Optical device
The optical device employs a superlattice structure in the n-type layer to overcome lattice relaxation issues, enabling thicker nitride semiconductor layers and reducing resistance, thus improving the performance of ultraviolet light-emitting diodes by lowering the laser oscillation threshold current density.
Patent Information
- Application Number
- PCT/JP2023/015889
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-21
- Publication Date
- 2024-10-24
AI Technical Summary
Conventional nitride semiconductor light-emitting devices face challenges in forming thicker n-type layers due to lattice relaxation, leading to increased element resistance and higher laser oscillation threshold current density, especially in ultraviolet light-emitting diodes (UV LEDs) and laser diodes (LDs).
The optical device incorporates an n-type layer with a superlattice structure made of AlxGa1-xN (0.5
This approach enables the creation of thicker n-type layers, lowering the laser oscillation threshold current density and preventing heat-induced device performance deterioration, making it suitable for ultraviolet LDs with emission wavelengths of 300 nm or less.
Smart Images

Figure JP2023015889_24102024_PF_FP_ABST
Abstract
Description
Optical Devices
[0001] The present invention relates to an optical device that emits light in the ultraviolet region.
[0002] Nitride semiconductors, such as AlN, GaN, InN, and their alloys, are characterized by their large bandgap energy and direct transition type semiconductor materials. For this reason, these nitride semiconductors have attracted attention as materials for semiconductor light-emitting devices, such as light-emitting diodes (LEDs) and laser diodes (LDs), which can emit light over a wide wavelength range from ultraviolet to red.
[0003] In recent years, various research institutes have been vigorously researching and developing semiconductor light-emitting devices that emit light in the deep ultraviolet region (wavelength: 200 nm to 350 nm), which are expected to be applied in a wide range of fields such as virus inactivation, sterilization, water purification, microfabrication, various medical fields, and high-speed decomposition treatment of pollutants by shortening the emission wavelength of light-emitting devices that use nitride semiconductors.
[0004] For example, a technology for oscillating a current injection type LD in the ultraviolet region using a nitride semiconductor has been disclosed (Non-Patent Document 1). In this technology, a 350 nm thick Si-doped AlN substrate is formed as an n-type layer. 0.7 Ga 0.3 In this technique, however, it is difficult to thicken the n-type layer from the viewpoint of lattice relaxation, which poses the problem of increased device resistance. In LDs that emit light at ultraviolet wavelengths, it is preferable to thicken the n-type layer to reduce device resistance and achieve oscillation characteristics with a lower threshold current density in order to prevent degradation of device performance due to heat.
[0005] Z. Zhang et al., "A 271.8 nm deep-ultraviolet laser diode for room temperature operation", Applied Physics Express, vol. 12, 124003, 2019.
[0006] As described above, the conventional technology has a problem in that the device resistance increases because it is difficult to make the n-type layer using AlGaN thicker.
[0007] The present invention has been made to solve the above problems, and has as its object to make it possible to form a thicker n-type layer in an optical device using AlGaN.
[0008] The optical device according to the present invention comprises an n-type layer having a superlattice structure made of a nitride semiconductor formed on a substrate, a p-type layer made of a nitride semiconductor formed on the substrate, and an active layer made of a nitride semiconductor formed between the n-type layer and the p-type layer, wherein the n-type layer is Al x Ga 1-x N (0.5<x≦0.87) and Al y Ga 1-y N (0.91<y≦1) units are repeated.
[0009] As described above, according to the present invention, the n-type layer is x Ga 1-x N (0.5<x≦0.87) and Al y Ga 1-y N (0.91<y≦1) units are repeated, so that the n-type layer of an optical device using AlGaN can be formed thicker.
[0010] Fig. 1 is a cross-sectional view showing the configuration of an optical device according to an embodiment of the present invention. Fig. 2 is a cross-sectional view showing a partial configuration of an optical device according to an embodiment of the present invention. Fig. 3 is a photograph showing a partial configuration of an optical device according to an embodiment of the present invention. Fig. 4 is a cross-sectional view showing the configuration of another optical device according to an embodiment of the present invention.
[0011] An optical device according to an embodiment of the present invention will be described below with reference to FIGS. 1 and 2. This optical device includes an n-type layer 102, a p-type layer 104, and an active layer 103 formed on a substrate 101. This optical device can be, for example, an LED (light-emitting diode). Furthermore, by combining it with a resonator, it can be made into an LD (laser diode).
[0012] The substrate 101 may be, for example, a SiC substrate or an AlN substrate, or may be a sapphire substrate, a GaN substrate, an MgAlO substrate, a SiO substrate, an MgO substrate, a ZnO substrate, an NdGaO substrate, an ScAlMgO substrate, a ZnS substrate, a GaAs substrate, or a Si substrate.
[0013] The n-type layer 102 has a superlattice structure made of nitride semiconductors. As shown in FIG. x Ga 1-x The first layer 121 is made of N (0.5<x≦0.87) and the second layer 122 is made of Al y Ga 1-y The n-type layer 102 has a repeating structure (periodic structure) with a first layer 121 and a second layer 122 of N (0.91<y≦1) as a unit. The n-type layer 102 may have a periodic structure with a first layer 121 and a second layer 122 as a unit, for example, so that the first layer 121 is formed in contact with the active layer 103. The p-type layer 104 is formed on the substrate 101 and is made of a nitride semiconductor. The p-type layer 104 may be made of AlGaN with a predetermined composition ratio. The active layer 103 is made of a nitride semiconductor and is formed between the n-type layer 102 and the p-type layer 104. The active layer 103 may be made of AlGaN with a predetermined composition ratio. The n-type layer 102, the p-type layer 104, and the active layer 103 are stacked on the substrate 101.
[0014] In the periodic structure of the first layer 121 and the second layer 122, Al y Ga 1-y N (0.91<y≦1) and Al x Ga 1-x Since the band gaps of N (0.5<x≦0.87) are different in magnitude, a band offset occurs in the conduction band.
[0015] The second layer 122 [Al y Ga 1-y N (0.91<y≦1)], the ionization energy of the donor is sufficiently smaller than the energy of the band offset, so the donor in the second layer 122 doped with the donor impurity is activated and x Ga 1-xN (0.5<x≦0.87)] and the second layer 122 [Al y Ga 1-y N (0.91<y≦1)], resulting in a high electron concentration.
[0016] In the n-type layer 102 of the optical device according to the embodiment, the Al y Ga 1-y It is preferable that N satisfies 0.91<y≦1. If y≦0.91, lattice relaxation occurs. Therefore, when the optical device according to the embodiment is used as an LD, there is a risk of an increase in the laser oscillation threshold current density. A more preferable Al composition is 0.93≦y≦1, and an even more preferable Al composition is 0.97<y≦1.
[0017] Al of the first layer 121 x Ga 1-x The Al composition of N is preferably 0.5<x≦0.87. When x≦0.5, lattice relaxation occurs. Therefore, when this optical device is used as an LD, there is a risk of an increase in the laser oscillation threshold current density. Furthermore, when x>0.87 is used, Al y Ga 1-y N and Al x Ga 1-x There is a risk that the donors will not be sufficiently activated, resulting in a decrease in the electron concentration, due to a small band offset with respect to N. A more preferable Al composition is 0.54<x<0.82, and an even more preferable Al composition is 0.58<x≦0.74.
[0018] In the n-type layer 102 having an n-type AlN-based superlattice structure, the thickness of each first layer 121 is preferably 0.8 to 17 nm, and the thickness of each second layer 122 is preferably 0.3 to 8 nm. If the thickness of the first layer 121 is less than 0.8 nm and the thickness of the second layer 122 is less than 0.3 nm, there is a risk of a decrease in the electron concentration in the n-type layer 102. Furthermore, if the thickness of the first layer 121 exceeds 17 nm and the thickness of the second layer 122 exceeds 8 nm, there is a risk of an increase in the device resistance.
[0019] In addition, optical devices having an n-type layer 102 with an n-type AlN-based superlattice structure are generally formed by epitaxial growth on a buffer layer made of AlN. Therefore, even if the n-type layer 102 is thickened to 400 nm or more, lattice relaxation does not occur and pseudomorphic (pseudomorphic) growth is possible. In Non-Patent Document 1, a 350 nm Si-doped Al 0.7 Ga 0.3 Although an N mixed crystal is used, in this case, it is difficult to make the n-type layer thick from the viewpoint of lattice relaxation.
[0020] According to the embodiment, the n-type layer 102 can be made thicker, which makes it possible to reduce the device resistance. Therefore, for example, when this optical device is used as an LD, the oscillation threshold current density can be reduced. y Ga 1-y N(0.91<y≦1) / Al x Ga 1-x The total thickness of the n-type layer 102 having a periodic structure of N (0.5<x≦0.87) is preferably 400 to 3100 nm. If the thickness (total thickness) of the n-type layer 102 is less than 400 nm, the device resistance may increase. If the thickness of the n-type layer 102 exceeds 3100 nm, lattice relaxation may occur. The thickness of the n-type layer 102 is more preferably 520 to 2600 nm, and even more preferably 640 to 1620 nm.
[0021] The n-type layer 102, which is an n-type AlN-based superlattice, is doped with a donor impurity. Although Si is generally used as the donor impurity, it is not limited thereto and may be any of the donor impurities Ge, Sn, C, O, etc. The concentration of the donor impurity is 2×10 16 cm -3 2 x 10 or more 20 cm -3 The donor impurity concentration is preferably 2×10 or less. 16 cm -3 If the concentration of the donor impurity is less than 2×10, the electron concentration may decrease, and the efficiency of electron injection into the active layer 103 by the n-type layer 102 may decrease. 20 cm -3If the concentration exceeds this value, the electron concentration will be significantly reduced due to a self-compensation effect, which may result in high resistance of the n-type layer 102. The concentration of donor impurities in the n-type layer 102 can be confirmed by secondary ion mass spectrometry (SIMS).
[0022] Furthermore, it is preferable that the n-type layer 102 has a single crystal structure throughout the first layer 121 and the second layer 122, which are made into a repeating structure, but polycrystalline or amorphous regions may be unevenly distributed in some areas to the extent that the various properties of a crystalline nitride semiconductor are not lost.
[0023] The cross-sectional structure of the n-type layer 102 can be clearly observed using a transmission electron microscope (TEM). TEM allows for the observation of the sample's microstructure by irradiating a thinly processed sample with an electron beam and imaging the transmitted or diffracted electron beam. High-magnification observations allow for the observation of the arrangement of atoms in the crystal (lattice fringes) (lattice image). Polycrystals and crystal defects can also be observed. Furthermore, electron diffraction patterns can be used to identify materials and analyze their crystalline state. The elemental distribution can be determined by elemental analysis using energy-dispersive X-ray spectroscopy (EDS). EDS measurements are performed using an EDS measurement device attached to the STEM device. SIMS is another elemental analysis method.
[0024] Lattice relaxation of nitride semiconductors can be confirmed by reciprocal space mapping (RSM) using X-ray diffraction (XRD). By analyzing reciprocal lattice mapping data in the vicinity of a diffraction peak obtained using an asymmetric plane as a diffraction plane, it is possible to confirm whether lattice relaxation has occurred relative to the underlayer and to obtain the Al composition of AlGaN.
[0025] Next, the p-type layer 104 will be described. The p-type layer 104 is preferably a multi-layer structure of compositionally graded AlGaN layers. In particular, it is preferable to insert a compositionally graded AlGaN layer with a thickness of 50 nm or less on the side closer to the active layer 103 to form a multi-layer structure. By forming the p-type layer 104 closer to the active layer 103 as a compositionally graded AlGaN layer with a thickness of 50 nm or less, hole injection efficiency can be improved. As a result, for example, when this optical device is used as an LD, the oscillation threshold current density of the LD can be reduced.
[0026] Each layer constituting the optical device according to the embodiment can be formed by epitaxial growth. The epitaxial growth can be, for example, MOVPE (metal organic vapor phase epitaxy). The epitaxial growth can be, for example, HVPE (hydride vapor phase epitaxy), MBE (molecular beam epitaxy), sputtering, or the like, without being limited to MOVPE.
[0027] For example, after preparing a growth substrate, the growth substrate is introduced into an epitaxial growth apparatus and layered by epitaxial growth. When an MOVPE apparatus is used as the epitaxial growth apparatus, trimethylaluminum (TMAl) can be used as the source gas for Al. Trimethylgallium (TMGa) can be used as the source gas for Ga. NH can be used as the source gas for N. Silane (SiH) can be used as the source gas for Si, which is an impurity contributing to n-type conductivity. Examples of carrier gases that can be used include H gas, N gas, and a mixture of H gas and N gas. The source gases are not particularly limited, and examples include triethylgallium (TEGa) as the source gas for Ga and hydrazine derivatives as the source gas for N. The n-type impurity refers to a donor impurity, such as Si.
[0028] Incidentally, each layer of the optical device according to the embodiment can be epitaxially grown on the (0001) plane, but can also be epitaxially grown on other crystal planes, such as the (000-1) plane or the (1-102) plane.
[0029] The electron concentration of the n-type layer 102 can be measured by the Hall effect measurement method. Details will be described later. 18 cm -3 When the activation energy of the electron concentration is 30 meV or less, good light emission characteristics are likely to be obtained when the optical device according to the embodiment is used as an ultraviolet light emitting device. The activation energy is determined by measuring the Hall effect of the layer to be measured at different temperatures and plotting the logarithm of the carrier concentration against the reciprocal of the temperature (Arrhenius plot), and then determining the slope of the plot.
[0030] The n-type layer 102 is 1×10 18 cm -3 Since a high electron concentration as high as or higher can be obtained and pseudomorphic growth occurs even when the thickness is increased, the film can be suitably used in ultraviolet LDs with an emission wavelength of 300 nm or less.
[0031] EXAMPLES The following will be described in more detail using examples. First, an n-type layer 102 having an n-type AlN-based superlattice structure that was actually fabricated will be described.
[0032] 3, the n-type layer 102 [AlN (1.3 nm) / AlN (1.3 nm)] is formed with x=0.74, y=1, and the thickness of each first layer 121 is 4.2 nm, and the thickness of each second layer 122 is 1.3 nm. 0.74 Ga 0.26 The analysis was performed using a H-9000UHR (Hitachi) microscope at an accelerating voltage of 300 kV.
[0033] Furthermore, an AlN buffer layer was grown by MOVPE on a substrate made of semi-insulating 4H—SiC (0001), and an AlN (1.3 nm) / Al 0.74 Ga 0.26 A periodic structure of N (4.2 nm) was grown 100 times to form the n-type layer 102. The total thickness of the n-type layer 102 was 550 nm.
[0034] From the X-ray reciprocal lattice mapping in the asymmetric plane (-1-124), it was found that the n-type layer 102 [AlN (1.3 nm) / Al 0.74 Ga 0.26 It was confirmed that the periodic structure of AlN (4.2 nm) in the first layer 102 was pseudomorphically grown. x Ga 1-x The Al composition of N was confirmed to be 0.74. The Si doping amount was 1.5×10 19 cm -3 The SIMS measurement was performed using ADEPT1010 (manufactured by ULVAC PHI).
[0035] The average Al composition of the n-type layer 102 forming the n-type superlattice is (1×L AlN +0.74 x L AlGaN ) / (L AlN +L AlGaN ) is calculated to be approximately 0.8. AlGaN is Al x Ga 1-x The thickness of the first layer made of N, L AlN is the thickness of the second layer 122 made of AlN. 0.74 Ga 0.26 The interface with the N layer is abrupt, and the AlN (1.3 nm) / Al 0.74 Ga 0.26 It was confirmed that a periodic structure of N (4.2 nm) was formed.
[0036] Next, the above-mentioned Si-doped AlN (1.3 nm) / Al 0.74 Ga 0.26 The electron concentration of the n-type layer 102 having a periodic structure (100 periods) of N (4.2 nm) will be described. The electron concentration of the fabricated n-type layer 102 was measured using the Van der Pauw method and found to be 1.2×10 19 cm -3 It was.
[0037] The Hall effect measurement device used was a "Resi Test 8300" manufactured by Toyo Corporation, and the measurement conditions were room temperature (approximately 25°C), approximately 0.25 [T], and approximately 10 -4~10 -9 [A] (AC magnetic field Hall measurement). The sample shape was approximately 5 mm x 5 mm in plan view.
[0038] In addition, Si-doped AlN (1.3 nm) / Al 0.74 Ga 0.26 For the n-type layer 102 with a periodic structure (100 periods) of N (4.2 nm), the temperature was changed from room temperature to 500 K to measure the temperature dependence of the electron concentration. According to the formula n = n0exp(-Ea / kT), the horizontal axis is the reciprocal of the temperature, and the vertical axis is the logarithm of the electron concentration. The slope (activation energy = Ea) was calculated to be 8 meV. Here, "T" is temperature, "n" is the electron concentration at temperature T, "n0" is a constant, "Ea" is the activation energy, and "k" is the Boltzmann constant.
[0039] Next, the configuration of this optical device as an ultraviolet LD will be described with reference to Fig. 4. This ultraviolet LD includes a substrate 201 made of AlN and having a (0001) plane as its main surface, a buffer layer 202 made of AlN formed on the substrate 201, and an n-type layer 203, an active layer 205, and a p-type layer 207 formed on the buffer layer 202.
[0040] The active layer 205 is sandwiched between a first guide layer 204 and a second guide layer 206, and is formed between an n-type layer 203 and a p-type layer 207. In addition, a compositionally graded layer 208 and a contact layer 209 are formed on the p-type layer 207.
[0041] Furthermore, a portion of the n-type layer 203 is thinned and exposed in a plan view, and an n-electrode 210 is formed in the exposed region. For example, first, the above-mentioned layers are formed by epitaxial growth on the substrate 201. Next, a mask pattern is formed on the contact layer 209 using a known lithography technique, and this mask pattern is used as a mask to etch away part of the n-type layer 203. This allows a portion of the n-type layer 203 to be exposed. Furthermore, a p-electrode 211 is formed on the contact layer 209.
[0042] The n-type layer 203 is Al y Ga 1-y N(0.91<y≦1) / Al xGa 1-x N (0.5<x≦0.87) periodic structure, and Si is 1.5×10 19 cm -3 It is doped to be n-type.
[0043] The first guide layer 204 is made of undoped Al 0.52 Ga 0.48 The active layer 205 is made of AlGaN and has a multi-quantum well structure with two well layers. The second guide layer 206 is made of undoped Al 0.52 Ga 0.48 It is made of N and has a thickness of 50 nm.
[0044] The p-type layer 207 is an undoped Al-doped layer with a composition gradient in which the Ga composition ratio gradually increases with increasing distance from the active layer 205. x Ga 1-x As will be described later, the p-type layer 207 is composed of a single undoped compositionally graded AlN (x: 1 → 0.7). x Ga 1-x The p-type layer 207 can be made of a plurality of undoped composition-graded AlN (x: 1 → 0.7). x Ga 1-x In addition, a nitride semiconductor having a polar or semipolar crystal growth plane can be made p-type even when undoped due to polarization charge at the heterojunction plane.
[0045] The composition gradient layer 208 is a Mg-doped composition gradient Al layer in which the Ga composition ratio gradually increases with increasing distance from the p-type layer 207. x Ga 1-x The contact layer 209 is made of GaN doped with Mg. x Ga 1-x The compositionally graded layer 208 made of N (x: 0.7→0) is made of GaN at the interface with the contact layer 209. The n-electrode 210 is made of a V-based electrode material, and the p-electrode 211 is made of Ni / Pt / Au.
[0046] Here, the following samples 1, 2, 3, 4, 5, 6, 7, and 8 were fabricated. From the X-ray reciprocal lattice mapping in the asymmetric plane (-1-124), it was found that the Si-doped AlN constituting the n-type layer 203 was different from the AlN buffer layer 202. y Ga 1-y N(0.91<y≦1) / Al x Ga 1-x It was confirmed that the periodic structure of N (0.5<x≦0.87) was pseudomorphically grown, and the Al composition of AlGaN in each sample was determined.
[0047] In sample 1, the n-type layer 203 is AlN (1.3 nm) / Al doped with Si. 0.64 Ga 0.36 The n-type layer 203 has a periodic structure of 4.0 nm, and the number of periods is 288. In this case, the total thickness of the n-type layer 203 is 1526.4 nm, and the average Al composition is about 73%. 0.4 Ga 0.6 N (3 nm) / Al 0.52 Ga 0.48 The p-type layer 207 is a 20 nm thick undoped AlN (6 nm) multi-quantum well with two quantum well layers. x Ga 1-x N (x: 1 → 0.7) layer and an undoped compositionally graded Al layer with a thickness of 300 nm formed thereon. x Ga 1-x A two-layer structure was formed with an N (x: 1 → 0.7) layer.
[0048] In sample 2, the n-type layer 203 is AlN (1.3 nm) / Al doped with Si. 0.6 Ga 0.4 The periodic structure is N (3.0 nm), and the number of periods is 200. In this case, the total thickness of the n-type layer 203 is 860 nm. The active layer 205 is made of Al 0.4 Ga 0.6 N (2 nm) / Al 0.52 Ga 0.48 The p-type layer 207 is a 20 nm thick undoped AlN (6 nm) multi-quantum well with two quantum well layers. x Ga 1-xN (x: 1 → 0.7) layer and an undoped compositionally graded Al layer with a thickness of 300 nm formed thereon. x Ga 1-x A two-layer structure was formed with an N (x: 1 → 0.7) layer.
[0049] In sample 3, the n-type layer 203 is AlN (0.8 nm) / Al doped with Si. 0.67 Ga 0.33 The periodic structure is N (3.0 nm), and the number of periods is 300. In this case, the total thickness of the n-type layer 203 is 1140 nm. The active layer 205 is made of Al 0.4 Ga 0.6 N (2 nm) / Al 0.52 Ga 0.48 The p-type layer 207 is a 20 nm thick undoped AlN (6 nm) multi-quantum well with two quantum well layers. x Ga 1-x N (x: 1 → 0.7) layer and an undoped compositionally graded Al layer with a thickness of 20 nm formed thereon. x Ga 1-x N (x: 1 → 0.7) layer and an undoped compositionally graded Al layer with a thickness of 280 nm formed thereon. x Ga 1-x A three-layer structure was formed with a N (x: 1 → 0.7) layer.
[0050] In sample 4, the n-type layer 203 is AlN (1.3 nm) / Al doped with Si. 0.74 Ga 0.26 The periodic structure is 288. In this case, the total thickness of the n-type layer 203 is 1584 nm. 0.4 Ga 0.6 N (3 nm) / Al 0.52 Ga 0.48 The p-type layer 207 is a 50 nm thick undoped AlN (6 nm) multi-quantum well with two quantum well layers. x Ga 1-x N (x: 1 → 0.7) layer and an undoped compositionally graded Al layer with a thickness of 270 nm formed thereon. x Ga 1-x A two-layer structure was formed with an N (x: 1 → 0.7) layer.
[0051] Sample 5 has an n-type layer 203 of AlN (1.3 nm) / Al doped with Si. 0.72 Ga 0.28 The periodic structure is 288. In this case, the total thickness of the n-type layer 203 is 1584 nm. 0.4 Ga 0.6 N (3 nm) / Al 0.52 Ga 0.48 The p-type layer 207 is a 20 nm thick undoped AlN (6 nm) multi-quantum well with two quantum well layers. x Ga 1-x N (x: 1 → 0.7) layer and an undoped compositionally graded Al layer with a thickness of 20 nm formed thereon. x Ga 1-x N (x: 1 → 0.7) layer and an undoped compositionally graded Al layer with a thickness of 280 nm formed thereon. x Ga 1-x A three-layer structure was formed with a N (x: 1 → 0.7) layer.
[0052] Sample 6 has an n-type layer 203 of AlN (1.3 nm) / Al doped with Si. 0.78 Ga 0.22 The periodic structure is 288. In this case, the total thickness of the n-type layer 203 is 1584 nm. 0.4 Ga 0.6 N (3 nm) / Al 0.52 Ga 0.48 The p-type layer 207 is a 20 nm thick undoped AlN (6 nm) multi-quantum well with two quantum well layers. x Ga 1-x N (x: 1 → 0.7) layer and an undoped compositionally graded Al layer with a thickness of 300 nm formed thereon. x Ga 1-x A two-layer structure was formed with an N (x: 1 → 0.7) layer.
[0053] Sample 7 has an n-type layer 203 of AlN (1.3 nm) / Al doped with Si. 0.78 Ga 0.22 The periodic structure is 288. In this case, the total thickness of the n-type layer 203 is 1584 nm. 0.4 Ga0.6 N (3 nm) / Al 0.52 Ga 0.48 The p-type layer 207 is a 320 nm thick undoped AlN (6 nm) multi-quantum well with two quantum well layers. x Ga 1-x A single-layer structure was formed with N (x: 1 → 0.7) layers.
[0054] In sample 8, the n-type layer 203 is an Al doped with Si. 0.98 Ga 0.02 N(1.7nm) / Al 0.78 Ga 0.22 The periodic structure is N (4.0 nm), and the number of periods is 240. In this case, the total thickness of the n-type layer 203 is 1368 nm. The active layer 205 is made of Al 0.4 Ga 0.6 N (3 nm) / Al 0.52 Ga 0.48 The p-type layer 207 is a 20 nm thick undoped AlN (6 nm) multi-quantum well with two quantum well layers. x Ga 1-x N (x: 1 → 0.7) layer and an undoped compositionally graded Al layer with a thickness of 300 nm formed thereon. x Ga 1-x A two-layer structure was formed with an N (x: 1 → 0.7) layer.
[0055] For comparison, the following comparative samples 1, 2, and 3 were also prepared. In the comparative samples, x-ray reciprocal lattice mapping in the asymmetric plane (-1-124) confirmed that the bulk layer of Si-doped AlGaN mixed crystal constituting the n-type layer 203 was lattice relaxed.
[0056] Comparative sample 1 has an n-type layer 203 made of Si-doped Al 0.73 Ga 0.27 The active layer 205 is a bulk layer of N with a thickness of 1520 nm. 0.4 Ga 0.6 N (3 nm) / Al 0.52 Ga 0.48 The p-type layer 207 is a 20 nm thick undoped AlN (6 nm) multi-quantum well with two quantum well layers. x Ga 1-xN (x: 1 → 0.7) layer and an undoped compositionally graded Al layer with a thickness of 300 nm formed thereon. x Ga 1-x A two-layer structure was formed with an N (x: 1 → 0.7) layer.
[0057] Comparative sample 2 has an n-type layer 203 made of Si-doped Al 0.7 Ga 0.3 The active layer 205 is a bulk layer of N with a thickness of 1250 nm. 0.4 Ga 0.6 N (3 nm) / Al 0.52 Ga 0.48 The p-type layer 207 is a 320 nm thick undoped AlN (6 nm) multi-quantum well with two quantum well layers. x Ga 1-x A single-layer structure was formed with N (x: 1 → 0.7) layers.
[0058] Comparative sample 3 has an n-type layer 203 made of Si-doped Al 0.75 Ga 0.25 The active layer 205 is a bulk layer of N with a thickness of 1250 nm. 0.4 Ga 0.6 N (3 nm) / Al 0.52 Ga 0.48 The p-type layer 207 is a 320 nm thick undoped AlN (6 nm) multi-quantum well with two quantum well layers. x Ga 1-x A single-layer structure was formed with N (x: 1 → 0.7) layers.
[0059] For each sample, the substrate 201 was divided into stripes by cleaving in the <11-20> direction to form individual LDs with m-plane mirror end faces. The contact area of the p-electrode 211 with the contact layer 209 in plan view was 4 μm × 450 μm for Samples 1 to 3 and Comparative Samples 1 to 3, 6 μm × 450 μm for Sample 4, 8 μm × 450 μm for Samples 5 and 8, and 4 μm × 500 μm for Samples 6 and 7, which were used as the device size. The current density was calculated by dividing the supplied current by the contact area of the p-electrode 211 with the contact layer 209 in plan view. The electrical characteristics of each sample's LD were investigated using room-temperature pulse operation (current pulse width: 50 ns, period: 500 μs). Furthermore, the emission spectrum from one of the m-plane mirror end faces was measured using a spectrometer. The measurement results are shown in Tables 1, 2, 3, 4, and 5 below.
[0060] For example, the LD of sample 1 has an injection current density of 16.3 kA / cm 2 A rapid increase in the emission intensity was observed at this current density, and a steep spectrum characteristic of laser oscillation was confirmed from the spontaneous emission light. The laser oscillation peak wavelength was 283.6 nm, the peak width (FWHM) was 0.47 nm, and the threshold current density for oscillation was 16.3 kA / cm. 2 The element resistance was 12.3Ω.
[0061] Furthermore, when each of the LDs of Samples 2 to 8 was evaluated by room temperature pulse driving (current pulse width 50 ns, period 500 μs), a steep spectrum characteristic of laser oscillation was observed. The results of the peak wavelength of laser oscillation, peak width (FWHM), threshold current density of oscillation, and element resistance are shown in Tables 1 to 4.
[0062]
[0063]
[0064]
[0065]
[0066] On the other hand, in the comparative example, the injection current density was 70 kA / cm 2 Even after this, no sudden increase in the emission intensity was observed, and laser oscillation was not observed.2 At the above current density, the LD structure was destroyed by heat. The element resistance of Comparative Example 1 was 21.6 Ω.
[0067] In Comparative Examples 2 and 3, the Al composition and thickness of the Si-doped AlGaN mixed crystal constituting the n-type layer and the composition of the p-type layer were changed from those in Comparative Example 1, but the same structure was grown by MOVPE. LDs in Comparative Examples 2 and 3 were fabricated and evaluated in the same manner as in Comparative Example 1. The injection current density was 70 kA / cm. 2 Even after this time, no laser oscillation was observed, and the LD structure was destroyed by heat. The results of the element resistance are shown in Table 5.
[0068]
[0069] As described above, according to the present invention, the n-type layer is x Ga 1-x N (0.5<x≦0.87) and Al y Ga 1-y The repeating structure of units of y and y (0.91<y≦1) allows the n-type layer of an optical device using AlGaN to be formed thicker. According to the present invention, it is possible to thicken the n-type layer (thick film) with a high electron concentration, which was difficult to achieve with n-type AlGaN mixed crystals, and, for example, laser oscillation with a low threshold current density can be realized. Optical devices using an n-type layer based on an n-type AlN-based superlattice can be suitably used for ultraviolet LDs with an emission wavelength of 300 nm or less.
[0070] When an AlGaN alloy bulk layer is used for the n-type layer of an ultraviolet LD, lattice relaxation occurs, making it difficult to thicken the n-type layer. In contrast, using an n-type AlN-based superlattice allows pseudomorphic growth on the underlying buffer layer without lattice relaxation, even when the n-type layer is thicker. Increasing the thickness of the n-type layer contributes to reducing the device resistance of the LD and suppressing heat generation. This prevents degradation of device performance due to heat and reduces the laser oscillation threshold current density of the ultraviolet LD.
[0071] It should be noted that the present invention is not limited to the embodiments described above, and it is clear that many modifications and combinations can be made by a person having ordinary knowledge in the art within the technical concept of the present invention.
[0072] 101...substrate, 102...n type layer, 103...active layer, 104...p type layer, 121...first layer, 122...second layer.
Claims
1. A semiconductor device comprising: an n-type layer having a superlattice structure made of a nitride semiconductor formed on a substrate; a p-type layer made of a nitride semiconductor formed on the substrate; and an active layer made of a nitride semiconductor formed between the n-type layer and the p-type layer, wherein the n-type layer is Al x G 1-x N (0.5<x≦0.87) and Al y G 1-y N (0.91<y≦1) is a unit of a repeating structure of the optical device.
2. An optical device according to claim 1, wherein said n-type layer, said p-type layer and said active layer are stacked on said substrate.
3. An optical device according to claim 2, further comprising a buffer layer made of AlN formed on the substrate, the n-type layer, the p-type layer and the active layer being formed by epitaxial growth on the buffer layer.
4. The optical device according to any one of claims 1 to 3, further comprising a resonator.
Citation Information
Patent Citations
Nitride semiconductor light-emitting element
WO2017057149A1
Semiconductor device
WO2020175125A1
Cited By
SEMICONDUCTOR LIGHT EMITTING DEVICE HAVING 4H-SiC CONDUCTIVE SUBSTRATE AND MANUFACTURING METHOD THEREOF
TWI933739B