Separator, and battery comprising same

By designing a ceramic layer, a heat-resistant polymer layer and a coating layer in the lithium-ion battery separator, the problem of potential safety hazards of lithium-ion batteries at high temperatures is solved, achieving both high safety performance and fast charging capabilities of the battery.

WO2024222501A1PCT designated stage expired Publication Date: 2024-10-31ZHUHAI COSMX BATTERY CO LTD

Patent Information

Application Number
PCT/CN2024/087717
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-26
Filing Date
2024-04-15
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Lithium-ion batteries have safety risks during use, especially the insufficient heat resistance of the separator at high temperatures, leading to the risk of thermal runaway, fire or explosion, and it is difficult to balance fast charging capabilities and safety performance.

Method used

Design a diaphragm, including a ceramic layer, a heat-resistant polymer layer and a coating layer. The ceramic layer is composed of ceramic powder, binder and polymer microspheres. The heat-resistant polymer layer is composed of heat-resistant polymer. The coating layer It is composed of glue-coated polymers. The thickness of the ceramic layer is 1 μm to 10 μm. The ceramic powder is selected from a variety of ceramic powders. The particle size distribution of the binder and polymer microspheres is optimized to improve the heat shrinkage performance and safety of the separator.

Benefits of technology

It effectively improves the heat shrinkage performance and safety performance of the separator, and reduces the risk of short circuit and thermal runaway of the battery at high temperatures. The closing temperature of the separator is between 90°C and 130°C, and the membrane rupture temperature is greater than 230°C, ensuring that the battery can survive in high temperature environments. Safety and fast charging performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCTCN2024087717-FTAPPB-I100001
    Figure PCTCN2024087717-FTAPPB-I100001
  • Figure PCTCN2024087717-FTAPPB-I100002
    Figure PCTCN2024087717-FTAPPB-I100002
  • Figure PCTCN2024087717-FTAPPB-I100003
    Figure PCTCN2024087717-FTAPPB-I100003
Patent Text Reader

Abstract

Provided in the present disclosure are a separator and a battery comprising same. Polymer microspheres having a melting point ranging from 90℃ to 130℃ are added into a ceramic layer, such that pores in a separator are closed below 130℃, so as to stop the shuttling of lithium ions between positive and negative electrodes inside a battery, thereby achieving the aim of improving the safety. Moreover, the surface of the ceramic layer is coated with a heat-resistant polymer layer, such that it is ensured that the separator is not broken at a high temperature, thereby improving the separation effect of the separator at a high temperature and improving the safety performance of the battery. A negative active substance with a surface being coated with amorphous carbon is further applied, and the negative active substance can significantly improve the quick-charging performance of the battery, such that the prepared battery can achieve both the quick-charging performance and the safety performance.
Need to check novelty before this filing date? Find Prior Art

Description

A diaphragm and a battery comprising the same Technical Field

[0001] The present disclosure belongs to the technical field of secondary batteries, and particularly relates to a separator and a battery including the separator. Background Art

[0002] In recent years, lithium-ion batteries have been widely used in smartphones, tablets, smart wearables, power tools, and electric vehicles. With the widespread use of lithium-ion batteries, consumers' demands for their service life and application environment are constantly increasing. This requires lithium-ion batteries to have both high fast charging performance and good safety performance.

[0003] Currently, lithium-ion batteries present safety risks during use. For example, when the battery temperature rises to a certain level, the internal temperature can run away, which can easily lead to serious safety accidents, fires, or even explosions. The main causes of thermal runaway are, on the one hand, insufficient heat resistance of the separator, which causes it to shrink or even rupture at high temperatures, failing to isolate the positive and negative electrodes of the battery; on the other hand, the high temperature at which the separator closes its pores prevents it from closing before thermal runaway occurs, preventing it from blocking the ion channels within the battery in a timely manner.

[0004] Given this situation, there is an urgent need to develop lithium-ion batteries with high safety. For example, this can be achieved by coating the separator with a heat-resistant layer. However, coating the separator with a heat-resistant layer often only improves the separator's thermal shrinkage performance and cannot completely solve the battery safety problem. Therefore, developing lithium-ion batteries with excellent fast charging capabilities and high safety is currently a top priority.

[0005] Summary of the Invention

[0006] The purpose of the present disclosure is to solve the problems of safety hazards in the use of existing lithium-ion batteries and the inability to balance the fast charging capability and safety performance of the battery. A diaphragm and a battery including the diaphragm are provided, and the battery has excellent fast charging capability and high safety performance.

[0007] To achieve the above objectives, the present disclosure adopts the following technical solutions:

[0008] A diaphragm, comprising a diaphragm substrate, a ceramic layer, a heat-resistant polymer layer, and a coating layer; the ceramic layer is disposed on at least one surface of the diaphragm substrate, the heat-resistant polymer layer is disposed on a surface of the ceramic layer away from the substrate, and the coating layer is disposed on a surface of the heat-resistant polymer layer away from the substrate;

[0009] The ceramic layer comprises ceramic powder, a binder and polymer microspheres; the heat-resistant polymer layer comprises a heat-resistant polymer; and the adhesive layer comprises an adhesive polymer.

[0010] The present disclosure improves the thermal shrinkage performance of the battery separator by rationally designing the composition of the ceramic layer, heat-resistant polymer layer and adhesive layer in the battery separator, so that the separator can still play the role of isolating the positive and negative electrodes at high temperatures; it can also avoid the separator's closed-pore temperature being too high, so that the separator can be closed in time before thermal runaway, and the ion channels inside the battery can be blocked in time, thereby effectively improving the safety performance of the battery.

[0011] According to an embodiment of the present disclosure, the closed-pore temperature of the diaphragm is 90°C to 130°C, for example, 90°C, 100°C, 110°C, 120°C or 130°C. The closed-pore temperature refers to the temperature at which the micropores inside the diaphragm close. When the closed-pore temperature of the diaphragm is within the above range, the closed-pore temperature of the diaphragm is kept at a lower range, making it easier to close the diaphragm more quickly and timely when the thermal runaway temperature rises, thereby more promptly blocking the ion channels inside the battery, thereby further improving the safety performance of the battery and more effectively reducing the safety hazards of lithium-ion batteries during use.

[0012] According to an embodiment of the present disclosure, the rupture temperature of the diaphragm is greater than or equal to 230°C, for example, 230°C, 240°C, 250°C, 260°C, 270°C, 280°C, 290°C, 300°C, 310°C, 320°C, 330°C, 340°C or 350°C. The rupture temperature refers to the temperature at which the diaphragm with blocked pores ruptures (breaks) after the temperature rises further after the diaphragm is closed, that is, the temperature at which the appearance of the diaphragm is damaged. The high rupture temperature of the diaphragm enables the battery to still work normally in a high temperature environment, reduces the risk of thermal runaway or short circuit of the battery at high temperatures, and improves the safety of the battery.

[0013] According to an embodiment of the present disclosure, the thickness of the ceramic layer is 1 μm to 10 μm, for example, 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, or 10 μm. When the thickness of the ceramic layer is within the above range, the mechanical strength and thermal shrinkage performance of the separator can be improved, thereby reducing the risk of short circuit or thermal runaway of the battery.

[0014] According to an embodiment of the present disclosure, the ceramic powder is selected from at least one of aluminum oxide, boehmite, magnesium oxide, magnesium hydroxide, barium sulfate, barium titanate, zinc oxide, calcium oxide, silicon dioxide, silicon carbide, and nickel oxide. These various types of ceramic powder have excellent thermal and chemical stability, which can improve the heat resistance and mechanical strength of the separator, thereby enhancing battery safety.

[0015] According to an embodiment of the present disclosure, the Dv50 of the ceramic powder is 0.5 μm-5 μm. The Dv50 of the ceramic powder is tested for particle size distribution using a Malvern laser particle size analyzer.

[0016] According to an embodiment of the present disclosure, the binder is selected from at least one of polytetrafluoroethylene, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polyimide, polyacrylonitrile, polymethyl (meth)acrylate, aramid resin, poly(meth)acrylic acid, styrene-butadiene rubber (SBR), polyvinyl alcohol, polyvinyl acetate, carboxymethyl cellulose (CMC), sodium carboxymethyl cellulose (CMC-Na), and carboxyethyl cellulose. The role of the binder in the diaphragm is to bond the ceramic powder and polymer microspheres together to form a strong ceramic layer. The above-mentioned binder has good bonding properties, which can enhance the stability and durability of the ceramic layer and improve the heat resistance and mechanical strength of the diaphragm.

[0017] According to an embodiment of the present disclosure, the polymer microspheres are made of at least one material selected from polyethylene, polymethacrylic acid, polymethacrylate, polypropylene, and polyvinylidene fluoride, and have a melting point of 90°C to 130°C.

[0018] According to an embodiment of the present disclosure, the molecular weight of the polymer microspheres is 50,000 to 500,000, for example, 50,000, 100,000, 150,000, 200,000, 250,000, 300,000, 350,000, 400,000, 450,000, or 500,000. When the molecular weight of the polymer microspheres is within the above range, they have a better melting effect.

[0019] According to an embodiment of the present disclosure, the polymer microspheres have a Dv50 of 0.1 μm to 10 μm (e.g., 0.1 μm, 0.2 μm, 0.5 μm, 0.8 μm, 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, or 10 μm). When the Dv50 of the polymer microspheres is within the above range, they have a relatively good dispersion effect in the ceramic layer.

[0020] According to an embodiment of the present disclosure, the melting point of the polymer microspheres is 90°C to 130°C (e.g., 90°C, 100°C, 110°C, 120°C, or 130°C). The same polymer microspheres can have different melting points, for example, polyethylene polymer microspheres have melting points of 120°C, 124°C, and 128°C. When the melting point of the polymer microspheres is within the above range, the closed-pore temperature of the separator can be lowered, thereby maintaining the closed-pore temperature of the separator in a lower range, thereby improving the safety performance of the battery.

[0021] According to an embodiment of the present disclosure, in the ceramic layer, the mass percentage of ceramic powder is 50% to 80% (such as 50%, 55%, 60%, 65%, 70%, 75%, 80%), the mass percentage of binder is 5% to 40% (such as 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%), and the mass percentage of polymer microspheres is 10% to 45% (10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%). In the ceramic layer, when the mass percentage of each component is within the above range, the separator can have good heat resistance and mechanical strength, as well as a lower closed-cell temperature, further improving the safety performance of the battery.

[0022] According to an embodiment of the present disclosure, the thickness of the heat-resistant polymer layer is 1 μm to 10 μm, for example, 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, or 10 μm. When the thickness of the heat-resistant polymer layer is within the above range, the heat-resistant polymer layer can better play its role, improve the heat resistance of the separator, enable the separator to have a higher rupture temperature, improve the separator's barrier effect at high temperatures, and thus improve the safety of the battery.

[0023] According to an embodiment of the present disclosure, the heat-resistant polymer is made of at least one material selected from aramid, polyimide, polyurethane, chlorophosphazene polymer, boron nitrogen polymer, polysulfone, and polybenzimidazole. These heat-resistant polymers have excellent heat resistance, chemical resistance, and mechanical strength, and can maintain stability at high temperatures, thereby improving the heat resistance of the separator and making it less susceptible to deformation at high temperatures, thereby enhancing the safety of the battery.

[0024] According to an embodiment of the present disclosure, the thickness of the adhesive layer is 1 μm to 10 μm, for example, 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, or 10 μm. When the thickness of the adhesive layer is within the above range, both battery energy density and good bonding effect can be taken into account.

[0025] According to an embodiment of the present disclosure, the coating polymer is made of at least one material selected from polytetrafluoroethylene, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene modified and copolymers thereof, polyimide, polyacrylonitrile, polymethyl methacrylate, and polyacrylic acid. The coating polymer made of the above materials has excellent chemical solvent resistance and good bonding properties.

[0026] According to an embodiment of the present disclosure, the solvent used to prepare the ceramic layer, the heat-resistant polymer layer and the adhesive layer is selected from at least one of acetone, tetrahydrofuran, dichloromethane, chloroform, dimethylformamide, N,N-dimethylacetamide (DMAc), N-methyl-2-pyrrolidone, cyclohexane, methanol, ethanol, isopropanol and water.

[0027] The present disclosure also provides a battery, comprising the above-mentioned separator.

[0028] According to an embodiment of the present disclosure, the battery includes a positive electrode sheet, a negative electrode sheet, a separator disposed between the positive electrode sheet and the negative electrode sheet, and a non-aqueous electrolyte.

[0029] According to an embodiment of the present disclosure, the battery is a high-safety lithium-ion battery with excellent fast charging capability.

[0030] According to an embodiment of the present disclosure, the positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer coated on one or both sides of the positive electrode current collector, wherein the positive electrode active material layer includes a positive electrode active material, a conductive agent, and a binder. The binder may include at least one of polyvinylidene fluoride (PVDF), hexafluoroethylene, polytetrafluoroethylene, methacrylate, and styrene-butadiene rubber. The binder may include at least one of polyvinylidene fluoride (PVDF), hexafluoroethylene, polytetrafluoroethylene, methacrylate, and styrene-butadiene rubber.

[0031] According to the embodiment of the present disclosure, the positive electrode active material is selected from lithium cobalt oxide or lithium cobalt oxide doped with two or more elements selected from Al, Mg, Mn, Cr, Ti, and Zr. The chemical formula of the lithium cobalt oxide doped with two or more elements selected from Al, Mg, Mn, Cr, Ti, and Zr is Li x Co1-y1-y2-y3-y4A y1 B y2 C y3 D y4 O2; 0.95≤x≤1.05, 0.01≤y1≤0.1, 0.01≤y2≤0.1, 0≤y3≤0.1, 0≤y4≤0.1, A, B, C, D are two or more elements selected from Al, Mg, Mn, Cr, Ti, Zr.

[0032] According to an embodiment of the present disclosure, the negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer coated on one or both sides of the negative electrode current collector, the negative electrode active material layer includes a negative electrode active material, a conductive agent and a binder; the surface of the negative electrode active material is coated with amorphous carbon.

[0033] According to an embodiment of the present disclosure, the negative electrode active material is selected from at least one of graphite coated with amorphous carbon, a composite material of graphite coated with amorphous carbon and silicon oxide, and a composite material of graphite coated with amorphous carbon and nano-silicon. The amorphous carbon coating can increase the conductivity of the negative electrode active material, improve the electronic conductivity of the electrode, reduce the internal resistance of the electrode during rapid charge and discharge, and thus enhance the fast-charging performance of the battery.

[0034] The composite material of graphite coated with amorphous carbon and silicon oxide has a silicon oxide content of 1 wt% to 15 wt%, for example, 1 wt%, 2 wt%, 4 wt%, 5 wt%, 6 wt%, 8 wt%, 12 wt%, and 15 wt%. When the silicon oxide content is within this range, the battery has advantages such as high energy density, fast charging, and excellent battery cycle performance.

[0035] In a composite material of graphite coated with amorphous carbon and nano-silicon, the nano-silicon content is 1wt% to 15wt%, for example, 1wt%, 2wt%, 4wt%, 5wt%, 6wt%, 8wt%, 12wt%, and 15wt%. When the nano-silicon content is within this range, the battery exhibits high energy density, fast charging, and excellent cycle performance.

[0036] Beneficial effects of the present disclosure:

[0037] (1) The diaphragm provided by the present invention, by rationally designing the composition of the ceramic layer, the heat-resistant polymer layer and the adhesive layer in the battery diaphragm, and coating a heat-resistant polymer layer on the surface of the ceramic layer, ensures that the diaphragm will not rupture at high temperatures, improves the barrier effect of the diaphragm at high temperatures, and enhances the safety performance of the battery, which can effectively improve the safety performance of the battery.

[0038] (2) Furthermore, the diaphragm provided by the present disclosure achieves closed pores before 130°C by adding polymer microspheres with a melting point between 90°C and 130°C in the ceramic layer, thereby isolating the lithium ions from shuttling between the positive and negative electrodes inside the battery, thereby achieving the purpose of improving battery safety.

[0039] (3) Furthermore, the diaphragm provided by the present disclosure is combined with a graphite containing amorphous carbon coated on the surface as a negative electrode active material. The negative electrode active material can significantly improve the fast charging performance of the battery, so that the prepared battery can take into account both fast charging performance and safety performance. DETAILED DESCRIPTION

[0040] The present disclosure will be further described in detail below with reference to specific embodiments. It should be understood that the following embodiments are merely illustrative and explanations of the present disclosure and should not be construed as limiting the scope of protection of the present disclosure. All technologies implemented based on the above content of the present disclosure are included within the scope of protection intended by the present disclosure.

[0041] Unless otherwise specified, the experimental methods used in the following examples are conventional methods; the reagents, materials, etc. used in the following examples are all commercially available unless otherwise specified.

[0042] Comparative Examples 1-4 and Examples 1-9

[0043] The lithium-ion batteries of Comparative Examples 1-4 and Examples 1-9 were all prepared according to the following preparation method, with the only difference being the selection of the separator and the negative electrode. The specific differences are shown in Table 1.

[0044] (1) Preparation of positive electrode sheet

[0045] The positive electrode active material LiCoO2, the binder polyvinylidene fluoride (PVDF), and the conductive agent acetylene black are mixed in a weight ratio of 97:1.0:2.0, and N-methylpyrrolidone (NMP) is added and stirred under the action of a vacuum mixer until the mixed system becomes a positive electrode slurry with uniform fluidity; the positive electrode slurry is evenly coated on an aluminum foil with a thickness of 10 μm; the coated aluminum foil is baked in an oven with 5 different temperature gradients, and then dried in an oven at 120°C for 8 hours, and then rolled and cut to obtain the required positive electrode sheet.

[0046] (2) Preparation of negative electrode sheet

[0047] A slurry consisting of 96% artificial graphite negative electrode material, 0.2% single-walled carbon nanotube (SWCNT) conductive agent, 1.0% conductive carbon black (SP) conductive agent, 1% sodium carboxymethyl cellulose (CMC) binder, and 1.8% styrene-butadiene rubber (SBR) binder was prepared using a wet process. The slurry was then applied to the surface of the negative electrode current collector copper foil. The negative electrode sheet was then dried (temperature: 85°C, time: 5 hours), rolled, and die-cut. The artificial graphite negative electrode material was specifically selected from artificial graphite 1 and artificial graphite 2. Artificial graphite 1 was purchased from commercial sources and had no surface coating. Artificial graphite 2 was purchased from commercial sources and had a layer of amorphous carbon coated on its surface. See Table 1 for details.

[0048] (3) Preparation of non-aqueous electrolyte

[0049] In an argon-filled glove box (moisture <10 ppm, oxygen <1 ppm), ethylene carbonate (EC), propylene carbonate (PC), and propyl propionate (PP) were mixed in a mass ratio of 2:1.5:2. 14 wt.% of LiPF6 based on the total mass of the non-aqueous electrolyte was slowly added to the mixed solution and stirred to obtain a non-aqueous electrolyte.

[0050] (4) Preparation of diaphragm

[0051] The polymer microspheres, alumina, polymethacrylic acid and water were mixed and recorded as solution T; the heat-resistant polymer and DMAc solvent were mixed and recorded as solution N; the coating polymer and DMAc solution were mixed and recorded as solution P;

[0052] Solution T was coated on both sides of a 5 μm thick diaphragm substrate PE by a gravure roller coating method, and after drying, a diaphragm with a 2 μm thick ceramic layer on each side was obtained, which was recorded as diaphragm TP; solution N was coated on both sides of the diaphragm TP by a gravure roller coating method, and after drying, a diaphragm with a 2 μm thick ceramic layer on each side and a 2 μm thick heat-resistant polymer layer was obtained, which was recorded as diaphragm NP; solution P was coated on both sides of the diaphragm NP by a gravure roller coating method, and after drying, a diaphragm with a 2 μm thick ceramic layer on each side, a 2 μm thick heat-resistant polymer layer and a 1 μm thick rubber coating layer was obtained.

[0053] The types of polymer microspheres in the ceramic layer, the ratio of polymer microspheres, the melting point of the polymer, the type of heat-resistant polymer and the type of the coating polymer are shown in Table 1.

[0054] (5) Preparation of lithium-ion batteries

[0055] The positive electrode sheet, separator and negative electrode sheet prepared above are wound to obtain a bare cell without liquid injection; the bare cell is placed in an outer packaging foil, and the prepared electrolyte is injected into the dried bare cell. After vacuum packaging, standing, formation, shaping, sorting and other processes, the required lithium-ion battery is obtained.

[0056] The electrochemical performance of the batteries obtained in the above comparative examples and examples was tested, and the relevant descriptions are as follows:

[0057] 1) 25°C cycle test: The batteries obtained in the above examples and comparative examples were placed in a (25±2)°C environment and allowed to stand for 2-3 hours. When the battery body reached (25±2)°C, the battery was charged at a 3C constant current with a cutoff current of 0.05C. After the battery was fully charged, it was left for 5 minutes and then discharged at a 3C constant current to a cutoff voltage of 3.0V. The highest discharge capacity of the first three cycles was recorded as the initial capacity Q. When the cycle reached 1000 times, the last discharge capacity Q of the battery was recorded. The recorded results are shown in Table 3.

[0058] The calculation formula used is as follows: Capacity retention rate (%) = Q1 / Q×100%;

[0059] 2) 150°C thermal shock test: The batteries obtained in the above examples and comparative examples were heated using convection or a circulating hot air oven at a starting temperature of (25±3)°C at a temperature ramp rate of (5±2)°C / min. The temperature was raised to (150±2)°C and maintained for 60 min before the test was terminated. The battery status results were recorded as shown in Table 3.

[0060] 3) Closed cell test:

[0061] The membranes obtained in the above examples and comparative examples were baked at a certain temperature for 10 minutes. The air permeability of the membranes before and after baking was measured. If the air permeability increased 10-fold before and after baking, the membrane was considered to be starting to close, 100-fold before and after baking, the membrane was considered to be substantially closed, and 1000-fold before and after baking, the membrane was considered to be completely closed. The baking temperature corresponding to the complete closure of the membrane was recorded as the membrane's closed temperature.

[0062] 4) Membrane rupture test:

[0063] The membranes obtained from the above examples and comparative examples were subjected to thermomechanical analysis (TMA) testing. The samples were cut into 4 mm wide and 8 mm long samples and tested at a heating rate of 5°C / min and an applied force of 0.01 N. The temperature at which the membrane was broken was recorded as the membrane rupture temperature.

[0064] Table 1 Composition of the batteries of Comparative Examples 1-4 and Examples 1-9

[0065] Example 10 Group

[0066] The same procedure was carried out as in Example 1, except that the negative electrode active material was different:

[0067] Example 10a: The composite material of graphite coated with amorphous carbon and silicon oxide was replaced with equal amounts of artificial graphite 2, with the content of silicon oxide being 10 wt %;

[0068] Example 10b: The composite material of graphite with amorphous carbon coating on the surface and nano-silicon was used in equal amounts to replace the artificial graphite 2, and the content of nano-silicon was 5 wt%.

[0069] Table 2 Diaphragm performance test data results of Comparative Examples 1-4 and Examples 1-9

[0070] Table 3 Performance test results of batteries of Comparative Examples 1-4 and Examples 1-9

[0071] By comparing Comparative Example 1 and Comparative Example 2, it can be found that when the conventional diaphragm and artificial graphite 1 are assembled, the battery obtained can pass the furnace temperature test, but the fast charging capability of the battery is greatly reduced. After the battery has been cycled 1000 times, the battery has no capacity, indicating that it cannot meet 1000 cycles; the fast charging capability of the battery obtained after the conventional diaphragm and artificial graphite 2 are assembled is significantly improved. After the battery has been cycled 1000 times, the capacity retention rate can reach 74.65%, but the safety performance of the battery is greatly reduced and cannot pass the furnace temperature test. This also shows that the introduction of a fast-charging negative electrode can deteriorate the safety performance of the battery. By comparing Comparative Examples 2-4 with Example 1, it is found that the safety performance of the battery of the present application can be significantly improved while taking into account the fast charging capability of the battery, thereby obtaining a battery that can take into account both battery safety performance and rate performance.

[0072] By comparing Examples 1 to 8, it is found that by adjusting the composition of the ceramic layer, heat-resistant polymer layer and rubber coating layer of the diaphragm within a reasonable range, a battery that can take into account both battery safety performance and rate performance can be obtained. By comparing Example 1 and Example 9, it is found that when the diaphragm of the present application and artificial graphite 2 are assembled, the safety performance of the battery obtained can be significantly improved while maintaining the fast charging capability of the battery. This shows that the use of the diaphragm of the present application can avoid the adverse effects of the fast-charging negative electrode on the safety performance of the battery.

[0073] In summary, it can be seen from the comparative examples and embodiments that the lithium-ion battery assembled with the diaphragm disclosed in the present invention can effectively improve the battery's fast-charging cycle life while taking into account the battery's safety performance.

[0074] The above describes the embodiments of the present disclosure. However, the present disclosure is not limited to the above embodiments. Any modifications, equivalent replacements, improvements, etc. made within the spirit and principles of the present disclosure shall be included in the scope of protection of the present disclosure.

Claims

1. A diaphragm, characterized in that: The diaphragm comprises a diaphragm substrate, a ceramic layer, a heat-resistant polymer layer and a coating layer; the ceramic layer is arranged on at least one side surface of the diaphragm substrate, the heat-resistant polymer layer is arranged on the surface of the ceramic layer away from the substrate, and the coating layer is arranged on the surface of the heat-resistant polymer layer away from the substrate; The ceramic layer comprises ceramic powder, a binder and polymer microspheres; the heat-resistant polymer layer comprises a heat-resistant polymer; and the adhesive layer comprises an adhesive polymer.

2. The diaphragm according to claim 1, characterized in that The diaphragm has a closed cell temperature of 90°C to 130°C.

3. The diaphragm according to claim 1 or 2, characterized in that: The rupture temperature of the diaphragm is greater than or equal to 230°C.

4. The diaphragm according to any one of claims 1 to 3, characterized in that: In the ceramic layer, the mass percentage of ceramic powder is 50% to 80%, the mass percentage of binder is 5% to 40%, and the mass percentage of polymer microspheres is 10% to 45%.

5. The diaphragm according to any one of claims 1 to 4, characterized in that: The thickness of the ceramic layer is 1 μm to 10 μm.

6. The diaphragm according to any one of claims 1 to 5, characterized in that: The ceramic powder is selected from at least one of aluminum oxide, boehmite, magnesium oxide, magnesium hydroxide, barium sulfate, barium titanate, zinc oxide, calcium oxide, silicon dioxide, silicon carbide, and nickel oxide; And / or, the material of the polymer microspheres is selected from at least one of polyethylene, polymethacrylic acid, polymethacrylate, polypropylene, and polyvinylidene fluoride; And / or, the binder is selected from at least one of polytetrafluoroethylene, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polyimide, polyacrylonitrile, polymethyl (meth)acrylate, aramid resin, poly (meth)acrylic acid, styrene-butadiene rubber, polyvinyl alcohol, polyvinyl acetate, carboxymethyl cellulose, sodium carboxymethyl cellulose, and carboxyethyl cellulose.

7. The diaphragm according to any one of claims 1 to 6, characterized in that: The molecular weight of the polymer microspheres is 50,000 to 500,000; and / or, the Dv50 of the polymer microspheres is 0.1 μm to 10 μm; And / or, the melting point of the polymer microspheres is 90°C to 130°C.

8. The diaphragm according to any one of claims 1 to 7, characterized in that: The thickness of the heat-resistant polymer layer is 1 μm to 10 μm; And / or, the material of the heat-resistant polymer is selected from at least one of aramid, polyimide, polyurethane, chlorophosphazene polymer, boron nitrogen polymer, polysulfone, and polybenzimidazole.

9. The diaphragm according to any one of claims 1 to 7, characterized in that: The thickness of the coating layer is 1 μm to 10 μm; And / or, the material of the coating polymer is selected from at least one of polytetrafluoroethylene, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene modification and copolymers thereof, polyimide, polyacrylonitrile, polymethyl methacrylate, and polyacrylic acid.

10. A battery, characterized in that: The battery comprises the separator according to any one of claims 1 to 9.

11. The battery according to claim 10, characterized in that The battery comprises a positive electrode sheet, a negative electrode sheet, a separator disposed between the positive electrode sheet and the negative electrode sheet, and a non-aqueous electrolyte; The negative electrode sheet comprises a negative electrode current collector and a negative electrode active material layer coated on one side or both sides of the negative electrode current collector, wherein the negative electrode active material layer comprises a negative electrode active material, a conductive agent and a binder; and the surface of the negative electrode active material is coated with amorphous carbon.

12. The battery according to claim 10 or 11, characterized in that: The negative electrode active material is selected from at least one of graphite with amorphous carbon coated on the surface, a composite material of graphite with amorphous carbon coated on the surface and silicon oxide, and a composite material of graphite with amorphous carbon coated on the surface and nano-silicon.

13. The battery according to any one of claims 10 to 12, characterized in that: In the composite material of graphite with amorphous carbon coated on the surface and silicon oxide, the content of silicon oxide is 1wt% to 15wt%.

14. The battery according to any one of claims 1 to 12, characterized in that: In the composite material of graphite with amorphous carbon coated on the surface and silicon oxide, and in the composite material of graphite with amorphous carbon coated on the surface and nano-silicon, the content of nano-silicon is 1wt% to 15wt%.

Citation Information

Patent Citations

  • Method for preparing ceramic composite diaphragm having high-adhesive polymer coating film

    CN110444718A

  • Separator for rechargeable lithium battery and rechargeable lithium battery including same

    CN112054150A

  • Lithium ion battery isolating membrane

    CN112652861A

  • Ceramic diaphragm with multi-layer composite structure and battery using ceramic diaphragm

    CN113224465A

  • Diaphragm and battery comprising same

    CN116435713A

Cited By

  • Composite powder for battery diaphragm, preparation method of composite powder, battery diaphragm, battery and electrochemical device

    CN119864597A

  • Separator, preparation method, and use thereof

    WO2026097569A1

  • Coating slurry, separator, preparation method for separator, and battery

    WO2026123675A1