Workpiece having a hard material layer

A workpiece with a metal nitride hard material layer (Alx,Cry,Tiz,Mob)N, incorporating specific alloying elements, addresses the thermal stability and oxidation resistance issues of existing coatings, achieving improved tool performance and extended lifetime by maintaining cubic phase stability and reducing hexagonal phase formation.

WO2024227809A1PCT designated stage expired Publication Date: 2024-11-07VOESTALPINE EIFELER VACOTEC GMBH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/EP2024/061960
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-02
Filing Date
2024-04-30
Publication Date
2024-11-07

AI Technical Summary

Technical Problem

Existing hard material coatings for machining tools, such as (Al,Cr)N-based coatings, have limited thermal stability and oxidation resistance at high temperatures, leading to decomposition and reduced tool lifetime, and require improved mechanical properties and reduced thermal conductivity for enhanced performance.

Method used

A workpiece with a hard material layer composed of a metal nitride layer (Alx,Cry,Tiz,Mob)N, optionally including alloying elements like Nb, B, and Si, with a nitrogen ratio between 45 to 55 at.%, is used, which is deposited using physical vapor deposition or chemical vapor deposition to enhance thermal stability, abrasion resistance, and oxidation resistance.

Benefits of technology

The solution provides improved thermal stability, reduced thermal conductivity, and enhanced mechanical properties, leading to increased tool lifetime and performance in high-temperature machining applications by maintaining the cubic phase stability and minimizing hexagonal phase formation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure EP2024061960_07112024_PF_FP_ABST
    Figure EP2024061960_07112024_PF_FP_ABST
Patent Text Reader

Abstract

A workpiece includes a substrate and a hard material layer disposed over the substrate. The hard material layer includes either (A) a metal nitride layer having a composition (A1x, Cry, Tiz, Mob) N with optionally added alloying elements Nb, B, Si, the metal nitride layer having a nitrogen ratio in a range of 45 to 55 at.% of the total lattice.
Need to check novelty before this filing date? Find Prior Art

Description

WORKPIECE HAVING A HARD MATERIAL LAYER Technical Field

[0001] This disclosure relates to a workpiece having a hard material layer formed over a substrate, and in particular to a workpiece used as a tool for machining or forming operations. Background

[0002] The use of protective coatings on tools for machining, cutting or forming applications is known. Such tools compromise a substrate and a hard material coating to protect the substrate and to improve operational performance.

[0003] Several properties of the hard material coating may be important in practice. In many applications, the material of the coating should have a high thermal stability and a low thermal conductivity in order to allow higher machining speeds and longer tool lifetime. Further aspects which may be of importance are a high abrasion resistance and a low surface roughness. Moreover, the protective coating should have excellent adhesion to the substrate in order to avoid chipping. Other aspects, which may be of importance depending on the application, are a high resistance to oxidation, a low defect concentration and low intrinsic stress. In some applications, the hard material coating should have a good suitability for de-coating, allowing the tool to be recoated and used multiple times.

[0004] (Al,Cr)N-based coatings are frequently used in the art to reduce the wear and increase the lifetime of a tool. However, the composition (Al,Cr)N is metastable and decomposes at elevatedtemperatures (about 900°C) into c-CrN and h-AlN. For a high temperature suitability it may therefore be desirable to shift this decomposition to higher temperatures (i.e., to improve the thermal stability of the coating).

[0005] Further, it may be desirable to provide a coating showing improved oxidation resistance, reduced thermal conductivity, improved mechanical properties (e.g., hardness and elastic modulus) and high performance in machining or cutting applications at high temperatures. Summary

[0006] According to an aspect of the disclosure a workpiece comprises a substrate. A hard material layer is disposed over the substrate. The hard material layer includes a metal nitride layer having a composition (Alx,Cry,Tiz,Mob)N with optionally added alloying elements Nb, B, Si, the metal nitride layer having a nitrogen ratio in a range of 45 to 55 at.% of the total lattice.

[0007] According to another aspect of the disclosure a method of manufacturing a workpiece comprising a substrate and a hard material layer disposed over the substrate as described above uses physical vapor deposition and / or chemical vapor deposition to generate the hard material layer over the substrate. Brief description of the drawings

[0008] The elements of the drawings are not necessarily to scale relative to each other. Like reference numerals designate corresponding similar parts. The features of the various illustrated examples can be combined unless they exclude eachother and / or can be selectively omitted if not described to be necessarily required. Examples are depicted in the drawings and are exemplarily detailed in the description which follows.

[0009] Figure 1 is an illustration of an exemplary tool used for hobbing, showing a sectional view and a perspective view of the tool and an enlarged view of a gear of the tool.

[0010] Figure 2 illustrates X-ray diffraction (XRD) diagrams of two examples of hard material layer compositions.

[0011] Figure 3 illustrates examples of a hard material layer on a substrate of a workpiece.

[0012] Figure 4 illustrates various layer stack architectures in connection with Figure 3. Detailed description

[0013] The words “over” or “on” or “beneath” with regard to a part, element or material layer formed or located or disposed or arranged or placed “over” or “on” or “beneath” a surface may be used herein to mean that the part, element, or material layer be located (e.g. placed, formed, arranged, disposed, etc.) “directly on” or “directly under”, e.g. in direct contact with, the implied surface. The word “over” or “on” or “beneath” used with regard to a part, element, or material layer formed or located or disposed or arranged or placed “over” or “on” or “beneath” a surface may, however, either be used herein to mean that the part, element or material layer be located (e.g. placed, formed, arranged, deposited, etc.) “indirectly on” or “indirectly under” the implied surface, with one or more additional parts, elements ormaterial layers being arranged between the implied surface and the part, element or material layer.

[0014] Figure 1 illustrates an exemplary tool or workpiece 100 used for metal cutting operations. In the example shown, the workpiece 100 is a HSS (high speed steel) hob cutter. However, many other tools such as, e.g. ball head cutters, planar or profile cutters, inserts for turning or milling applications, forming dies, etc., may be examples for workpieces 100 disclosed herein. In particular, workpieces 100 described herein may be designed to be used in metal machining or metal cutting applications in which high temperatures may be created and / or are present. Other applications include the machining or cutting of plastics, for example.

[0015] The workpiece 100 includes a substrate 110 and a hard material layer 120 disposed over the substrate 110. For example, the substrate 110 may be made of metal, in particular steel, e.g. HSS, cemented carbide, or MC90. The hard material layer 120 is used as a coating to protect the substrate 110 and thereby to extend the lifetime of the workpiece 100 as well as to improve its performance.

[0016] During operation the workpiece 100 may suffer wear and / or damage. Figure 1 illustrates damages such as cutting edge rounding 122, flank wear 124, chipping 126 and cratering 128 that can occur over time during operation of the tool.

[0017] To avoid such damages, or for other reasons, several aspects related to the hard material layer 120 may be important:

[0018] The hard material layer 120 should have a good abrasion resistance. A low surface roughness (Rz,Ra) may be desired. For many applications the defect concentration should be low, and the oxidation resistance (at high operational temperatures) should be high.

[0019] For the hard material layer 120, an increase in phase stability (i.e., thermal stability) and a reduction in compressive lattice stress caused by ion bombardment during deposition of the hard material layer may be particularly desirable. In addition, a decrease in thermal conductivity may be particularly desirable because the lower the thermal conductivity, the better the protection of the substrate 110 from thermal damage.

[0020] These and other properties are strongly dependent on the chemical and physical parameters of the hard material layer 120, especially on its composition and layer structure.

[0021] According to the disclosure, the hard material layer 120 may comprise a metal nitride layer having a composition (Alx,Cry,Tiz,Mob)N with optionally added alloying elements Nb, B, Si.

[0022] Here and in the following, a notation is used in which the indices of the elements refer to the content of the element in the so-called metal sub-lattice of the composition, i.e. to the composition term placed in parentheses. That is, the indices (here: x, y, z, b) of the elements placed in parenthesis add up to 1 (corresponding to 100 at.%) except that optional alloying elements (here: Nb, B, Si) are added. Hence, the composition (Alx,Cry,Tiz,Mob)N with optionally added alloying elements Nb, B,Si can also be written as (Alx,Cry,Tiz,Nba,Mob,Bc,Sid)N, with a+ b + c + d + x + y + z = 1 (and, e.g., a = c = d = 0 if no (optional) alloying element is added). It is to be noted that other notations such as those without indices and / or without commas for the metal sub-lattice (e.g., (AlCrTiMo)N or AlCrTiMoN for (Alx,Cry,Tiz,Mob)N) are also common in the art. Further, as can be seen from the above, not all elements of the metal sub- lattice need to be metals.

[0023] Further, it is to be noted that irrespective of the composition of the metal sub-lattice (i.e., the composition term placed in parenthesis), the composition is essentially stoichiometric, i.e. about 50 at.% (ideally, exactly 50%) of the atoms of the total lattice is N and the rest is the metal sub- lattice. However, as the composition may slightly deviate from stoichiometry, the content of N may be, e.g., in a range of 45 to 55 at.% of the total lattice, which may still be referred to as an “essentially stoichiometric nitrogen ratio”.

[0024] The effects of the elements of the metal sub-lattice in relation to their content are described below.

[0025] Aluminum (Al) is a main group metal. Al forms preferably the wurtzite (hexagonal) AlN structure with nitrogen (also referred to as h-AlN). Al increases the oxidation resistance of the cubic transition metal (TM) aluminum nitride structure (referred to in the following as c-(TM,Al)N structure), as a protective Al2O3scale can form. On the other hand, Al mobility (diffusion) is the main effect for the decomposition of the material system at elevated temperatures.

[0026] Al may be, e.g., used in a range between 50 at.% and 72 at.%. Preferably, 65 at.% Al may be used, as this offers the highest hardness. Above 69 at.% Al the thermal stability decreases significantly. Below 50 at.% Al the oxidation resistance decreases.

[0027] Chromium (Cr) is a transition metal (TM). Cr forms preferably the cubic CrN structure (also referred to as c-CrN) with nitrogen. Cr increases the oxidation resistance of the c- (TM,Al)N structure, as a protective Cr2O3scale can form. Hexagonal Cr2N formation is the one of the decomposition products of the material system at elevated temperatures and detrimental for the thermal stability.

[0028] Cr may be, e.g., used in a range between 7 at.% and 26 at.%. Above 26 at.% the formation of hexagonal Cr2N is more detrimental than the desired stabilization of the cubic phase. Preferably about 20 at.% Cr may be used as this offers the highest hardness. Above 24 at.% Cr the thermal stability decreases significantly. Below 10 at.% Cr the wear resistance does not improve.

[0029] Titanium (Ti) is a transition metal (TM). Ti forms preferably with nitrogen the cubic TiN structure. Ti strains the atomic lattice and increases the phase stability (as is needed for high temperature operations). On the other hand, Ti decreases the oxidation resistance of the c-(TM,Al)N structure, as a porous TiO2scale can form. Ti oxidation can be one of the main effects for coating failure of the material system at elevated temperatures.

[0030] Above 24 at.% the oxidation of Ti (during operation) may be more detrimental than the stabilization of the cubic phase (during deposition), i.e. the negative effect may be larger than the positive effect. A preferred range of Ti may be between 5 and 20 at.%. In some examples, about 9 at.% Ti may be used as this offers the highest hardness. In other examples, a specifically preferred range of Ti may be between 12 and 15 at.%, as this still offers a high hardness while providing higher phase stability and still high oxidation resistance at elevated operational temperatures. Above 20 at.% Ti the oxidation resistance decreases slightly, above 24 at.% it may decrease significantly. Below about 1 at.% Ti the wear resistance may not improve by the addition of Ti.

[0031] Molybdenum (Mo) is a transition metal (TM). Mo forms preferably the Mo2N phase with nitrogen. Mo improves the wear resistance of the c-(TM,Al)N structure drastically, as a lubricious oxide of MoO3forms that enables less friction during operation. That is, Mo reduces the coefficient of friction, enabling less material adhesion on the hard material layer (i.e., the protective coating).

[0032] Preferably, about 6 at.% Mo may be used as this may offer the highest hardness. A specifically preferred range of Mo may be between 4 and 6 at.%, as this offers high hardness and low friction during operation while still providing high thermal stability. Above 12 at.% Mo the thermal stability decreases slightly, above 20 at.% Mo the thermal stability (i.e. phase stability) decreases significantly. Below 1 at.% Mo the wear resistance does not improve by the addition of Mo.

[0033] Niobium (Nb) is a transition metal (TM). Nb forms with nitrogen preferably the hexagonal NbN phase. Nb may improve the wear resistance of the c-(TM,Al)N structure drastically, as the hardness increases with Nb addition. Further, Nb increases the ductility of the c-(TM,Al)N structure. Nb increases the thermal stability of c-(TM,Al)N significantly. Nb forms a lubricating oxide.

[0034] Preferably, about 3 at.% Nb may be used as this offers the highest hardness. Above 5 at.% Nb the oxidation resistance decreases slightly, above 8 at.% it decreases significantly, and above 12 at.% it decreases too much. The thermal stability, which is increased by Nb, starts to decrease only for Nb addition greater than 10 at.%. Below 1 at.% Nb the wear resistance does not improve by the addition of Nb. A preferred range of Nb may be between 2 and 8 at.%, more preferably between 4 and 5 at.%, as this may allow high hardness, high ductility, and high thermal stability without significant loss of oxidation resistance.

[0035] Boron (B) is a main group nonmetal. B forms preferably the hexagonal BN phase with nitrogen. B reduces the crystallite (grain) size, thereby decreasing the thermal conductivity. B improves the wear resistance of the c-(TM,Al)N structure drastically, as the hardness and elastic modulus improve with B addition.

[0036] Preferably, about 3 at.% B may be used as this offers the highest hardness. Above 6 at.% B the thermal stability decreases significantly. Below 1 at.% B the wear resistance does not improve by the addition of B. A preferred range of B may be between 1 and 4 at.%, as this offers increased hardness and lowered thermal conductivity virtually without loss of thermalstability. A specifically preferred range of B may be between 2 and 3 at.%.

[0037] Silicon (Si) is a main group nonmetal. Si forms preferably the amorphous Si3N4 phase with nitrogen. Si improves the oxidation resistance of the c-(TM,Al)N structure drastically, as a mixture of SiO2and TiO2forms an oxygen diffusion barrier at the surface of the hard material layer. In the bulk hard material layer, the formation of the SiNxtissue phase is one of the main effects for enhanced hardness of the c-(TM,Al)N structure. Further, Si reduces the crystallite (grain) size, thereby decreasing the thermal conductivity. Si segregates to grain boundaries, thereby limiting material transport.

[0038] Preferably, about 10 at.% Si may be used as this offers the highest hardness for a monolayer. Above 15 at.% Si the oxidation resistance still increases, however the hardness may decrease. Above 20 at.%, the decrease in hardness may be too significant. Below 1 at.% Si the oxidation resistance does not improve by the addition of Si. A preferred range of Si may be between 1 and 15 at.%, as this offers oxidation resistance without significant loss of hardness. A specifically preferred range of Si may be between 2 and 10 at.%.

[0039] Nitrogen (N) is a main group nonmetal. It is not part of the metal sub-lattice. N forms preferably a nitride with the here presented metal sub-lattice elements (X) in the X-N and X-N2structure. N increases the mechanical properties of the metals.

[0040] Coatings as described herein may not form a stoichiometric nitride. It is possible to form nitrides over- stoichiometric (more than 50 at.%) and under-stoichiometric (lessthan 50 at.%). Both scenarios (not = 50 at.%, i.e. not (ideally) stoichiometric) decrease the mechanical properties and decrease the phase stability as vacancies (metal vacancies if nitrogen is over-stoichiometric and nitrogen vacancies if nitrogen is under- stoichiometric) form. It is also possible to substitute N with oxygen and / or carbon to a small extent.

[0041] Preferably, 50 at.% N is used, as this offers the highest elastic modulus and hardness. Above 51 at.% N the thermal stability decreases. Below 49 at.% N the mechanical properties decrease. A preferred range of N may be between 45 and 55 at.%, more preferably between 48 and 52 at.%, as this may promote the elastic modulus and hardness (which, however, can also be affected by other elements as described above).

[0042] Table 1 summarizes exemplary chemical compositions of the metal sub-lattice of the hard material layer 120 according to the disclosure (upper and lower limits, preferred upper and lower limits, specifically preferred upper and lower limits). Table 1: Exemplary chemical compositions of the hard material layer (in at.%) Al Cr Ti Nb Mo B Si Upper limit 72 26 24 12 20 6 20 Pref. upper limit69 23 20 8 8 4 15Spec. pref. upper limit 67 20 15 5 6 3 10 Spec. pref. lower limit 63 19 12 4 4 2 2 Pref. lower limit 58 10 5 2 2 1 1 Lower limit 50 7 1 0 1 0 0

[0043] In particular in view of Mo and / or B, micro-alloying may be beneficial, i.e. little contents of Mo and / or B are already effective in terms of improving the wear resistance. Therefore, in view of Mo, 0.01 ≤ b ≤ 0.20 is used. Further, the alloying elements (Nba,Bc,Sid) optionally added to the composition(Alx,Cry,Tiz,Mob)N may, e.g., fulfil 0 ≤ a0.12 and / or 0.01 ≤ c ≤ 0.06 and / or 0 ≤ d0.20, for example. Any other individual or combined ranges based on any of the above exemplary limits are also possible.

[0044] Some elements could optionally be added or used as substitute elements in the metal sub-lattice: V (stabilizes the fcc lattice as well, enhances gliding properties with lubricious oxides), Zr, Y, Hf, Ta, W, and Ni, in general all elements of the th th 5 and 6 main group of the periodic table. EXAMPLES

[0045] In Table 2, examples of c-(Al,Cr,Ti,Mo)N layer compositions and layer thickness (in µm) are set out. Table 2: Chemical compositions (in at.%) of examples according to the present disclosure Al Cr Ti Nb Mo B Si Layer thickness [µm] Example 1 61 14 10 4 5 3 3 3 Example 2 65 16 10 0 4 2 3 5 Example 3 62 21 11 0 2 3 1 4 Example 463 17 8 3 3 4 2 4

[0046] In Table 3, examples of c-(Al,Cr,Ti,Mo)N layer compositions not according to exemplary Table 1 compositions are set out.Table 3: Chemical compositions (in at.%) of examples not falling within all ranges of Table 1 Al Cr Ti Nb Mo B Si Example 5 64 20 8 4 0 4 0 Example 6 45 18 15 6 7 3 5 Example 7 75 8 7 3 3 1 2 Example 8 55 36 4 0 2 2 1 Example 9 67 33 0 0 0 0 0

[0047] In Table 3, composition values that fall outside the ranges of Table 1 are in bold. In Example 5, Mo had not been added. In Example 6, the Al content is lower and in Example 7 it is higher than laid out in Table 1. Examples 8 and 9 exhibit Cr contents higher than laid out in Table 1. The oxidation resistance of the layer of Example 6 was poor. The layer of Example 7 showed relatively low thermal stability. The high Cr content of Example 8 also resulted in a significant decrease in thermal stability. Example 9 consists of cubic phase only, but tool lifetime is decreased in comparison to Example 2.

[0048] More specifically, a Titanium-Milling-Test with a Chiron Mill 800 was performed with a milling tool (which is the “workpiece” of the description) having a hard material layer according to Example 2 and a milling workpiece having a hard material layer according to Example 9. The following cutting parameters were used: Vc = 80 Cutting speed (m / min) n = 2546 Spindle speed (rev / min) vf = 509 Feed speed (mm / min) ap = 5.0 Axial depth of cut (mm) ae = 3.1 Radial depth of cut (mm) f = 0.2 Feed per rev (mm / rev)z = 4 Number of teeth fz = 0.05 Feed per tooth (mm / tooth) D = 10 Cutter diameter (mm).

[0049] Stopping criteria were set to flank wear > 0.10 mm or fracture. The workpiece of Example 2 exhibited a 74.2 min tool lifetime, while the workpiece of Example 9 exhibited a 49.5 min tool lifetime.

[0050] Further, a Tooth-Impact-Test / Fly-hobbing-test was performed with the two above-mentioned workpieces (according to Example 2 and 9) to obtain the cutting performance per tooth: The test yielded a depth of crater wear at 11 m / tooth of 40 µm for the workpiece according to Example 2 and of 110 µm for the workpiece according to Example 9.

[0051] Figure 2 illustrates X-ray diffraction (XRD) diagrams (diffractograms) of Examples 2 and 7. Peaks in the diffractograms (intensity in arbitrary units versus twice the theta angle) were characterized with reference to the Crystallography Open Database (COD), the corresponding datasets having the numbers COD-9008619 for c-CrN (which represents the desired cubic / fcc phase) and COD- 9008860 for h-AlN (which is the undesired hexagonal phase). As apparent from Figure 2, the hard material layer of Example 2 (upper diffractogram) exhibits cubic phases only, while the hard material layer of Example 7 (lower diffractogram) exhibits both the cubic phase and, to a low extent, the unwanted hexagonal phase.

[0052] The settings of the primary optics in the XRD measurements were as follows: Cu Kalpha radiation, X-ray mirror, Ni filter, divergence slit 0.5°, anti-scatter slit 1.4°, mask10 mm. The following settings of the secondary optics were used: parallel plate collimator 0.18°, soller slit 0.04rad, proportional counter. The measurements were performed in grazing incidence geometry, incidence angle 1°.

[0053] Generally, a hard material layer in accordance with the disclosure may preferably have only cubic crystalline phases or, optionally, additionally a hexagonal phase (h-AlN) wherein the hexagonal phase fraction is less than 0.5 vol.%, preferably 0.2 vol.% measured by XRD by ratio of peak areas.

[0054] Figures 3 illustrates an illustrative example of a hard material layer 120 which could be used for coating the substrate 110 of a workpiece 100 (see, e.g., Figure 1).

[0055] In all examples disclosed herein, the hard material layer 120 is the functional layer of the workpiece 100. In Figure 3 the hard material layer 120 comprises or is a metal nitride layer (in this example, also referred to by the reference sign 120) having a composition (Alx,Cry,Tiz,Mob)N with optionally added alloying elements Nb, B, Si. The metal nitride layer 120 has an essentially stoichiometric nitrogen ratio.

[0056] In some examples, the metal nitride layer 120 may be monolithic, i.e. may have a composition which is constant along the layer thickness. In other examples the metal nitride layer 120 may comprise or be a metal nitride Si-gradient layer. In a metal nitride Si-gradient layer 120, the content d of Si increases along a direction facing away from the substrate 110, see arrow A. For example, d may increase from the bottom to the top of the metal nitride Si-gradient layer 120 over any of the ranges set out in Table 1. For example, d may increase from thebottom to the top of the metal nitride Si-gradient layer 120 from 0 to 10 at.%. In particular, the metal nitride Si-gradient layer 120 may have a composition which is constant along the layer thickness except for Si.

[0057] The Si-gradient may be helpful because Si is particularly beneficial at the upper surface of the hard material layer 120 to improve the oxygen diffusion barrier by generating a SiO2surface layer which impedes oxygen diffusion into the hard material layer 120. Further, such a SiO2surface layer has a very high thermal stability. For example, the Si-gradient may extend over the full thickness or over a partial thickness of the hard material layer 120.

[0058] Optionally, an adhesion layer 310 may be disposed between the substrate 110 and the hard material layer 120. The adhesion layer 310 may have a composition (Alx’,Cry’,Tiz’,Nba’,Mob’,Bc’,Sid’)N, with 0.00 ≤ x’ ≤ 0.72, 0.07 ≤ y’ ≤ 1.00, 0.00 ≤ z’ ≤ 0.24, 0.00 ≤ a’ ≤ 0.12, 0.00 ≤ b’ ≤ 0.07, 0.00 ≤ c’ ≤ 0.06, and 0.00 ≤ d’ ≤ 0.20, e.g. (Alx’,Cry’)N or (Alx’,Cry’,Bc’)N or (Alx’,Cry’,Bc’,Sid’)N. In particular, the adhesion layer 310 may, e.g., be a CrN, (AlCr)N, (AlCrB)N, (AlCrSi)N or (AlCrTiMoBSi)N layer within the above limits.

[0059] Specific examples of adhesion layers 310 are given by: Example Ad1: x’=50, y’=50, z’=a’=b’=c’= d’=0; Example Ad2: x’=0, y’=100, z’=a’=b’=c’=d’=0; Example Ad3: x’=40, y’=40, z’=15, b’=5, a’=c’=d’=0; Example Ad4: x’=40, y’=57, c’=3, z’= a’=b’=d’=0

[0060] Adhesion layers 310 of (AlCr)N, (AlCrB)N, (AlCrSi)N or (AlCrTiMoBSi)N within the above limits may have a higher oxidation resistance than a conventional CrN adhesion layer used in the art. Further, these adhesion layers 310 may form a better lattice match between the substrate 110 and the hard material layer 120 than a conventional CrN adhesion layer.

[0061] In particular, 0.5 ^ x’ ^ 0.6 and / or 0.4 ^ y’ ^ 0.5 may be used. In other examples, a metallic Cr-layer may be used as an adhesion layer 310.

[0062] In the example of Figure 3 and in all other examples disclosed herein, the hard material layer 120 may have a thickness in a range between 100 nm and 10,000 nm, preferably between 2,000 nm and 4,000 nm. The adhesion layer 310 may have a thickness in a range between 10 nm and 200 nm, preferably about 30 nm.

[0063] The hard material layers 120 described above may each have their respective composition according to any of the ranges shown in Table 1 (hard material layer 120).

[0064] The hard material layers 120 described above may be provided with an optional decorative top coating 130. The decorative top coating 130 may comprise or consist of, for example, Ti(O,C,N). TiN, for example, results in a golden coating. With a Ti(O,N) coating, the color can be adjusted by the oxygen content. A Ti(C,N) coating has a pink color. The (optional) decorative top coating 130 may have a layer thickness in a range between, e.g., 10 nm and 1,000 nm. Preferably, the layer thickness may be, e.g., about 100 nm.

[0065] Figure 4 illustrates various layer architectures in connection with Figure 3. The monolithic layer architecture of Figure 3 with constant layer composition is referred to by reference sign 410. The Si-gradient layer architecture of Figure 3 is referred to by reference sign 430.

[0066] As mentioned above, each of the layer architectures 410, 430 may be provided with a lower adhesion layer 310 between the substrate 110 and the hard material layer 120 and / or an optional decorative top coating 130, which are not shown in Figure 4.

[0067] A method of manufacturing a workpiece comprising a substrate and a hard material layer as described above may use a PVD (Physical Vapor Deposition) process to generate the adhesion layer 310, the hard material layer 120, and the top coating 130 over the substrate 110. Specifically, cathodic arc deposition and / or sputtering and / or magnetron deposition may be used, for example. Alternatively or in addition, the process may include CVD (Chemical Vapor Deposition) since, e.g., in particular Si, B, Ti can be added via the gas phase. For example, CVD allows to form gradient layers such as, e.g., the Si-gradient layer described above, by, e.g., increasing the partial pressure of the Si precursor gas during layer deposition. By PVD, gradient layers may be deposited by appropriately tuning the corresponding deposition rates (e.g., sputter rates). Further, the process may additionally include ALD (Atomic Laser Deposition), for example.

[0068] In some examples, the substrate 110 is preheated before starting PVD and / or CVD. That way, the compressive stress in the hard material layer 120 may be reduced by ensuring good CTE (Coefficient of Thermal Expansion) compensation between thesubstrate 110 and the adhesion layer 310 and / or the hard material layer 120. On a microscopic scale, the intrinsic compressive stress in the hard material layer 120 may be reduced by aiming for an (ideally) stoichiometric composition, i.e. by providing a low defect concentration.

[0069] Although specific examples have been illustrated and described herein, it will be appreciated by those of ordinary skill in the art that a variety of alternate and / or equivalent implementations may be substituted for the specific examples shown and described without departing from the scope of the present invention. This application is intended to cover any adaptations or variations of the specific examples discussed herein. Therefore, it is intended that this invention be limited only by the claims and the equivalents thereof.

Claims

Claims 1. A workpiece comprising: a substrate, and a hard material layer disposed over the substrate, wherein the hard material layer comprises a metal nitride layer having a composition (Alx,Cry,Tiz,Mob)N with optionally added alloying elements (Nba,Bc,Sid), the metal nitride layer having a nitrogen ratio in a range of 45 to 55 at.% of the total lattice.

2. The workpiece of claim 1, wherein the composition fulfils the following requirements: 0.5 ≤ x ≤ 0.72, 0.07 ≤ y ≤ 0.26, 0.01 ≤ z ≤ 0.24, 0 ≤ a ≤ 0.12, 0.01 ≤ b ≤ 0.20, 0 ≤ c ≤ 0.06, 0 ≤ d ≤ 0.

20.

3. The workpiece of claim 1 or 2, wherein the metal nitride layer is alloyed with Si, wherein a content of Si in the metal nitride layer increases along a direction facing away from the substrate.

4. The workpiece of any of the preceding claims, further comprising an adhesion layer disposed between the substrate and the hard material layer, the adhesion layer having a composition (Alx’,Cry’,Tiz’,Nba’,Mob’,Bc’,Sid’)N, with 0.00 ≤ x’ ≤ 0.72, 0.07 ≤ y’ ≤ 1.00, 0.00 ≤ z’ ≤ 0.24,0.00 ≤ a’ ≤ 0.12, 0.00 ≤ b’ ≤ 0.07, 0.00 ≤ c’ ≤ 0.06, 0.00 ≤ d’ ≤ 0.

20.

5. The workpiece of claim 4, wherein the composition of the adhesion layer fulfils the requirements: 0.50 ≤ x’ ≤ 0.60, 0.40 ≤ y’ ≤ 0.

50.

6. The workpiece of one of the preceding claims, wherein the workpiece is a tool, in particular a hob cutter, a ball head cutter, a planar or profile cutter, an insert for turning or milling applications or a forming die.

7. A method of manufacturing a workpiece comprising a substrate, and a hard material layer disposed over the substrate, wherein the hard material layer comprises a metal nitride layer having a composition (Alx,Cry,Tiz,Mob)N with optionally added alloying elements (Nba,Bc,Sid), the metal nitride layer having a nitrogen ratio in a range of 45 to 55 at.% of the total lattice, the method comprising: using physical vapor deposition and / or chemical vapor deposition to generate the hard material layer over the substrate.

8. The method of claim 7, the composition fulfils the following requirements: 0.5 ≤ x ≤ 0.72, 0.07 ≤ y ≤ 0.26, 0.01 ≤ z ≤ 0.24, 0 ≤ a ≤ 0.12,01 ≤ b ≤ 0.20, ≤ c ≤ 0.06, ≤ d ≤ 0.20.

Citation Information

Patent Citations

  • Sliding element with max phase coating

    CN109642305A

  • Surface-coated cutting tool and process for producing the same

    EP1842610A1

  • Coated cutting tool

    EP3346026A1

  • Multilayer NANO hard coating film for tooth-shaped forming tool

    WO2020230994A1