High-strength bridge steel and manufacturing method therefor

Through specific chemical composition and manufacturing process, the problems of low-temperature impact and welding performance of bridge steel are solved, high strength and high toughness are achieved, and the welding performance and market competitiveness of bridge steel are improved.

WO2024221568A1PCT designated stage expired Publication Date: 2024-10-31NANJING IRON & STEEL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/100370
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-26
Filing Date
2023-06-15
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

It is difficult to achieve a -40°C low-temperature impact energy of more than 120J while ensuring the strength of bridge steel with existing technology. It also takes into account the processing performance and welding performance of the steel plate, especially the production of extra-thick bridge steel.

Method used

Adopting specific chemical composition ratio and manufacturing process, including using boron element to replace Mo element, combining with Nb-Ti-B composite alloy, using magnesium metallurgy technology to improve welding performance, using two-stage rolling process and high-temperature tempering treatment to form a granular shape The metallographic structure of bainite + acicular ferrite improves the mechanical properties and welding performance of the steel plate.

Benefits of technology

The low-temperature impact absorption energy of high-strength bridge steel is more than 47J, and there are no obvious cracks on the 180-degree bending outer surface, which improves the use effect and market competitiveness of bridge steel, ensures high strength and high toughness performance, and improves welding performance. and reprocessing performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023100370_31102024_PF_FP_ABST
    Figure CN2023100370_31102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of steel production. Disclosed are high-strength bridge steel and a manufacturing method therefor. The chemical components, in percentage by mass, of the high-strength bridge steel are as follows: C: 0.04%-0.09%; Si: 0.10%-0.40%; Mn: 1.00%-1.40%; P≤0.015%; S≤0.003%; Nb: 0.010%-0.030%; V: 0.010%-0.030%; Ti: 0.008%-0.030%; Cr: 0.30%-0.50%; Ni: 0.30%-0.50%; Cu: 0.10%-0.30%; B: 0.0005%-0.0020%; Mg: 0.0008%-0.0015%; Al: 0.015%-0.030%; the remainder being Fe and inevitable impurities. An element Mo is replaced with a boron element; a method for using an Nb-Ti-B composite alloy is researched; the hardenability of a steel plate is improved by means of the precipitation hardening effect; the alloy design costs are reduced; the market competitiveness is improved.
Need to check novelty before this filing date? Find Prior Art

Description

High-strength bridge steel and manufacturing method thereof Technical Field

[0001] The present invention relates to the technical field of steel production, in particular to a high-strength bridge steel and a manufacturing method thereof. Background Art

[0002] With the rapid development of my country's economy, infrastructure construction has also been vigorously developed. Among them, the bridge industry is developing rapidly. With the continuous improvement of bridge quality, heavy load, high speed and large span have become the main development directions. The new generation of high-performance bridge steel that integrates high strength, high toughness, low yield ratio, easy welding and other properties is the preferred material for key components of large-span and heavy-load railway steel bridges. The demand is clear and urgent.

[0003] The continuous improvement of bridge quality requires a qualitative change in steel quality, especially for extra-thick bridge steel. It is extremely difficult to achieve a low-temperature impact strength of -40°C exceeding 120J while maintaining strength. At the same time, the processing and welding properties of the steel plate must also be taken into consideration. Therefore, the development of efficient and easy-to-weld bridge products is crucial to the company's future development.

[0004] Summary of the Invention

[0005] In view of the above technical problems, the present invention overcomes the shortcomings of the prior art and provides a high-strength bridge steel, whose chemical composition and mass percentage are as follows: C: 0.04%~0.09%, Si: 0.10%~0.40%, Mn: 1.00%~1.40%, P≤0.015%, S≤0.003%, Nb: 0.010%~0.030%, V: 0.010%~0.030%, Ti: 0.008%~0.030%, Cr: 0.30%~0.50%, Ni: 0.30%~0.50%, Cu: 0.10%~0.30%, B: 0.0005%~0.0020%, Mg: 0.0008%~0.0015%, Al: 0.015%~0.030%, and the balance is Fe and unavoidable impurities.

[0006] The technical solution further defined in the present invention is:

[0007] The chemical composition and mass percentage of the high-strength bridge steel mentioned above are as follows: C: 0.04%~0.07%, Si: 0.20%~0.40%, Mn: 1.20%~1.40%, P≤0.013%, S≤0.002%, Nb: 0.020%~0.030%, V: 0.020%~0.030%, Ti: 0.010%~0.030%, Cr: 0.40%~0.50%, Ni: 0.40%~0.50%, Cu: 0.20%~0.30%, B: 0.0010%~0.0020%, Mg: 0.0010%~0.0015%, Al: 0.020%~0.025%, and the remainder is Fe and unavoidable impurities.

[0008] The chemical composition and mass percentage of the high-strength bridge steel mentioned above are as follows: C: 0.05%~0.09%, Si: 0.10%~0.30%, Mn: 1.10%~1.30%, P≤0.014%, S≤0.003%, Nb: 0.015%~0.025%, V: 0.015%~0.025%, Ti: 0.010%~0.020%, Cr: 0.35%~0.45%, Ni: 0.35%~0.45%, Cu: 0.15%~0.25%, B: 0.0008%~0.0015%, Mg: 0.0009%~0.0013%, Al: 0.018%~0.028%, and the remainder is Fe and unavoidable impurities.

[0009] Another object of the present invention is to provide a method for manufacturing high-strength bridge steel, comprising the following steps:

[0010] S1. Boron, nickel and copper are smelted in a steelmaking furnace together with scrap steel. Aluminum is used for deoxidation of steel tapped from the steelmaking furnace and lime and refined slag are added to form slag.

[0011] S2, adopt LF+RH vacuum method for refining, after vacuum treatment, simmer in magnesium wire for treatment, and promote the floating removal of inclusions through static stirring;

[0012] S3, using a vertical bending continuous casting machine for casting, stretching 0.6-1.3m / min, superheat 10-30 degrees, using weak cooling mode for cooling, combined with dynamic soft reduction;

[0013] S4, after the billet is cooled, it is sent to the heating furnace for heating at a temperature of 1220±20 degrees and a heating time of 10 to 15 min / cm;

[0014] S5, adopt two-stage rolling process, the second rolling temperature is 800-900 degrees, the final rolling temperature is 770-870 degrees, the cooling temperature is 740-800 degrees, and the red-returning temperature is 400-600 degrees;

[0015] S6. The rolled steel plate is sent to heat treatment for tempering treatment, with a tempering temperature of 550 degrees, a heating rate of 2.3 hours, and a holding time of 30±10 minutes;

[0016] S7. After heat treatment, the steel plates are sampled, marked, inspected and put into storage.

[0017] In the above-mentioned method for manufacturing high-strength bridge steel, the thickness of the steel plate is 5 to 100 mm.

[0018] In the aforementioned method for manufacturing high-strength bridge steel, the metallographic structure of the steel plate is mainly granular bainite + acicular ferrite.

[0019] The aforementioned method for manufacturing high-strength bridge steel has a steel grade of Q420~Q690MPa, and the steel plate has the following properties: yield strength 410~690MPa, tensile strength 540~770MPa, elongation after fracture >14%, -40 degree impact absorption energy >47J, and no cracks visible to the naked eye on the outer surface when bent at 180 degrees.

[0020] The beneficial effects of the present invention are:

[0021] (1) The present invention uses boron to replace Mo, studies the use of Nb-Ti-B composite alloy, improves the hardenability of steel plates through precipitation strengthening, reduces alloy design costs, and improves market competitiveness;

[0022] (2) The present invention adopts magnesium metallurgy technology to improve the adverse effects of boron on welding performance, solve the harm of sulfide to steel plate performance, stabilize the mechanical properties of the product, and also improve the welding performance of the product and the use effect of bridge steel;

[0023] (3) The present invention adopts a two-stage rolling process. The rough rolling stage is carried out in the austenite region, which ensures that the boron element precipitates in the ferrite, forms BN and other complexes at the grain boundary interface, and is pinned around the grain boundary, slowing down the austenite recrystallization rate and grain growth size. At the same time, the precipitated elemental boron strengthens the organizational properties; the finishing rolling is carried out in the non-recrystallized austenite region, and the chromium, nickel, and boron elements improve the product hardenability, ensuring the stability of the mechanical properties of the high-strength bridge;

[0024] (4) The present invention adopts a high-temperature tempering process to solve the internal stress of the high-strength steel plate and improve the reprocessing performance of the product. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 is the metallographic structure of the steel plate. DETAILED DESCRIPTION

[0026] Example 1

[0027] The present embodiment provides a high-strength bridge steel, whose chemical composition and mass percentage are as follows: C: 0.06%, Si: 0.31%, Mn: 1.29%, P: 0.010%, S: 0.001%, Nb: 0.019%, V: 0.023%, Ti: 0.018%, Cr: 0.43%, Ni: 0.36%, Cu: 0.19%, B: 0.0013%, Mg: 0.0011%, Al: 0.022%, and the remainder is Fe and unavoidable impurities.

[0028] The manufacturing method comprises the following steps:

[0029] S1. Boron, nickel and copper are smelted in a steelmaking furnace together with scrap steel. Aluminum is used for deoxidation of steel tapped from the steelmaking furnace and lime and refined slag are added to form slag.

[0030] S2, adopt LF+RH vacuum method for refining, after vacuum treatment, simmer in magnesium wire for treatment, and promote the floating removal of inclusions through static stirring;

[0031] S3, using a vertical bending continuous casting machine for casting, stretching 0.65m / min, superheat 23 degrees, using weak cooling mode for cooling, combined with dynamic soft reduction;

[0032] S4, after the billet is cooled, it is sent to the heating furnace for heating at a temperature of 1230 degrees and a heating time of 13 min / cm;

[0033] S5, adopts two-stage rolling process, second rolling temperature is 810 degrees, final rolling temperature is 778 degrees, cooling temperature is 749 degrees, and returning to red temperature is 430 degrees;

[0034] S6. The rolled steel plate is sent to heat treatment for tempering treatment, with a tempering temperature of 550 degrees, a heating rate of 2.3 hours, and a holding time of 36 minutes;

[0035] S7. After heat treatment, the steel plates are sampled, marked, inspected and put into storage.

[0036] Example 2

[0037] The present embodiment provides a high-strength bridge steel, whose chemical composition and mass percentage are as follows: C: 0.05%, Si: 0.26%, Mn: 1.15%, P: 0.011%, S: 0.001%, Nb: 0.016%, V: 0.017%, Ti: 0.015%, Cr: 0.46%, Ni: 0.43%, Cu: 0.23%, B: 0.0017%, Mg: 0.0009%, Al: 0.022%, and the balance is Fe and unavoidable impurities.

[0038] The manufacturing method comprises the following steps:

[0039] S1. Boron, nickel and copper are smelted in a steelmaking furnace together with scrap steel. Aluminum is used for deoxidation of steel tapped from the steelmaking furnace and lime and refined slag are added to form slag.

[0040] S2, adopt LF+RH vacuum method for refining, after vacuum treatment, simmer in magnesium wire for treatment, and promote the floating removal of inclusions through static stirring;

[0041] S3, using a vertical bending continuous casting machine for casting, stretching 0.70m / min, superheat 19 degrees, using weak cooling mode for cooling, combined with dynamic soft reduction;

[0042] S4, after the billet is cooled, it is sent to the heating furnace for heating at a temperature of 1233 degrees and a heating time of 13 min / cm;

[0043] S5, adopts two-stage rolling process, second opening temperature is 836 degrees, final rolling temperature is 786 degrees, opening cooling temperature is 753 degrees, and returning to red temperature is 461 degrees;

[0044] S6. The rolled steel plate is sent to heat treatment for tempering treatment, with a tempering temperature of 550 degrees, a heating rate of 2.3 hours, and a holding time of 38 minutes;

[0045] S7. After heat treatment, the steel plates are sampled, marked, inspected and put into storage.

[0046] Example 3

[0047] The present embodiment provides a high-strength bridge steel, whose chemical composition and mass percentage are as follows: C: 0.06%, Si: 0.18%, Mn: 1.09%, P: 0.012%, S: 0.001%, Nb: 0.017%, V: 0.022%, Ti: 0.0190%, Cr: 0.44%, Ni: 0.38%, Cu: 0.17%, B: 0.0013%, Mg: 0.0011%, Al: 0.021%, and the balance is Fe and unavoidable impurities.

[0048] The manufacturing method comprises the following steps:

[0049] S1. Boron, nickel and copper are smelted in a steelmaking furnace together with scrap steel. Aluminum is used for deoxidation of steel tapped from the steelmaking furnace and lime and refined slag are added to form slag.

[0050] S2, adopt LF+RH vacuum method for refining, after vacuum treatment, simmer in magnesium wire for treatment, and promote the floating removal of inclusions through static stirring;

[0051] S3, using a vertical bending continuous casting machine for casting, stretching 0.85m / min, superheat 23 degrees, using weak cooling mode for cooling, combined with dynamic soft reduction;

[0052] S4, after the billet is cooled, it is sent to the heating furnace for heating at a temperature of 1217 degrees and a heating time of 12 min / cm;

[0053] S5, adopts two-stage rolling process, second rolling temperature is 868 degrees, final rolling temperature is 796 degrees, cooling temperature is 780 degrees, and returning to red temperature is 530 degrees;

[0054] S6. The rolled steel plate is sent to heat treatment for tempering treatment, with a tempering temperature of 550 degrees, a heating rate of 2.3 hours, and a holding time of 30±10 minutes;

[0055] S7. After heat treatment, the steel plates are sampled, marked, inspected and put into storage.

[0056] The properties of the steel plates of Examples 1, 2, and 3 are as follows:

[0057] In addition to the above embodiments, the present invention may also have other implementations. Any technical solution formed by equivalent replacement or equivalent transformation falls within the scope of protection required by the present invention.

Claims

1. A high-strength bridge steel, characterized in that: Its chemical composition and mass percentage are as follows: C: 0.04% ~ 0.09%, Si: 0.10% ~ 0.40%, Mn: 1.00% ~ 1.40%, P ≤ 0.015%, S ≤ 0.003%, Nb: 0.010% ~ 0.030%, V: 0.010% ~ 0.030%, Ti: 0.008% ~ 0.030%, Cr: 0.30% ~ 0.50%, Ni: 0.30% ~ 0.50%, Cu: 0.10% ~ 0.30%, B: 0.0005% ~ 0.0020%, Mg: 0.0008% ~ 0.0015%, Al: 0.015% ~ 0.030%, and the balance is Fe and unavoidable impurities.

2. The high-strength bridge steel according to claim 1, characterized in that: Its chemical composition and mass percentage are as follows: C: 0.04% ~ 0.07%, Si: 0.20% ~ 0.40%, Mn: 1.20% ~ 1.40%, P≤0.013%, S≤0.002%, Nb: 0.020% ~ 0.030%, V: 0.020% ~ 0.030%, Ti: 0.010% ~ 0.030%, Cr: 0.40% ~ 0.50%, Ni: 0.40% ~ 0.50%, Cu: 0.20% ~ 0.30%, B: 0.0010% ~ 0.0020%, Mg: 0.0010% ~ 0.0015%, Al: 0.020% ~ 0.025%, and the balance is Fe and unavoidable impurities.

3. The high-strength bridge steel according to claim 1, characterized in that: Its chemical composition and mass percentage are as follows: C: 0.05% ~ 0.09%, Si: 0.10% ~ 0.30%, Mn: 1.10% ~ 1.30%, P ≤ 0.014%, S ≤ 0.003%, Nb: 0.015% ~ 0.025%, V: 0.015% ~ 0.025%, Ti: 0.010% ~ 0.020%, Cr: 0.35% ~ 0.45%, Ni: 0.35% ~ 0.45%, Cu: 0.15% ~ 0.25%, B: 0.0008% ~ 0.0015%, Mg: 0.0009% ~ 0.0013%, Al: 0.018% ~ 0.028%, and the balance is Fe and unavoidable impurities.

4. A method for manufacturing high-strength bridge steel, characterized in that: Applicable to any one of claims 1 to 3, comprising the following steps: S1. The steelmaking furnace is used for smelting. Boron, nickel and copper are put into the furnace together with scrap steel for smelting. The steelmaking furnace uses aluminum deoxidation and adds lime and refined slag to make slag; S2, LF+RH vacuum refining is adopted, and after vacuum treatment, magnesium wire is put into the steel for treatment, and static stirring is used to promote the floating and removal of inclusions; S3, use vertical bending continuous casting machine for casting, stretching 0.6 ~ 1.3m / min, superheat 10 ~ 30 degrees, use weak cooling mode for cooling, and use dynamic soft pressure; S4, after the billet is cooled, it is sent to the heating furnace for heating, the heating temperature is 1220±20 degrees, and the heating time is 10~15min / cm; S5, adopt two-stage rolling process, the second rolling temperature is 800-900 degrees, the final rolling temperature is 770-870 degrees, the cooling temperature is 740-800 degrees, and the red-returning temperature is 400-600 degrees; S6. The rolled steel plate is sent to heat treatment for tempering, the tempering temperature is 550 degrees, the heating rate is 2.3h, and the holding time is 30±10min; S7. After heat treatment, the steel plates are sampled, marked, inspected and put into storage.

5. The method for manufacturing high-strength bridge steel according to claim 4, characterized in that: The thickness of the steel plate is 5 to 100 mm.

6. The method for manufacturing high-strength bridge steel according to claim 4, characterized in that: The metallographic structure of the steel plate is mainly granular bainite + acicular ferrite.

7. The method for manufacturing high-strength bridge steel according to claim 4, characterized in that: The steel grade is Q420~Q690MPa, and the properties of the steel plate are: yield strength 410~690MPa, tensile strength 540~770MPa, elongation after fracture>14%, -40 degree impact absorption energy>47J, and no cracks visible to the naked eye on the outer surface of 180 degree bending.

Citation Information

Patent Citations

  • 500MPa-grade weather-resistant bridge steel and manufacturing method thereof

    CN113025880A

  • 345MPa-grade weather-resistant bridge steel and manufacturing method thereof

    CN113046627A

  • 420 MPa-grade weather-proof bridge steel and manufacturing method thereof

    CN113046652A

  • Efficient welding bridge steel and manufacturing method thereof

    CN113234999A

  • Low-yield-ratio high-strength steel sheet excellent in toughness of welding-heat-affected part and its production method