Perovskite material mass production method
The method of stirring a precursor solution with controlled solvent pressures and solvents allows for high-yield, high-crystallinity perovskite production without heat treatment, addressing the challenges of toxic solvent use and scalability in perovskite solar cell production.
Patent Information
- Application Number
- PCT/KR2024/004129
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-20
- Filing Date
- 2024-04-01
- Publication Date
- 2024-10-24
AI Technical Summary
Current methods for producing perovskite crystalline precursors face challenges in achieving high yield and purity while minimizing the use of toxic solvents and avoiding heat treatment, which are essential for large-scale commercialization of perovskite solar cells.
A method involving the continuous stirring of a precursor solution containing a combination of metal and organic halides with a good solvent and an anti-solvent, where the partial pressure of the anti-solvent is maintained at 0.1 atm or more, allowing for the precipitation of perovskite crystalline precursors without heat treatment, using solvents like chloroform, ethyl alcohol, and isopropyl alcohol, and collecting the precipitate using a pressure reduction filter.
This method enables the high-yield production of perovskite crystalline precursors with high crystallinity in kg quantities in a short time, reducing the use of toxic solvents and eliminating the need for heat treatment, thus enhancing industrial applicability and environmental sustainability.
Smart Images

Figure KR2024004129_24102024_PF_FP_ABST
Abstract
Description
Mass production method of perovskite materials
[0001] The present invention relates to a method for synthesizing a large quantity of perovskite crystal precursors at the kg level in a short period of time with a high yield without heat treatment.
[0002] Recently, organic-inorganic hybrid perovskite materials have been highlighted as key materials for next-generation photovoltaic devices due to their advantages such as high light absorbance, high external quantum efficiency (EQE), fast charge transfer rate, and solution processability. Over the past decade, extensive research has been conducted on perovskite materials, focusing on solar cells, and commercialization is imminent with a peak photoelectric conversion efficiency of 25%. However, many challenges remain for the commercialization of perovskite solar cells, such as improving stability against light, heat, and moisture, improving charge transfer efficiency, reducing toxic substances, and developing low-cost, large-area perovskite thin film manufacturing methods. Therefore, active research is being actively conducted.
[0003] Perovskite thin films are manufactured from a perovskite precursor solution prepared by dissolving a perovskite precursor in a solvent. The perovskite precursor is prepared by crystallizing a mixture of organic halides and metal halides in the solution. To manufacture a perovskite precursor with high purity and crystallinity, the precursor solution is heated to crystallize, taking advantage of the reduced solubility of perovskite crystals at high temperatures. However, in the process of removing impurities from the perovskite crystals, large amounts of toxic nonsolvents such as diethyl ether are used. This poses a significant obstacle to environmental pollution issues related to perovskite technology.
[0004] Research on improving the yield, purity, and reducing environmental pollutants of the above crystallization process is still insufficient, and is emerging as a key research for future commercialization of perovskite.
[0005] The purpose of the present invention is to provide a method for mass producing a perovskite precursor, which can produce a large quantity of perovskite precursor in units of kg in a short period of time with a high yield without heat treatment.
[0006] Another object of the present invention is to provide a method for mass producing a perovskite precursor having high crystallinity while using a small amount of toxic solvent.
[0007] A method for mass producing a perovskite precursor according to the present invention comprises the steps of (S1) preparing a precursor solution by mixing at least one halide selected from the group consisting of a combination of a first metal halide and an organic halide; a second metal halide; and a first solvent; (S2) continuously stirring the precursor solution while adding a second solvent in a gaseous state; and (S3) obtaining a perovskite crystalline precursor precipitated from the precursor solution; wherein the first solvent is a good solvent for the halide and the second metal halide, and the second solvent is an antisolvent for the halide and the second metal halide.
[0008] In the mass production method of a perovskite precursor according to the present invention, the partial pressure of the second solvent in the gas phase of step (S2) may be 0.1 atm or more based on atmospheric pressure.
[0009] In the mass production method of a perovskite precursor according to the present invention, the second solvent may be at least one solvent selected from the group consisting of a combination of chloroform, diethyl ether, ethyl acetate, ethyl alcohol, and isopropyl alcohol.
[0010] In the mass production method of the perovskite precursor according to the present invention, the second metal halide is Pb 2+ , Sn 2+ , Bi 2+ , Ge 2+ , Mn 2+ and Cu 2+ It may contain one or more divalent metal cations selected from the group consisting of combinations of;
[0011] In the mass production method of a perovskite precursor according to the present invention, the organic halide may contain at least one monovalent cation selected from the group consisting of a combination of methylammonium and formamidinium.
[0012] In the mass production method of a perovskite precursor according to the present invention, the first metal halide is Li + ; Na + ; K + ; Rb + ; Cs + ; Fr + ; Cu(I) + ; Ag(I) + and Au(I) + It may contain one or more monovalent metal cations selected from the group consisting of combinations of .
[0013] In the mass production method of a perovskite precursor according to the present invention, collection of the perovskite crystal precursor in the step (S3) can be performed using a pressure reducing filter.
[0014] In the mass production method of a perovskite precursor according to the present invention, the concentration of the precursor solution in step (S1) may be 0.4 M or more.
[0015] In the mass production method of a perovskite precursor according to the present invention, the weight of the perovskite crystal precursor obtained in the step (S3) may be 85 parts by weight or more relative to 100 parts by weight of the mixture of solutes used in the step (S1).
[0016] In the mass production method of a perovskite precursor according to the present invention, the volume of the precursor solution may be 100 ml or more.
[0017] In the mass production method of a perovskite precursor according to the present invention, the stirring in step (S2) can be performed at a stirring speed of 100 to 500 RPM.
[0018] In the mass production method of a perovskite precursor according to the present invention, the peak of X-ray diffraction analysis of the perovskite crystal precursor can satisfy the following equation 1.
[0019] (Formula 1)
[0020] I2 / I1> 10
[0021] (In the above equation 1, I1 is the peak intensity at 2θ of 12.8±0.5°, and I2 is the peak intensity at 13.8±0.5°.)
[0022] The method for mass-producing a perovskite precursor according to the present invention has high industrial applicability due to the small amount of toxic solvent used, and can produce a large-capacity perovskite precursor at the kg level with high crystallinity at a high yield in a short time without heat treatment.
[0023] FIG. 1 is a drawing showing the X-ray diffraction peaks of perovskite crystal precursors according to Example 1 (chloroform), Example 2 (ethyl alcohol), Example 3 (isopropyl alcohol), Example 4 (ethyl acetate), Example 5 (diethyl ether), Comparative Example 1 (Boil), Comparative Example 2 (ethyl alcohol not stirred), and Comparative Example 3 (isopropyl alcohol not stirred) measured using X-ray diffraction (XRD).
[0024] The embodiments described herein may be modified in various different forms, and the technology according to one embodiment is not limited to the embodiments described below. In addition, the embodiments of one embodiment are provided to more completely explain the present disclosure to a person with average knowledge in the relevant technical field. In this case, unless there is a different definition for the technical and scientific terms used, they have the meaning commonly understood by a person with ordinary skill in the technical field to which this invention belongs, and in the following description and the attached drawings, descriptions of well-known functions and configurations that may unnecessarily obscure the gist of the present invention are omitted.
[0025] Additionally, the singular forms used in this specification and the appended claims are intended to include the plural forms as well, unless the context clearly dictates otherwise.
[0026] Additionally, in this specification and the appended claims, the terms first, second, etc. are not used in a limiting sense, but are used for the purpose of distinguishing one component from another.
[0027] Additionally, in this specification and the appended claims, when a part such as a film (layer), region or component is said to be located “on,” “above,” “upper,” “lower,” “lower” or “lower” another part, this includes not only cases where one part is in contact with another part, but also cases where another part exists between the two parts.
[0028] In addition, the terms “about,” “substantially,” and the like used in this specification and the appended claims are used in a meaning that is at or close to the numerical value when manufacturing and material tolerances inherent in the meanings stated are presented, and are used to prevent unscrupulous infringers from unfairly utilizing the disclosure in which exact or absolute values are mentioned in order to aid in the understanding of this specification and the appended claims.
[0029] Additionally, the numerical ranges used herein include lower and upper limits and all values within that range, increments logically derived from the shape and width of the defined range, all doubly defined values, and all possible combinations of upper and lower limits of numerical ranges defined in different shapes.
[0030] Furthermore, terms such as “include” or “have” in this specification and the appended claims mean that a feature or component described in the specification is present, and unless specifically limited, do not preclude the possibility that one or more other features or components may be added.
[0031] Hereinafter, a method for mass producing a perovskite precursor of the present invention will be described in detail.
[0032] The present invention provides a method for mass-producing a perovskite precursor, the method for mass-producing a perovskite precursor comprising: (S1) preparing a precursor solution by mixing at least one halide selected from the group consisting of a combination of a first metal halide and an organic halide; a second metal halide; and a first solvent; (S2) continuously stirring the precursor solution while adding a second solvent in a gaseous state; and (S3) obtaining a perovskite crystalline precursor precipitated from the precursor solution; wherein the first solvent is a good solvent for the halide and the second metal halide, and the second solvent is an antisolvent for the halide and the second metal halide.
[0033] The above perovskite refers to a crystal having a perovskite crystal structure, which may be a three-dimensional perovskite structure satisfying the chemical formula ABX3, or a two-dimensional planar perovskite structure satisfying the chemical formula A2BX4. In the chemical formula, A may be a monovalent organic or metal cation, B may be a divalent metal cation, and X may be I - , Br - , Cl - Or it may be a halogen anion which is a combination of these.
[0034] According to one embodiment, the precursor solution may contain a first metal halide and a second metal halide. For example, the first metal halide may be a metal halide including a monovalent metal cation. The monovalent metal cation may be Li. + ; Na + ; K + ; Rb + ; Cs + ; Fr + ; Cu(I) + ; Ag(I) + and Au(I) +It may be at least one selected from the group consisting of a combination of. In addition, the second metal halide may be a metal halide containing a divalent metal cation. The divalent metal cation is Pb 2+ , Sn 2+ , Bi 2+ , Ge 2+ , Mn 2+ and Cu 2+ It may be at least one selected from the group consisting of a combination of the first metal halide and the second metal halide. The first metal halide and the second metal halide may be dissolved together in a solvent and then crystallized to produce a perovskite crystal.
[0035] In addition, according to one embodiment, the precursor solution may contain a first organic halide and a second metal halide. For example, the first organic halide may contain one or more monovalent cations selected from the group consisting of a combination of a methylammonium-based monovalent cation and a formamidinium-based monovalent cation. In addition, it goes without saying that the second metal halide may include the above-described divalent metal cation.
[0036] As described above, the precursor solution may contain a halide containing a monovalent cation and a halide containing a divalent metal cation. The chemical species and metal ions contained in the first metal halide, the first organic halide, and the second metal halide contained in the precursor solution described above are described only to explain the present invention in detail, and the present invention is not limited thereto. Therefore, the first metal halide, the first organic halide, and the second metal halide may be any chemical species that can be dissolved in the precursor solution and then crystallized to form a perovskite crystal.
[0037] According to one embodiment, the concentration of the precursor solution in step (S1) may be 0.4 M or more. The perovskite crystal precursor is a process in which the halide and the second metal halide dissolved in the precursor solution come into contact with the second solvent, which is an antisolvent, and are crystallized. Therefore, the yield and crystallinity of the perovskite crystal precursor may vary depending on the concentration of the precursor solution. The concentration of the precursor solution may be 0.01 M or more, 0.1 M or more, 0.2 M or more, 0.3 M or more, or 0.4 M or more, and the upper limit may be 5 M or less, 4 M or less, 2 M or less, 1 M or less, or 0.8 M or less. Specifically, it may be 0.01 to 5 M, 0.1 to 4 M, 0.2 to 2 M, 0.3 to 1 M, or 0.4 to 0.8 M. When the precursor solution satisfies the above-described concentration range, the yield of the perovskite crystal precursor may be high, and a perovskite crystal precursor having a high crystallinity may be obtained.
[0038] According to one embodiment, the volume of the precursor solution may be 100 ml or more. The precursor solution may be selected to have a volume required for mass production of the perovskite crystal precursor. The volume of the precursor solution may be 50 ml or more, 100 ml or more, 200 ml or more, 500 ml or more, or 1,000 ml or more, and an upper limit may be 50,000 ml or less, 30,000 ml or less, 10,000 ml or less, 5,000 ml or less, or 2,000 ml or less. Specifically, the volume may be 50 to 50,000 ml, 100 to 30,000 ml, 200 to 10,000 ml, 500 to 5,000 ml, or 1,000 to 2,000 ml. The volume of the precursor solution can obtain a large amount of perovskite crystal precursor in one process within the above-described range. If the volume of the precursor solution is less than the above-described range, the yield of the perovskite crystal precursor may be low, and if it exceeds the above-described range, the yield of the perovskite crystal precursor may be reduced. Therefore, it may be advantageous to use a precursor solution having a volume within the above-described range.
[0039] The first solvent is advantageously a solvent that can easily dissolve the halide and the second metal halide. Accordingly, the solubility of each of the first metal halide, the first organic halide, or the second metal halide in the first solvent may be 5 parts by weight or more, 10 parts by weight or more, 20 parts by weight or more, or 30 parts by weight or more, based on 100 parts by weight of the first solvent at 25°C, and the upper limit may be 200 parts by weight or less, 150 parts by weight or less, 100 parts by weight or less, or 50 parts by weight or less. Specifically, the solubility may be 5 to 200 parts by weight, 10 to 150 parts by weight, 20 to 100 parts by weight, or 30 to 50 parts by weight. A solvent having the above-described solubility may be referred to as a good solvent, and when the first solvent has the above-described solubility, it may be advantageous for preparing the precursor solution by dissolving the first metal halide, the first organic halide, and the second metal halide. As a non-limiting example, the first solvent may be at least one solvent selected from the group consisting of a combination of 2-methoxyethanol (2-ME), dimethylformamide (DMF), and dimethyl sulfoxide (DMSO), but the present invention is not limited thereto, and the first solvent may be a good solvent having the above-described solubility range.
[0040] In addition, as described above, since the second solvent has low solubility in each of the halide and the second metal halide, it is advantageous if it is a solvent in which the halide and the organic halide contained in the precursor solution are crystallized when the precursor solution and the second solvent come into contact. The solubility of each of the first metal halide, the first organic halide, or the second metal halide in the second solvent may be 3 parts by weight or less, 1 part by weight or less, 0.5 parts by weight or less, or 0.1 part by weight or less, with respect to 100 parts by weight of the second solvent at 25°C, and the lower limit may be 0.001 part by weight or more. Specifically, it may be 0.001 to 3 parts by weight, 0.001 to 1 part by weight, 0.001 to 0.5 parts by weight, or 0.001 to 0.1 part by weight. A solvent having the above-described solubility can be called an anti-solvent.
[0041] According to one embodiment, the second solvent may be at least one solvent selected from the group consisting of a combination of chloroform, diethyl ether, ethyl acetate, ethyl alcohol, and isopropyl alcohol. The above-described solvent may be an antisolvent for each of the halide and the second metal halide, and thus may be advantageous in obtaining the perovskite crystal precursor, and may have a higher yield of the perovskite crystal precursor compared to other solvents.
[0042] The stirring in the above step (S2) refers to a process in which the precursor solution located inside the reactor is physically stirred and mixed. According to one embodiment, the stirring may be performed using any method used in the art for stirring, such as impeller stirring, propeller stirring, and magnetic stirring. The stirring can increase the speed of crystallization when the second solvent comes into contact with the precursor solution and the halide and second metal halide contained in the precursor solution are crystallized, and can prevent the formation of an undesired layer or undesired concentration. This can be advantageous in that it increases the yield and production speed of the perovskite crystal precursor.
[0043] According to one embodiment, the stirring in step (S2) may be performed at a stirring speed of 100 to 500 RPM (revolutions per minute). The stirring speed may be 100 RPM or more, 200 RPM or more, or 250 RPM or more, and an upper limit may be 2,000 RPM or less, 1,000 RPM or less, or 500 RPM or less. Specifically, it may be 100 to 2,000 RPM, 200 to 1,000 RPM, or 250 to 500 RPM. When the stirring in step (S2) is performed within the stirring speed described above using the above-described stirring method, the yield and reaction speed of the perovskite crystal precursor may be advantageously high.
[0044] As a non-limiting example, the above-described stirring method can be variously selected depending on process conditions such as the volume and viscosity of the precursor solution; and the shape of the reactor; and thus, the above-described stirring speed can be the rotation speed of the magnetic bar of the magnetic stirrer, and when using a stirring method other than the magnetic stirring, a stirring speed having the same force as the shear force due to the rotation of the magnetic bar can be selected.
[0045] According to one embodiment, the partial pressure of the second solvent in the gas phase of step (S2) may be 0.1 atm based on atmospheric pressure. Since the second solvent is an antisolvent of the halide and the second metal halide, the second solvent in the gas phase may contact the precursor solution and crystallization may occur from the surface of the precursor solution, thereby producing the perovskite crystal precursor. The step (S2) may be performed in a reactor under an atmospheric pressure of 1 atm, and the partial pressure of the second solvent in the gas phase may be 0.001 atm or more, 0.01 atm or more, 0.05 atm or more, or 0.1 atm or more based on atmospheric pressure, and an upper limit may be 0.99 atm or less, 0.9 atm or less, 0.5 atm or less, or 0.2 atm or less. Specifically, it can be 0.001 to 0.99 atm, 0.01 to 0.9 atm, 0.05 to 0.5 atm, or 0.1 to 0.2 atm. When the partial pressure of the second solvent in the gas phase satisfies the above-described range, the yield and yield speed of the perovskite crystal precursor can be advantageously increased. The partial pressure can be achieved by increasing the injection amount of the second solvent in the gas phase in a reactor of a certain size, reducing the size of the reactor, or performing stirring.
[0046] According to one embodiment, the weight of the perovskite crystal precursor obtained in the step (S3) may be 80 parts by weight or more relative to 100 parts by weight of the mixture of solutes used in the step (S1). The mixture of solutes used in the step (S1) refers to a mixture of one or more halides selected from the group consisting of a combination of a first metal halide and an organic halide; and a second metal halide. The yield of the perovskite crystal precursor, that is, the weight of the perovskite crystal precursor relative to 100 parts by weight of the mixture introduced in the step (S1), may be 50 parts by weight or more, 70 parts by weight or more, 80 parts by weight or more, or 85 parts by weight or more, and an upper limit may be 99 parts by weight or less, 98 parts by weight or less, 95 parts by weight or less, or 90 parts by weight or less. Specifically, it may be 50 to 99 parts by weight, 70 to 98 parts by weight, 80 to 95 parts by weight, or 85 to 90 parts by weight. As described above, the yield may vary depending on the concentration of the precursor solution, the chemical species of the second solvent, the partial pressure of the second solvent in the gas phase, etc., but it may be advantageous when the yield falls within the above-described range.
[0047] According to one embodiment, the collection of the perovskite crystal precursor in step (S3) may be performed using a vacuum filter. Since the perovskite crystal precursor in step (S3) may further include a first solvent and a second solvent, the first solvent and the second solvent may be filtered using a vacuum filter to obtain the perovskite crystal precursor. Of course, the perovskite crystal precursor obtained using the vacuum filter may further undergo a drying process to further remove impurities on the first solvent, the second solvent, and the precursor surface.
[0048] According to one embodiment, the X-ray diffraction peak of the perovskite crystal precursor can satisfy the following equation 1.
[0049] (Formula 1)
[0050] I2 / I1> 10
[0051] (In the above equation 1, I1 is the peak intensity at 2θ of 12.8±0.5°, and I2 is the peak intensity at 13.8±0.5°.)
[0052] In describing the above perovskite photoelectric device, the perovskite thin film, etc. includes the contents of the method for manufacturing a perovskite crystal precursor and the method for manufacturing a perovskite thin film described above, and therefore the perovskite photoelectric device according to the present invention includes all contents described above in the method for manufacturing a perovskite crystal precursor and the method for manufacturing a perovskite thin film.
[0053] Hereinafter, the perovskite photovoltaic device of the present invention will be described in more detail.
[0054] According to one embodiment, the peak intensity at 2θ of 12.8±0.5° refers to the lead iodide (PbI2) peak included in the perovskite thin film. The perovskite thin film may include a lead halide that has not been crystallized or a lead halide generated when perovskite is decomposed by an external environment, and the higher the lead iodide, i.e., the lead halide peak, the lower the crystallinity of the perovskite thin film.
[0055] In addition, the peak intensity at 2θ of 13.8±0.5° refers to the alpha-phase peak of the perovskite crystal included in the perovskite thin film. The alpha-phase peak is a hexagonal perovskite crystal, and the higher the alpha-phase peak, the higher the crystallinity of the perovskite crystal included in the perovskite thin film.
[0056] The ratio I2 / I1 of the I1 to the I2 may be 10 or more, 20 or more, 30 or more, 40 or more, or 50 or more, and may have an upper limit of 10,000 or less, 1,000 or less, 500 or less, 300 or less, or 100 or less. Specifically, it may be 10 to 10,000, 20 to 1,000, 30 to 500, 40 to 300, or 50 to 100. When the I2 / I1 satisfies the above-described range, more alpha-phase perovskite crystals may be included in the perovskite thin film, and the crystallinity of the perovskite thin film may increase, thereby significantly increasing device efficiency and stability. As a non-limiting example, it may be advantageous when the I1 peak is not detected.
[0057] According to one embodiment, the X-ray diffraction peak may further have a peak at 2θ of 11.8±0.5°. The peak intensity at 2θ of 11.8±0.5° refers to a delta phase (δ peak) of a perovskite crystal. The delta phase peak is a cubic non-perovskite crystal, and the alpha phase perovskite crystal may be converted to the delta phase when influenced by an external environment. As a non-limiting example, the X-ray diffraction peak of the perovskite crystal precursor may satisfy the following equation 1.
[0058] (Formula 2)
[0059] I2 / I3> 10
[0060] (In the above equation 2, I3 is the peak intensity at 2θ of 11.8±0.5°, and I2 is the peak intensity at 13.8±0.5°.)
[0061] The ratio I2 / I3 of the I3 to the I2 may be 10 or more, 20 or more, 30 or more, 40 or more, or 50 or more, and may have an upper limit of 10,000 or less, 1,000 or less, 500 or less, 300 or less, or 100 or less. Specifically, it may be 10 to 10,000, 20 to 1,000, 30 to 500, 40 to 300, or 50 to 100. When the I2 / I3 satisfies the above-described range, more alpha-phase perovskite crystals may be included in the perovskite thin film, and the crystallinity of the perovskite thin film may increase, thereby significantly increasing device efficiency and stability. As a non-limiting example, it may be advantageous when the I3 peak is not detected.
[0062] Hereinafter, specific examples and experimental examples will be described. However, the examples and experimental examples described below are only illustrative, and the technology described in this specification is not limited thereto.
[0063]
[0064] (Example 1)
[0065] A precursor solution was prepared by dissolving 3.36 g of formamidinium iodide (FAI) and 9 g of lead(II) iodide in 10 ml of 2-methoxyethanol (2ME). The precursor solution was loaded into a 70 ml vial and continuously stirred at 250 rpm using a magnetic stirrer.
[0066] The above vial was placed in a 100 ml beaker with the lid open, 25 ml of chloroform was added to the beaker, and the beaker was sealed. At this time, the partial pressure of the chloroform in the beaker was 0.1 atm. The stirring was continued for 8 hours at room temperature (25°C).
[0067] Thereafter, the perovskite crystals precipitated in the vial were filtered through a depressurizing filter to obtain a perovskite crystal precursor. The perovskite crystal precursor was heat-treated at 150°C for 10 minutes using a hot plate, and further heat-treated at 170°C for 10 minutes using a hot press to produce a perovskite crystal precursor.
[0068] 0.8 g of the above perovskite crystal precursor was dissolved in a mixed solvent of 0.8 ml of dimethylformamide (DMF) and 0.1 ml of dimethylsulfoxide (DMSO), and the solution was dropped onto a glass substrate, followed by spin coating at 500 rpm for 5 seconds, 1000 rpm for 8 seconds, and 5000 rpm for 60 seconds consecutively. When the spin coating was performed for 25 seconds, 1 ml of diethyl ether was dropped during the spin coating.
[0069] After the spin coating was completed, the glass substrate was heat-treated at 100°C for 40 minutes and then heat-treated at 150°C for 5 minutes to produce a perovskite thin film.
[0070]
[0071] (Example 2)
[0072] In Example 1, a perovskite crystal precursor and a perovskite thin film were manufactured in the same manner as in Example 1, except that 25 ml of ethyl alcohol was added to the beaker and the beaker was sealed.
[0073]
[0074] (Example 3)
[0075] In Example 1, a perovskite crystal precursor and a perovskite thin film were manufactured in the same manner as in Example 1, except that 25 ml of isopropyl alcohol was added to the beaker and the beaker was sealed.
[0076]
[0077] (Example 4)
[0078] In Example 1, a perovskite crystal precursor and a perovskite thin film were manufactured in the same manner as in Example 1, except that 25 ml of ethyl acetate was added to the beaker and the beaker was sealed.
[0079]
[0080] (Example 5)
[0081] In Example 1, a perovskite crystal precursor and a perovskite thin film were manufactured in the same manner as in Example 1, except that 25 ml of diethyl ether was added to the beaker and the beaker was sealed.
[0082]
[0083] (Example 6)
[0084] In Example 5, a perovskite crystal precursor and a perovskite thin film were prepared in the same manner as in Example 5, except that a precursor solution was prepared by dissolving 16.8 g of formamidinium iodide (FAI) and 45 g of lead(II) iodide in 50 ml of 2-methoxyethanol (2ME), the precursor solution was loaded into a 300 ml vial, the vial was placed in a 500 ml beaker with the lid open, and 125 ml of diethyl ether was placed in the beaker and then the beaker was sealed.
[0085]
[0086] (Example 7)
[0087] In Example 5, a perovskite crystal precursor and a perovskite thin film were manufactured in the same manner as in Example 5, except that a precursor solution was prepared by dissolving 168 g of formamidinium iodide (FAI) and 450 g of lead(II) iodide in 500 ml of 2-methoxyethanol (2ME), the precursor solution was loaded into a 3,000 ml vial, the vial was placed in a 5,000 ml beaker with the lid open, and 1,250 ml of diethyl ether was placed in the beaker and then the beaker was sealed.
[0088]
[0089] (Example 8)
[0090] In Example 5, a perovskite crystal precursor and a perovskite thin film were prepared in the same manner as in Example 5, except that the precursor solution was continuously stirred at 500 rpm.
[0091]
[0092] (Comparative Example 1)
[0093] A precursor solution was prepared by dissolving 3.36 g of formamidinium iodide (FAI) and 9 g of lead(II) iodide in 10 ml of 2-methoxyethanol (2ME).
[0094] After stirring the precursor solution for 30 minutes, the precursor solution was heated to 172°C for 10 minutes to prepare a crystalline precursor. Heating was stopped before all of the 2-methoxyethanol evaporated, the remaining 2-methoxyethanol was removed using a pipette, and 100 ml of ethyl alcohol was mixed with the crystalline precursor to remove impurities. Thereafter, the ethyl alcohol containing impurities was removed to obtain a crystalline precursor.
[0095] The above crystal precursor was filtered under reduced pressure to remove the 2-methoxyethanol and the ethyl alcohol, thereby obtaining a perovskite crystal precursor.
[0096] The perovskite crystal precursor (0.8 g) was dissolved in a mixed solvent of 0.8 ml of dimethylformamide (DMF) and 0.1 ml of dimethylsulfoxide (DMSO), and the solution was dropped onto a glass substrate, followed by spin coating at 500 rpm for 5 seconds, 1000 rpm for 8 seconds, and 5000 rpm for 60 seconds. When the spin coating was performed for 25 seconds, 1 ml of diethyl ether was dropped during the spin coating.
[0097] After the spin coating was completed, the glass substrate was heat-treated at 100°C for 40 minutes and then heat-treated at 150°C for 5 minutes to produce a perovskite thin film.
[0098]
[0099] (Comparative Example 2)
[0100] In Example 2, a perovskite crystal precursor and a perovskite thin film were prepared in the same manner as in Example 2, except that the stirring was not performed.
[0101]
[0102] (Comparative Example 3)
[0103] In Example 3, a perovskite crystal precursor and a perovskite thin film were prepared in the same manner as in Example 3, except that the stirring was not performed.
[0104]
[0105] (Comparative Example 4)
[0106] In Example 5, a perovskite crystal precursor and a perovskite thin film were prepared in the same manner as in Example 5, except that the stirring was not performed.
[0107]
[0108] (Comparative Example 5)
[0109] In Example 6, a perovskite crystal precursor and a perovskite thin film were prepared in the same manner as in Example 6, except that the stirring was not performed.
[0110]
[0111] (Comparative Example 6)
[0112] In Example 7, a perovskite crystal precursor and a perovskite thin film were prepared in the same manner as in Example 7, except that the stirring was not performed.
[0113] (Comparative Example 7)
[0114] In Example 5, a perovskite crystal precursor and a perovskite thin film were prepared in the same manner as in Example 5, except that the precursor solution was continuously stirred at 1,000 rpm.
[0115]
[0116] (Experimental Example 1) Yield according to nonsolvent during stirring
[0117] The yields of perovskite crystal precursors according to Examples 1, 2, 3, 4, 5, and Comparative Example 1 were measured. The yields were as shown in Table 1 below.
[0118] Yield (%) Example 195.6 Example 292.1 Example 389.7 Example 491.5 Example 590.7 Comparative Example 184.3
[0119] The yield of the perovskite crystal precursor prepared by the method of Example 1 was confirmed to be 95.6% due to the high partial pressure of chloroform in the beaker caused by the high volatility of chloroform.
[0120] (Experimental Example 2) Yield according to non-solvent in comparison group
[0121] In order to confirm the effect of stirring the precursor solution of the present invention, the yield of the perovskite crystal precursor manufactured by the method according to Example 2, Example 3, Comparative Example 1, Comparative Example 2, and Comparative Example 3 was measured. The yield was as shown in Table 2 below.
[0122] Yield (%) Example 292.1 Example 389.7 Comparative Example 184.3 Comparative Example 278.3 Comparative Example 384.1
[0123] It was confirmed that the manufacturing methods according to Example 2 (ethyl alcohol) and Example 3 (isopropyl alcohol) showed very low yields when stirring was not performed due to the low volatility of the ethyl alcohol and isopropyl alcohol.
[0124] (Experimental Example 3) Yield and reaction time according to solution volume
[0125] In order to confirm the effect of stirring the precursor solution of the present invention, the yield and reaction time of the perovskite crystal precursor according to Examples 5 to 8 and Comparative Examples 4 to 7 were measured. The yield and reaction time were as shown in Table 3 below.
[0126] Yield (%) Reaction time (hours, h) Example 5908 Comparative Example 48417 Example 68815 Comparative Example 58050 Example 78540 Comparative Example 655250
[0127] It was confirmed that the perovskite crystal precursors manufactured by the methods according to Comparative Examples 4 to 7 had a significantly reduced yield and a rapidly increased reaction time as the volume of the precursor solution increased. On the other hand, it was confirmed that the perovskite crystal precursors manufactured by the methods according to Examples 5 to 8 had a significantly shorter reaction time and a significantly increased yield compared to the methods according to Comparative Examples 4 to 7 even when the volume of the precursor solution increased due to the effect of the stirring described above.
[0128] (Experimental Example 4) Yield and reaction time according to stirring speed
[0129] The yields and reaction times of the perovskite crystal precursors according to Example 5, Example 8, Comparative Example 4, and Comparative Example 7 were measured. The yields and reaction times were as shown in Table 4 below.
[0130] Yield (%) Reaction time (hours, h) Example 5908 Example 8878 Comparative Example 48417 Comparative Example 78015
[0131] (Experimental Example 5) - XRD data analysis results according to non-solvent
[0132] Using X-ray diffraction (XRD), the X-ray diffraction peaks of the perovskite crystal precursors according to Example 1 (chloroform), Example 2 (ethyl alcohol), Example 3 (isopropyl alcohol), Example 4 (ethyl acetate), Example 5 (diethyl ether), Comparative Example 1 (Boil), Comparative Example 2 (ethyl alcohol not stirred), and Comparative Example 3 (isopropyl alcohol not stirred) were measured and shown in Fig. 1.
[0133] The peak at 2θ±0.5° corresponds to the residual lead iodide (PbI2) that has not been converted into a perovskite crystal. The larger the residual lead iodide peak, the lower the crystallinity of the perovskite crystal, and the lower the photoelectric conversion efficiency of the perovskite device.
[0134] In addition, the peak at 2θ±0.5° corresponds to the α phase of perovskite. Perovskite α phase is a perovskite with a cubic crystal structure, and the more α phase contained in perovskite, the higher the photoelectric conversion efficiency of the perovskite and the higher the stability from the external environment.
[0135] According to FIG. 1, it was found that the perovskite crystal precursor according to Example 1 had a high intensity and ratio of the peak at the 2θ±0.5° position. The intensity of the peak at the 2θ±0.5° position and the intensity of the peak at the 2θ±0.5° position were as shown in FIG. 1 and Table 5 below.
[0136] Thin film peak I1(au)I2(au)I2 / I1Example 57861491518.9Comparative example 19231032511.2Comparative example 48071104013.7
[0137] Although the present invention has been described in this specification with specific details and limited examples, these are provided only to help a more general understanding of the present invention, and the present invention is not limited to the above examples, and those skilled in the art to which the present invention pertains can make various modifications and variations based on these descriptions. Therefore, the ideas described in this specification should not be limited to the described examples, and all things that are equivalent or equivalent to the claims below, as well as the claims, are considered to fall within the scope of the ideas described in this specification.
Claims
1. (S1) A step of preparing a precursor solution by mixing at least one halide selected from the group consisting of a combination of a first metal halide and an organic halide; a second metal halide; and a first solvent; (S2) a step in which the precursor solution is continuously stirred and a second solvent in the gas phase is added; and (S3) a step of obtaining a precipitated perovskite crystal precursor from the precursor solution; comprising; The above first solvent is a good solvent of the above halide and the above second metal halide, A method for mass production of a perovskite precursor, wherein the second solvent is an anti-solvent of the halide and the second metal halide.
2. In paragraph 1, A method for mass production of a perovskite precursor, wherein the partial pressure of the second solvent in the gas phase of the above (S2) step is 0.1 atm or more based on atmospheric pressure.
3. In paragraph 1, A method for mass production of a perovskite precursor, wherein the second solvent is at least one solvent selected from the group consisting of a combination of chloroform, diethyl ether, ethyl acetate, ethyl alcohol, and isopropyl alcohol.
4. In paragraph 1, The above second metal halide is Pb 2+ , Sn 2+ , Bi 2+ , Ge 2+ , Mn 2+ and Cu 2+ A method for mass producing a perovskite precursor, comprising at least one divalent metal cation selected from the group consisting of a combination of; 5. In paragraph 1, A method for mass producing a perovskite precursor, wherein the organic halide contains at least one monovalent cation selected from the group consisting of a combination of methylammonium and formamidinium.
6. In paragraph 1, The above first metal halide is Li + ; Na + ; K + ; Rb + ; Cs + ; Fr + ; Cu(I) + ; Ag(I) + and Au(I) + A method for mass production of a perovskite precursor containing one or more monovalent metal cations selected from the group consisting of combinations of .
7. In paragraph 1, A method for mass production of a perovskite precursor, wherein collection of the perovskite crystal precursor in the above step (S3) is performed using a pressure reducing filter.
8. In paragraph 1, A method for mass production of a perovskite precursor, wherein the concentration of the precursor solution in the above (S1) step is 0.4 M or more.
9. In paragraph 1, A method for mass production of a perovskite precursor, wherein the weight of the perovskite crystal precursor obtained in the above step (S3) is 85 parts by weight or more relative to 100 parts by weight of the mixture of solutes used in the above step (S1).
10. In paragraph 9, A method for mass production of a perovskite precursor, wherein the volume of the precursor solution is 100 ml or more.
11. In paragraph 10, A method for mass production of a perovskite precursor, wherein the stirring in the above step (S2) is performed at a stirring speed of 100 to 500 RPM.
12. In paragraph 1, A method for mass production of a perovskite precursor, wherein the peak of the X-ray diffraction analysis of the above perovskite crystal precursor satisfies the following equation 1. (Formula 1) I2 / I1> 10 (In the above equation 1, I1 is the peak intensity at 2θ of 12.8±0.5°, and I2 is the peak intensity at 13.8±0.5°.)
Citation Information
Patent Citations
Precursor of inorganic / organic hybrid perovskite compound
KR1020180085833A
Display substrate, repair method of display substrate
KR1020210134268A
Door lock device
KR1020230025569A
Preparation method for perovskite nanoparticles and optoelectronic device comprising the perovskite nanoparticles manufactured thereby
KR102243623B1
Chlorine disinfectant constant temparature maintenance system
KR102388705B1