AI Technical Summary
Conventional cutting tools face challenges in achieving long tool life, especially in high-speed, low-feed machining and low-speed, high-feed machining, due to limitations in wear resistance and temperature stability, leading to reduced performance and increased costs.
A cutting tool with a multilayer coating structure, comprising TiAlN and TiAlBN layers with specific thickness and composition, alternately laminated to enhance hardness, wear resistance, and temperature stability, suppressing crack propagation and improving crater wear resistance.
The cutting tool exhibits improved wear resistance, extended tool life, and balanced crater and chipping resistance, enabling efficient performance in various machining conditions.
Smart Images

Figure JP2023016836_31102024_PF_FP_ABST
Abstract
Description
cutting tools
[0001] The present disclosure relates to cutting tools.
[0002] Conventionally, in order to improve the performance of cutting tools, development has been underway for coatings that coat the surfaces of substrates made of cemented carbide, cubic boron nitride sintered bodies, etc. (for example, Patent Documents 1 and 2).
[0003] JP 2017-193004 A JP 2011-224717 A
[0004] A cutting tool according to the present disclosure is a cutting tool including a substrate and a coating provided on the substrate, wherein the coating includes a first layer, the first layer having a multilayer structure in which first unit layers and second unit layers are alternately stacked, the first unit layers having an average thickness of 2 nm or more and 50 nm or less, the second unit layers having an average thickness of 2 nm or more and 50 nm or less, the first layer having an average thickness of 1.0 μm or more and 20 μm or less, and the first unit layers being made of Ti. a Al 1-a-b B b N, wherein 0.30≦a≦0.50 and 0<b≦0.10 are satisfied, and the second unit layer is composed of Ti c Al 1-c N, wherein 0.70≦c≦1.00 is satisfied, and in the first layer, a percentage (T2 / T1)×100 of the number of titanium atoms T2 to the total number T1 of titanium and aluminum atoms is 60% or more.
[0005] FIG. 1 is a schematic cross-sectional view showing an example of the configuration of a cutting tool according to a first embodiment. FIG. 1A is a schematic cross-sectional view showing an example of the configuration of a cutting tool according to a second embodiment. FIG. 2 is a diagram for explaining a measurement area when measuring the diameter of the largest inscribed circle of a crystal grain in a first layer. FIG. 3 is a diagram for explaining a method for measuring the diameter of the largest inscribed circle of a crystal grain in a first layer, and is a diagram schematically showing a bright-field image of a measurement field. FIG. 3A is a diagram for explaining the positional relationship between the crystal grain and the first and second unit layers. FIG. 4 is a schematic cross-sectional view showing an example of the configuration of a film-forming apparatus. FIG. 5 is a schematic cross-sectional view showing an example of the configuration of a film-forming apparatus.
[0006] [Problem to be Solved by the Present Disclosure] In recent years, there has been an increasing demand for cost reduction, and there is a demand for longer tool life. For example, there is a demand for cutting tools with long tool life in both high-speed, low-feed cutting and low-speed, high-feed cutting.
[0007] Therefore, an object of the present disclosure is to provide a cutting tool having a long tool life.
[0008] Effect of the Present Disclosure The cutting tool of the present disclosure can have a long tool life.
[0009] [Description of Embodiments of the Present Disclosure] First, embodiments of the present disclosure will be listed and described. (1) A cutting tool of the present disclosure is a cutting tool including a substrate and a coating provided on the substrate, wherein the coating includes a first layer, the first layer having a multilayer structure in which first unit layers and second unit layers are alternately stacked, the first unit layers having an average thickness of 2 nm to 50 nm, the second unit layers having an average thickness of 2 nm to 50 nm, the first layer having an average thickness of 1.0 μm to 20 μm, and the first unit layers having a thickness of Ti. a Al 1-a-b B b N, wherein 0.30≦a≦0.50 and 0<b≦0.10 are satisfied, and the second unit layer is composed of Ti c Al 1-c N, wherein 0.70≦c≦1.00 is satisfied, and in the first layer, a percentage (T2 / T1)×100 of the number of titanium atoms T2 to the total number T1 of titanium and aluminum atoms is 60% or more.
[0010] The cutting tools of the present disclosure can have a long tool life.
[0011] (2) In the above (1), the first layer may have a nanoindentation hardness of 30 GPa or more at 25° C. This improves the wear resistance of the cutting tool.
[0012] (3) A cutting tool according to the present disclosure is a cutting tool including a substrate and a coating provided on the substrate, wherein the coating includes a first A layer, the first A layer having a multilayer structure in which first unit layers and third unit layers are alternately stacked, the first unit layers having an average thickness of 2 nm or more and 50 nm or less, the third unit layers having an average thickness of 2 nm or more and 50 nm or less, the first A layer having an average thickness of 1.0 μm or more and 20 μm or less, and the first unit layers being made of Ti. a Al 1-a-b B b N, wherein 0.30≦a≦0.50 and 0<b≦0.10 are satisfied, and the third unit layer is made of Ti d Al 1-d-e B e wherein 0.70≦d<1.00, 0<e≦0.10 are satisfied, and in the 1A layer, a percentage (T4 / T3)×100 of the number of titanium atoms T4 to the total number T3 of titanium and aluminum atoms is 60% or more.
[0013] The cutting tools of the present disclosure can have a long tool life.
[0014] (4) In the above (3), the nanoindentation hardness of the first A layer may be 30 GPa or more at 25° C. This improves the wear resistance of the cutting tool.
[0015] [Details of the Embodiments of the Present Disclosure] Specific examples of cutting tools according to the present disclosure will be described below with reference to the drawings. In the drawings of the present disclosure, the same reference numerals represent the same or corresponding parts. Furthermore, dimensional relationships such as length, width, thickness, and depth have been appropriately changed for clarity and simplification of the drawings, and do not necessarily represent actual dimensional relationships.
[0016] In the present disclosure, the notation in the form of "A to B" means the upper and lower limits of a range (i.e., A or more and B or less), and when no unit is specified for A and a unit is specified only for B, the units of A and B are the same.
[0017] In the present disclosure, when a compound or the like is represented by a chemical formula, unless the atomic ratio is particularly limited, it is understood to include any conventionally known atomic ratio and is not necessarily limited to only those within the stoichiometric range. For example, when "TiN" is described, the ratio of the numbers of atoms constituting TiN includes any conventionally known atomic ratio.
[0018] In the present disclosure, when one or more numerical values are recited as the lower limit and the upper limit of a numerical range, a combination of any one numerical value recited as the lower limit and any one numerical value recited as the upper limit is also considered to be disclosed. For example, when a1 or more, b1 or more, and c1 or more are recited as the lower limit and a2 or less, b2 or less, and c2 or less are recited as the upper limit, a1 or more and a2 or less, a1 or more and b2 or less, a1 or more and c2 or less, b1 or more and a2 or less, b1 or more and b2 or less, b1 or more and c2 or less, c1 or more and a2 or less, c1 or more and b2 or less, and c1 or more and c2 or less are considered to be disclosed.
[0019] [Embodiment 1: Cutting Tool] A cutting tool according to one embodiment of the present disclosure (hereinafter also referred to as "Embodiment 1") is a cutting tool including a substrate and a coating provided on the substrate, wherein the coating includes a first layer, the first layer having a multilayer structure in which first unit layers and second unit layers are alternately stacked, the first unit layers having an average thickness of 2 nm or more and 50 nm or less, the second unit layers having an average thickness of 2 nm or more and 50 nm or less, the first layer having an average thickness of 1.0 μm or more and 20 μm or less, and the first unit layers comprising Ti a Al 1-a-b B b N, wherein 0.30≦a≦0.50 and 0<b≦0.10 are satisfied, and the second unit layer is composed of Ti c Al 1-c N, wherein 0.70≦c≦1.00 is satisfied, and in the first layer, a percentage (T2 / T1)×100 of the number of titanium atoms T2 to the total number T1 of titanium and aluminum atoms is 60% or more.
[0020] The cutting tool of the present disclosure can have a long tool life, and the reason for this is presumably as follows.
[0021] (i) The coating of the cutting tool disclosed herein includes a first layer having a multilayer structure in which first unit layers and second unit layers are alternately stacked. The first unit layers and second unit layers have different compositions. This allows for the suppression of crack propagation from the surface of the coating near the interface between the first unit layers and the second unit layers during use of the cutting tool. Furthermore, the average thickness of each of the first unit layers and the second unit layers is 2 nm to 50 nm, and the average thickness of the first layer is 1.0 μm to 20 μm. This increases the number of first unit layers and second unit layers stacked in the first layer, further improving the crack propagation suppression effect. This prevents large-scale damage to the coating and extends the tool life of the cutting tool.
[0022] (ii) The first unit layer is Ti a Al 1-a-b B b The first unit layer is made of TiAlN (where 0.30≦a≦0.50, 0<b≦0.10). The hardness of the first unit layer is improved by adding a small amount of boron (B) to TiAlN. The second unit layer is made of Ti c Al 1-c N (where 0.70≦c≦1.00 is satisfied). The second unit layer has a high titanium (Ti) content and has excellent high-temperature stability. In the present disclosure, the first layer has a multilayer structure in which high-hardness first unit layers and second unit layers with excellent high-temperature stability are alternately stacked, thereby providing stable hardness even at high temperatures and improving crater wear resistance. Crater wear is wear that occurs mainly on the rake face of a cutting tool due to frictional heat between the cutting tool and the chips. Furthermore, the first layer has a multilayer structure in which high-hardness first unit layers and second unit layers with a lower hardness than the first unit layers are alternately stacked, thereby improving chipping resistance. Therefore, the crater wear resistance and chipping resistance of the coating are improved in a balanced manner, and the tool life of the cutting tool is extended.
[0023] (iii) The first unit layer and the second unit layer have different Ti and Al contents, which results in different crystal lattices between the first unit layer and the second unit layer, causing distortion of the crystal lattice in the first layer, thereby enabling the first layer to have high hardness.
[0024] (iv) In the first layer, the percentage (T2 / T1)×100 of the number of titanium atoms T2 to the total number of titanium and aluminum atoms T1 is 60% or more, which allows the first layer to have excellent crater wear resistance and extends the tool life of the cutting tool.
[0025] <Cutting Tool> The cutting tool of embodiment 1 is not particularly limited in shape, use, etc., as long as it is a cutting tool. The cutting tool of embodiment 1 may be, for example, a drill, an end mill, an indexable insert for milling, an indexable insert for turning, a metal saw, a gear cutting tool, a reamer, a tap, or an insert for pin milling of a crankshaft.
[0026] 1 is a schematic partial cross-sectional view showing an example of the configuration of a cutting tool according to embodiment 1. The cutting tool 100 includes a substrate 10 and a coating 20 provided on the substrate 10. The coating 20 includes a first layer 21, which has a multilayer structure in which first unit layers 1 and second unit layers 2 are alternately stacked.
[0027] <<Substrate>> The substrate 10 is not particularly limited. The substrate 10 may be made of, for example, cemented carbide, cermet, high-speed steel, ceramics, cubic boron nitride sintered body, diamond sintered body, or the like. The substrate 10 is preferably made of cemented carbide. This is because cemented carbide has excellent wear resistance.
[0028] A cemented carbide is a sintered body whose main component is tungsten carbide (WC) particles. The cemented carbide includes a hard phase and a binder phase. The hard phase contains WC particles. The binder phase bonds the WC particles together. The binder phase contains, for example, cobalt (Co). The binder phase may further contain titanium carbide (TiC), tantalum carbide (TaC), niobium carbide (NbC), or the like.
[0029] The cemented carbide may contain impurities that are inevitably mixed in during the manufacturing process. The cemented carbide may also contain free carbon or an abnormal layer called an "η layer" in its structure. Furthermore, the cemented carbide may be subjected to a surface modification treatment. For example, the cemented carbide may include a de-β layer on its surface.
[0030] The cemented carbide may contain 85% by mass or more and 98% by mass or less of WC grains and 2% by mass or more and 15% by mass or less of Co. The WC grains may have an average grain size of 0.2 μm or more and 4 μm or less.
[0031] Co is softer than WC particles. As described below, the soft Co can be removed by subjecting the surface of the substrate 10 to ion bombardment treatment. When the cemented carbide has the above composition and the WC particles have the above average particle size, appropriate irregularities are formed on the surface after the Co is removed. It is believed that forming the coating 20 on such a surface produces an anchor effect, improving the adhesion between the coating 20 and the substrate 10.
[0032] Here, the grain size of a WC grain refers to the diameter of a circle circumscribing a two-dimensional projected image of the WC grain. The grain size is measured using a scanning electron microscope (SEM) or a transmission electron microscope (TEM). That is, the cemented carbide is cut and the cut surface is observed using an SEM or TEM. In the observed image, the diameter of the circle circumscribing the WC grain is regarded as the grain size of the WC grain. In the observed image, the grain sizes of 10 or more (preferably 50 or more, more preferably 100 or more) randomly selected WC grains are measured, and the arithmetic mean value is taken as the average grain size of the WC grains. Before the observation, it is desirable to process the cut surface with a cross section polisher (CP) or a focused ion beam (FIB) or the like.
[0033] <Coating> The coating 20 is provided on the substrate 10. The coating 20 may be provided on a portion of the surface of the substrate 10, or may be provided on the entire surface. However, the coating 20 is provided on at least a portion of the surface of the substrate 10 that corresponds to the cutting edge. In the present disclosure, the portion of the surface of the substrate 10 that corresponds to the cutting edge refers to an area on the surface of the substrate 10 that is at least 500 μm or 2 mm away from the cutting edge ridge. As long as the effects of the present disclosure are not impaired, it does not deviate from the scope of the present disclosure even if a coating is not formed on at least a portion of the portion that corresponds to the cutting edge.
[0034] The coating 20 includes a first layer 21. The coating 20 may include other layers in addition to the first layer 21, as long as the effects of the present disclosure are not impaired. For example, the coating 20 may include one or both of a second layer 22 provided between the substrate 10 and the first layer 21 and a third layer 23 provided on the outermost surface of the coating 20. A known underlayer can be applied to the second layer. Examples of such underlayers include a TiCN layer, a TiN layer, or a TiCNO layer. A known surface layer can be applied to the third layer. Examples of such surface layers include a TiC layer, a TiN layer, or a TiCN layer.
[0035] The layer structure of the coating 20 does not need to be uniform over the entire coating 20, and the layer structure may be partially different.
[0036] The thickness of the coating 20 may be 1.0 μm or more and 25 μm or less. When the thickness of the coating 20 is 1.0 μm or more, wear resistance is improved. When the thickness of the coating 20 is 25 μm or less, chipping resistance is improved. The thickness of the coating 20 may be 2.0 μm or more and 16 μm or less, or 3.0 μm or more and 12 μm or less. Here, the thickness of the coating means the sum of the thicknesses of the layers that make up the coating. Examples of the "layers that make up the coating" include the first layer, second layer, third layer, etc.
[0037] The thickness of each layer constituting the coating is measured by obtaining a thin section sample (hereinafter also referred to as a "cross-sectional sample") of a cross section parallel to the normal direction of the surface of the cutting tool and observing the cross-sectional sample with a scanning transmission electron microscope (STEM). An example of a scanning transmission electron microscope is the JEM-2100F (trade name) manufactured by JEOL Ltd. The cross-sectional sample is observed at a magnification of 5,000 to 10,000 times, and the thickness of each layer is measured at five locations, and the arithmetic average value is taken as the "thickness of each layer."
[0038] It has been confirmed that as long as measurements are made using the same cutting tool, there is no variation in the measurement results even if the measurement location is selected arbitrarily.
[0039] <First Layer> The first layer 21 has a multilayer structure in which first unit layers 1 and second unit layers 2 are alternately stacked. The number of stacked layers is not particularly limited, as long as the average thickness of each of the first unit layers 1 and second unit layers 2 is 2 nm or more and 50 nm or less, and the average thickness of the first layer is 1.0 μm or more and 20 μm or less. The number of stacked layers refers to the number of first unit layers 1 and second unit layers 2 included in the first layer 21. The number of stacked layers may be 10 or more and 5,000 or less, 200 or more and 5,000 or less, 400 or more and 2,000 or less, or 500 or more and 1,000 or less. In the first layer 21, the layer closest to the substrate 10 may be either the first unit layer 1 or the second unit layer 2. In the first layer 21, the layer farthest from the substrate 10 may be either the first unit layer 1 or the second unit layer 2.
[0040] The average thickness of the first layer is 1.0 μm or more and 20 μm or less. When the average thickness of the first layer is 1.0 μm or more, wear resistance is improved. When the average thickness of the first layer is 20 μm or less, chipping resistance is improved. The lower limit of the average thickness of the first layer is 1.0 μm or more, or may be 2.0 μm or more, or 3.0 μm or more. The upper limit of the average thickness of the first layer is 20 μm or less, or may be 18 μm or less, or may be 16 μm or less, or may be 12 μm or less. The average thickness of the first layer is 1.0 μm or more and 20 μm or less, or may be 2.0 μm or more and 16 μm or less, or may be 3.0 μm or more and 12 μm or less.
[0041] <Average Thickness of First Unit Layer and Second Unit Layer> The average thickness of the first unit layer 1 is 2 nm or more and 50 nm or less, and the average thickness of the second unit layer 2 is 2 nm or more and 50 nm or less. By alternately stacking such thin layers in the first layer, crack propagation can be suppressed. If the average thickness of one or both of the first unit layer 1 and the second unit layer 2 is less than 2 nm, the compositions of the first unit layer 1 and the second unit layer 2 may be mixed, potentially reducing the effect of suppressing crack propagation. If the average thickness of one or both of the first unit layer 1 and the second unit layer 2 exceeds 50 nm, the effect of suppressing delamination may be reduced. The average thickness of the first unit layer and the average thickness of the second unit layer may be the same or different.
[0042] The lower limit of the average thickness of the first unit layer is 2 nm or more, or may be 4 nm or more, 6 nm or more, or 8 nm or more. The upper limit of the average thickness of the first unit layer is 50 nm or less, or may be 46 nm or less, or may be 40 nm or less, or may be 30 nm or less. The average thickness of the first unit layer is 2 nm or more and 50 nm or less, or may be 4 nm or more and 40 nm or less, or may be 6 nm or more and 30 nm or less.
[0043] The lower limit of the average thickness of the second unit layer is 2 nm or more, or may be 4 nm or more, 6 nm or more, or 8 nm or more. The upper limit of the average thickness of the second unit layer is 50 nm or less, or may be 46 nm or less, or may be 40 nm or less, or may be 30 nm or less. The average thickness of the second unit layer is 2 nm or more and 50 nm or less, or may be 4 nm or more and 40 nm or less, or may be 6 nm or more and 30 nm or less.
[0044] The method for measuring the average thickness of each of the first unit layer and the second unit layer is as follows. A thin section sample (hereinafter also referred to as a "cross-sectional sample") of the cutting tool cross section parallel to the normal direction of the surface of the cutting tool is obtained. The cross-sectional sample is observed with a scanning transmission electron microscope (STEM). An example of a scanning transmission electron microscope is the JEM-2100F (product name) manufactured by JEOL Ltd. The observation magnification of the cross-sectional sample is adjusted appropriately depending on the thickness of the first unit layer 1 and the second unit layer 2. For example, the observation magnification can be approximately 1,000,000 times. The thickness is measured at five locations for one first unit layer. The arithmetic mean value of the thicknesses of the five locations of the first unit layer is calculated, and this arithmetic mean value is defined as the average thickness of the first unit layer. The thickness is measured at five locations for one second unit layer.
[0045] For each of five different first unit layers, the average thickness of the first unit layer is measured using the above procedure. The arithmetic mean value of the average thicknesses of the five first unit layers is determined. In the present disclosure, this arithmetic mean value is referred to as the average thickness of the first unit layer. For each of five different second unit layers, the average thickness of the second unit layer is measured using the above procedure. The arithmetic mean value of the average thicknesses of the five second unit layers is determined. In the present disclosure, this arithmetic mean value is referred to as the average thickness of the second unit layer.
[0046] It has been confirmed that as long as measurements are made using the same cutting tool, there is no variation in the measurement results even if the measurement location is selected arbitrarily.
[0047] <Composition of First Unit Layer and Second Unit Layer> In the cutting tool of the present disclosure, the first unit layer comprises Ti a Al 1-a-b B b N, where 0.30≦a≦0.50, 0<b≦0.10 are satisfied, and the second unit layer is Ti c Al 1-c N, where 0.70≦c≦1.00 is satisfied. The first unit layer may be made of Ti as long as it does not impair the effect of the present disclosure. a Al 1-a-b B b The first unit layer may contain impurities together with N. a Al 1-a-b B bThe second unit layer may be composed of N and impurities. c Al 1-c The second unit layer may contain impurities together with N. c Al 1-c It can be composed of N and impurities, such as carbon (C) and oxygen (O).
[0048] In the first unit layer, the lower limit of a is 0.30 or more, or may be 0.35 or more, or 0.37 or more. The upper limit of a is 0.50 or less, or may be 0.45 or less, or may be 0.40 or less. a may be 0.35≦a≦0.45, or 0.37≦a≦0.40.
[0049] In the first unit layer, the lower limit of b is greater than 0, and may be 0.01 or greater, 0.02 or greater, or 0.04 or greater. The upper limit of b is 0.10 or less, 0.08 or less, or 0.07 or less. b may satisfy 0.01≦b≦0.08 or 0.02≦b≦0.07.
[0050] In the second unit layer, the lower limit of c is 0.70 or more, or may be 0.75 or more, or 0.80 or more. The upper limit of c is 1.00 or less, or may be 0.95 or less, or may be 0.90 or less. c may be in the range of 0.75≦d≦0.95, or 0.80≦d≦0.90.
[0051] Ti of the first unit layer a Al 1-a-b B b a, b and second unit layer Ti in N c Al 1-c The c in N is determined by measuring the composition of each layer using energy dispersive X-ray spectrometry (EDX). An EDX (TEM-EDX) attached to a transmission electron microscope (TEM) is used for the composition analysis. An example of an EDX device is the JED-2300 (trademark) manufactured by JEOL Ltd.
[0052] The composition analysis is performed as follows: A thin section sample (hereinafter also referred to as a "cross-sectional sample") of a cross section parallel to the normal direction of the surface of the cutting tool is obtained. While observing the cross-sectional sample with a TEM, EDX analysis is performed at five arbitrarily selected points within one first unit layer 1 or one second unit layer 2. The first unit layer and the second unit layer can be distinguished by the difference in contrast. Here, the "five arbitrarily selected points" are selected from different crystal grains. The composition ratios of each element obtained from the measurements at the five points are arithmetically averaged to identify the respective compositions of the first unit layer and the second unit layer.
[0053] For each of five different first unit layers, the composition of the first unit layer is determined using the above procedure. In the present disclosure, the average of the compositions of the five first unit layers is taken as the composition of the first unit layer, and a and b are determined based on this. For each of five different second unit layers, the composition of the second unit layer is determined using the above procedure. In the present disclosure, the average of the compositions of the five second unit layers is taken as the composition of the second unit layer, and c is determined based on this.
[0054] It has been confirmed that as long as measurements are taken using the same cutting tool, there is no variation in the measurement results even if the measurement points are selected arbitrarily.
[0055] <Composition of First Layer> In the first layer, the percentage (T2 / T1) × 100 (hereinafter also referred to as "percentage (T2 / T1) × 100") of the number of titanium atoms T2 relative to the total number of titanium and aluminum atoms T1 is 60% or more. This allows the first layer to have excellent crater wear resistance. From the viewpoint of improving crater wear resistance, the lower limit of percentage (T2 / T1) × 100 is 60% or more, or may be 63% or more, or 66% or more. From the viewpoint of improving oxidation resistance, the upper limit of percentage (T2 / T1) × 100 may be 80% or less, 77% or less, or 75% or less. Percentage (T2 / T1) × 100 may be 60% or more and 80% or less, or 63% or more and 77% or less, or 66% or more and 75% or less.
[0056] The percentage (T2 / T1) x 100 in the first layer is measured by TEM-EDX. An example of an EDX device is the JED-2300 (product name) manufactured by JEOL Ltd. The percentage (T2 / T1) x 100 is measured by the following procedure.
[0057] A thin section sample (hereinafter also referred to as a "cross-sectional sample") of a cross section parallel to the normal direction of the cutting tool surface is obtained. While observing the cross-sectional sample with a TEM, EDX analysis is performed on five arbitrarily selected fields within the first layer to measure the percentage (T2 / T1) x 100 of the number of titanium atoms T2 relative to the total number of titanium and aluminum atoms T1. Here, the "five arbitrarily selected fields" are set so that they do not overlap with each other. The range of one field is 200 x 200 nm. In the present disclosure, the arithmetic mean of the percentages (T2 / T1) x 100 obtained by measuring the five fields is defined as the percentage (T2 / T1) x 100 in the first layer.
[0058] It has been confirmed that as long as measurements are taken using the same cutting tool, there is no variation in the measurement results even if the measurement points are selected arbitrarily.
[0059] <Nanoindentation hardness of first layer> The nanoindentation hardness of the first layer at 25°C may be 30 GPa or more. This improves the wear resistance of the cutting tool. The lower limit of the nanoindentation hardness may be 32 GPa or more, or 34 GPa or more. The upper limit of the nanoindentation hardness is not particularly limited, but from a manufacturing standpoint, it may be 60 GPa or less, 40 GPa or less, or 36 GPa or less. The nanoindentation hardness may be 30 GPa or more and 60 GPa or less, 32 GPa or more and 60 GPa or less, or 34 GPa or more and 60 GPa or less.
[0060] The nanoindentation hardness of the first layer at 25°C is measured by the nanoindentation method in accordance with the standard procedure defined in "ISO 14577-1: 2015 Metallic materials - Instrumented indentation test for hardness and materials parameters -." The measuring instrument used is an "ENT-1100a" manufactured by Elionix. The indenter load is 1 g. In a cross section parallel to the normal direction of the cutting tool surface, the indenter is pressed against the first layer in the direction perpendicular to the cross section (i.e., parallel to the surface of the cutting tool).
[0061] The above measurement is performed at five locations on one measurement sample. The average value of the nanoindentation hardness at the five locations is taken as the nanoindentation hardness of the first layer. Note that data that appear to be abnormal at first glance are to be excluded.
[0062] It has been confirmed that as long as measurements are taken using the same cutting tool, there is no variation in the measurement results even if the measurement points are selected arbitrarily.
[0063] <Diameter of the largest inscribed circle of the crystal grains in the first layer> The first layer may be composed of a plurality of crystal grains, and the diameter of the largest inscribed circle of the crystal grains may be 5 nm or more and 500 nm or less. This improves the crater wear resistance of the cutting tool. The first layer of the present disclosure may include, in addition to the plurality of crystal grains, regions that do not constitute crystal grains (regions with random atomic arrangement), as long as the effects of the present disclosure are not impaired.
[0064] The upper limit of the diameter of the maximum inscribed circle of the crystal grain may be 500 nm or less, 450 nm or less, or 400 nm or less from the viewpoint of improving wear resistance and chipping resistance. The lower limit of the diameter of the maximum inscribed circle of the crystal grain may be 5 nm or more, 7 nm or more, or 10 nm or more from the viewpoint of suppressing a decrease in film hardness due to excessive crystal grain refinement. The diameter of the maximum inscribed circle of the crystal grain may be 5 nm or more and 500 nm or less, 7 nm or more and 450 nm or less, or 10 nm or more and 400 nm or less.
[0065] The diameter of the maximum inscribed circle of the crystal grain is measured as follows. A thin section sample (thickness: approximately 10 to 100 nm, hereinafter also referred to as the "cross-sectional sample") of the cutting tool cross section parallel to the normal direction of the cutting tool surface is obtained. The cross-sectional sample is observed with a transmission electron microscope (TEM) to obtain a bright-field image. The observation magnification is 1,000,000 to 5,000,000 times. As shown in Figure 2, the bright-field image is obtained so as to include an area A sandwiched between a line L2 that is 0.2 μm away from a line L1 indicating the center of the average thickness direction of the first layer toward the substrate side, and a line L3 that is 0.2 μm away from the line L1 toward the surface side of the coating. A rectangular measurement field of 150 nm x 150 nm is arbitrarily set within the area A.
[0066] In the above measurement field of view, a region where the atomic arrangement is ±0.5° or less is identified and this region is defined as a crystal grain. The method for identifying the region where the atomic arrangement is ±0.5° or less and the crystal grain will be described with reference to FIG. 3.
[0067] FIG. 3 is a schematic diagram showing an example of a bright-field image of the above-mentioned measurement field. In FIG. 3, atoms are indicated by black dots with the reference numeral 50. Note that FIG. 3 shows only a portion of the atoms. In the bright-field image, regularly arranged atoms 50 are connected by line segments that provide the shortest interatomic distances. In FIG. 3, the line segments are indicated by L10 to L14, L20 to L22, and L30 to L34. Regions where the angle between the line segments is ±0.5° or less (i.e., −0.5° or more and 0.5° or less) are defined as crystal grains.
[0068] In Figure 3, the angle between line segments L10 to L14 is ±0.5° or less, and the region containing these line segments corresponds to crystal grain 24a. The angle between line segments L20 to L22 is ±0.5° or less, and the region containing these line segments corresponds to crystal grain 24b. The angle between line segments L30 to L34 is ±0.5° or less, and the region containing these line segments corresponds to crystal grain 24c.
[0069] The diameter of the largest inscribed circle of each crystal grain in the measurement field is determined. The diameter of the largest inscribed circle means the diameter of the largest inscribed circle that can be drawn inside the crystal grain and that contacts at least a part of the outer edge of the crystal grain.
[0070] In Fig. 3, the diameter of the maximum inscribed circle 25a of crystal grain 24a is D1. The diameter of the maximum inscribed circle 25b of crystal grain 24b is D2. The diameter of the maximum inscribed circle 25c of crystal grain 24c is D3. When D1, D2, and D3 are all 50 nm or less, it is confirmed that the first layer shown in Fig. 3 is made up of a plurality of crystal grains, and the diameters of the maximum inscribed circles of the crystal grains are 50 nm or less.
[0071] It has been confirmed that, as long as the measurement is performed using the same cutting tool, there is no variation in the measurement results of the diameter of the maximum inscribed circle of the crystal grain, even if the measurement field is set arbitrarily.
[0072] In Figure 3, there are spaces between crystal grains 24a, 24b, and 24c, but in reality, crystal grains exist in the spaces. Because the thickness of a cross-sectional sample for TEM is approximately 10 to 100 nm, the bright-field image also reflects information in the depth direction. In areas where multiple crystal grains overlap in the thickness direction of the sample, a regular atomic arrangement cannot be confirmed in the bright-field image. Therefore, the areas where multiple crystal grains overlap are not identified as crystal grains using the above identification method.
[0073] <Positional Relationship Between Crystal Grains and First and Second Unit Layers> The positional relationship between crystal grains and first and second unit layers will be described using FIG. 3A . FIG. 3A is a schematic diagram showing a cross section of the first layer of embodiment 1 along the film thickness direction. As shown in FIG. 3A , the first layer 21 has a multilayer structure in which first unit layers 1 and second unit layers 2 are alternately stacked. FIG. 3A shows a plurality of crystal grains 24, and the boundaries between the crystal grains 24 are shown as crystal grain boundaries 25. Each crystal grain 24 can be composed of only the first unit layer or only the second unit layer. Furthermore, each crystal grain 24 can exist across one or more first unit layers and one or more second unit layers. That is, each crystal grain 24 can have a lamellar structure in which first unit layers and second unit layers are alternately stacked.
[0074] [Embodiment 2: Cutting Tool] A cutting tool according to one embodiment of the present disclosure (hereinafter also referred to as "Embodiment 2") is a cutting tool including a substrate and a coating provided on the substrate, wherein the coating includes a first A layer, the first A layer having a multilayer structure in which first unit layers and third unit layers are alternately stacked, the first unit layers having an average thickness of 2 nm or more and 50 nm or less, the third unit layers having an average thickness of 2 nm or more and 50 nm or less, the first A layer having an average thickness of 1.0 μm or more and 20 μm or less, and the first unit layers being made of Ti. a Al 1-a-b B b N, wherein 0.30≦a≦0.50 and 0<b≦0.10 are satisfied, and the third unit layer is made of Ti d Al 1-d-e B e wherein 0.70≦d<1.00, 0<e≦0.10 are satisfied, and in the 1A layer, a percentage (T4 / T3)×100 of the number of titanium atoms T4 to the total number T3 of titanium and aluminum atoms is 60% or more.
[0075] The cutting tool of the present disclosure can have a long tool life, and the reason for this is presumably as follows.
[0076] (i) The coating of the cutting tool disclosed herein includes a first A layer having a multilayer structure in which first unit layers and third unit layers are alternately stacked. The first unit layers and third unit layers have different compositions. This allows for the suppression of crack propagation from the coating surface near the interface between the first unit layers and the third unit layers during use of the cutting tool. Furthermore, because the average thickness of each of the first and third unit layers is 2 nm to 50 nm, and the average thickness of the first A layer is 1.0 μm to 20 μm, the first A layer contains a large number of first unit layers and third unit layers, further improving the crack propagation suppression effect. This prevents large-scale damage to the coating and extends the tool life of the cutting tool.
[0077] (ii) The first unit layer is Ti a Al 1-a-b B bThe first unit layer is made of TiAlN (where 0.30≦a≦0.50, 0<b≦0.10). The hardness of the first unit layer is improved by adding a small amount of boron (B) to TiAlN. The third unit layer is made of Ti d Al 1-d-e B e N (where 0.70≦d<1.00, 0<e≦0.10 are satisfied). The third unit layer has improved hardness due to the addition of a small amount of boron (B) to TiAlN. The third unit layer has a high Ti content and excellent high-temperature stability. In the present disclosure, the 1A layer has a multilayer structure in which high-hardness first unit layers and third unit layers with excellent high-temperature stability are alternately stacked, thereby obtaining stable hardness even at high temperatures and improving crater wear resistance. Furthermore, the 1A layer has a multilayer structure in which high-hardness first unit layers and third unit layers with a lower hardness than the first unit layers are alternately stacked, thereby improving fracture resistance. Therefore, the crater wear resistance and fracture resistance of the coating are improved in a balanced manner, and the tool life of the cutting tool is extended.
[0078] (iii) The first unit layer and the third unit layer have different Ti and Al contents, which results in different crystal lattices between the first unit layer and the third unit layer, causing distortion of the crystal lattice in the first A layer, and allowing the first A layer to have high hardness.
[0079] (iv) In the 1A layer, the percentage (T4 / T3)×100 of the number of titanium atoms T4 to the total number of titanium and aluminum atoms T3 is 60% or more, which allows the 1A layer to have excellent crater wear resistance and fracture resistance, thereby extending the tool life of the cutting tool.
[0080] <Cutting Tool> The cutting tool of embodiment 2 can have basically the same configuration as the cutting tool of embodiment 1, except for the configuration of the 1A layer. Fig. 1A is a schematic partial cross-sectional view showing an example of the configuration of the cutting tool of embodiment 2. The cutting tool 100 includes a substrate 10 and a coating 20 provided on the substrate 10. The coating 20 includes a 1A layer 21A, which has a multilayer structure in which first unit layers 1 and third unit layers 3 are alternately stacked.
[0081] In the second embodiment, the cutting tool and the substrate may have the same configuration as in the first embodiment. In the second embodiment, the configuration of the coating may be the same as in the first embodiment, except for the configuration of the first A layer. The "first A layer" will be described below.
[0082] <<First A Layer>> The first A layer 21A has a multilayer structure in which first unit layers 1 and third unit layers 3 are alternately stacked. The number of stacked layers is not particularly limited, as long as the average thickness of each of the first unit layers 1 and the third unit layers 3 is 2 nm or more and 50 nm or less, and the average thickness of the first A layer is 1.0 μm or more and 20 μm or less. The number of stacked layers refers to the number of first unit layers 1 and the number of third unit layers 3 included in the first A layer 21A. The number of stacked layers may be 10 or more and 5,000 or less, 200 or more and 5,000 or less, 400 or more and 2,000 or less, or 500 or more and 1,000 or less. In the first A layer, the layer closest to the substrate 10 may be either the first unit layer 1 or the third unit layer 3. In the first A layer, the layer farthest from the substrate 10 may be either the first unit layer 1 or the third unit layer 3.
[0083] The average thickness of the first A layer is 1.0 μm or more and 20 μm or less. When the average thickness of the first A layer is 1.0 μm or more, wear resistance is improved. When the average thickness of the first A layer is 20 μm or less, chipping resistance is improved. The lower limit of the average thickness of the first A layer is 1.0 μm or more, or may be 2.0 μm or more, or 3.0 μm or more. The upper limit of the average thickness of the first A layer is 20 μm or less, or may be 18 μm or less, or may be 16 μm or less, or may be 12 μm or less. The average thickness of the first A layer is 1.0 μm or more and 20 μm or less, or may be 2.0 μm or more and 16 μm or less, or may be 3.0 μm or more and 12 μm or less.
[0084] <<Average Thickness of First Unit Layer and Third Unit Layer>> The average thickness of the first unit layer can be as described in the first embodiment.
[0085] The lower limit of the average thickness of the third unit layer is 2 nm or more, or may be 4 nm or more, 6 nm or more, or 8 nm or more. The upper limit of the average thickness of the third unit layer is 50 nm or less, or may be 46 nm or less, or may be 40 nm or less, or may be 30 nm or less. The average thickness of the third unit layer is 2 nm or more and 50 nm or less, or may be 4 nm or more and 40 nm or less, or may be 6 nm or more and 30 nm or less.
[0086] The average thickness of each of the first and third unit layers may be the same or different from that of the first unit layer and the third unit layer, and is measured by replacing the second unit layer with the third unit layer in the method for measuring the average thickness of each of the first and second unit layers described in embodiment 1.
[0087] <Composition of First Unit Layer and Third Unit Layer> In the cutting tool of the present disclosure, the first unit layer comprises Ti a Al 1-a-b B b N, where 0.30≦a≦0.50, 0<b≦0.10 are satisfied, and the third unit layer is Ti d Al 1-d-e B e N, where 0.70≦d<1.00, 0<e≦0.10 are satisfied. The first unit layer may be made of Ti as long as the effect of the present disclosure is not impaired. a Al 1-a-b B b The first unit layer may contain impurities together with N. a Al 1-a-b B b The third unit layer may be composed of N and impurities. d Al 1-d-e B e The third unit layer can contain impurities together with N. d Al 1-d-e B e It can be composed of N and impurities, such as carbon (C) and oxygen (O).
[0088] The composition of the first unit layer may be the same as that described in the first embodiment.
[0089] In the third unit layer, the lower limit of d is 0.70 or more, or may be 0.75 or more, or 0.80 or more. The upper limit of d is less than 1.00, or may be 0.99 or less, or may be 0.95 or less, or may be 0.90 or less. d may be in the range of 0.70≦d≦0.99, 0.75≦d≦0.99, or 0.80≦d≦0.95.
[0090] In the third unit layer, the lower limit of e is greater than 0, and may be 0.01 or greater, 0.02 or greater, or 0.04 or greater. The upper limit of b is 0.10 or less, 0.08 or less, or 0.06 or less. b may satisfy 0.01≦b≦0.08 or 0.02≦b≦0.06.
[0091] Ti of the first unit layer a Al 1-a-b B b Ti of a, b and third unit layer in N d Al 1-d-e B e The d and e in N are determined by measuring the composition of each layer using energy dispersive X-ray spectrometry (EDX). Specifically, they are measured by replacing the second unit layer with the third unit layer in the method for measuring the compositions of the first unit layer and the second unit layer described in embodiment 1.
[0092] <Composition of Layer 1A> In Layer 1A, the percentage (T4 / T3) × 100 (hereinafter also referred to as "percentage (T4 / T3) × 100") of the number of titanium atoms T4 relative to the total number of titanium and aluminum atoms T3 is 60% or more. This allows Layer 1A to have excellent crater wear resistance. From the viewpoint of improving crater wear resistance, the lower limit of percentage (T4 / T3) × 100 is 60% or more, or may be 63% or more, or 66% or more. From the viewpoint of improving oxidation resistance, the upper limit of percentage (T4 / T3) × 100 may be 80% or less, 77% or less, or 75% or less. Percentage (T4 / T3) × 100 may be 60% or more and 80% or less, or 63% or more and 77% or less, or 66% or more and 75% or less.
[0093] The percentage (T4 / T3)×100 in the 1A layer is measured by TEM-EDX. Specifically, it is measured by substituting the 1A layer for the 1A layer in the method for measuring the percentage (T2 / T1)×100 in the 1A layer described in embodiment 1.
[0094] <Nanoindentation hardness of Layer 1A> The nanoindentation hardness of Layer 1A at 25°C may be 30 GPa or more. This improves the wear resistance of the cutting tool. The lower limit of the nanoindentation hardness may be 32 GPa or more, or 34 GPa or more. The upper limit of the nanoindentation hardness is not particularly limited, but from a manufacturing standpoint, it may be 60 GPa or less, 40 GPa or less, or 36 GPa or less. The nanoindentation hardness may be 30 GPa or more and 60 GPa or less, 32 GPa or more and 60 GPa or less, or 34 GPa or more and 60 GPa or less.
[0095] The nanoindentation hardness of the first A layer at 25°C is measured by the method for measuring the nanoindentation hardness of the first layer at 25°C described in embodiment 1, but replacing the first layer with the first A layer.
[0096] <Diameter of the largest inscribed circle of the crystal grains in the 1A layer> The 1A layer may be composed of a plurality of crystal grains, and the diameter of the largest inscribed circle of the crystal grains may be 5 nm or more and 500 nm or less. This improves the crater wear resistance of the cutting tool. The 1A layer of the present disclosure may include, in addition to the plurality of crystal grains, regions that do not constitute crystal grains (regions with a random atomic arrangement), as long as the effects of the present disclosure are not impaired.
[0097] The upper limit of the diameter of the maximum inscribed circle of the crystal grain may be 500 nm or less, 450 nm or less, or 400 nm or less from the viewpoint of improving wear resistance and chipping resistance. The lower limit of the diameter of the maximum inscribed circle of the crystal grain may be 5 nm or more, 7 nm or more, or 10 nm or more from the viewpoint of suppressing a decrease in film hardness due to excessive crystal grain refinement. The diameter of the maximum inscribed circle of the crystal grain may be 5 nm or more and 500 nm or less, 7 nm or more and 450 nm or less, or 10 nm or more and 400 nm or less.
[0098] In the second embodiment, the diameter of the largest inscribed circle of the crystal grain is measured by the method for measuring the diameter of the largest inscribed circle of the crystal grain described in the first embodiment, except that the first layer is read as the firstA layer.
[0099] In embodiment 2, the positional relationship between the crystal grains and the first unit layer and the third unit layer can be explained by replacing the second unit layer with the third unit layer in the positional relationship between the crystal grains and the first unit layer and the second unit layer described in embodiment 1.
[0100] [Embodiment 3: Method for Manufacturing Cutting Tool] In embodiment 3, a method for manufacturing the cutting tools of embodiments 1 and 2 will be described. The manufacturing method of embodiment 3 can include a step of preparing a substrate and a step of forming a coating on the substrate. Details of each step will be described below.
[0101] <<Step of Preparing a Substrate>> In the step of preparing a substrate, a substrate 10 is prepared. As the substrate 10, the substrates described in the first and second embodiments can be used.
[0102] <<Coating Forming Step>> In the coating forming step, the coating 20 is formed on the substrate 10. In the third embodiment, the coating 20 can be formed by a physical vapor deposition (PVD) method. Specific examples of the PVD method include an arc ion plating (AIP) method, a balanced magnetron sputtering (BMS) method, and an unbalanced magnetron sputtering (UBMS) method. In the third embodiment, it is preferable to use arc ion plating.
[0103] In the AIP method, an arc discharge is generated using a target material as a cathode. This vaporizes and ionizes the target material. The ions are then deposited on the surface of the substrate 10 to which a negative bias voltage is applied. The AIP method is excellent in terms of the ionization rate of the target material.
[0104] A film formation apparatus used in the AIP method will be described with reference to Figures 4 and 5. As shown in Figure 4, the film formation apparatus 200 includes a chamber 201. The chamber 201 is provided with a gas inlet 202 for introducing a source gas into the chamber 201 and a gas outlet 203 for discharging the source gas from the chamber 201 to the outside. The gas outlet 203 is connected to a vacuum pump (not shown). The pressure inside the chamber 201 is adjusted by adjusting the amount of gas introduced and discharged.
[0105] A rotary table 204 is disposed within the chamber 201. A substrate holder 205 for holding the substrate 10 is attached to the rotary table 204. The substrate holder 205 is connected to the negative terminal of a bias power supply 206. The positive terminal of the bias power supply 206 is grounded.
[0106] As shown in Fig. 5, a plurality of targets 211, 212, 213, and 214 are attached to the side wall of the chamber 201. As shown in Fig. 4, each of the targets 211 and 212 is connected to the negative pole of a DC power supply 221 or 222, respectively. The DC power supplies 221 and 222 are variable power supplies, and their positive poles are grounded. Although not shown in Fig. 4, the same applies to the targets 213 and 214. Specific operations will be described below.
[0107] The substrate 10 is held by the substrate holder 205. The pressure in the chamber 201 is reduced to 1.0×10 using a vacuum pump. -4 While the turntable 204 is being rotated, the temperature of the substrate 10 is adjusted to 500° C. by a heater (not shown) attached to the film forming apparatus 200 .
[0108] Ar gas is introduced from the gas inlet 202, and the pressure inside the chamber 201 is adjusted to 3.0 Pa. While maintaining this pressure, the voltage of the bias power supply 206 is gradually changed and finally adjusted to −1000 V. Then, the surface of the substrate 10 is cleaned by ion bombardment treatment using Ar ions.
[0109] Next, if the coating includes the second layer 22, the second layer 22 is formed on the surface of the substrate 10. For example, a TiCN layer, a TiN layer, or a TiCNO layer is formed on the surface of the substrate 10.
[0110] Next, the first layer or the first A layer is formed on the surface of the substrate 10 or the surface of the second layer 22. The composition of each target material is selected so as to obtain the compositions of the first unit layer 1, the second unit layer 2, and the third unit layer 3. Each target material is set in a predetermined position, and nitrogen gas is introduced from the gas inlet 202 to form the first layer 21 or the first A layer 21A while rotating the turntable 204. The conditions for forming the first layer 21 and the first A layer are as follows:
[0111] <Conditions for forming the first layer and the first A layer> Substrate temperature: 400 to 800°C Bias voltage: -400 to -20 V Arc current: 80 to 200 A Reactive gas pressure: 2 to 10 Pa
[0112] The substrate temperature, reaction gas pressure, bias voltage and arc current are set to constant values within the above ranges, or are varied continuously within the above ranges.
[0113] A multilayer structure in which first unit layers and second unit layers are alternately stacked, or a multilayer structure in which first unit layers and third unit layers are alternately stacked, can be formed by appropriately combining the following methods (A) to (D): (A) In the AIP method, a plurality of target materials (sintered alloys) having different compositions are used; (B) In the AIP method, the bias voltage applied to the substrate 10 during film formation is changed within the bias voltage range described in the formation conditions for the first layer and the firstA layer above; (C) In the AIP method, the gas flow rate is changed; (D) In the AIP method, the substrate 10 is rotated and its rotation period is controlled.
[0114] Next, when the coating includes the third layer 23, for example, the third layer 23 is formed on the surface of the first layer 21 or the firstA layer 21A.
[0115] As described above, a cutting tool 100 including a substrate 10 and a coating 20 provided on the substrate 10 can be manufactured.
[0116] The present embodiment will be described in more detail with reference to examples, although the present embodiment is not limited to these examples.
[0117] Example 1 <Preparation of Cutting Tool> A cutting tool was prepared as follows, and the tool life was evaluated.
[0118] A cutting tip made of cemented carbide (model number: CNMG120408 (manufactured by Sumitomo Electric Hardmetal Corporation)) was prepared as a substrate. The cemented carbide contained WC particles (90% by mass) and Co (10% by mass). The average particle size of the WC particles was 1 to 2 μm.
[0119] A coating was formed on the substrate using a film-forming apparatus having the configuration shown in Figures 4 and 5. First, the surface of the substrate was cleaned by ion bombardment treatment with Ar ions. The specific conditions for the ion bombardment treatment were as described in embodiment 3.
[0120] Next, the target materials were set at predetermined positions in the film forming apparatus. The compositions of the target materials were adjusted so as to obtain the compositions of the first and second unit layers shown in Tables 1 and 2.
[0121] The first layer was formed by alternately forming first and second unit layers while introducing nitrogen gas through a gas inlet and rotating the turntable. The conditions for forming the first layer of each sample were a substrate temperature of 400 to 800°C, a bias voltage of -400 to -20 V, an arc current of 80 to 200 A, and a reactive gas pressure of 2 to 10 Pa. The substrate temperature, reactive gas pressure, bias voltage, and arc current were either constant within the above ranges or continuously varied within the above ranges. The thickness and number of layers of each of the first and second unit layers were adjusted by the rotation speed of the substrate.
[0122]
[0123]
[0124] <Evaluation> <Coating Composition> For each sample coating, the composition of the first unit layer and the second unit layer, the average thickness of the first unit layer, the average thickness of the second unit layer, the average thickness of the first layer, the number of stacked layers of each of the first unit layer and the second unit layer, the percentage of the number of titanium atoms relative to the total number of titanium and aluminum atoms in the first layer (shown as "(T2 / T1) x 100" in Tables 1 and 2), and the nanoindentation hardness of the first layer (shown as "Hardness" in Tables 1 and 2) were measured. The measurement method for each item was as described in embodiment 1. The results are shown in Tables 1 and 2. In Table 2, the notation "1" for "Number of stacked layers" indicates that only one first unit layer or one second unit layer was formed.
[0125] <Cutting Test 1> Turning was performed using the cutting tool of each sample under the following conditions, and the cutting distance until the crater wear width reached 0.3 mm was measured. The longer the cutting distance, the better the crater wear resistance and the longer the tool life. The results are shown in the "Cutting Test 1" column in Tables 1 and 2.
[0126] (Cutting conditions) Work material: SUS316 Cutting speed: 120 m / min Feed rate: 0.3 mm / rev Depth of cut: 2.0 mm Wet The above cutting conditions apply to turning of stainless steel (low speed, high feed rate cutting).
[0127] <Evaluation> Samples 1 to 15 correspond to Examples. Samples 101 to 117 correspond to Comparative Examples. It was confirmed that Samples 1 to 15 had longer tool life than Samples 101 to 117.
[0128] Example 2 <Preparation of Cutting Tool> A cutting tool was prepared as follows, and the tool life was evaluated.
[0129] The same substrate as in Example 1 was prepared. A coating was formed on the substrate using a film-forming apparatus having the configuration shown in Figures 4 and 5. First, the surface of the substrate was cleaned by ion bombardment treatment using Ar ions. The specific conditions for the ion bombardment treatment were as described in Example 3.
[0130] Next, the target materials were set at predetermined positions in the film forming apparatus. The compositions of the target materials were adjusted so as to obtain the compositions of the first and third unit layers shown in Tables 3 and 4.
[0131] Nitrogen gas was introduced through the gas inlet, and the first and third unit layers were alternately formed while the turntable was rotating, thereby forming the 1A layer. The conditions for forming the 1A layer for each sample were a substrate temperature of 400 to 800°C, a bias voltage of -400 to -20 V, an arc current of 80 to 200 A, and a reactive gas pressure of 2 to 10 Pa. The substrate temperature, reactive gas pressure, bias voltage, and arc current were either constant within the above ranges or continuously varied within the above ranges. The thickness and number of layers of the first and third unit layers were adjusted by the rotation speed of the substrate.
[0132]
[0133]
[0134] <Evaluation> <Coating Composition> For each sample coating, the composition of the first unit layer and the third unit layer, the average thickness of the first unit layer, the average thickness of the third unit layer, the average thickness of the 1A layer, the number of stacked layers of each of the first unit layer and the third unit layer, the percentage of the number of titanium atoms relative to the total number of titanium and aluminum atoms in the 1A layer (shown as "(T4 / T3) x 100" in Tables 3 and 4), and the nanoindentation hardness of the 1A layer (shown as "Hardness" in Tables 3 and 4) were measured. The measurement method for each item was as described in embodiment 1. The results are shown in Tables 3 and 4. In Table 4, the notation "1" for "Number of stacked layers" indicates that only one first unit layer or one third unit layer was formed.
[0135] <Cutting Test 2> Turning was performed using the cutting tool of each sample under the following conditions, and the cutting distance until the crater wear width reached 0.3 mm was measured. The longer the cutting distance, the better the crater wear resistance and the longer the tool life. The results are shown in the "Cutting Test 2" column in Table 2.
[0136] (Cutting conditions) Work material: SCM435 Cutting speed: 300 m / min Feed rate: 0.15 mm / rev Depth of cut: 1.0 mm Wet The above cutting conditions apply to turning of chromium molybdenum steel (high-speed, low-feed cutting).
[0137] <Evaluation> Samples 21 to 40 correspond to Examples. Samples 120 to 137 correspond to Comparative Examples. It was confirmed that Samples 11 to 40 had a longer tool life than Samples 120 to 137.
[0138] Although the embodiments and examples of the present disclosure have been described above, it is intended from the beginning that the configurations of the above-described embodiments and examples may be appropriately combined or modified in various ways. The embodiments and examples disclosed herein are illustrative in all respects and should not be considered limiting. The scope of the present disclosure is defined by the claims, not the above-described embodiments and examples, and is intended to include meanings equivalent to the claims and all modifications within the scope of the claims.
[0139] 1 First unit layer, 2 Second unit layer, 3 Third unit layer, 10 Substrate, 20 Coating, 21 First layer, 21A 1A layer, 22 Second layer, 23 Third layer, 24, 24a, 24b, 24c Crystal grain, 25 Crystal grain boundary, 50 Atom, 100 Cutting tool, 200 Film forming apparatus, 201 Chamber, 202 Gas inlet, 203 Gas exhaust port, 204 Rotary table, 205 Substrate holder, 206 Bias power supply, 211, 212, 213, 214 Target material, 221, 222 DC power supply
Claims
1. A cutting tool comprising a substrate and a coating provided on the substrate, the coating including a first layer, the first layer being a multilayer structure in which first unit layers and second unit layers are alternately laminated, the first unit layers having an average thickness of 2 nm to 50 nm, the second unit layers having an average thickness of 2 nm to 50 nm, the first layer having an average thickness of 1.0 μm to 20 μm, and the first unit layers being made of Ti. a A 1-a-b B b N, wherein 0.30≦a≦0.50 and 0<b≦0.10 are satisfied, and the second unit layer is made of Ti c A 1-c N, wherein 0.70≦c≦1.00 is satisfied, and in the first layer, a percentage (T2 / T1)×100 of a number of titanium atoms T2 to a total number T1 of titanium and aluminum atoms is 60% or more.
2. The cutting tool according to claim 1, wherein the nanoindentation hardness of the first layer at 25°C is 30 GPa or more.
3. A cutting tool comprising a substrate and a coating provided on the substrate, the coating including a first A layer, the first A layer being made of a multilayer structure in which a first unit layer and a third unit layer are alternately laminated, the average thickness of the first unit layer being 2 nm or more and 50 nm or less, the average thickness of the third unit layer being 2 nm or more and 50 nm or less, the average thickness of the first A layer being 1.0 μm or more and 20 μm or less, and the first unit layer being made of Ti. a A 1-a-b B b N, wherein 0.30≦a≦0.50 and 0<b≦0.10 are satisfied, and the third unit layer is made of Ti d A 1-d-e B e N, wherein 0.70≦d<1.00 and 0<e≦0.10 are satisfied, and in the 1A layer, a percentage (T4 / T3)×100 of the number of titanium atoms T4 to a total number T3 of the titanium and aluminum atoms is 60% or more.
4. A cutting tool according to claim 3, wherein the nanoindentation hardness of the first A layer at 25°C is 30 GPa or more.
Citation Information
Patent Citations
Surface-coated cutting tool
JP2011224717A
Surface coated cutting tool
JP2017193004A
Hard film excellent in wear resistance, hard film coated tool and hard film coated member
JP1995310171A
Surface coated high-speed tool steel-made gear cutting tool having hard coating layer exhibiting excellent wear resistance in high-speed gear cutting of alloy steel