. Under the protection of inert gas Ar / N2, heat it from room temperature at a rate of 5°C min -1 The temperature was raised to 950°C and carbonized at this temperature for 1 hour, followed by natural cooling to room temperature. Finally, the heteronuclear diatomic metal nitrogen-carbon catalyst (FePtSNC-3) was obtained.
[0478] Material characterization and performance testing are as follows:
[0479] FIG66 is a scanning electron microscope (SEM) image of the FePtSNC-3 diatomic material of Example 17.
[0480] Figure 67 shows the X-ray diffraction (XRD) patterns of the FePtSNC-3 obtained in step 13 of Example 17, the FeSNC-3 obtained in step 9, and the etched FeSNC-3 obtained in step 6. Figure 67 shows only two carbon peaks, indicating that there are no metal nanoparticles in the FeSNC-3, etched FeSNC-3, and FePtSNC-3.
[0481] Figure 68 shows the linear sweep polarization curves for oxygen reduction in the FePtSNC-3 bimetallic atomic material of Example 17, the FeSNC-3 obtained in Step 5, and the etched FeSNC-3 obtained in Step 9 under the alkaline conditions of 0.1 M KOH saturated with O2 at a rotation speed of 1600 rpm. As shown in Figure 68, the half-wave potential of the FePtSNC-3 bimetallic atomic material is 0.861 V, while the half-wave potential of FeSNC-3 is 0.833 V, and the half-wave potential of the etched FeSNC-3 is 0.824 V. A comparative analysis reveals that FePtSNC-3 has the highest half-wave potential, indicating that it has the best electrocatalytic oxygen reduction activity. This suggests that in the electrocatalytic oxygen reduction reaction, iron and platinum atoms have a synergistic effect, and the catalytic activity of the iron-platinum bimetallic atomic material is higher than that of the iron atoms.
[0482] The specific conditions of Examples 18 to 20 are as follows:
[0483] Example 18
[0484] The preparation method of the cobalt-iron metal diatomic material comprises the following steps:
[0485] 1. Dissolve the cobalt salt and zinc salt in 30 mL of formamide as the solvent. Ultrasonicate for 30 minutes to ensure that both salts are fully dissolved in the formamide. The resulting clear pink solution is the hydrothermal reaction mother liquor A. The molar ratio of the cobalt salt to the zinc salt is 1:10. The cobalt salt is anhydrous cobalt chloride with a molarity of 0.01 mol / L. The zinc salt is anhydrous zinc chloride with a molarity of 0.1 mol / L.
[0486] 2. Pour the above hydrothermal reaction mother solution A into a clean and dry closed reactor and carry out hydrothermal reaction at 180°C for 12 hours.
[0487] 3. After the hydrothermal reaction is completed, the sealed reactor is cooled naturally to room temperature, the reactor is opened, and the reaction liquid is filtered, and washed twice with deionized water and anhydrous ethanol to obtain a solid material B without formamide residue.
[0488] 4. Place solid material B in a 60°C forced air drying oven and dry for 2 hours until dry solid material C is obtained.
[0489] 5. Grind the obtained solid material C into fine powder, and place the fine powder in a porcelain boat. Start from room temperature under the protection of inert gas N2, and heat at 5℃min. -1 The temperature was raised at a heating rate of , and then carbonized at a constant temperature of 900 ° C for 2 hours. After the constant temperature was completed, it was naturally cooled to room temperature to obtain cobalt single-atom nitrogen-carbon material (CoNC-1).
[0490] 6. Measure 12.5 mL of ethanol and deionized water of equal volume, mix them into a solution, dissolve 50 mg of the cobalt single-atom nitrogen-carbon material (CoNC-1) synthesized above in the mixed solution D, and sonicate for 30 minutes until it is evenly dispersed.
[0491] 7. Place mixed solution D on a thermostatic stirring platform and stir for 10 minutes. During the stirring period, 0.250 mL of 30% (10 mol / L) hydrogen peroxide solution was evenly added dropwise to obtain a uniformly mixed reaction solution E. The concentration of hydrogen peroxide in reaction solution E was 0.1 mol / L.
[0492] 8. Transfer the reaction solution E to a high-pressure reactor, place it in an oven at 180°C, and react for 6 hours.
[0493] 9. After the reaction is completed, the solid material obtained in the high-pressure reactor is filtered, washed three times with deionized water, and placed in a vacuum freeze drying oven for overnight freeze drying to obtain the etched cobalt single-atom nitrogen-carbon material (etched CoNC-1).
[0494] 10. Weigh 50 mg of the dry solid of the etched CoNC-1 material and dissolve it in a mixed solution of equal volumes of 12.5 mL of anhydrous ethanol and 12.5 mL of deionized water.
[0495] 11. After ultrasonication for 1 hour, transfer to a constant temperature stirring table and weigh 0.1086g (0.75mg) of ferric chloride powder. Fe / mL) was dissolved in a mixed solution of equal volumes of 12.5mL anhydrous ethanol and 12.5mL deionized water, and ultrasonicated until dissolved.
[0496] 12. The hydroalcoholic solution for etching CoNC-1 was vigorously stirred for 2 hours, and then ferric chloride solution was evenly added dropwise to adsorb iron ions on the surface of the etched CoNC-1 material by an immersion method.
[0497] 13. After 2 hours of stirring, the mixture was filtered and washed, and the obtained solid material was vacuum freeze-dried.
[0498] 14. Place the solid material obtained after freeze drying in a porcelain boat. Under the protection of inert gas Ar / N2, heat it from room temperature at a rate of 5°C min -1 The temperature was raised to 900°C and carbonized at this temperature for 1 hour, followed by natural cooling to room temperature. Finally, a heteronuclear diatomic metal nitrogen-carbon catalyst (CoFeNC-1) was obtained.
[0499] First, characterize the above materials:
[0500] FIG69 is a scanning electron microscope (SEM) image of CoFeNC-1.
[0501] As shown in FIG69 , scanning electron microscopy (SEM) observations show that the morphology of the CoFeNC diatomic particles is amorphous and has a partial porous structure.
[0502] FIG70 is a transmission electron microscopy (TEM) of CoFeNC-1.
[0503] As shown in Figure 70: Transmission electron microscopy (TEM) shows that CoFeNC-1 diatoms are in the form of thin sheets and exhibit a multi-layer stacked sheet structure.
[0504] Figure 71 is a high-angle annular dark field scanning transmission electron microscopy (HAADF-STEM) image of CoFeNC-1.
[0505] Figure 71 confirms the presence of CoFeNC-1 diatomic atoms. The bright spots in the image represent metal atoms, most of which appear as pairs of cobalt-iron atoms, proving that the material is a cobalt-iron metal diatomic material.
[0506] The distance between the two atoms was measured by direct measurement analysis method, and the distance statistics between the two atoms are shown in Table 1 below.
[0507] Table 1
[0508] Table 1 above proves that the distance between all diatoms is less than or equal to 0.5 nm, that is, the distance between a single cobalt atom and a single iron atom is less than or equal to 0.5 nanometers, specifically 0.15 to 0.5 nm.
[0509] As shown in Figure 71, there are 29 pairs of bimetallic atomic pairs at a scale of 2 nanometers, that is, 280 square nanometers, and the density of atomic pairs is higher, indicating that this CoFeNC diatomic material and preparation method have unique advantages, and the success rate of bimetallic atomic pairs prepared by this method is higher.
[0510] Figure 1 shows a high-angle annular dark field scanning transmission image of the Fe1Co1-CNF bimetallic atom catalyst from Reference 1. As shown in Figure 1, at a 2-nanometer scale, there are nine pairs of bimetallic atoms within 156.11 square nanometers, a relatively small number of pairs. Comparing Figure 71 with Figure 1 demonstrates that the present material exhibits a higher number of diatomic sites. This demonstrates that the success rate of diatomic formation on the conductive carbon-nitrogen substrate is higher than that of bimetallic atoms prepared by a one-pot hydrothermal method.
[0511] In Figure 71 and Figure 1, the area of the pictures was calculated by the inventor based on the scale in the pictures and the actual size of the pictures.
[0512] FIG72 is an X-ray diffraction (XRD) pattern of CoFeNC-1, CoNC-1, and etched CoNC-1.
[0513] The X-ray diffraction (XRD) in Figure 72 shows that the CoFeNC-1 diatomic material exhibits only two diffraction peaks at 25° and 43°, which are the (002) and (100) planes of graphitic carbon, respectively, and there are no diffraction peaks of metallic cobalt and metallic iron nanoparticles. Therefore, the synthesized series of materials does not contain metal particles, and both cobalt and iron are in a single-atom dispersed state.
[0514] The X-ray diffraction (XRD) patterns of CoNC-1 and etched CoNC-1 in Figure 72 have only two carbon peaks, indicating that there are no metallic cobalt nanoparticles in CoNC-1 and etched CoNC-1, and cobalt is in a single-atom dispersed state.
[0515] Second, performance test:
[0516] The performance of the CoFeNC-1 obtained above was tested using a CHI three-electrode system, and a linear sweep voltage (LSV) test was performed at an O2-saturated 0.1 M KOH and a rotation speed of 1600 rpm.
[0517] Figure 73 shows the linear sweep polarization curves for oxygen reduction of the CoFeNC-1 diatomic material, etched CoNC-1, FeNC, CoNC-1, and 20 wt% Pt / C at 1600 rpm. Figure 73 demonstrates that under alkaline conditions of 0.1 M KOH, the half-wave potential of the CoFeNC-1 diatomic material is 0.897 V, far superior to that of single-atom-level CoNC-1, etched CoNC-1, and FeNC (the half-wave potential of etched CoNC-1 is 0.793 V, the half-wave potential of CoNC-1 is 0.801 V, and the half-wave potential of FeNC is 0.864 V). Furthermore, the half-wave potential of the CoFeNC-1 diatomic material is 25 mV higher than that of 20 wt% Pt / C (0.872 V). Figure 73 demonstrates that the addition of a second metal species to form a diatomic catalyst can significantly enhance the oxygen reduction performance of the single-atom catalyst and accelerate the oxygen reduction reaction rate. In Figure 73, the 20 wt% Pt / C material is a commercially available Pt / C material with a Pt content of 20%. The etched CoNC-1 source is the product obtained in step 9, as prepared in Example 18. The CoNC-1 source is the product obtained in step 5, as prepared in Example 18. The FeNC preparation method is as follows: The preparation of FeNC is identical to that of CoNC-1 in steps 1-5 of Example 18, except that the cobalt salt is replaced with an iron salt, namely, ferric acetylacetonate, at a molar concentration of 0.005 mol / L. The resulting material is FeNC.
[0518] Figure 74 shows the four-electron transfer number and hydrogen peroxide yield of the CoFeNC-1 diatomic material and 20wt% Pt / C material. Figure 74 demonstrates that, calculated from experimental data, the electron transfer number of the CoFeNC-1 diatomic material is 3.99, very close to the four-electron transfer number. Furthermore, the hydrogen peroxide yield is less than 1% over a wide potential range, demonstrating the high four-electron selectivity of the CoFeNC-1 diatomic material. In Figure 74, a 20wt% Pt / C material is used as a control material for comparison with the CoFeNC-1 diatomic material, demonstrating the excellent electrocatalytic oxygen reduction performance of the CoFeNC-1 diatomic material.
[0519] CoFeNC-1 diatomic materials and 20wt% Pt / C materials were tested under oxygen-saturated 0.1M KOH alkaline conditions. Figure 75 shows the oxygen reduction polarization curves of the CoFeNC-1 diatomic materials and the 20wt% Pt / C materials before and after 40,000 seconds of operation. Figure 75 shows that after 40,000 seconds of cycling, the half-wave potential of the CoFeNC-1 diatomic material shifted negatively by only 3 mV (an average of 0.75 mV over approximately 10,000 seconds of cycling), indicating negligible activity decay. In contrast, the half-wave potential of the 20wt% Pt / C material exhibited significant decay.
[0520] Figure 2 shows the oxygen reduction polarization curves of the Fe1Co1-CNF bimetallic atom catalyst from Reference 1 before and after 10,000 seconds at a potential of 0.5 V. The cycling stability of the Fe1Co1-CNF bimetallic atom catalyst is poor. After 10,000 seconds of CV cycling, the half-wave potential of the Fe1Co1-CNF bimetallic atom catalyst shifted negatively by 2 mV (Note: The smaller the negative shift of the half-wave potential, the longer the cycling time and the higher the cycling stability).
[0521] Comparison of Figure 75 and Figure 2 proves that the cyclic stability of the CoFeNC-1 diatomic material of the present invention is higher than that of the Fe1Co1-CNF bimetallic atom catalyst in the reference.
[0522] Example 19
[0523] The preparation method of the cobalt-iron metal diatomic material comprises the following steps:
[0524] 1. Dissolve the cobalt salt and zinc salt in 30 mL of formamide as the solvent. Ultrasonicate for 30 minutes to ensure that both salts are fully dissolved in the formamide. The resulting clear pink solution is the hydrothermal reaction mother liquor A. The molar ratio of the cobalt salt to the zinc salt is 1:4. The cobalt salt is cobalt nitrate with a molarity of 0.025 mol / L. The zinc salt is anhydrous zinc chloride with a molarity of 0.1 mol / L.
[0525] 2. Pour the above hydrothermal reaction mother solution A into a clean and dry closed reactor and carry out hydrothermal reaction at 160°C for 12 hours.
[0526] 3. After the hydrothermal reaction is completed, the sealed reactor is cooled naturally to room temperature, the reactor is opened, and the reaction liquid is filtered, and washed twice with deionized water and anhydrous ethanol to obtain a solid material B without formamide residue.
[0527] 4. Place solid material B in a 60°C forced air drying oven and dry for 2 hours until dry solid material C is obtained.
[0528] 5. Grind the obtained solid material C into fine powder, and place the fine powder in a porcelain boat. Start from room temperature under the protection of inert gas N2, and heat at 5℃min. -1 The temperature was raised at a heating rate of , and then carbonized at a constant temperature of 800 ° C for 2 hours. After the constant temperature was completed, it was naturally cooled to room temperature to obtain cobalt single-atom nitrogen-carbon material (CoNC-2).
[0529] 6. Measure 12.5 mL of ethanol and deionized water of equal volume, mix them into a solution, dissolve 50 mg of the cobalt single-atom nitrogen-carbon material (CoNC-2) synthesized above in the mixed solution D, and ultrasonicate for 30 minutes to make it evenly dispersed.
[0530] 7. Place mixed solution D on a thermostatic stirring platform and stir for 10 minutes. During the stirring period, 0.126 mL of 10 mol / L peroxodisulfate solution was evenly added dropwise to obtain a uniformly mixed reaction solution E. The concentration of hydrogen peroxide in reaction solution E was 0.05 mol / L.
[0531] 8. Transfer the reaction solution E to a high-pressure reactor, place it in an oven at 150°C, and react for 6 hours.
[0532] 9. After the reaction is completed, the solid material obtained in the high-pressure reactor is filtered, washed three times with deionized water, and placed in a vacuum freeze drying oven for overnight freeze drying to obtain the etched cobalt single-atom nitrogen-carbon material (etched CoNC-2).
[0533] 10. Weigh 200 mg of the dry solid of the etched CoNC-2 material and dissolve it in a mixed solution of equal volumes of 12.5 mL of anhydrous ethanol and 12.5 mL of deionized water.
[0534] 11. After ultrasonication for 1 hour, transfer to a constant temperature stirring table and weigh an equal amount of ferric chloride powder 0.1839g (i.e. 1.27mg Fe / mL), dissolved in a mixed solution of equal volumes of 12.5mL anhydrous ethanol and 12.5mL deionized water, and sonicated until dissolved.
[0535] 12. The hydroalcoholic solution for etching CoNC-2 was vigorously stirred for 2 hours, and then ferric chloride solution was evenly added dropwise to adsorb iron ions on the surface of the etched CoNC-2 material by an immersion method.
[0536] 13. After 2 hours of stirring, the mixture was filtered and washed, and the obtained solid material was vacuum freeze-dried.
[0537] 14. Place the solid material obtained after freeze drying in a porcelain boat. Under the protection of inert gas Ar / N2, heat it from room temperature at a rate of 5°C min -1 The temperature was raised to 900°C and carbonized at this temperature for 1 hour, followed by natural cooling to room temperature. Finally, a heteronuclear diatomic metal nitrogen-carbon catalyst (CoFeNC-2) was obtained.
[0538] Material characterization and performance testing are as follows:
[0539] FIG76 is a scanning electron microscope (SEM) image of the CoFeNC-2 diatomic material of Example 19.
[0540] Figure 77 shows the X-ray diffraction (XRD) patterns of CoFeNC-2 obtained in step 14 of Example 19, CoNC-2 obtained in step 9, and etched CoNC-2 obtained in step 5. Figure 11 shows only two carbon peaks, indicating the absence of metal nanoparticles in CoNC-2, etched CoNC-2, and CoFeNC-2.
[0541] Figure 78 is a high-angle annular dark-field scanning transmission electron microscopy (HAADF-STEM) image of the CoFeNC-2 diatomic material of Example 19. As shown in Figure 78, at a scale of 2 nanometers, or 280 square nanometers, there are 44 pairs of bimetallic atomic pairs, or 0.16 pairs per square nanometer, indicating a higher density of atomic pairs. This demonstrates the unique advantages of this CoFeNC diatomic material and preparation method, and the higher success rate of bimetallic atomic pairs prepared by this method. The image area was calculated by the inventors based on the scale and actual size of the image.
[0542] Figure 79 shows the linear sweep polarization curves of oxygen reduction of the CoFeNC-2 diatomic material obtained in step 14 of Example 19, the CoNC-2 obtained in step 5, the etched CoNC-2 and FeNC-2 obtained in step 9, and the 20 wt% Pt / C material under the alkaline conditions of O2-saturated 0.1 M KOH at a rotation speed of 1600 rpm.
[0543] The preparation method for FeNC-2 is as follows: The preparation of FeNC-2 is identical to the preparation of CoNC-2 in steps 1-5 of Example 19, except that the cobalt salt is replaced with an iron salt, namely, ferric acetylacetonate, at a molar concentration of 0.005 mol / L. The resulting material is FeNC-2. The 20 wt% Pt / C material is a commercially available Pt / C material with a Pt content of 20%.
[0544] As shown in Figure 79, the half-wave potential of the CoFeNC-2 diatomic material is 0.885 V, while the half-wave potentials of CoNC-2 and FeNC-2 are 0.802 V and 0.846 V, respectively. A comparison reveals that the CoFeNC-2 diatomic material has the highest half-wave potential, which is 13 mV higher than the half-wave potential of 20 wt% Pt / C (0.872 V), indicating that the CoFeNC-2 diatomic material has the best electrocatalytic oxygen reduction performance.
[0545] Example 20
[0546] The preparation method of the cobalt-iron metal diatomic material comprises the following steps:
[0547] 1. Dissolve the cobalt salt and zinc salt in 30 mL of formamide as a solvent and sonicate for 30 minutes to ensure that the two salts are fully dissolved in the formamide. The resulting clear pink solution is the hydrothermal reaction mother liquor A. The molar ratio of the cobalt salt to the zinc salt is 1:20. The above-mentioned cobalt salt is anhydrous cobalt sulfate, and the zinc salt is anhydrous zinc chloride.
[0548] 2. Pour the above hydrothermal reaction mother solution A into a clean and dry closed reactor and carry out hydrothermal reaction at 220°C for 12 hours.
[0549] 3. After the hydrothermal reaction is completed, the sealed reactor is cooled naturally to room temperature, the reactor is opened, and the reaction liquid is filtered, and washed twice with deionized water and anhydrous ethanol to obtain a solid material B without formamide residue.
[0550] 4. Place solid material B in a 60°C forced air drying oven and dry for 2 hours until dry solid material C is obtained.
[0551] 5. Grind the obtained solid material C into fine powder, and place the fine powder in a porcelain boat. Start from room temperature under the protection of inert gas N2, and heat at 5℃min. -1 The temperature was raised at a heating rate of 100 ℃, and then carbonized at a constant temperature of 1100 ℃ for 2 hours. After the constant temperature was completed, it was naturally cooled to room temperature to obtain cobalt single-atom nitrogen-carbon material (CoNC-3).
[0552] 6. Measure 12.5 mL of ethanol and deionized water of equal volume, mix them into a solution, dissolve 100 mg of the cobalt single-atom nitrogen-carbon material (CoNC-3) synthesized above in the mixed solution D, and ultrasonicate for 30 minutes to make it evenly dispersed.
[0553] 7. Place mixed solution D on a constant temperature stirring table and stir for 10 minutes. During the stirring period, 2.5 mL of 10 mol / L sodium persulfate solution was evenly added dropwise to obtain a uniformly mixed reaction solution E. The concentration of sodium persulfate in reaction solution E was 1.0 mol / L.
[0554] 8. Transfer the reaction solution E to a high-pressure reactor, place it in an oven at 200°C, and react for 8 hours.
[0555] 9. After the reaction is completed, the solid material obtained in the high-pressure reactor is filtered, washed three times with deionized water, and placed in a vacuum freeze drying oven for overnight freeze drying to obtain the etched cobalt single-atom nitrogen-carbon material (etched CoNC-3).
[0556] 10. Weigh 100 mg of the dry solid of the etched CoNC-3 material and dissolve it in a mixed solution of equal volumes of 12.5 mL of anhydrous ethanol and 12.5 mL of deionized water.
[0557] 11. After ultrasonication for 1 hour, transfer to a constant temperature stirring table and weigh an equal amount of ferric chloride powder 0.0460g (i.e. 0.3175mg Fe / mL), dissolved in a mixed solution of equal volumes of 12.5mL anhydrous ethanol and 12.5mL deionized water, and sonicated until dissolved.
[0558] 12. The hydroalcoholic solution for etching CoNC-3 was vigorously stirred for 2 hours, and then ferric chloride solution was evenly added dropwise to adsorb iron ions on the surface of the etched CoNC-3 material by an immersion method.
[0559] 13. After 2 hours of stirring, the mixture was filtered and washed, and the obtained solid material was vacuum freeze-dried.
[0560] 14. Place the solid material obtained after freeze drying in a porcelain boat. Under the protection of inert gas Ar / N2, heat it from room temperature at a rate of 5°C min -1 The temperature was raised to 900°C and carbonized at this temperature for 1 hour, followed by natural cooling to room temperature. Finally, a heteronuclear diatomic metal nitrogen-carbon catalyst (CoFeNC-3) was obtained.
[0561] Figure 80 is a scanning electron microscope (SEM) image of CoFeNC-3 of Example 20.
[0562] Figure 81 is the X-ray diffraction (XRD) pattern of CoFeNC-3 obtained in step 14 of Example 20, CoNC-3 obtained in step 5, and etched CoNC-3 obtained in step 9.
[0563] Figure 82 shows the linear sweep polarization curves of oxygen reduction of the CoFeNC-3 diatomic material of Example 20, the CoNC-3 obtained in step 5, and the etched CoNC-3 obtained in step 9 under the alkaline conditions of 0.1M KOH saturated with O2 and a rotation speed of 1600 rpm. Figure 82 shows that the half-wave potential of CoFeNC-3 is 0.819V, the half-wave potential of CoNC-3 is 0.788V, and the half-wave potential of etched CoNC-3 is 0.784V. Comparative analysis shows that the half-wave potential of CoFeNC-3 is the largest, indicating that it has the best electrocatalytic oxygen reduction activity. This shows that in the electrocatalytic oxygen reduction reaction, cobalt single atoms and iron single atoms have a synergistic effect, and the catalytic activity of cobalt-iron diatoms is higher than that of cobalt single atoms.
Claims
1. A metal diatomic material, characterized in that: The metal diatomic material comprises: a conductive substrate and a first metal single atom and a second metal single atom supported on the conductive substrate, wherein the distance between the first metal single atom and the second metal single atom is less than or equal to 0.5 nanometers.
2. The metal diatomic material according to claim 1, characterized in that: On a conductive substrate, the density of diatomic pairs is no less than 0.06 pairs / square nanometer.
3. The metal diatomic material according to claim 1, characterized in that: The first metal in the first metal single atom is selected from: one or more of cobalt, iron, zinc, nickel, manganese, platinum, ruthenium, iridium, gold, and silver; The second metal in the second metal single atom is selected from: one or more of cobalt, iron, zinc, nickel, manganese, platinum, ruthenium, iridium, gold, and silver.
4. The metal diatomic material according to claim 1, characterized in that: The conductive substrate is selected from: nitrogen-carbon material or sulfur-nitrogen-carbon material.
5. A method for preparing the metal diatomic material according to claims 1 to 4, characterized in that: The preparation method comprises the following steps: Etching: placing the conductive substrate loaded with the first metal single atom in a peroxide aqueous solution for etching to obtain an etched first metal single atom material; Preparation of metal diatomic material: The first metal single atom material obtained after etching is loaded with the second metal single atom to obtain the metal diatomic material.
6. The method for preparing a metal diatomic material according to claim 5, characterized in that: The specific method of etching is as follows: Step A, mixing alcohol and water into a solution, placing a conductive substrate loaded with a first metal single atom in the mixed solution, and performing ultrasound treatment; Step B, stirring the mixed solution obtained in step A and uniformly adding a peroxide aqueous solution to obtain a uniformly mixed reaction solution; Step C, transferring the reaction solution obtained in step B to a high-pressure reactor, placing it in an oven, setting the reaction temperature to 100-200° C., and reacting for 3-10 hours; after the reaction is completed, filtering and washing the solid material obtained in the high-pressure reactor, and vacuum freeze-drying it to obtain the first metal single atom material after etching.
7. The method for preparing a metal diatomic material according to claim 5, characterized in that: The specific method for preparing the metal diatomic material is as follows: The etched first metal single atom material is dissolved in a mixed solution of alcohol and water, and ultrasonicated until a uniformly dispersed turbid liquid is obtained, and an appropriate amount of the second metal precursor is weighed and added to the turbid liquid, mixed evenly, and the solid-liquid separation is performed, and the obtained solid material is vacuum freeze-dried; The solid material obtained after freeze-drying is placed in a porcelain boat, carbonized under the protection of an inert gas, and then naturally cooled to room temperature to finally obtain a metal diatomic material.
8. The method for preparing a metal diatomic material according to claim 5, characterized in that: The peroxide in the aqueous peroxide solution is selected from one or more of hydrogen peroxide, peroxodisulfate, persulfate, peracetate, peroxyphosphate or peroxycarbonate.
9. The method for preparing a metal diatomic material according to claim 5, characterized in that: When the conductive substrate is a nitrogen-carbon substrate, the preparation method of the conductive substrate loaded with the first metal single atom is as follows: (a) dissolving a first metal salt and a zinc salt in formamide as a solvent, and ultrasonicating to ensure that the two salts are fully dissolved in the formamide to obtain a hydrothermal reaction mother solution A, wherein the molar ratio of the first metal salt to the zinc salt is 1:4 to 1:20; (b) pouring the hydrothermal reaction mother solution A into a sealed reactor, carrying out a hydrothermal reaction at 160° C. to 220° C. and under autogenous pressure, and after completion, naturally cooling the sealed reactor to room temperature, separating the solid from the liquid, washing the solid, obtaining a solid material B without formamide residue, and drying the solid material B to obtain a solid material C; (c) Grinding the solid material C and placing it in a porcelain boat, heating it under the protection of an inert gas, and then maintaining the temperature at 800° C.-1100° C. for 2-6 hours. After the reaction is completed, naturally cooling it to room temperature to obtain the conductive substrate loaded with the first metal single atom.
10. The method for preparing a metal diatomic material according to claim 5, characterized in that: When the conductive substrate is a sulfur-nitrogen-carbon substrate, the preparation method of the conductive substrate loaded with the first metal single atom is as follows: (a) dissolving a first metal salt, a zinc salt and a sulfur source in formamide as a solvent, and ultrasonicating to ensure that the two salts are fully dissolved in formamide to obtain a hydrothermal reaction mother solution A, wherein the molar ratio of the first metal salt to the zinc salt is 1:4 to 1:20, and the molar amount of the sulfur source is consistent with that of the first metal salt; (b) pouring the hydrothermal reaction mother solution A into a sealed reactor, carrying out a hydrothermal reaction at 160° C. to 220° C. and under autogenous pressure, and after completion, naturally cooling the sealed reactor to room temperature, separating the solid from the liquid, washing the solid, obtaining a solid material B without formamide residue, and drying the solid material B to obtain a solid material C; (c) Grind the solid material C and place it in a porcelain boat, heat it under the protection of inert gas, and then The reaction mixture is kept at a constant temperature of 600° C. to 1100° C. for 1 to 4 hours, and then naturally cooled to room temperature after the reaction is completed to obtain the conductive substrate loaded with the first metal single atom.
11. The method for preparing a metal diatomic material according to claim 9, characterized in that: The first metal in the first metal salt is selected from one or more of cobalt, iron, zinc, nickel, manganese, platinum, ruthenium, iridium, gold and silver.
12. The method for preparing a metal diatomic material according to claim 7, characterized in that: The precursor of the second metal is a second metal salt, and the second metal is selected from: one or more of cobalt, iron, zinc, nickel, manganese, platinum, ruthenium, iridium, gold, and silver.
13. Use of the metal diatomic material according to any one of claims 1 to 4 for catalyzing oxygen reduction reactions.
Citation Information
Patent Citations
Preparation method of hierarchical porous three-dimensional structure graphene electrocatalyst
CN111250073A
Phosphorus and nitrogen co-doped iron monatomic carbon material as well as preparation method and application thereof
CN112938966A
Solvent circulation preparation method and application of metal atomic-scale dispersed nitrogen-carbon material
CN113373474A
Preparation method and application of bimetal monatomic loaded BCN aerogel catalyst
CN115155647A
Ni-Zn diatom electro-catalysis oxygen reduction reaction catalyst and preparation method and application thereof
CN115632134A
Cited By
Ordered macroporous carbon-supported bimetallic monatomic catalyst, and preparation method and application thereof
CN119852426A