Modified ABS plastic powder, preparation method therefor, ABS resin, and automotive interior part
By adding residual monosorbent and transition metal element doping modified titanium dioxide to ABS glue powder, and preparing it in combination with emulsion method, the problem of high odor and VOC content of ABS glue powder was solved, and low odor and low emanation modification was achieved ABS glue powder and ABS resin meet the strict air quality standards for vehicle interior parts.
Patent Information
- Application Number
- PCT/CN2023/137516
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-10
- Filing Date
- 2023-12-08
- Publication Date
- 2024-11-14
AI Technical Summary
The existing ABS glue powder has a high odor and VOC content in vehicle interior parts, which is difficult to meet the increasingly stringent air quality requirements, especially the benzene, alkanes, aldehydes, ketones, and thiols of volatile organic compounds. Emission standards.
Modified ABS glue powder is prepared by adding residual monosorbent adsorbents such as diatomaceous earth, molecular sieve, porous silicate, and doping modified titanium dioxide with transition metal elements, combined with emulsion method to reduce residual monosorb content and odor, forming Low odor, low-emission modified ABS glue powder and blended with SAN resin to prepare ABS resin.
The odor and VOC emissions of modified ABS glue powder and ABS resin are significantly reduced, and the odor test requirements of vehicle interior parts is less than or equal to 3.5 and VOC is less than 50g/L, broadening the application space of materials.
Smart Images

Figure PCTCN2023137516-FTAPPB-I100001 
Figure PCTCN2023137516-FTAPPB-I100002 
Figure PCTCN2023137516-FTAPPB-I100003
Abstract
Description
Modified ABS rubber powder and preparation method thereof, ABS resin and vehicle interior parts
[0001] Related applications
[0002] This application claims priority to Chinese patent application No. 202310527469X, filed on May 10, 2023, entitled “Modified ABS rubber powder and preparation method thereof, ABS resin and vehicle interior parts,” the entire text of which is hereby incorporated by reference. Technical Field
[0003] The present invention relates to the field of engineering plastics, and in particular to modified ABS rubber powder and a preparation method thereof, ABS resin and vehicle interior decoration parts. Background Art
[0004] As the automotive industry continues to raise its standards for interior air quality, more and more automakers are paying particular attention to the impact of interior odor and VOCs (volatile organic compounds, primarily consisting of benzene, alkanes, aldehydes, ketones, and mercaptans) on driver and passenger comfort. For example, some automakers require that vehicle interior components meet odor test levels of 3.5 or less and VOC levels of less than 50g / L. Therefore, low-odor and low-emission materials are becoming increasingly important for vehicle interiors.
[0005] ABS resin, or acrylonitrile-butadiene-styrene copolymer, is an important thermoplastic polymer with broad application prospects in vehicle interiors. By blending ABS rubber powder with SAN resin, the acrylonitrile, butadiene, and styrene content of ABS resin can be flexibly adjusted, broadening its application range. However, ABS rubber powder generally contains a high level of residual monomers, resulting in high odor and VOC levels.
[0006] Summary of the Invention
[0007] Based on this, the present invention provides a modified ABS rubber powder and a preparation method thereof, ABS resin and vehicle interior trim.
[0008] The first aspect of the present invention provides a modified ABS rubber powder, the technical solution of which is as follows:
[0009] A modified ABS rubber powder, comprising a residual adsorbent and titanium dioxide doped with a transition metal element;
[0010] The residual monomer adsorbent includes diatomaceous earth, molecular sieve, porous silicate or a combination thereof.
[0011] In some embodiments, the transition metal element is palladium, platinum or a combination thereof.
[0012] In some embodiments, in the transition metal element-doped modified titanium dioxide, the molar ratio of the transition metal element to the titanium element is 1:(1-5).
[0013] In some embodiments, one or more of the following conditions are met:
[0014] 1) The residual adsorbent accounts for 0.2 wt% to 1.5 wt% of the modified ABS rubber powder;
[0015] 2) The transition metal element doped modified titanium dioxide accounts for 0.2 wt% to 1.5 wt% of the modified ABS rubber powder;
[0016] 3) the content of polybutadiene in the modified ABS rubber powder is 50 wt% to 70 wt%; and
[0017] 4) The content of acrylonitrile-styrene copolymer in the modified ABS rubber powder is 27wt% to 49.6wt%; the polymerization monomers of the acrylonitrile-styrene copolymer include acrylonitrile monomer and styrene monomer in a weight ratio of (50-150):(250-350).
[0018] The second aspect of the present invention provides a method for preparing modified ABS rubber powder, and its technical solution is as follows:
[0019] mixing butadiene latex, acrylonitrile monomer and styrene monomer, performing emulsion graft copolymerization to obtain grafted latex, and flocculating the grafted latex to prepare a flocculated slurry;
[0020] mixing the washing liquid and the flocculated slurry, collecting the solid and drying it to prepare modified ABS rubber powder;
[0021] The washing liquid includes a residual single adsorbent and titanium dioxide doped and modified by a transition metal element;
[0022] The residual monomer adsorbent includes diatomaceous earth, molecular sieve, porous silicate or a combination thereof.
[0023] In some embodiments, the method for preparing the washing solution comprises the following steps:
[0024] Titanium dioxide gel doped with transition metal elements was prepared by a sol-gel method using tetrabutyl titanate as a precursor and transition metal salts as doping sources.
[0025] The transition metal element doped and modified titanium dioxide gel, residual monosorbent adsorbent and washing solvent are mixed to prepare a washing liquid.
[0026] In some embodiments, the method for preparing the washing solution satisfies one or more of the following conditions:
[0027] 1) The transition metal salt is a palladium salt, a platinum salt or a combination thereof;
[0028] 2) The molar ratio of the transition metal salt to the tetrabutyl titanate is 1:(1-5).
[0029] In some embodiments, the concentration of the residual adsorbent in the washing liquid is 0.5 wt % to 1 wt %.
[0030] In some embodiments, the concentration of the transition metal element-doped modified titanium dioxide in the washing solution is 0.5 wt % to 1 wt %.
[0031] In some embodiments, the volume ratio of the washing liquid to the flocculation slurry is 1:(1.5-2.5).
[0032] In some embodiments, one or more of the following conditions are met:
[0033] 1) The butadiene latex is prepared by emulsion polymerization of butadiene monomer;
[0034] 2) controlling the weight of the butadiene latex so that the content of polybutadiene in the modified ABS rubber powder is 50 wt% to 70 wt%;
[0035] 3) controlling the weight of the acrylonitrile monomer and the styrene monomer so that the content of the acrylonitrile-styrene copolymer in the modified ABS rubber powder is 27 wt % to 49.6 wt %, and the weight ratio of the acrylonitrile monomer to the styrene monomer is (50-150):(250-350);
[0036] 4) The chain transfer agent used in the emulsion graft copolymerization reaction is α-methylstyrene dimer
[0037] 5) The initiator used in the emulsion graft copolymerization reaction is selected from one or more of cumene hydroperoxide, sodium persulfate, potassium persulfate, ammonium persulfate and azobisisobutylnitrile;
[0038] 6) the emulsifier used in the emulsion graft copolymerization reaction is selected from one or more of sodium salt of pernaphthalenesulfonic acid formaldehyde condensate, potassium salt of naphthalenesulfonic acid formaldehyde condensate, potassium oleate, potassium stearate, potassium disproportionated rosin acid, sodium dodecylbenzenesulfonate and sodium dodecylsulfonate;
[0039] 7) The reducing agent used in the emulsion graft copolymerization reaction is selected from one or more of sodium ethylenediaminetetraacetate, ferrous sulfate, glucose, sodium pyrophosphate and sodium sulfite;
[0040] 8) The solvent used in the emulsion graft copolymerization reaction is water; and
[0041] 9) The flocculant used in the flocculation treatment is one or more selected from magnesium sulfate, sulfuric acid and calcium chloride.
[0042] The third aspect of the present invention provides an ABS resin, and its technical solution is as follows:
[0043] An ABS resin comprises the modified ABS rubber powder or the modified ABS rubber powder prepared by the above-mentioned preparation method, and SAN resin.
[0044] A fourth aspect of the present invention provides a vehicle interior trim, the technical solution of which is as follows:
[0045] A vehicle interior trim part, comprising the modified ABS rubber powder, the modified ABS rubber powder prepared by the preparation method, or the ABS resin.
[0046] The details of one or more embodiments of the present application are set forth in the description below, and other features, objects, and advantages of the application will become apparent from the description and from the claims thereof. DETAILED DESCRIPTION
[0047] The present invention will be further described in detail below with reference to specific embodiments. The present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to provide a more thorough and comprehensive understanding of the present disclosure.
[0048] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in this specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention.
[0049] the term
[0050] Unless otherwise specified or incompatible herewith, the terms and phrases used herein shall have the following meanings:
[0051] In the present invention, "plurality", "multiple", "multiple times", "multiple", etc., unless otherwise specified, refer to a number greater than or equal to 2. For example, "one or more" means one or more than or equal to two.
[0052] In the present invention, “preferred”, “better”, “more preferred” and “suitable” are only used to describe implementation methods or examples with better effects, and it should be understood that they do not constitute a limitation on the scope of protection of the present invention.
[0053] In the present invention, the terms “further”, “further”, “particularly”, etc. are used for descriptive purposes to indicate differences in content, but should not be construed as limiting the scope of protection of the present invention.
[0054] In this disclosure, the terms "optionally," "optional," and "optional" are optional and refer to either option, i.e., to the selection of either option from the two parallel options of "optional" or "optional." If multiple "optional" terms appear in a technical solution, each "optional" term is independent unless otherwise specified and there are no conflicts or constraints.
[0055] In the present invention, in the "first aspect," "second aspect," "third aspect," "fourth aspect," etc., the terms "first," "second," "third," "fourth," etc. are used for descriptive purposes only and should not be understood as indicating or implying relative importance or quantity, nor as implicitly indicating the importance or quantity of the technical features indicated. Furthermore, "first," "second," "third," "fourth," etc. serve only as non-exhaustive enumeration and description and should be understood not to constitute a closed-ended limitation on quantity.
[0056] In the present invention, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.
[0057] In the present invention, when referring to a numerical interval (i.e., a numerical range), unless otherwise specified, the optional numerical distribution is considered continuous within the above numerical interval and includes the two numerical endpoints of the numerical range (i.e., the minimum value and the maximum value), as well as each numerical value between the two numerical endpoints. Unless otherwise specified, when a numerical interval refers only to integers within the numerical interval, it includes the two endpoint integers of the numerical range, as well as each integer between the two endpoints. In this article, it is equivalent to directly listing each integer, such as t is an integer selected from 1 to 10, indicating that t is any integer selected from the group of integers consisting of 1, 2, 3, 4, 5, 6, 7, 8, 9 and 10. In addition, when multiple ranges are provided to describe features or characteristics, these ranges can be merged. In other words, unless otherwise specified, the ranges disclosed herein should be understood to include any and all subranges included therein.
[0058] The temperature parameters in the present invention, unless otherwise specified, may be either constant temperature or fluctuating within a certain temperature range. It should be understood that the constant temperature treatment allows for temperature fluctuations within the precision range of the instrument control. Fluctuations within ranges such as ±5°C, ±4°C, ±3°C, ±2°C, and ±1°C are permitted.
[0059] In the present invention, when referring to percentage concentration, unless otherwise specified, it refers to the final concentration. The final concentration refers to the percentage of the added component in the system after the addition of the component.
[0060] In the present invention, wt% represents weight percentage, and wt‰ represents weight thousandth.
[0061] In the present invention, the proportion of residual single adsorbent and transition metal element doped modified titanium dioxide in the modified ABS rubber powder is measured by the following method:
[0062] Take 5g of ABS rubber powder and test its ash content according to GB / T 9345-2008. Specifically, calcine the powder in a muffle furnace at 850°C for 30 minutes. Measure the total ash content, and then calculate the ash content (w).
[0063] The content of Ti and transition metal elements in the ash was tested using inductively coupled plasma optical emission spectrometry (ICP-OES) according to the GB / T 30902-2014 method. Combined with the molecular weight of TiO2, the content of transition metal element-doped modified TiO2, w1, was calculated.
[0064] The content of residual adsorbent w2 = w-w1.
[0065] One embodiment of the present invention provides a modified ABS rubber powder, wherein the modified ABS rubber powder contains a residual adsorbent and titanium dioxide modified by doping with transition metal elements, wherein the residual adsorbent includes diatomaceous earth, molecular sieve, porous silicate or a combination thereof.
[0066] The modified ABS rubber powder of this embodiment contains a residual monolactic acid adsorbent and transition metal-doped titanium dioxide. The residual monolactic acid adsorbent comprises diatomaceous earth, molecular sieves, porous silicates, or a combination thereof. The residual monolactic acid adsorbent physically adsorbs residual monolactic acid in the modified ABS rubber powder. Simultaneously, the transition metal-doped titanium dioxide continuously decomposes the residual monolactic acid adsorbed by the residual monolactic acid adsorbent. Since titanium dioxide takes time to decompose residual monolactic acid, the physical adsorption of the residual monolactic acid by the residual monolactic acid adsorbent provides more time for the titanium dioxide to decompose the residual monolactic acid, promoting the decomposition of more residual monolactic acid by the titanium dioxide. This reduces the residual monolactic acid content of the modified ABS rubber powder of this embodiment, resulting in low odor and low emissions. When blended with SAN resin, it facilitates achieving the low odor and low emissions properties of ABS resin, as well as its wider application.
[0067] Optionally, the modified ABS rubber powder includes polybutadiene and acrylonitrile-styrene copolymer.
[0068] Optionally, the modified ABS rubber powder can be modified ABS high-rubber powder or modified ABS low-rubber powder. Preferably, the modified ABS rubber powder is modified ABS high-rubber powder, and the polybutadiene content is 50wt% to 70wt%.
[0069] In this embodiment, the modified ABS rubber powder can be prepared by an emulsion method, which can achieve a polybutadiene content of 50wt% to 70wt% in the modified ABS rubber powder. By dispersing the aforementioned residual monobutylene adsorbent and transition metal-doped modified titanium dioxide, the residual monobutylene content in the modified ABS rubber powder can be reduced, thereby reducing the odor and VOC emissions of the product.
[0070] Optionally, the content of acrylonitrile-styrene copolymer in the modified ABS rubber powder is 27wt% to 49.6wt%; the polymerization monomers of the acrylonitrile-styrene copolymer include acrylonitrile monomer and styrene monomer in a weight ratio of (50-150):(250-350).
[0071] In this embodiment, the residual monolite adsorbent can effectively adsorb residual monolite small molecules through physical adsorption, thereby reducing residual monolite, odor and VOC.
[0072] Optionally, the residual adsorbent accounts for 0.2 wt% to 1.5 wt% of the modified ABS rubber powder.
[0073] The diatomaceous earth in this embodiment has a porous structure and can effectively adsorb residual small molecules through physical adsorption.
[0074] Unlike simply adding a residual monolite adsorbent for adsorption, this embodiment adds titanium dioxide doped with transition metal elements to continuously decompose the residual monolite adsorbed by the residual monolite adsorbent, preventing the adsorbed residual monolite from being released and diffused during subsequent injection molding, extrusion or melt processing, causing odor or VOC to exceed the standard in subsequent steps.
[0075] In this embodiment, the titanium dioxide doped and modified with transition metal elements has the function of decomposing residues. It can not only play the role of decomposing residues under the action of light, but also play the role of decomposing residues under the action of heat separated from light by doping and modifying the titanium dioxide with transition metal elements.
[0076] Optionally, the transition metal element is palladium, platinum or a combination thereof.
[0077] Optionally, in the transition metal element-doped modified titanium dioxide, the molar ratio of the transition metal element to the titanium element is 1:(1-5).
[0078] Optionally, the transition metal element-doped modified titanium dioxide accounts for 0.2 wt% to 1.5 wt% of the modified ABS rubber powder.
[0079] Generally speaking, ABS resin can be prepared by either the emulsion method or the bulk method. The emulsion method uses more additives during the synthesis process. Therefore, compared to ABS resin obtained by the bulk method, the amount of residual singlet obtained by the emulsion method is relatively higher, and the odor and VOC are greater. Therefore, ABS resin produced by the bulk method is more commonly used. However, due to the limitations of the bulk method itself, the glue content in the ABS resin product obtained is limited and relatively fixed. It is difficult to obtain ABS resin with a high glue content, and its performance in aspects such as coating performance is poor. In addition, the flexibility of ingredients and the room for modification are relatively small. Therefore, the emulsion method is still used in the production of ABS resin materials for some vehicle interior parts. As a result, how to reduce the residual singlet in the emulsion method has become an important research topic.
[0080] By blending ABS rubber powder with SAN resin, the acrylonitrile, butadiene, and styrene content can be flexibly adjusted, providing a wide range of modification options. ABS rubber powder can be prepared using an emulsion process to obtain ABS rubber powder with a flexible polybutadiene content.
[0081] In one embodiment of the present invention, a method for preparing modified ABS rubber powder is provided, comprising the following steps:
[0082] mixing butadiene latex, acrylonitrile monomer and styrene monomer, performing emulsion graft copolymerization to obtain grafted latex, and flocculating the grafted latex to prepare a flocculated slurry;
[0083] mixing the washing liquid and the flocculated slurry, collecting the solid and drying it to prepare modified ABS rubber powder;
[0084] The washing liquid includes a residual single adsorbent and titanium dioxide doped and modified by a transition metal element;
[0085] The residual monomer adsorbent includes diatomaceous earth, molecular sieve, porous silicate or a combination thereof.
[0086] In this embodiment, the modified ABS rubber powder is prepared by an emulsion method. In the presence of a reducing agent, an emulsifier, an initiator, a chain transfer agent, and a solvent, butadiene latex, acrylonitrile monomer, and styrene monomer undergo an emulsion graft copolymerization reaction to obtain a grafted latex.
[0087] Optionally, the butadiene latex is prepared by emulsion polymerization of butadiene monomer.
[0088] Alternatively, butadiene monomer is subjected to emulsion polymerization in the presence of an electrolyte, an initiator, an emulsifier and a chain transfer agent to obtain butadiene latex.
[0089] Optionally, the reaction time of the emulsion polymerization reaction is 20 hours to 40 hours, and the reaction temperature is 51° C. to 93° C.
[0090] In some examples, the method for preparing the butadiene latex comprises the following steps:
[0091] The butadiene monomer, electrolyte, initiator, emulsifier and chain transfer agent are mixed, and the temperature of the obtained mixed system is raised from 51° C. to 61° C. to 83° C. to 93° C. within 20 h to 40 h.
[0092] Optionally, the initiator used in the emulsion polymerization is one or more selected from the group consisting of cumene hydroperoxide, sodium persulfate, potassium persulfate, ammonium persulfate and azobisisobutylnitrile.
[0093] Optionally, the initiator accounts for 0.2 wt% to 1.5 wt% of the butadiene monomer.
[0094] Optionally, the electrolyte used in the emulsion polymerization is selected from one or more of sodium carbonate, sodium bicarbonate, sodium hydroxide, potassium carbonate, and potassium hydroxide.
[0095] Optionally, the electrolyte accounts for 2 wt% to 15 wt% of the butadiene monomer.
[0096] Optionally, the emulsifier used in the emulsion polymerization is one or more selected from the group consisting of sodium salt of naphthalenesulfonic acid formaldehyde condensate, potassium salt of naphthalenesulfonic acid formaldehyde condensate, potassium oleate, potassium stearate, potassium disproportionated rosin acid, sodium dodecylbenzenesulfonate and sodium dodecylsulfonate.
[0097] Optionally, the emulsifier accounts for 2 wt% to 15 wt% of the butadiene monomer.
[0098] Optionally, the chain transfer agent used in the emulsion polymerization is one or more selected from tert-dodecyl mercaptan, n-dodecyl mercaptan, tetradecyl mercaptan, tridecyl mercaptan, undecyl mercaptan and decanyl mercaptan.
[0099] Optionally, the chain transfer agent accounts for 0.5 wt% to 5 wt% of the butadiene monomer.
[0100] Optionally, the reaction time of the emulsion graft copolymerization reaction is 5 hours to 9 hours, and the reaction temperature is 10° C. to 72° C.
[0101] In some examples, the method for preparing the grafted latex comprises the following steps:
[0102] Mix butadiene latex and reducing agent, heat the resulting mixed system to 62°C to 72°C, add acrylonitrile monomer, styrene monomer, emulsifier, initiator, chain transfer agent and solvent, keep warm for 1 to 3 hours, and naturally cool and react for 4 to 6 hours.
[0103] Optionally, the weight of the butadiene latex is controlled so that the content of polybutadiene in the modified ABS rubber powder is 50 wt % to 70 wt %.
[0104] Optionally, the solid content of the butadiene latex is 50 wt% to 65 wt%.
[0105] Optionally, the weights of acrylonitrile monomer and styrene monomer are controlled so that the content of acrylonitrile-styrene copolymer in the modified ABS rubber powder is 27 wt % to 49.6 wt %, and the weight ratio of acrylonitrile monomer to styrene monomer is (50-150):(250-350).
[0106] Optionally, the chain transfer agent used in the emulsion graft copolymerization reaction is α-methylstyrene dimer, which is sulfur-free, odorless, safe and environmentally friendly, and meets FDA requirements. Compared with using tert-dodecyl mercaptan, it has much lower odor.
[0107] Optionally, the chain transfer agent accounts for 0.2 wt‰ to 10 wt‰ of the total amount of the polybutadiene, acrylonitrile monomer and styrene monomer.
[0108] Optionally, the initiator used in the emulsion graft copolymerization reaction is one or more selected from cumene hydroperoxide, sodium persulfate, potassium persulfate, ammonium persulfate and azobisisobutylnitrile;
[0109] Optionally, the initiator accounts for 1 wt‰ to 10 wt‰ of the total amount of the polybutadiene, acrylonitrile monomer and styrene monomer.
[0110] Optionally, the emulsifier used in the emulsion graft copolymerization reaction is selected from one or more of sodium salt of pernaphthalenesulfonic acid formaldehyde condensate, potassium salt of naphthalenesulfonic acid formaldehyde condensate, potassium oleate, potassium stearate, potassium disproportionated rosin acid, sodium dodecylbenzenesulfonate and sodium dodecylsulfonate.
[0111] Optionally, the emulsifier accounts for 2 wt‰ to 20 wt‰ of the total amount of the polybutadiene, acrylonitrile monomer and styrene monomer.
[0112] Optionally, the reducing agent used in the emulsion graft copolymerization reaction is one or more selected from the group consisting of sodium ethylenediaminetetraacetate, ferrous sulfate, glucose, sodium pyrophosphate and sodium sulfite.
[0113] Optionally, the reducing agent accounts for 0.01 wt‰ to 0.05 wt‰ of the total amount of the polybutadiene, acrylonitrile monomer and styrene monomer.
[0114] Optionally, the solvent used in the emulsion graft copolymerization reaction may be water.
[0115] In this embodiment, a flocculant is added to the obtained graft latex to perform flocculation treatment to prepare a flocculated slurry.
[0116] Optionally, the flocculation treatment time is 2 hours to 6 hours, and the reaction temperature is 70°C to 100°C.
[0117] Optionally, the flocculant used in the flocculation treatment is selected from one or more of magnesium sulfate, sulfuric acid and calcium chloride.
[0118] Optionally, the weight ratio of the grafted latex to the flocculant is 1000:(40-50).
[0119] It can be understood that the flocculant is added to the graft latex in the form of an aqueous flocculant solution.
[0120] In some examples, the method for preparing the flocculated slurry comprises the following steps:
[0121] The grafted latex is heated to 70-80° C., and a flocculant aqueous solution is added. The flocculant aqueous solution is added within 1-3 hours, and then the temperature is raised to 90-100° C. and kept warm for 1-3 hours.
[0122] Optionally, the concentration of the flocculant in the flocculant aqueous solution is 0.5 wt% to 5 wt%.
[0123] In this embodiment, the flocculated slurry is washed with a washing liquid containing a residual monosorbent adsorbent and titanium dioxide doped with transition metal elements. This washing process allows the residual monosorbent adsorbent and the titanium dioxide doped with transition metal elements to be fully dispersed in the modified ABS rubber powder. In their experiments, the inventors investigated numerous methods for incorporating residual monosorbent adsorbents and titanium dioxide doped with transition metal elements into ABS rubber powder. Experimental verification revealed that adding both to the washing liquid and then mixing the washing liquid into the flocculated slurry is beneficial for their dispersion in the modified ABS rubber powder. The better the dispersion of the residual monosorbent adsorbent and titanium dioxide doped with transition metal elements in the modified ABS rubber powder, the better the odor and VOC reduction effects. The method of this embodiment can produce a modified ABS rubber powder with low odor and low emissions.
[0124] Optionally, the preparation method of the washing solution comprises the following steps:
[0125] Titanium dioxide gel doped with transition metal elements was prepared by a sol-gel method using tetrabutyl titanate as a precursor and transition metal salts as doping sources.
[0126] The transition metal element doped and modified titanium dioxide gel, residual monosorbent adsorbent and washing solvent are mixed to prepare a washing liquid.
[0127] In this embodiment, the transition metal-doped titanium dioxide gel prepared by the sol-gel method contains transition metal-doped titanium dioxide. After mixing the gel with a residual monoadsorbent and a washing solvent, the gel is diluted and can be used as a washing liquid. The washing liquid contains the residual monoadsorbent, the transition metal-doped titanium dioxide, and the washing solvent.
[0128] Further optionally, tetrabutyl titanate is used as a precursor and a transition metal salt is used as a doping source, and the preparation of transition metal element-doped titanium dioxide gel by a sol-gel method comprises the following steps:
[0129] Mix hydrochloric acid, transition metal salt and ethanol, add tetrabutyl titanate, and then add water to adjust the pH value to 3-4.
[0130] Further optionally, the transition metal salt is a palladium salt, a platinum salt or a combination thereof, such as palladium chloride PdCl2, H2PtCl6.
[0131] Further optionally, the molar ratio of the transition metal salt to the tetrabutyl titanate is 1:(1-5).
[0132] In this embodiment, a transition metal-doped titanium dioxide gel, a residual monoadsorbent, and a washing solvent are mixed. Optionally, the concentration of the residual monoadsorbent in the washing solution is 0.5 wt% to 1 wt%. Optionally, the concentration of the transition metal-doped titanium dioxide in the washing solution is 0.5 wt% to 1 wt%. Optionally, the washing solvent can be water.
[0133] In this embodiment, the residual single adsorbent is as described above and will not be described again here.
[0134] In this embodiment, the flocculated slurry is washed by mixing a washing liquid with the flocculated slurry. Optionally, the flow ratio of the washing liquid to the flocculated slurry is 1:(1.5-2.5). Optionally, the washing time is 20-40 minutes. After washing, the solids can be collected by centrifugation, filtration, or other means and dried to obtain modified ABS rubber powder.
[0135] In this embodiment, the content of the transition metal element-doped modified titanium dioxide and the residual monoadsorbent in the modified ABS rubber powder can be controlled by controlling the concentration of the transition metal element-doped modified titanium dioxide and the residual monoadsorbent in the washing liquid, the flow rate of the washing liquid and the flocculation slurry, and the washing time. However, the above methods are not limited to the above.
[0136] Through the preparation method of this embodiment, the residual adsorbent accounts for 0.2wt% to 1.5wt% in the modified ABS rubber powder; the transition metal element-doped modified titanium dioxide accounts for 0.2wt% to 1.5wt% in the modified ABS rubber powder.
[0137] The preparation method of this embodiment requires less modification to the original emulsion production line, has less impact on the production cycle and energy consumption, and is conducive to continuous large-scale production.
[0138] In one embodiment of the present invention, an ABS resin is provided, which includes the modified ABS rubber powder or the modified ABS rubber powder prepared by the above preparation method, and SAN resin.
[0139] Optionally, the amount of modified ABS rubber powder and SAN resin added can be adjusted according to actual use requirements. In some embodiments, the weight ratio of modified ABS rubber powder to SAN resin can be (15-35): (65-85).
[0140] It is understood that the ABS resin can be prepared by extruding and pelletizing a powder containing modified ABS rubber powder and SAN resin. Optionally, the extrusion temperature is 180°C to 210°C, the screw speed is 200 rpm to 300 rpm, and the screw aspect ratio is (35-45):1.
[0141] In one embodiment of the present invention, a vehicle interior trim is provided, comprising the modified ABS rubber powder, the modified ABS rubber powder obtained by the above preparation method, or the above ABS resin.
[0142] The vehicle interior decoration part of this embodiment has low odor and low emission, and is widely used.
[0143] The following is further described in conjunction with specific examples and comparative examples. The raw materials involved in the following specific examples and comparative examples, unless otherwise specified, can be derived from commercial sources. The instruments used, unless otherwise specified, can be derived from commercial sources. The processes involved, unless otherwise specified, are routinely selected by those skilled in the art. The parts involved in the following examples and comparative examples, unless otherwise specified, are all parts by weight.
[0144] Among them, butadiene monomer is industrial-grade butadiene with a purity greater than 96%, sourced from Huarui Chemical; styrene monomer has a purity greater than or equal to 99%, sourced from Aladdin Reagent Company; acrylonitrile monomer has a purity greater than or equal to 99%, sourced from Aladdin Reagent Company; tert-dodecyl mercaptan TDM is a chain transfer agent; α-methylstyrene dimer AMSD is a chain transfer agent; SAN resin is a styrene-acrylonitrile copolymer with the brand PN-128, sourced from Taiwan Chi Mei.
[0145] Example 1
[0146] This embodiment provides a modified ABS rubber powder and a preparation method thereof, an ABS resin and a preparation method thereof, and the steps are as follows:
[0147] Step 1: Preparation of butadiene latex
[0148] 100 parts of butadiene monomer, 0.5 parts of sodium persulfate (initiator), 5 parts of sodium carbonate (electrolyte), 5 parts of potassium disproportionate rosin acid (emulsifier) and 2 parts of tert-dodecyl mercaptan (chain transfer agent) were mixed, the temperature was raised to 56°C to start the emulsion polymerization reaction, and the temperature was continuously raised to 88°C within 30 hours. The reaction was completed after 30 hours to obtain a butadiene latex with a particle size of 310 nm and a solid content of 58 wt%.
[0149] Step 2: Preparation of flocculation slurry
[0150] A butadiene latex containing 600 parts of polybutadiene was added to a reactor, 0.015 parts of ferrous sulfate was added to the reactor and stirred evenly, the reactor was heated to 67°C, and 2.51 parts of cumene hydroperoxide, 100 parts of acrylonitrile monomer, 300 parts of styrene monomer, 1.5 parts of AMSD, 5 parts of potassium disproportionate rosinate and 175 parts of deionized water were added, and the addition was continued dropwise for 2 hours. After heating was completed, the reaction was continued for 5 hours to obtain a grafted latex.
[0151] Take 1000 parts of grafted latex and add it to the flocculation reactor, start stirring and heat to 75°C, gradually add 450 parts of 10wt% magnesium sulfate aqueous solution, add it over 2 hours, and heat to 95°C and maintain the temperature for 2 hours. Filter the product with a 325-mesh filter to obtain a flocculation slurry.
[0152] Step 3: Prepare washing solution
[0153] At room temperature, 3g of PdCl2 was dissolved in 20ml of 10% hydrochloric acid, and 80ml of anhydrous ethanol was added and mixed thoroughly. Under vigorous stirring, 20ml of tetrabutyl titanate was slowly added dropwise to the above solution to form a homogeneous solution. Deionized water was added to adjust the pH of the system to about 4, and stirring was continued until a Pd-doped TiO2 gel was formed.
[0154] Diatomaceous earth and deionized water were added to the Pd-doped modified TiO2 gel to prepare a washing solution, wherein the concentration of the Pd-doped modified TiO2 in the washing solution was 0.5 wt %, and the concentration of the diatomaceous earth in the washing solution was 0.5 wt %.
[0155] Step 4: Prepare modified ABS rubber powder
[0156] The washing liquid and the flocculated slurry were mixed and washed for 30 minutes at a flow rate of 2 tons / h for the flocculated slurry and 1 ton / h for the washing liquid. The mixed solution was then washed with water via vacuum turbines and then centrifuged for dehydration. After dehydration, it was dried in a fluidized bed at 60°C for 6 hours to obtain a modified ABS rubber powder 1 having a moisture content of <1 wt%. The proportions of Pd-doped TiO2 and diatomaceous earth in the modified ABS rubber powder 1 were measured, as shown in Table 1.
[0157] Step 5: Preparation of ABS resin
[0158] 25 parts of the modified ABS rubber powder 1 and 75 parts of SAN resin were mixed, extruded through a twin-screw extruder, cooled, and pelletized to obtain ABS resin 1, wherein the extrusion temperature was 200°C, the screw speed was 250 r / min, and the screw aspect ratio was 40:1.
[0159] Example 2
[0160] This example provides a modified ABS rubber powder and a preparation method thereof, as well as an ABS resin and a preparation method thereof. These methods are substantially the same as those of Example 1, differing primarily in that, in step 3, the concentration of Pd-doped TiO₂ and the concentration of diatomaceous earth in the washing liquid are set to 1 wt %. Modified ABS rubber powder 2 and ABS resin 2 were produced in this example, and the proportions of Pd-doped TiO₂ and diatomaceous earth in modified ABS rubber powder 2 were measured. The results are shown in Table 1.
[0161] Example 3
[0162] This example provides a modified ABS rubber powder and a preparation method thereof, as well as an ABS resin and a preparation method thereof. These methods are substantially the same as those of Example 1, differing primarily in that, in step 3, the concentration of Pd-doped TiO₂ and the concentration of diatomaceous earth in the washing liquid are set to 0.8 wt %. This example produced modified ABS rubber powder 3 and ABS resin 3. The proportions of Pd-doped TiO₂ and diatomaceous earth in modified ABS rubber powder 3 were measured, as shown in Table 1.
[0163] Example 4
[0164] This example provides a modified ABS rubber powder and a preparation method thereof, as well as an ABS resin and a preparation method thereof. These methods are substantially the same as those in Example 1, differing primarily in that, in step 3, 3g of PdCl2 is replaced with 7g of H2PtCl6. This example produced modified ABS rubber powder 4 and ABS resin 4. The proportions of Pt-doped TiO2 and diatomaceous earth in modified ABS rubber powder 4 were measured, as shown in Table 1.
[0165] Example 5
[0166] This embodiment provides a modified ABS rubber powder and a preparation method thereof, as well as an ABS resin and a preparation method thereof. These methods are substantially the same as those of Example 1, with the primary difference being that, in Step 3, porous silicate and deionized water are added to the Pd-doped TiO2 gel to prepare a washing solution, wherein the concentration of the Pd-doped TiO2 and the porous silicate in the washing solution is set to 0.5 wt %. This embodiment produced modified ABS rubber powder 5 and ABS resin 5. The proportions of Pd-doped TiO2 and porous silicate in the modified ABS rubber powder 5 were measured, as shown in Table 1.
[0167] Example 6
[0168] This embodiment provides a modified ABS rubber powder and a preparation method thereof, and an ABS resin and a preparation method thereof, which are substantially the same as those in Example 1, with the main difference being that Pd-doped modified TiO2 and diatomaceous earth are added in step 2. Steps 2 and 3 of this embodiment are as follows:
[0169] Step 2: Prepare flocculation slurry
[0170] A butadiene latex containing 600 parts of polybutadiene was added to a reactor, 0.015 parts of ferrous sulfate was added to the reactor and stirred evenly, the reactor was heated to 67°C, and 2.51 parts of cumene hydroperoxide, 100 parts of acrylonitrile monomer, 300 parts of styrene monomer, 1.5 parts of AMSD, 5 parts of potassium disproportionate rosinate and 175 parts of deionized water were added, and the addition was continued dropwise for 2 hours. After heating was completed, the reaction was continued for 5 hours to obtain a grafted latex.
[0171] 1000 parts of the grafted latex were added to a flocculation reaction kettle, stirred and heated to 75°C. 450 parts of a 10 wt% aqueous solution of magnesium sulfate, 0.5 parts of Pd-doped TiO2, and 0.5 parts of diatomaceous earth were gradually added over a period of 2 hours. The mixture was then heated to 95°C and maintained at that temperature for 2 hours. The product was filtered through a 325-mesh filter to obtain a flocculated slurry. The preparation method of the Pd-doped TiO2 is as follows:
[0172] Under room temperature, 3g of PdCl2 was dissolved in 20ml of 10% hydrochloric acid, and then added into 80ml of anhydrous ethanol and mixed thoroughly. Under vigorous stirring, 20ml of tetrabutyl titanate was slowly added dropwise into the above solution to form a homogeneous solution. 1 part of deionized water was added to adjust the pH of the system to about 4. Stirring was continued until a Pd-doped TiO2 gel was formed. After dilution with water, the mixture was dehydrated and dried to obtain Pd-doped TiO2.
[0173] Step 3: Prepare modified ABS rubber powder
[0174] The flocculated slurry was washed with deionized water at a flow rate of 2 tons / h and 1 ton / h of water. After washing, the mixture was centrifuged for dehydration and then dried in a fluidized bed at 60°C for 6 hours, yielding modified ABS rubber powder 6 with a moisture content of <1 wt%. The proportions of Pd-doped TiO2 and diatomaceous earth in the modified ABS rubber powder 6 were measured, as shown in Table 1.
[0175] Referring to step 5 of Example 1, ABS resin 6 of this example was prepared.
[0176] Example 7
[0177] This embodiment provides a modified ABS rubber powder and a preparation method thereof, and an ABS resin and a preparation method thereof, which are substantially the same as those in Example 1, with the primary difference being that Pd-doped modified TiO2 and diatomaceous earth are added after water washing in step 4. Step 3 of this embodiment is as follows:
[0178] Step 3: Prepare modified ABS rubber powder
[0179] The flocculated slurry from step 2 was washed with deionized water at a flow rate of 2 tons / h and 1 ton / h of water. After washing, the mixed solution was centrifuged for dehydration and then dried in a fluidized bed at 60°C for 6 hours to obtain a rubber powder with a moisture content of less than 1 wt%. Pd-doped TiO2 and diatomaceous earth were added to the rubber powder to a concentration of 0.51 wt% of the Pd-doped TiO2 and 0.48 wt% of the diatomaceous earth. Mechanical stirring was performed to obtain modified ABS rubber powder 7, where the Pd-doped TiO2 was the same as that in Example 6.
[0180] Referring to step 5 of Example 1, ABS resin 7 of this example was prepared.
[0181] Example 8
[0182] This example provides a modified ABS rubber powder and a preparation method thereof, as well as an ABS resin and a preparation method thereof. These methods are substantially the same as those in Example 1, differing primarily in that AMSD is replaced with TDM in Step 2. This example produced modified ABS rubber powder 8 and ABS resin 8. The proportions of Pd-doped TiO2 and diatomaceous earth in modified ABS rubber powder 8 were measured, as shown in Table 1.
[0183] Comparative Example 1
[0184] This comparative example provides an ABS rubber powder and a preparation method thereof, and an ABS resin and a preparation method thereof. These methods are essentially the same as those in Example 1, with the primary difference being that the washing solution is deionized water, and that Pd-doped TiO2 and diatomaceous earth are not added. This comparative example produces ABS rubber powder 9 and ABS resin 9.
[0185] Comparative Example 2
[0186] This comparative example provides an ABS rubber powder and a preparation method thereof, an ABS resin and a preparation method thereof, which are basically the same as those in Example 1, with the main difference being that the preparation of the washing liquid in step 3 is different. Step 3 of this comparative example is as follows:
[0187] Step 3: Prepare washing solution
[0188] At room temperature, add 80 ml of anhydrous ethanol to 20 ml of 10% hydrochloric acid and mix thoroughly. Under vigorous stirring, slowly add 20 ml of tetrabutyl titanate dropwise to the above solution to form a homogeneous solution. Add deionized water to adjust the system pH to about 4. Continue stirring until TiO2 gel is formed.
[0189] Diatomaceous earth and deionized water were added to the TiO2 gel to prepare a washing solution, wherein the concentration of TiO2 in the washing solution was 0.5 wt %, and the concentration of diatomaceous earth in the washing solution was 0.5 wt %.
[0190] Referring to steps 4 and 5 of Example 1, ABS rubber powder 10 and ABS resin 10 of this comparative example were prepared, and the proportions of TiO2 and diatomaceous earth in the modified ABS rubber powder 10 were measured. The results are shown in Table 2.
[0191] Comparative Example 3
[0192] This comparative example provides an ABS rubber powder and a preparation method thereof, an ABS resin and a preparation method thereof, which are basically the same as those in Example 1, with the main difference being that the preparation of the washing liquid in step 3 is different. Step 3 of this comparative example is as follows:
[0193] Step 3: Prepare washing solution
[0194] At room temperature, 3g of PdCl2 was dissolved in 20ml of 10% hydrochloric acid, and 80ml of anhydrous ethanol was added and mixed thoroughly. Under vigorous stirring, 20ml of tetrabutyl titanate was slowly added dropwise to the above solution to form a homogeneous solution. Deionized water was added to adjust the pH of the system to about 4, and stirring was continued until a Pd-doped TiO2 gel was formed.
[0195] Deionized water was added to the Pd-doped modified TiO2 gel to prepare a washing solution, and the concentration of the Pd-doped modified TiO2 in the washing solution was set to 1 wt%.
[0196] Referring to steps 4 and 5 of Example 1, ABS rubber powder 11 and ABS resin 11 of this comparative example were prepared, and the proportion of Pd-doped TiO2 in the modified ABS rubber powder 11 was measured. The results are shown in Table 2.
[0197] The ABS resins of the above embodiments and comparative examples were subjected to performance tests. The test items and methods are as follows. The test results are shown in Tables 1 and 2.
[0198] Odor: Tested according to PV3900-2000;
[0199] Total carbon (TVOC): tested according to PV3341;
[0200] Remaining order test conditions:
[0201] Headspace injection: HS-10 thermostated oven at 80°C, sample flow path at 210°C, transfer line at 215°C. Inlet: 230°C, split ratio 100:1, injection time 1 min, septum purge flow rate 3 ml / min. Column oven: initial temperature 60°C, retention time 1 min, first-step ramp rate 5°C / min, final temperature 80°C, hold time 0 min, second-step ramp rate 1°C / min, final temperature 85°C, hold time 0 min. Third-step ramp rate 5°C / min, final temperature 100°C, hold time 0 min, fourth-step ramp rate 40°C / min, final temperature 225°C, hold time 5 min. Front detector (FID): 320°C, makeup gas N2: 24 ml / min. Gas pressure and flow rate: APC1 pressure 260.0 kPa.
[0202] Quantitative method: internal standard method
[0203] Weigh 0.5 g of the sample, accurate to 0.1 mg, into a headspace bottle, add 10 ml of o-dichlorobenzene (containing 5 mg / L n-butanol), seal the bottle, place it in an oscillator at 60°C for 2 hours, and take it out for analysis.
[0204] Table 1
[0205] Table 2
[0206] As can be seen from Table 1 and Table 2, the odor of the ABS resin prepared from the modified ABS rubber powder of Examples 1-8 is between 3 and 3.7, the TVOC is between 13 and 38 μg / g, the residual styrene is between 280 and 390 ppm, the residual ethylbenzene is between 32 and 56 ppm, and the residual acrylonitrile is between 20 and 29 ppm. It shows a lower residual monohydrate content, low odor, and less TVOC. The chain transfer agent used in Example 8 is different from that in Example 1, and has relatively more TVOC and odor. In Examples 6 and 7, the residual monohydrate adsorbent and the titanium dioxide doped with transition metal elements are added before and after washing, respectively, but the effect is not as good as that of adding them in the washing liquid. Adding the residual monohydrate adsorbent and the titanium dioxide doped with transition metal elements to the washing liquid has a better dispersion effect on the two in the rubber powder, and a better effect on reducing the residual monohydrate content, odor, and VOC.
[0207] In Comparative Example 1, no residual monohydrate adsorbent and transition metal element-doped modified titanium dioxide were added, in Comparative Example 2, titanium dioxide was not modified, and in Comparative Example 3, only Pd-doped modified TiO2 gel was added without adding residual monohydrate adsorbent. The ABS resins prepared from the ABS rubber powders of Comparative Examples 1, 2 and 3 had poor effects on reducing residual monohydrate content, odor and VOC.
[0208] The technical features of the above-mentioned embodiments can be combined arbitrarily. In order to make the description concise, not all possible combinations of the technical features in the above-mentioned embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0209] The above-described embodiments merely illustrate several implementations of the present invention, and while their descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the patent. It should be noted that a person skilled in the art would be able to make numerous variations and improvements without departing from the spirit of the present invention, all of which fall within the scope of protection of the present invention. Therefore, the scope of protection of the patent for this invention shall be determined by the appended claims.
Claims
1. A modified ABS rubber powder, It is characterized in that The modified ABS rubber powder contains residual single adsorbent and transition metal element doped modified titanium dioxide; The residual monomer adsorbent includes diatomaceous earth, molecular sieve, porous silicate or a combination thereof.
2. The modified ABS rubber powder according to claim 1, It is characterized in that The transition metal element is palladium, platinum or a combination thereof.
3. The modified ABS rubber powder according to any one of claims 1-2, It is characterized in that In the transition metal element doped modified titanium dioxide, the molar ratio of the transition metal element to the titanium element is 1:(1-5).
4. The modified ABS rubber powder according to any one of claims 1 to 3, It is characterized in that One or more of the following conditions are met: 1) The residual adsorbent accounts for 0.2wt% to 1.5wt% of the modified ABS rubber powder; 2) The transition metal element doped modified titanium dioxide accounts for 0.2wt% to 1.5wt% of the modified ABS rubber powder; 3) the content of polybutadiene in the modified ABS rubber powder is 50wt% to 70wt%; and 4) The content of acrylonitrile-styrene copolymer in the modified ABS rubber powder is 27wt% to 49.6wt%; the polymerization monomers of the acrylonitrile-styrene copolymer include acrylonitrile monomer and styrene monomer in a weight ratio of (50-150):(250-350).
5. A method for preparing modified ABS rubber powder, It is characterized in that The following steps are involved: Mixing butadiene latex, acrylonitrile monomer and styrene monomer, performing emulsion graft copolymerization reaction to obtain grafted latex, and flocculating the grafted latex to prepare flocculated slurry; Mixing the washing liquid and the flocculated slurry, collecting the solid and drying it to prepare modified ABS rubber powder; The washing liquid comprises a residual single adsorbent and titanium dioxide doped and modified by transition metal elements; The residual monomer adsorbent includes diatomaceous earth, molecular sieve, porous silicate or a combination thereof.
6. The method for preparing the modified ABS rubber powder according to claim 5, It is characterized in that The preparation method of the washing liquid comprises the following steps: Using tetrabutyl titanate as a precursor and transition metal salt as a doping source, a transition metal element-doped titanium dioxide gel was prepared by a sol-gel method. The transition metal element doped modified titanium dioxide gel, residual adsorbent and washing solvent are mixed to prepare a washing liquid.
7. The method for preparing the modified ABS rubber powder according to claim 6, It is characterized in that The preparation method of the washing liquid meets one or more of the following conditions: 1) The transition metal salt is a palladium salt, a platinum salt or a combination thereof; 2) The molar ratio of the transition metal salt to the tetrabutyl titanate is 1:(1-5).
8. A method for preparing the modified ABS rubber powder according to any one of claims 5 to 7, It is characterized in that The concentration of the residual adsorbent in the washing liquid is 0.5 wt % to 1 wt %.
9. A method for preparing the modified ABS rubber powder according to any one of claims 5 to 7, It is characterized in that The concentration of the titanium dioxide doped with transition metal elements in the washing liquid is 0.5 wt % to 1 wt %.
10. A method for preparing the modified ABS rubber powder according to any one of claims 8 to 9, It is characterized in that The volume ratio of the washing liquid to the flocculation slurry is 1:(1.5-2.5).
11. A method for preparing the modified ABS rubber powder according to any one of claims 5 to 10, It is characterized in that One or more of the following conditions are met: 1) The butadiene latex is prepared by emulsion polymerization of butadiene monomer; 2) controlling the weight of the butadiene latex so that the content of polybutadiene in the modified ABS rubber powder is 50wt% to 70wt%; 3) controlling the weight of the acrylonitrile monomer and the styrene monomer so that the content of the acrylonitrile-styrene copolymer in the modified ABS rubber powder is 27wt% to 49.6wt%, and the weight ratio of the acrylonitrile monomer to the styrene monomer is (50 to 150): (250~350); 4) The chain transfer agent used in the emulsion graft copolymerization reaction is α-methylstyrene dimer; 5) The initiator used in the emulsion graft copolymerization reaction is selected from one or more of cumene hydroperoxide, sodium persulfate, potassium persulfate, ammonium persulfate and azobisisobutylnitrile; 6) the emulsifier used in the emulsion graft copolymerization reaction is selected from one or more of sodium salt of pernaphthalenesulfonic acid formaldehyde condensate, potassium salt of naphthalenesulfonic acid formaldehyde condensate, potassium oleate, potassium stearate, potassium disproportionated rosin acid, sodium dodecylbenzene sulfonate and sodium dodecyl sulfonate; 7) The reducing agent used in the emulsion graft copolymerization reaction is selected from one or more of sodium ethylenediaminetetraacetate, ferrous sulfate, glucose, sodium pyrophosphate and sodium sulfite; 8) The solvent used in the emulsion graft copolymerization reaction is water; and 9) The flocculant used in the flocculation treatment is one or more selected from magnesium sulfate, sulfuric acid and calcium chloride.
12. An ABS resin, It is characterized in that The composition comprises the modified ABS rubber powder described in any one of claims 1 to 4 or the modified ABS rubber powder prepared by the preparation method described in any one of claims 5 to 11, and SAN resin.
13. A vehicle interior component, It is characterized in that Its components include the modified ABS rubber powder described in any one of claims 1 to 4, the modified ABS rubber powder prepared by the preparation method described in any one of claims 5 to 11, or the ABS resin described in claim 12.
Citation Information
Patent Citations
Preparation method of monolithic catalyst for degrading VOCS (Volatile Organic Compounds)
CN103100386A
Metal modified titanium dioxide aqueous sol with high visible light activity, as well as synthesis and application of metal modified titanium dioxide aqueous sol
CN106111126A
Low-odor sterilization reinforced ABS (acrylonitrile butadiene styrene) automobile rearview mirror frame material and method for preparing same
CN107915948A
ABS rubber powder with low impurity content, and preparation method thereof, and ABS resin
CN110964133A
Modified ABS (Acrylonitrile Butadiene Styrene) rubber powder and preparation method thereof, ABS resin and vehicle interior trim part
CN116554409A