Method for manufacturing thin film transistor, sputtering target, and sintered body
By integrating In, Zn, and Al in the oxide semiconductor and gas barrier layers within specific atomic percentage ranges, the method addresses hydrogen and oxygen infiltration issues in thin film transistors, enhancing stability and carrier mobility for improved performance in thin film transistors.
Patent Information
- Application Number
- PCT/JP2024/009593
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-02-06
- Filing Date
- 2024-03-12
- Publication Date
- 2024-10-24
AI Technical Summary
Thin film transistors with oxide semiconductor layers, particularly those containing In, Zn, and Fe, face instability due to hydrogen desorption and diffusion from protective layers, leading to shifts in threshold voltage and reduced operational stability.
Incorporating In, Zn, and Al in the oxide semiconductor and gas barrier layers to suppress hydrogen and oxygen infiltration, with specific atomic percentage ranges for these elements to enhance carrier mobility and stability, and using a sputtering target with similar compositions to form these layers.
The method improves operational stability and optical stress resistance of thin film transistors by effectively preventing hydrogen and oxygen infiltration, thereby maintaining stable electrical characteristics and carrier mobility.
Smart Images

Figure JP2024009593_24102024_PF_FP_ABST
Abstract
Description
Thin film transistor manufacturing method, sputtering target and sintered body
[0001] The present disclosure relates to a method for manufacturing a thin film transistor, a sputtering target, and a sintered body.
[0002] Thin film transistors (TFTs) are becoming increasingly popular as active elements used in flat panel displays such as organic electroluminescence (EL) displays. Known types of thin film transistors include top-gate (staggered) and bottom-gate (reverse-staggered) types.
[0003] Such thin film transistors are required to have operational stability. Thin film transistors with improved operational stability due to increased carrier mobility and light stress resistance are known (see JP 2020-194945 A).
[0004] Japanese Patent Application Laid-Open No. 2020-194945
[0005] The thin-film transistor of Patent Document 1 has improved operational stability by including an oxide semiconductor layer containing In, Zn, and Fe. SiN is often used as the protective layer of thin-film transistors. Protective layers containing SiN have a high hydrogen content, and hydrogen may be desorbed from the protective layer and diffuse due to thermal history during the manufacturing process. If this hydrogen penetrates the oxide semiconductor layer of the thin-film transistor, it may deteriorate characteristics such as Vth shift of the thin-film transistor. Such deterioration in characteristics has a significant impact on thin-film transistors including oxide semiconductor layers with high carrier mobility, which tend to make their operation unstable. There is a need to reduce the effects of hydrogen and improve the operational stability of thin-film transistors including oxide semiconductor layers.
[0006] The present disclosure has been made in view of the above circumstances, and aims to provide a method for manufacturing a thin-film transistor that can improve operational stability, and a sputtering target for forming an oxide semiconductor layer and an oxide gas barrier layer of a thin-film transistor with high operational stability.
[0007] A method for manufacturing a thin film transistor according to one aspect of the present disclosure is a method for manufacturing a thin film transistor having at least an oxide semiconductor layer, a protective layer, a gate insulating layer, a gate electrode, a source electrode, and a drain electrode on a substrate, the method including the steps of: forming the oxide semiconductor layer containing In, Zn, and Al as metal elements on the substrate; and forming the protective layer containing SiN on the oxide semiconductor layer.
[0008] A method for manufacturing a thin film transistor according to another aspect of the present disclosure is a method for manufacturing a thin film transistor having at least an oxide semiconductor layer, an oxide gas barrier layer, a protective layer, a gate insulating layer, a gate electrode, a source electrode, and a drain electrode on a substrate, the method including the steps of: forming the oxide semiconductor layer on the substrate; forming the oxide gas barrier layer containing In, Zn, and Al as metal elements on the oxide semiconductor layer; and forming the protective layer containing SiN on the oxide gas barrier layer.
[0009] A sputtering target according to yet another embodiment of the present disclosure is a sputtering target for forming at least one of an oxide semiconductor layer and an oxide gas barrier layer used in a thin film transistor, the sputtering target containing In, Zn, and Al as metal elements, wherein the contents of In, Zn, and Al relative to the total of all contained metal elements are In: 40 atomic % or more and 75 atomic % or less, Zn: 15 atomic % or more and 45 atomic % or less, and Al: 0.5 atomic % or more and 20 atomic % or less.
[0010] A method for manufacturing a thin film transistor according to one aspect of the present disclosure can improve the operational stability of the thin film transistor. A sputtering target according to another aspect of the present disclosure can form an oxide semiconductor layer and an oxide gas barrier layer of a thin film transistor with high operational stability.
[0011] FIG. 1 is a schematic cross-sectional view showing a top-gate thin-film transistor according to an embodiment of the present disclosure. FIG. 2 is a schematic cross-sectional view showing a top-gate thin-film transistor different from that shown in FIG. 1 . FIG. 3 is a schematic cross-sectional view showing a top-gate thin-film transistor different from that shown in FIGS. 1 and 2 . FIG. 4 is a graph showing the results of measuring the Id-Vg characteristics of a thin-film transistor of Sample 15 having a channel length of 10 μm and an oxide semiconductor layer containing In and Zn. FIG. 5 is a graph showing the results of measuring the Id-Vg characteristics of a thin-film transistor of Sample 16 having a channel length of 10 μm and an oxide semiconductor layer containing In, Zn, and Al. FIG. 6 is a graph showing the results of measuring the Id-Vg characteristics of a thin-film transistor of Sample 15 having a channel length of 10 μm and an oxide semiconductor layer containing In and Zn, and comparing the light stress resistance in a negative gate bias and light irradiation (Negative Bias Temperature Illumination Stress (NBTIS) test. FIG. 7 is a graph showing the results of measuring the Id-Vg characteristics of a thin film transistor of Sample 16, which has a channel length of 10 μm and includes an oxide semiconductor layer containing In, Zn, and Al, and comparing the light stress resistance through an NBTIS test. FIG. 8 is a graph showing the results of measuring the Id-Vg characteristics of thin film transistors in which the channel length of the oxide semiconductor layer containing In and Zn is changed. FIG. 9 is a graph showing the results of measuring the Id-Vg characteristics of thin film transistors in which the channel length of the oxide semiconductor layer containing In, Zn, and Al is changed. FIG. 10 is a graph showing the results of measuring the Id-Vg characteristics of a thin film transistor of Sample 27, which has a channel length of 10 μm and includes an oxide semiconductor layer containing In, Zn, and Al. FIG. 11 is a graph showing the results of measuring the Id-Vg characteristics of thin film transistors in which the channel length of the oxide semiconductor layer containing In, Zn, and Al is changed.
[0012] [Description of Embodiments of the Present Disclosure] First, embodiments of the present disclosure will be listed and described.
[0013] As described above, hydrogen (H 2 ) penetrates into the oxide semiconductor layer, or this hydrogen turns into moisture (H 2As a result of extensive research by the present inventors, it has been found that by adding indium (In), zinc (Zn), and aluminum (Al) to the oxide semiconductor layer, H 2 and H 2 By providing a thin film transistor with an oxide gas barrier layer containing In, Zn, and Al, it is possible to prevent the intrusion of O into the oxide semiconductor layer. 2 and H 2 It was found that the Al can suppress the penetration of O. At the same time, it was found that the Al can suppress the desorption of Zn, which may be desorbed from the layer due to aging or the like.
[0014] (1) A method for manufacturing a thin film transistor according to one aspect of the present disclosure is a method for manufacturing a thin film transistor having at least an oxide semiconductor layer, a protective layer, a gate insulating layer, a gate electrode, a source electrode, and a drain electrode on a substrate, the method including the steps of: forming the oxide semiconductor layer containing In, Zn, and Al as metal elements on the substrate; and forming the protective layer containing SiN on the oxide semiconductor layer.
[0015] In the method for manufacturing a thin film transistor, an oxide semiconductor layer containing In, Zn, and Al is formed on a substrate. Therefore, H diffused in the oxide semiconductor layer 2 and H 2 The penetration of O can be suppressed, and the operational stability of the resulting thin film transistor can be improved.
[0016] (2) A method for manufacturing a thin film transistor according to another aspect of the present disclosure is a method for manufacturing a thin film transistor having at least an oxide semiconductor layer, an oxide gas barrier layer, a protective layer, a gate insulating layer, a gate electrode, a source electrode, and a drain electrode on a substrate, the method including the steps of: forming the oxide semiconductor layer on the substrate; forming the oxide gas barrier layer containing In, Zn, and Al as metal elements on the oxide semiconductor layer; and forming the protective layer containing SiN on the oxide gas barrier layer.
[0017] In the method for manufacturing a thin film transistor, an oxide gas barrier layer containing In, Zn, and Al is formed on an oxide semiconductor layer, and therefore, H diffused into the oxide semiconductor layer is prevented from being generated. 2 and H 2 The penetration of O can be suppressed, and the operational stability of the resulting thin film transistor can be improved.
[0018] (3) In the above (2), the oxide semiconductor layer may contain In, Zn, and Al as metal elements. By doing so, H 2 and H 2 The diffusion of O can be further suppressed.
[0019] (4) In the above (1), (2), and (3), the content of the metal elements may be 40 atomic % or more and 75 atomic % or less of In, 15 atomic % or more and 45 atomic % or less of Zn, and 0.5 atomic % or more and 20 atomic % or less of Al, relative to the total content of the metal elements. In this way, when the contents of the In, Zn, and Al in the metal elements are within the above ranges, H is not formed in the oxide semiconductor layer. 2 and H 2 While effectively suppressing the intrusion of O, it is possible to promote optimization of the carrier mobility and threshold voltage of the thin film transistor.
[0020] (5) In the above (1), (2), and (3), the oxide semiconductor layer and the oxide gas barrier layer may be amorphous layers. 2 and H 2 The effect of suppressing the diffusion of O can be improved.
[0021] (6) In the above (1) to (5), the oxide semiconductor layer and the oxide gas barrier layer are formed by H 2 and H 2 In other words, the oxide semiconductor layer itself may be formed as a barrier layer against at least one of H and O. 2 and H 2 The insulating layer may also function as a gas barrier layer that suppresses the penetration of at least one of O and SiO.
[0022] (7) In the above (1) to (6), the Al in the oxide semiconductor layer and the oxide gas barrier layer may suppress the desorption of Zn, i.e., the Al may be contained as a metal element that suppresses the desorption of Zn.
[0023] A sputtering target according to yet another embodiment of the present disclosure is a sputtering target for forming at least one of an oxide semiconductor layer and an oxide gas barrier layer used in a thin film transistor, the sputtering target containing In, Zn, and Al as metal elements, wherein the contents of In, Zn, and Al relative to the total of all contained metal elements are In: 40 atomic % or more and 75 atomic % or less, Zn: 15 atomic % or more and 45 atomic % or less, and Al: 0.5 atomic % or more and 20 atomic % or less.
[0024] The sputtering target is a target for forming H in the oxide semiconductor layer. 2 and H 2 An oxide semiconductor layer and an oxide gas barrier layer that can suppress the diffusion of O can be formed.
[0025] A sintered body according to yet another aspect of the present disclosure is a sintered body for forming the sputtering target.
[0026] That is, the sputtering target may be formed of a sintered body.
[0027] [Details of the embodiment of the present disclosure] Hereinafter, the embodiment of the present disclosure will be described in detail with reference to the drawings as appropriate. Note that with respect to the numerical values described in this specification, it is possible to adopt only one of the upper limit value and the lower limit value described, or to arbitrarily combine the upper limit value and the lower limit value. In this specification, all numerical ranges from the upper limit value to the lower limit value that can be combined are described as suitable ranges.
[0028] First Embodiment FIG. 1 shows a top-gate thin-film transistor 10 (hereinafter simply referred to as "thin-film transistor 10") as an example of a thin-film transistor obtained by the thin-film transistor manufacturing method (hereinafter simply referred to as "the manufacturing method"). The thin-film transistor 10 has an oxide semiconductor layer 12, a protective layer 13, a gate insulating layer 14, a gate electrode 15, a source electrode 16, and a drain electrode 17 on a substrate 11. The protective layer 13 of the thin-film transistor 10 in FIG. 1 includes a first protective layer 131 containing silicon oxide (SiOx) and a second protective layer 132 containing silicon nitride (SiN) and stacked on the first protective layer 131. The gate insulating layer 14 and the gate electrode 15 are disposed within the protective layer 13 (first protective layer 131). The gate insulating layer 14 is stacked on the oxide semiconductor layer 12, and the gate electrode 15 is stacked on the gate insulating layer 14. The source electrode 16 and the drain electrode 17 are arranged so that parts of them are in contact with the conductive S / D regions of the oxide semiconductor layer 12. The region of the oxide semiconductor layer 12 where the gate insulating layer 14 is stacked is a channel region that is not conductive.
[0029] The thin film transistor 10 is obtained by a manufacturing method including the steps of forming an oxide semiconductor layer 12 containing In, Zn, and Al as metal elements on a substrate 11, and forming a protective layer 13 containing SiN on the oxide semiconductor layer 12. Between these two steps, the manufacturing method includes the steps of forming a gate insulating layer 14 on the oxide semiconductor layer 12 and forming a gate electrode 15 on the gate insulating layer 14. The manufacturing method also includes the steps of forming a source electrode 16 and a drain electrode 17 after the step of forming the protective layer 13.
[0030] [Step of Forming Oxide Semiconductor Layer] In the step of forming the oxide semiconductor layer 12, the oxide semiconductor layer 12 containing In, Zn, and Al as metal elements is formed on the substrate 11.
[0031] (Substrate) The substrate 11 is not particularly limited, and examples thereof include a glass substrate and a silicon substrate. Examples of glass used for the glass substrate include alkali-free glass, high strain point glass, soda lime glass, etc. Alternatively, the substrate 11 may be a metal substrate such as a stainless steel sheet, or a resin substrate such as a polyethylene terephthalate (PET) film.
[0032] From the viewpoint of workability, the average thickness of the substrate 11 is preferably 0.001 mm or more and 10 mm or less. The size and shape of the substrate 11 can be set depending on the size of the display, etc.
[0033] (Oxide Semiconductor Layer) The oxide semiconductor layer 12 contains In, Zn, and Al as metal elements. By containing these metal elements, the oxide semiconductor layer 12 can withstand H diffused from the second protective layer 132 containing SiN, which will be described later. 2 It is possible to prevent the diffused H 2 combines with oxygen, and H 2 In other words, the oxide semiconductor layer 12 can be prevented from penetrating into the interior as H 2 and H 2 It functions as a barrier layer against O gas.
[0034] <In> In is H 2 and H 2 In is an element that suppresses the penetration of O into the oxide semiconductor layer 12 and also contributes to improving the conductivity (electrical conductivity). The greater the content of In, the more the conductivity of the oxide semiconductor layer 12 improves, and the more the carrier density and carrier mobility improve.
[0035] The lower limit of the In content relative to the total metal elements in the oxide semiconductor layer 12 is preferably 40 atomic %. The upper limit of the content is preferably 75 atomic %, more preferably 65 atomic %. By setting the In content within the above range, H 2 and H 2 This can improve the reliability of the effect of suppressing the intrusion of O into the oxide semiconductor layer 12, and can also ensure sufficient carrier mobility and the like.
[0036] <Zn> Zn is H 2 and H 2 O is an element that inhibits the intrusion of O into the oxide semiconductor layer 12 and also affects the processing characteristics of the oxide semiconductor layer 12 .
[0037] The lower limit of the Zn content relative to the total metal elements in the oxide semiconductor layer 12 is preferably 15 atomic %, more preferably 25 atomic %. The upper limit of the content is preferably 45 atomic %, more preferably 35 atomic %. By setting the Zn content within the above range, H 2 and H 2 This can improve the reliability of the effect of suppressing the penetration of O into the oxide semiconductor layer 12, and also makes it easier to ensure the processability and uniformity of the oxide semiconductor layer 12.
[0038] <Al> Al is H 2 and H 2 Al is an element that suppresses the penetration of O into the oxide semiconductor layer 12 and also suppresses the desorption of Zn from the oxide semiconductor layer 12. Specifically, Zn may be desorbed from the oxide semiconductor layer 12 due to aging or the like. By including Al, the desorption of Zn can be suppressed. Furthermore, by including Al in the oxide semiconductor layer 12, the light stress resistance of the thin film transistor 10 can be improved.
[0039] The lower limit of the Al content relative to the total metal elements in the oxide semiconductor layer 12 is preferably 0.5 atomic %, more preferably 1.5 atomic %. The upper limit of the Al content is preferably 20 atomic %, more preferably 10 atomic %. By setting the Al content within the above range, H 2 and H 2 This can improve the reliability of the effect of suppressing the intrusion of O into the oxide semiconductor layer 12 and also improve the reliability of the effect of suppressing the desorption of Zn.
[0040] The reason why Al can suppress the desorption of Zn is thought to be as follows: Zn in the oxide layer is absorbed by H contained in the oxide layer. 2 and H 2It is known that the oxide layer is desorbed after the release of O. When Al is added, the oxide layer is 2 and H 2 In addition to the function of preventing O from penetrating into the oxide layer (gas barrier function), 2 and H 2 This provides a function of suppressing the release of O. It is therefore believed that adding Al to the oxide layer can suppress the desorption of Zn from the oxide layer.
[0041] In the oxide semiconductor layer 12, elements other than those mentioned above are O (oxygen) and inevitable impurities. The inevitable impurities may be contained due to raw materials, materials, manufacturing equipment, etc. Examples of the inevitable impurities include Pb, Si, Fe, Ni, Ti, Mg, Cr, and Zr. The content of the inevitable impurities in the oxide semiconductor layer 12 is preferably 1 mass% or less for each element, and more preferably 500 mass ppm or less. In this configuration, the contents of In, Zn, and Al in the oxide semiconductor layer 12 can also be considered as proportions of all elements excluding O.
[0042] The average thickness of the oxide semiconductor layer 12 can be determined based on the condition that the drain current can be turned off when the oxide semiconductor layer 12 is used as a switching element. The lower limit of the average thickness of the oxide semiconductor layer 12 is preferably 10 nm, more preferably 15 nm. On the other hand, the upper limit of the average thickness is preferably 60 nm, more preferably 50 nm. In this specification, the term "average thickness" refers to the average value of thicknesses at any five points.
[0043] The oxide semiconductor layer 12 is preferably an amorphous layer. Alternatively, it is preferable that at least a portion of the oxide semiconductor layer 12 is formed as an amorphous layer. That is, it is preferable that the oxide forming the oxide semiconductor layer 12 is amorphous or at least a portion of the oxide is amorphous. Even when the oxide semiconductor layer 12 has such a configuration, it can sufficiently increase the carrier mobility compared to general-purpose amorphous silicon. Furthermore, by having such a configuration, it is possible to easily and reliably increase the optical band gap.
[0044] In general, the denser the oxide layer, the better the gas barrier function. The denser the oxide layer, the more the oxide layer can be made amorphous rather than polycrystalline with many grain boundaries. In oxide has gas barrier function, but tends to crystallize the oxide layer. On the other hand, adding Zn can promote the amorphization of the oxide layer. Al is a metal oxide that can be used as a barrier against H 2 When the oxide layer reacts with O to become partially an Al oxide, it tends to crystallize that portion, but Al can promote the amorphization of the oxide layer. Therefore, the oxide layer containing In, Zn, and Al promotes the amorphization, and H 2 and H 2 It is believed that a suitable gas barrier function against O can be exhibited.
[0045] The oxide semiconductor layer 12 can be made into an amorphous layer by controlling the gas pressure to a range of 1 mTorr to 5 mTorr, for example, and by performing a surface treatment with plasma or a reducing gas after film formation.
[0046] The upper limit of the sheet resistance of the oxide semiconductor layer 12 (the sheet resistance of the S / D region after surface treatment) is preferably 1.0 kΩ / □, and more preferably 0.5 kΩ / □. When the oxide semiconductor layer 12 has a sheet resistance after surface treatment that is equal to or less than the upper limit, the S / D region can be easily and reliably made conductive. The sheet resistance can be a value measured using a four-probe resistance meter.
[0047] The oxide semiconductor layer 12 is formed by sputtering using a sputtering target. After the oxide semiconductor layer 12 is formed, it is patterned by photolithography or the like. Immediately after this patterning, it is preferable to perform a heat treatment (pre-annealing treatment) to improve the film quality.
[0048] <<Sputtering Target>> The oxide semiconductor layer 12 can be formed using a sputtering target containing In, Zn, and Al as metal elements, with the In, Zn, and Al contents being 40 atomic % to 75 atomic % of In, 15 atomic % to 45 atomic % of Zn, and 0.5 atomic % to 20 atomic % of Al relative to the total of all metal elements contained. Elements other than those mentioned above in the sputtering target are unavoidable impurities. The content of each element in the sputtering target can be the same as the range described for the oxide semiconductor layer 12.
[0049] The sputtering target material formed in the sputtering target can be used to form the oxide semiconductor layer 12 and can also be used to form the oxide gas barrier layer described later. The sputtering target material contains the same metal elements as the sputtering target described above, and the content of the metal elements is approximately the same. 2 and H 2 It can have a gas barrier function against O.
[0050] <<Sintered Body>> The sputtering target is formed of a sintered body.
[0051] [Step of Forming Gate Insulating Layer] In the step of forming the gate insulating layer 14, the gate insulating layer 14 is formed on the oxide semiconductor layer 12. The gate insulating layer 14 is formed on the oxide semiconductor layer 12 after the pre-annealing treatment.
[0052] The gate insulating layer 14 may be, for example, a silicon oxide layer, a silicon nitride layer, a silicon oxynitride layer, or an Al 2 O 3 Ya Y 2 O 3 Examples of the gate insulating layer 14 include a metal oxide layer such as a SiO 2 film or a SiO 3 film. The gate insulating layer 14 can be formed by a CVD method, a PECVD method, or the like. The gate insulating layer 14 may be a single layer or a multilayer body having two or more layers. When the gate insulating layer 14 is a multilayer body having two or more layers, it is preferable that the first layer and the second and subsequent layers have different components.
[0053] The lower limit of the average thickness of the gate insulating layer 14 is preferably 50 nm, more preferably 100 nm. On the other hand, the upper limit of the average thickness of the gate insulating layer 14 is preferably 300 nm, more preferably 250 nm. If the average thickness is less than the lower limit, the withstand voltage of the gate insulating layer 14 may be insufficient. Conversely, if the average thickness exceeds the upper limit, the capacitance of the capacitor formed between the gate electrode 15 and the oxide semiconductor layer 12 may be insufficient, resulting in insufficient drain current. Note that when the gate insulating layer 14 is multilayered, the "average thickness of the gate insulating layer" refers to the average thickness of the entire gate insulating layer.
[0054] [Step of Forming Gate Electrode] In the step of forming the gate electrode 15, the gate electrode 15 is formed on the gate insulating layer 14. After the gate electrode 15 is formed, the gate insulating layer 14 and the gate electrode 15 are patterned by photolithography or the like.
[0055] (Gate electrode) The gate electrode 15 is conductive. The gate electrode 15 is formed, for example, after forming the gate insulating layer 14 and then subjecting the oxide semiconductor layer 12 to a heat treatment (annealing treatment). The gate electrode 15 is not particularly limited, but may be made of a metal with low electrical resistivity such as Al or Cu, or an alloy of a high-melting-point metal with high heat resistance such as Mo, Cr, or Ti.
[0056] The lower limit of the average thickness of the gate electrode 15 is preferably 50 nm, more preferably 80 nm. By setting the average thickness to be equal to or greater than the lower limit, it is possible to suppress an increase in the resistance of the gate electrode 15 and to suppress an increase in power consumption in the gate electrode 15. On the other hand, from the viewpoint of processability and the like, the upper limit of the average thickness of the gate electrode 15 is preferably 500 nm, more preferably 400 nm.
[0057] [Step of Forming Protective Layer] In the step of forming the protective layer 13, the protective layer 13 containing SiN is formed on the oxide semiconductor layer 12. This step in the present embodiment includes a procedure of forming a first protective layer 131 containing SiOx on the oxide semiconductor layer 12 so as to cover the gate insulating layer 14 and the gate electrode 15, and a procedure of forming a second protective layer 132 containing SiN on the first protective layer 131.
[0058] The first protective layer 131 is formed after patterning the gate insulating layer 14 and the gate electrode 15 and after performing a surface treatment on the oxide semiconductor layer 12. The surface treatment of the oxide semiconductor layer 12 is performed to make the S / D region conductive, and can be performed by, for example, ion implantation, element diffusion, reduction with a reducing gas, plasma treatment, or the like.
[0059] The first protective layer 131 and the second protective layer 132 can be formed by using a CVD method, a PECVD method, etc. After the film formation, contact holes for disposing the source electrode 16 and the drain electrode 17 are formed by photolithography or the like.
[0060] The first protective layer 131 contains SiOx, and the second protective layer 132 contains SiN, i.e., the first protective layer 131 is a silicon oxide layer, and the second protective layer 132 is a silicon nitride layer.
[0061] By providing the protective layer 13, it is possible to reduce the influence of the external environment on the oxide semiconductor layer 12, the gate electrode 15, etc. The second protective layer 132 containing SiN is 2 On the other hand, the second protective layer 132 containing SiN is suitable for reducing the influence of H 2 Because it contains a lot of H, the heat history during the manufacturing process 2 This released H 2 If H penetrates into the oxide semiconductor layer 12, the electrical characteristics of the thin film transistor 10 may be degraded. 2 Therefore, by disposing the insulating layer between the oxide semiconductor layer 12 and the second protective layer 132, the intrusion of H released from the second protective layer 132 can be suppressed. 2The thin film transistor 10 further includes the oxide semiconductor layer 12 having a gas barrier function, and therefore, H 2 The penetration of the oxygen into the oxide semiconductor layer 12 can be further suppressed.
[0062] [Step of Forming Electrodes] In the step of forming electrodes, the source electrode 16 and the drain electrode 17 are formed. Specifically, the source electrode 16 and the drain electrode 17 are formed in the contact holes so that parts of the electrodes are in contact with the S / D regions of the oxide semiconductor layer 12. After being formed, the source electrode 16 and the drain electrode 17 are patterned by photolithography or the like.
[0063] The source electrode 16 and the drain electrode 17 are conductive. The source electrode 16 and the drain electrode 17 are not particularly limited, but may be made of a metal with low electrical resistivity such as Al or Cu, a high-melting-point metal with high heat resistance such as Mo, Cr or Ti, or an alloy of these.
[0064] The source electrode 16 and the drain electrode 17 cover a part of the protective layer 13 and fill the contact holes. By providing them in this manner, the source electrode 16 and the drain electrode 17 are electrically connected to the oxide semiconductor layer 12 at both ends of the channel region of the thin film transistor 10.
[0065] The lower limit of the average thickness of the source electrode 16 and the drain electrode 17 is preferably 100 nm, more preferably 150 nm. By setting the average thickness to be equal to or greater than the lower limit, it is possible to prevent the resistance of the source electrode 16 and the drain electrode 17 from increasing, and to prevent an increase in power consumption. The upper limit of the average thickness of the source electrode 16 and the drain electrode 17 is desirably greater than the total thickness of the gate insulating layer 14 and the gate electrode 15, and is, for example, preferably 1000 μm, more preferably 800 μm.
[0066] <Advantages> The manufacturing method includes a step of forming an oxide semiconductor layer 12 containing In, Zn, and Al as metal elements on a substrate 11, and a step of forming a protective layer 13 containing SiN on the oxide semiconductor layer 12. Therefore, H diffused from the protective layer 13 due to the thermal history during the manufacturing process can be prevented. 2 This can prevent the oxide semiconductor layer 12 from penetrating. Therefore, the resulting thin film transistor 10 has high carrier mobility and excellent operational stability.
[0067] The sputtering target is suitable for producing the oxide semiconductor layer 12 .
[0068] Second Embodiment Another embodiment of the method for manufacturing the thin film transistor will be described below. Note that the same components as those in the first embodiment are denoted by the same reference numerals and will not be described again.
[0069] 2 shows a top-gate thin-film transistor 20 (hereinafter simply referred to as "thin-film transistor 20") obtained by the thin-film transistor manufacturing method (hereinafter simply referred to as "the manufacturing method"). The thin-film transistor 20 has an oxide semiconductor layer 22, an oxide gas barrier layer 27, a protective layer 13, a gate insulating layer 14, a gate electrode 15, a source electrode 16, and a drain electrode 17 on a substrate 11. The protective layer 13 includes a first protective layer 131 containing SiOx and a second protective layer 132 containing SiN and stacked on the first protective layer 131.
[0070] The thin film transistor 20 includes a step of forming an oxide semiconductor layer 22 on a substrate 11, a step of forming an oxide gas barrier layer 27 containing In, Zn, and Al as metal elements on the oxide semiconductor layer 22, and a step of forming a protective layer 13 containing SiN on the oxide gas barrier layer 27. The manufacturing method includes a step of forming a gate insulating layer 14 on the oxide semiconductor layer 22 and a step of forming a gate electrode 15 on the gate insulating layer 14 between the step of forming the oxide semiconductor layer and the step of forming the oxide gas barrier layer. The manufacturing method also includes a step of forming a source electrode 16 and a drain electrode 17 after the step of forming the protective layer 13.
[0071] [Step of Forming Oxide Semiconductor Layer] In the step of forming an oxide semiconductor layer, an oxide semiconductor layer 22 is formed on the substrate 11. The metal elements contained in this oxide semiconductor layer 22 are not particularly limited, and it is not necessary for the oxide semiconductor layer 22 to contain any or all of In, Zn, and Al.
[0072] Next, the gate insulating layer 14 and the gate electrode 15 are formed on the oxide semiconductor layer 22 .
[0073] [Step of Forming Oxide Gas Barrier Layer] In the step of forming the oxide gas barrier layer, the oxide gas barrier layer 27 containing In, Zn, and Al as metal elements is formed on the oxide semiconductor layer 22. Specifically, the oxide gas barrier layer 27 is formed so as to cover the gate insulating layer 14 and the gate electrode 15 formed on the oxide semiconductor layer 22.
[0074] The oxide gas barrier layer 27 contains In, Zn, and Al as metal elements. The content of each of the In, Zn, and Al relative to the total content of these metal elements can be the same as that of the oxide semiconductor layer 12 described in the first embodiment. The oxide gas barrier layer 27 is preferably an amorphous layer. Alternatively, it is preferable that at least a part of the oxide gas barrier layer 27 is formed as an amorphous layer. The oxide gas barrier layer 27 is preferably a layer containing H 2 and H 2 It functions as a barrier layer against O gas. The Al prevents the Zn from being desorbed from the oxide gas barrier layer 27.
[0075] [Step of Forming Protective Layer] In the step of forming the protective layer 13, the protective layer 13 containing SiN is formed on the oxide gas barrier layer 27. This step in the present embodiment includes a procedure of forming a first protective layer 131 containing SiOx on the oxide gas barrier layer 27, and a procedure of forming a second protective layer 132 containing SiN on this first protective layer 131.
[0076] After the protective layer 13 is formed, contact holes are formed, and a source electrode 16 and a drain electrode 17 are formed in the contact holes.
[0077] <Advantages> The manufacturing method includes the steps of forming an oxide semiconductor layer 22 on a substrate 11, forming an oxide gas barrier layer 27 containing In, Zn, and Al as metal elements on the oxide semiconductor layer 22, and forming a protective layer 13 containing SiN on the oxide gas barrier layer 27. That is, the manufacturing method can obtain a thin film transistor 20 in which the oxide gas barrier layer 27 containing In, Zn, and Al is formed between the oxide semiconductor layer 22 and the protective layer 13 containing SiN. Therefore, H diffused from the protective layer 13 due to the thermal history during the manufacturing process can be prevented from being oxidized. 2 This can prevent the oxide semiconductor layer 22 from penetrating.
[0078] [Other Embodiments] The above-described embodiments do not limit the configuration of the present invention. Therefore, the above-described embodiments may include omissions, substitutions, or additions of components based on the description in this specification and common general technical knowledge, and all of these should be construed as falling within the scope of the present invention.
[0079] The oxide semiconductor layer of the thin film transistor (second embodiment) having an oxide gas barrier layer may contain In, Zn, and Al. Furthermore, as shown in FIG. 3 , when an oxide semiconductor layer 12 containing In, Zn, and Al is used, the oxide gas barrier layer 27 of the thin film transistor 30 may be disposed within the protective layer 13 (between the first protective layer 131 and the second protective layer 132).
[0080] The specific configuration of the thin film transistor is not limited to the configurations shown in Figures 1, 2, and 3. For example, the protective layer may be only a protective layer containing SiN. Furthermore, the thin film transistor may be a bottom-gate type.
[0081] In the thin film transistor, another layer such as a buffer layer may be provided between the substrate and the oxide semiconductor layer to improve adhesion or as a buffer material.
[0082] The present invention will be described in detail below based on examples, but the present invention should not be construed as being limited by the descriptions of these examples.
[0083] H by oxide layers containing In, Zn and Al2 and H 2 Samples 1 to 14 were prepared to evaluate the gas barrier resistance to O. Each sample was prepared by forming a second protective layer (containing SiN) having a thickness of 150 nm on a silicon substrate having a thickness of 525 μm, forming a first protective layer (containing SiO) having a thickness of 200 nm on the second protective layer, and then forming oxide layers having varying contents of In, Zn, and Al on the first protective layer.
[0084] The film formation conditions and thickness (film thickness) of the oxide layer of each sample are shown below: (1) Samples 1 to 12 Film formation method: DC (direct current) sputtering method Apparatus: CS200 manufactured by ULVAC, Inc. Film formation temperature: room temperature Gas pressure: 1 mTorr Carrier gas: Ar Oxygen partial pressure: 100×O 2 / (Ar + O 2 ) = 4 vol% Film formation power density: 2.55 W / cm 2 Film thickness: 15 nm (2) Samples 13 and 14 Film formation method: DC (direct current) sputtering method Apparatus: CS200 manufactured by ULVAC, Inc. Film formation temperature: room temperature Gas pressure: 1 mTorr Carrier gas: Ar Oxygen partial pressure (first partial pressure): 100×O 2 / (Ar + O 2 ) = 0% by volume Oxygen partial pressure (second partial pressure): 100 × O 2 / (Ar + O 2 ) = 4 vol% Film formation power density: 2.55 W / cm 2 Film thickness: 10 nm was formed at the first partial pressure, and then 15 nm was formed at the second partial pressure (total 25 nm).
[0085] Each sample was analyzed by TDS (Thermal Desorption Spectrometry) to determine the H 2 and H 2 The gas barrier resistance was determined from the amount of O.
[0086] The gas barrier resistance was evaluated by TDS analysis as follows: (1) H 2 :A, B or C was determined based on whether the ion current [A] below was exceeded in the temperature range of 300℃ to 450℃. "A" indicates H 2 "C" indicates good gas barrier resistance, and "H" indicates good gas barrier resistance.2 The gas barrier resistance is poor, and "B" means an intermediate evaluation between A and C. -9 [A] Super: C 5E -10 [A] Super: B 5E -10 [A] Below: A (2) H 2 O: The following temperature range and ion current [A] were used to determine whether the temperature is A, B, or C. "A" indicates H 2 O gas barrier resistance is good, "C" is H 2 1E indicates poor gas barrier resistance, and "B" indicates an intermediate evaluation between A and C. -9 Temperature exceeding [A] is 300°C or higher and lower than 350°C: C 1E -9 Temperature exceeding [A] is 350°C or higher and lower than 400°C: B 1E -9 [A] Temperature exceeding 400 ° C or more and less than 450 ° C: A
[0087] After the TDS analysis, the resistance value of the oxide layer of each sample was measured. Resistance values less than 100 Ωcm were rated "A," and resistance values of 100 Ωcm or more were rated "B." Oxide layers rated "B" are considered to be difficult to use as semiconductor layers.
[0088] Measurements were performed as follows: (1) Measurement of ion current Analytical device: TDS1200II (manufactured by Denshi Kagaku Co., Ltd.) Temperature conditions: RT-500°C (60°C / min) at set temperature USC temperature Sample stage: quartz stage Quadrupole mass spectrometer Ionization method: electron ionization Measurement mode: SIM mode (selective mass number measurement mode) (2) Measurement of resistance Analytical device: MCP-HT450 (manufactured by Nitto Seiko Analytech Co., Ltd.) Measurement method: constant voltage application, leakage current measurement method
[0089] The In, Zn, and Al contents and measurement results for each sample are shown in Table 1. In Table 1, the numerical values represent the In, Zn, and Al contents, and "-" indicates that the element is not contained.
[0090]
[0091] From Table 1, it can be seen that Samples 8, 9, 10 and 14 all received high marks.
[0092] Next, a thin film transistor (Sample 15) including an oxide semiconductor layer containing 65 atomic % In, 35 atomic % Zn, and 0 atomic % Al was fabricated; a thin film transistor (Sample 16) including an oxide semiconductor layer containing 65 atomic % In, 28 atomic % Zn, and 7 atomic % Al; and a thin film transistor (Sample 27) including an oxide semiconductor layer containing 64 atomic % In, 35 atomic % Zn, and 0.7 atomic % Al were fabricated. The Id-Vg characteristics of Samples 15, 16, and 27 were compared, and the light stress resistance of Samples 15 and 16 was compared. The results are shown in FIGS. 4 to 11.
[0093] The Id-Vg characteristics (drain current (Id) - gate voltage (Vg) characteristics) of Samples 15, 16, and 27 were compared with a channel length of 10 μm. The Id-Vg characteristics were measured three times for each sample. The results for Sample 15 are shown in Figure 4, those for Sample 16 in Figure 5, and those for Sample 27 in Figure 10.
[0094] 4, 5, and 10, the slope decreases (approaching parallel to the vertical axis) in the vicinity of Vg0 [V] in the order of Fig. 4 (Sample 15), Fig. 10 (Sample 27), and Fig. 5 (Sample 16). This suggests that the inclusion of Al and the increase in the Al content can improve the transfer characteristics (Id-Vg characteristics).
[0095] Next, the light stress resistance of Sample 15 and Sample 16 was compared. To evaluate the light stress resistance, a stress application test (NBTIS test) was conducted on each sample (thin film transistor: TFT) in which a negative bias was continuously applied to the gate electrode while irradiating the sample with light (white light), simulating the environment (stress) during actual liquid crystal panel operation. The variation in threshold voltage (Vth) before and after stress application (threshold voltage shift: ΔVth) was used as an index of light stress resistance in the TFT characteristics. Light stress resistance is one of the important characteristics for driving a liquid crystal display. The NBTIS test was conducted under the following conditions: Gate voltage: -20 V, Source / drain voltage: 10 V, Substrate temperature: 60°C, Stress application time: 2 hours, Light intensity during light stress: 25,000 nits, Light source during light stress: White LED (Light Emitting Diode).
[0096] The ΔVth of Sample 15 was 3.0 [V], and the ΔVth of Sample 16 was 1.8 [V]. The results of the light stress resistance of Sample 15 are shown in FIG. 6 , and the results of the light stress resistance of Sample 16 are shown in FIG. 7 . Comparing FIGS. 6 and 7 , around Vg0 [V], Sample 15 exhibited relatively large variations in the horizontal axis direction and a relatively large inclination (tilt angle) relative to the vertical axis. Sample 16 exhibited relatively small variations in the horizontal axis direction and a relatively small inclination relative to the vertical axis. This indicates that the inclusion of Al improves the light stress resistance. The numbers on the left in the graphs ( FIGS. 6 and 7 ) indicate the application time of the light stress. 0 sec indicates the start of the application of the light stress. Measurements were taken after 30 sec of application, then 100 sec, and then 300 sec, 1000 sec, 3600 sec, and 7200 sec, respectively.
[0097] Samples with different channel lengths (lengths of channel regions) were prepared for a thin film transistor including an oxide semiconductor layer containing 65 atomic % In, 35 atomic % Zn, and 0 atomic % Al, a thin film transistor including an oxide semiconductor layer containing 65 atomic % In, 28 atomic % Zn, and 7 atomic % Al, and a thin film transistor including an oxide semiconductor layer containing 64 atomic % In, 35 atomic % Zn, and 0.7 atomic % Al, and the channel length dependence was compared. Table 2 shows the contained metal elements and channel lengths for each sample number. Note that Sample 15 described above and Sample 19 in Table 2 are the same sample, Sample 16 described above and Sample 24 in Table 2 are the same sample, and Sample 27 described above and Sample 30 in Table 2 are the same sample.
[0098]
[0099] The transmission characteristics were measured and compared for Samples 17 to 26 and Samples 28 to 32. The results for Samples 17 to 21 are shown in Fig. 8, the results for Samples 22 to 26 in Fig. 9, and the results for Samples 28 to 32 in Fig. 11.
[0100] 8, 9, and 11, in the samples with a channel length of 8 μm or more, the slope decreases (approaching parallel to the vertical axis) in the order of FIG. 8, FIG. 11, and FIG. 9 near Vg0 [V]. This suggests that the inclusion of Al and the increase in Al content can improve the transfer characteristics (Id-Vg characteristics). Furthermore, when comparing Sample 17, Sample 22, and Sample 28, which have a channel length of 5 μm, a large shift (deviation) occurs in the horizontal axis direction near Vg0 [V] in Sample 17, whereas the shift is smaller in Samples 22 and 28. This suggests that the inclusion of Al in the oxide semiconductor layer can contribute to the miniaturization of thin film transistors.
[0101] As described above, the method for manufacturing a thin film transistor according to one embodiment of the present disclosure can provide a thin film transistor that has high operational stability and is suitable for organic EL displays and the like.
[0102] 10, 20, 30 Thin film transistor 11 Substrate 12, 22 Oxide semiconductor layer 13 Protective layer 131 First protective layer 132 Second protective layer 14 Gate insulating layer 15 Gate electrode 16 Source electrode 17 Drain electrode 27 Oxide gas barrier layer
Claims
1. A method for manufacturing a thin film transistor having at least an oxide semiconductor layer, a protective layer, a gate insulating layer, a gate electrode, a source electrode and a drain electrode on a substrate, the method comprising the steps of: forming the oxide semiconductor layer containing In, Zn and Al as metal elements on the substrate; and forming the protective layer containing SiN on the oxide semiconductor layer.
2. A method for manufacturing a thin film transistor having at least an oxide semiconductor layer, an oxide gas barrier layer, a protective layer, a gate insulating layer, a gate electrode, a source electrode and a drain electrode on a substrate, comprising the steps of: forming the oxide semiconductor layer on the substrate; forming the oxide gas barrier layer containing In, Zn and Al as metal elements on the oxide semiconductor layer; and forming the protective layer containing SiN on the oxide gas barrier layer.
3. The method for producing a thin film transistor according to claim 2, wherein the oxide semiconductor layer contains In, Zn and Al as metallic elements.
4. A method for manufacturing a thin film transistor according to claim 1, 2 or 3, wherein the content of the metal elements relative to the total is: In: 40 atomic % or more and 75 atomic % or less; Zn: 15 atomic % or more and 45 atomic % or less; and Al: 0.5 atomic % or more and 20 atomic % or less.
5. The method for producing a thin film transistor according to claim 1, wherein the oxide semiconductor layer is an amorphous layer.
6. The method for producing a thin film transistor according to claim 3, wherein at least one of the oxide semiconductor layer and the oxide gas barrier layer is an amorphous layer.
7. The oxide semiconductor layer is treated with H 2 and H 2 4. The method for producing a thin film transistor according to claim 1, wherein the barrier layer is formed against at least one of oxygen and oxygen.
8. The oxide gas barrier layer is treated with H 2 and H 2 4. The method for producing a thin film transistor according to claim 2, wherein the barrier layer is formed against at least one of oxygen and oxygen.
9. A sputtering target for forming at least one of an oxide semiconductor layer and an oxide gas barrier layer used in a thin film transistor, comprising In, Zn and Al as metal elements, the contents of the In, Zn and Al relative to the total of all metal elements contained being as follows: In: 40 atomic % or more and 75 atomic % or less, Zn: 15 atomic % or more and 45 atomic % or less, and Al: 0.5 atomic % or more and 20 atomic % or less.
10. A sintered body for forming the sputtering target according to claim 9.
Citation Information
Patent Citations
Electronic display
JP2009021554A
Thin film field effect transistor and display using the same
JP2009212497A
Semiconductor device and touch panel
JP2016201539A