Conductive paste composition

The conductive paste composition, featuring a high epoxy equivalent epoxy resin and phenolic ester curing agent, effectively addresses the challenge of achieving thermal shock and moist heat resistance while maintaining electrical properties, enhancing the performance of epoxy resin-based compositions.

WO2024236964A1PCT designated stage expired Publication Date: 2024-11-21KYOTO ELEX
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/014649
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-12
Filing Date
2024-04-11
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Conductive paste compositions containing epoxy resin struggle to achieve both thermal shock resistance and moist heat resistance while maintaining good electrical properties, as improving thermal shock resistance often compromises heat and humidity resistance.

Method used

A conductive paste composition with a resin component that includes an epoxy resin with an epoxy equivalent of 500 g/eq or more, a phenolic ester compound as the curing agent, and a curing accelerator, which provides a cured product with both good thermal shock resistance and moist heat resistance.

Benefits of technology

The composition achieves excellent thermal shock resistance and moist heat resistance while maintaining good electrical properties, addressing the limitations of existing epoxy resin-based conductive paste compositions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024014649_21112024_PF_FP_ABST
    Figure JP2024014649_21112024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a conductive paste composition that contains an epoxy resin as a resin component and that is capable of realizing favorable thermal shock resistance and favorable moist heat resistance after curing. The conductive paste composition contains (A) a conductive powder, (B) an epoxy resin which serves as a resin component, (C) a curing agent, and (D) a curing accelerator. The (B) epoxy resin includes at least one type of epoxy resin having an epoxy equivalent of 500 g / eq or more. The (C) curing agent is a phenolic ester compound having a structure represented by formula (1). In the formula, R is a C1 to C10 alkyl group, a phenyl group, an aralkyl group, an alkoxyl group, or a halogen atom. In the formula, X is a hydrogen atom or an ester structure represented by -C(=O)-A (where A is a C1 to C6 alkyl group). In the formula, Z is a C1 to C15 divalent hydrocarbon group. In the formula, m is an integer from 0 to 4, and n is a number having an average value from 0 to 2.
Need to check novelty before this filing date? Find Prior Art

Description

Conductive paste composition

[0001] The present invention relates to a thermosetting conductive paste composition, and in particular to a conductive paste composition that can be suitably used in the field of electronic components.

[0002] In the field of electronic components, a technique using a conductive paste composition has been widely used as one of the methods for forming electrical connections. Various types of such conductive paste compositions are known, and an example of a thermosetting conductive paste composition is a composition containing a conductive powder and an epoxy resin as a resin component.

[0003] Epoxy resins have advantages such as good adhesion to metals constituting electronic components, good heat resistance, and relatively little volume shrinkage upon curing, and therefore are widely used as the resin component of conductive paste compositions.

[0004] In recent years, there has been an increasing demand for electronic components to be smaller, lighter, more precise, and more reliable. Therefore, various studies have been conducted on conductive paste compositions to meet these requirements. For example, Patent Document 1 discloses a conductive adhesive that uses a liquid epoxy resin and a solid epoxy resin in combination to achieve both stress relaxation and heat resistance when mounting chip components on a substrate.

[0005] Japanese Patent Application Laid-Open No. 2007-277384

[0006] Here, a conductive paste composition containing an epoxy resin as a resin component is required to have both thermal shock resistance and moist heat resistance after curing. However, when the resin component is an epoxy resin, an attempt to improve the thermal shock resistance tends to result in a decrease in moist heat resistance.

[0007] In recent years, as described above, higher requirements have been placed on electronic components, and therefore conductive paste compositions are required to have both thermal shock resistance and moist heat resistance. However, no conductive paste composition containing an epoxy resin has been known that can achieve both of these properties more effectively. For example, the conductive adhesive described in Patent Document 1 aims to achieve both stress relaxation and heat resistance as described above, but no consideration has been given to thermal shock resistance or moist heat resistance.

[0008] The present invention has been made to solve these problems, and an object of the present invention is to provide a conductive paste composition containing an epoxy resin as a resin component, which is capable of realizing good thermal shock resistance and good moist heat resistance after curing.

[0009] In order to solve the above-mentioned problems, the conductive paste composition according to the present disclosure contains (A) a conductive powder and a resin component, the resin component contains (B) an epoxy resin, (C) a curing agent, and (D) a curing accelerator, the (B) epoxy resin contains at least one epoxy resin having an epoxy equivalent of 500 g / eq or more, and the (C) curing agent is a compound represented by the following general formula (1):

[0010]

[0011] (wherein R in formula (1) is an alkyl group having 1 to 10 carbon atoms, a substituted or unsubstituted phenyl group, a substituted or unsubstituted aralkyl group, an alkoxyl group, or a halogen atom; X in formula (1) is a hydrogen atom or an ester structure represented by the following general formula (2); A in formula (2) is an alkyl group having 1 to 6 carbon atoms;

[0012] Z in formula (1) is a divalent hydrocarbon group having 1 to 15 carbon atoms, m in formula (1) is an integer of 0 to 4, n in formula (1) is a number of 0 to 2 on average, R, X, Z, and A included in formula (1) may be the same substituent or atom or may be different substituents or atoms, and m in formula (1) may be the same integer or may be different integers.

[0013] According to the above configuration, the (B) epoxy resin contained as the resin component is one or more epoxy resins having an epoxy equivalent of 500 g / eq or more, and the (C) curing agent is a phenolic ester compound of the general formula (1). This allows the resulting cured product of the conductive paste composition to have good thermal shock resistance and good moist heat resistance while maintaining good electrical properties. Therefore, a conductive paste composition containing an epoxy resin as a resin component can be obtained that can achieve good thermal shock resistance and good moist heat resistance after curing.

[0014] In the conductive paste composition having the above-described configuration, the epoxy resin (B) may contain 30 mass % or more of an epoxy resin having an epoxy equivalent of 500 g / eq or more.

[0015] In the conductive paste composition having the above-described configuration, the esterification rate of the curing agent (C) may be 70% or more.

[0016] In addition, the conductive paste composition having the above-described configuration may be configured such that the (C) curing agent is blended in an amount within the range of 3 to 150 parts by mass with respect to 100 parts by mass of the (B) epoxy resin.

[0017] In addition, in the conductive paste composition having the above configuration, the (A) conductive powder may be at least one selected from the group consisting of silver powder, copper powder, silver-coated copper powder, silver-coated nickel powder, silver-coated aluminum powder, and silver-coated glass powder.

[0018] The conductive paste composition having the above-described structure may be used by being applied to a substrate using a printer, a dispenser, or by dipping.

[0019] The conductive paste composition having the above-described structure may be used by being applied to an electrode of an electronic component.

[0020] The present invention has the above-described configuration, which has the effect of providing a conductive paste composition containing an epoxy resin as a resin component, which can achieve good thermal shock resistance and good moist heat resistance after curing.

[0021] 1 is a plan view showing the shape of a conductor pattern for evaluating the conductor resistance of a conductor pattern (cured product) obtained by curing a conductive paste composition according to an embodiment of the present disclosure, and FIG. 2 is a model diagram schematically showing the configuration of an evaluation sample used to evaluate the connection resistance and adhesive strength of the conductive paste composition after curing in an embodiment of the present disclosure.

[0022] Representative embodiments of the present disclosure will be described below. The conductive paste composition according to the present disclosure contains (A) a conductive powder and a resin component, and the resin component contains (B) an epoxy resin, (C) a curing agent, and (D) a curing accelerator. The (B) epoxy resin contains at least one epoxy resin having an epoxy equivalent of 500 g / eq or more. Furthermore, the (C) curing agent is a compound having a structure represented by the general formula (1) described below, i.e., a compound obtained by esterifying the phenolic hydroxyl group of a polyhydric phenol compound. In the present disclosure, this compound is referred to as a phenolic ester compound.

[0023] [(A) Conductive Powder] The specific constitution of the conductive powder (A) contained in the conductive paste composition according to the present disclosure is not particularly limited, and conductive powders known in the field of conductive paste compositions can be suitably used. Representative examples include at least one selected from the group consisting of silver powder, copper powder, silver-coated copper powder, silver-coated nickel powder, silver-coated aluminum powder, and silver-coated glass powder.

[0024] In the examples described later in this disclosure, flake-shaped or spherical silver powder or spherical silver-coated copper powder is exemplified as a representative (A) conductive powder. Therefore, in this disclosure, a powder containing at least silver is used as the (A) conductive powder. For convenience of explanation, a powder containing silver will be referred to as a "silver-based powder" as appropriate.

[0025] Specific examples of silver-based powders include silver powders that are essentially composed of silver, silver-coated powders in which silver is coated on the surface of powder (main powder) that is composed of a material other than silver, and silver alloy powders that are composed of an alloy containing silver (silver alloy).

[0026] Silver powder is a powder composed only of silver, but it goes without saying that it may contain known unavoidable impurities. In addition, even if it is a silver alloy powder, if it has a purity that is recognized as "silver" according to various known standards, it can be treated as silver powder in this disclosure.

[0027] The specific composition of the silver-coated powder is not particularly limited, and the main powder composed of a material other than silver may be a metal or a material other than a metal. Examples of the material other than a metal include known resin materials, known ceramic materials, and glass. When the main powder is a resin material, it is sufficient that the resin material has heat resistance sufficient to maintain the powder shape (particle shape) even at the heating temperature used to harden the conductive paste composition according to the present disclosure.

[0028] Silver-coated powders in which the main powder is a metal, i.e., silver-coated metal powders, include, but are not limited to, silver-coated copper powders, silver-coated copper alloy powders, silver-coated nickel powders, silver-coated aluminum powders, etc. Silver-coated powders in which the main powder is glass, i.e., silver-coated glass powders, are not particularly limited to the specific type of glass. Examples include various known glass powders coated with silver.

[0029] Examples of silver-coated powders in which the main powder is a resin, i.e., silver-coated resin powders, include, but are not limited to, silver-coated silicone resin powders, etc. Examples of silver-coated powders in which the main powder is a ceramic material, i.e., silver-coated ceramic powders, include, but are not limited to, silver-coated alumina powders, etc.

[0030] When the silver-based powder is a silver-coated powder, the amount of silver coated on the surface of the main powder, i.e., the silver coating amount, is not particularly limited and can be set appropriately depending on various conditions. The silver coating amount can be increased or decreased depending on the volume resistivity required for the application of the conductive paste composition according to the present disclosure (application of the cured product). Alternatively, the silver coating amount can be increased or decreased depending on the material (conductivity) of the main powder. The silver coating amount can be expressed as the ratio of the mass of coated silver to the total mass of the silver-coated powder (mass ratio, for example, percentage (mass%), etc.).

[0031] The specific shape of the silver-based powder (or other conductive powder) is not particularly limited, and may be spherical (granular) or flake-like (thin or scale-like). Note that the flake-like powder may be powder that has a shape similar to a flat plate or a thin rectangular parallelepiped when viewed as a whole, even if it has partial irregularities and deformations. The spherical powder may be powder that has a three-dimensional shape closer to a cube than a rectangular parallelepiped when viewed as a whole, even if it has partial irregularities and deformations.

[0032] The specific physical properties of the silver-based powder (or other conductive powder) are not particularly limited, and the average particle size, specific surface area, tap density, etc. may be within known ranges. For example, if the silver-based powder is a flake-shaped powder, the average particle size D50 may be within a range of, for example, 0.5 to 20 μm, and the BET specific surface area may be within a range of, for example, 0.1 to 2.0 m. 2 / g, and the tap density is, for example, 0.5 to 10 g / cm 3 The aspect ratio may be within a range of, for example, 5 to 15. If the silver-based powder is a spherical powder, the average particle size D50 may be within a range of 0.1 to 10 μm, and the BET specific surface area may be within a range of 0.5 to 2.0 m. 2 / g, and the tap density is, for example, 1.0 to 10 g / cm 3 Conductive powders other than silver-based powders may also be used as long as they fall within the range of these physical properties.

[0033] The method for measuring (evaluating) the average particle size D50 of the conductive powder is not particularly limited, but in the present disclosure, it may be measured (evaluated) by laser diffraction using a Microtrac particle size distribution analyzer, as in the Examples described below. The method for evaluating the BET specific surface area of ​​the conductive powder is also not particularly limited, but it may be measured and evaluated by the BET single-point method using nitrogen adsorption using a known specific surface area meter, as in the Examples described below. The method for evaluating the tap density of the conductive powder is also not particularly limited, but it may be evaluated by tapping under specified conditions using a known tap density measuring device, and calculating the sample mass relative to the sample volume after tapping, as in the Examples described below.

[0034] The various conditions in the various measurement or evaluation methods for the (A) conductive powder containing these silver-based powders can be conditions known in the field of resin-type conductive pastes (for example, conditions described in the published patent applications of the applicant of the present application).

[0035] Whether the silver-based powder is a silver powder (or a silver alloy powder) or a silver-coated powder, or whether the shape of the silver-based powder is flake-like or spherical, the method for producing the powder is not particularly limited, and any known method can be used.

[0036] When the silver powder (or silver alloy powder) is a flake powder, for example, a spherical powder produced by a known method can be used as a base powder and subjected to a known mechanical treatment to produce the flake powder. The particle size, degree of aggregation, and other physical properties of the base powder can be appropriately selected depending on, for example, the intended use of the conductive paste composition (such as the type of electrode or electrical wiring that is the cured product, or the type of electronic component or electronic device that includes such an electrode or electrical wiring).

[0037] Furthermore, when the silver powder (or silver alloy powder) is a spherical powder, the method for producing it is not particularly limited, and examples thereof include powder produced by a wet reduction method, and spherical powder produced by other known methods such as an electrolytic method or an atomization method. In the case of a silver-coated powder, the surface of the flake-shaped or spherical main powder produced as described above may be coated with silver by a known method.

[0038] In the conductive paste composition according to the present disclosure, at least a silver-based powder may be used as the conductive powder (A), but a conductive powder other than the silver-based powder may also be used in combination. Examples of such other conductive powders include, but are not limited to, gold powder, copper powder, palladium powder, nickel powder, aluminum powder, lead powder, and carbon powder. A representative example is copper powder.

[0039] When multiple types of powders are used in combination as the (A) conductive powder, the blending ratio (blending amount) is not particularly limited. For example, when a silver-based powder is used in combination with a conductive powder other than the silver-based powder, the silver-based powder may be contained in at least more than 10 mass% of all the (A) conductive powders, and may be contained in 50 mass% or more, 90 mass% or more, or 95 mass% or more. The blending amount when using other conductive powders in combination can be appropriately set depending on the conditions required for the resulting cured product.

[0040] [(B) Epoxy Resin] The specific structure of the (B) epoxy resin used as one of the resin components in the present disclosure is not particularly limited, but as the (B) epoxy resin, at least one epoxy resin having an epoxy equivalent of 500 g / eq or more is used.

[0041] For convenience of explanation, an epoxy resin having an epoxy equivalent of 500 g / eq or more will be referred to as a “first epoxy resin,” and an epoxy resin having an epoxy equivalent of less than 500 g / eq will be referred to as a “second epoxy resin.” In the present disclosure, as the (B) epoxy resin, only the first epoxy resin may be used, or the first epoxy resin and the second epoxy resin may be used in combination.

[0042] When the first epoxy resin is used as the (B) epoxy resin, and a phenolic ester compound is used as the (C) curing agent, as described below, the resulting cured product of the conductive paste composition can have both good thermal shock resistance and good moist heat resistance while maintaining good electrical properties.

[0043] When the first epoxy resin and the second epoxy resin are used in combination, the content of the first epoxy resin in all of the epoxy resins (B) is not particularly limited, but is typically 30% by mass or more. When the content of the first epoxy resin is 30% by mass or more, both the thermal shock resistance and the moist heat resistance can be more favorably achieved.

[0044] In the present disclosure, as the (B) epoxy resin, only one type of first epoxy resin may be used, or two or more types may be used in appropriate combination. Furthermore, when a second epoxy resin is used in combination as the (B) epoxy resin, only one type of second epoxy resin may be used, or two or more types may be used in appropriate combination.

[0045] In the present disclosure, regardless of whether it is the first epoxy resin or the second epoxy resin, the specific type of epoxy resin used as the epoxy resin (B) is not particularly limited. A representative example is a polyhydric epoxy resin having two or more oxirane rings (epoxy groups) in one molecule.

[0046] Examples of such polyhydric epoxy resins include glycidyl ether type, glycidyl amine type, glycidyl ester type, and alicyclic type. Glycidyl ether type resins can be obtained, for example, by reacting epichlorohydrin with novolak, polyhydric phenol, polyhydric alcohol, etc. Examples of novolak include phenol novolak and cresol novolak. Examples of polyhydric phenols include bisphenol A, hydrogenated bisphenol A, bisphenol F, bisphenol AD, and resorcinol. Examples of polyhydric alcohols include ethylene glycol, neopentyl glycol, glycerin, trimethylolpropane, pentaerythritol, triethylene glycol, and polypropylene glycol. Examples of monofunctional glycidyl ether type epoxy resins include phenyl glycidyl ether. Glycidyl amine type resins can be obtained, for example, by reacting epichlorohydrin with a polyamino compound such as ethylenediamine, triethylenetetramine, or aniline. Glycidyl ester type epoxy resins can be obtained, for example, by reacting epichlorohydrin with a polycarboxylic acid compound such as adipic acid, phthalic acid, or isophthalic acid. Alicyclic type epoxy resins can be synthesized by oxidizing olefins. These epoxy resins can be used alone or in combination of two or more.

[0047] In the examples described below, a commercially available bisphenol A epoxy resin is used as the first epoxy resin (epoxy equivalent: 500 g / eq or more), and a commercially available bisphenol A epoxy resin, bisphenol F epoxy resin, or phenol novolac epoxy resin is used as the second epoxy resin (epoxy equivalent: less than 500 g / eq).

[0048] [(C) Curing Agent] In the present disclosure, the (C) curing agent used as one of the resin components together with the (B) epoxy resin is a compound obtained by esterifying the phenolic hydroxyl group of a polyhydric phenol compound with an organic acid. More specifically, the (C) curing agent according to the present disclosure may be a phenol ester compound having a structure represented by the following general formula (1):

[0049]

[0050] In general formula (1), R is an alkyl group having 1 to 10 carbon atoms, a substituted or unsubstituted phenyl group, a substituted or unsubstituted aralkyl group, an alkoxyl group, or a halogen atom. Furthermore, X in general formula (1) is a hydrogen atom or an ester structure represented by the following general formula (2). In general formula (2), A is an alkyl group having 1 to 6 carbon atoms. Furthermore, Z in general formula (1) is a divalent hydrocarbon group having 1 to 15 carbon atoms.

[0051]

[0052] The R, X, Z, and A contained in the general formula (1) may each independently be the substituent or atom described above. That is, in the general formula (1), the R, X, Z, and A may each be the same substituent or atom, or may each be a different substituent or atom (including the case where some of the R, X, Z, and A in the molecule are the same and the other parts are different substituents or atoms).

[0053] Furthermore, m in general formula (1) is an integer of 0 to 4, and n in general formula (1) is an average value of 0 to 2. All m in formula (1) may be the same integer, or may be different integers (including the case where some m in a molecule are the same integer and other m are different integers).

[0054] By using such a phenolic ester compound as the curing agent (C) for the epoxy resin (B) containing the first epoxy resin, the resulting cured product of the conductive paste composition can achieve good electrical properties as well as good thermal shock resistance and good moist heat resistance.

[0055] The esterification rate of the phenolic ester compound as the (C) curing agent is not particularly limited, but typically 70% or more, or may be 80% or more, or may be 90% or more. When the esterification rate of the phenolic ester compound is 70% or more, when the phenolic ester compound is used as the (C) curing agent for the (B) epoxy resin containing at least one first epoxy resin as the (B) epoxy resin, it is possible to easily achieve good thermal shock resistance and good moist heat resistance in the cured product of the obtained conductive paste composition.

[0056] The synthesis method (production method) of the phenolic ester compound represented by general formula (1) is not particularly limited, and known methods can be suitably used. For example, in the examples described later, a commercially available phenolic resin (e.g., phenol novolac resin or cresol novolac resin) is reacted with a carboxylic acid anhydride (e.g., acetic anhydride or propionic anhydride) by a known method to synthesize the phenolic ester compound. The esterification rate of the phenolic ester compound used in the examples described later is 90% or more (95% or 93%).

[0057] In the present disclosure, the amount of the (C) curing agent used (the amount of the (C) curing agent blended in the conductive paste composition) is not particularly limited. Typically, the amount of the (C) curing agent blended may be in the range of 3 to 150 parts by mass when the total amount of the (B) epoxy resin contained in the conductive paste composition is taken as 100 parts by mass. In the examples described below, the amount of the (C) curing agent used per 100 parts by mass of the (B) epoxy resin is exemplified as 4.1 to 33.3 parts by mass.

[0058] In the present disclosure, the phenol compound before esterification used in the synthesis of the phenol ester compound as the curing agent (C) is not particularly limited. Specific examples include known polyhydric phenol compounds such as phenol novolac resin, cresol novolac resin, aromatic hydrocarbon formaldehyde resin-modified phenol resin, dicyclopentadiene phenol adduct resin, phenol aralkyl resin (Xyloc resin), naphthol aralkyl resin, triphenylol methane resin, tetraphenylol ethane resin, naphthol novolac resin, naphthol-phenol co-condensed novolac resin, naphthol-cresol co-condensed novolac resin, and terpene phenol resin.

[0059] The organic acid used to esterify these phenolic compounds is not particularly limited. Representative examples include acetic acid, propionic acid, butyric acid, valeric acid, oxalic acid, succinic acid, maleic acid, phthalic acid, and benzoic acid. These organic acids may be anhydrides, as described above.

[0060] The phenol ester compound (C) may be used alone or in combination of two or more. A known curing agent other than the phenol ester compound may also be used in combination, provided that it does not affect the physical properties of the resulting conductive paste composition or the cured product thereof.

[0061] [(D) Curing Accelerator] In the present disclosure, a (D) curing accelerator is used as a resin component together with the (B) epoxy resin and the (C) curing agent. The specific (D) curing accelerator is not particularly limited, and may be a known compound used to cure the first epoxy resin used as the (B) epoxy resin, or the first epoxy resin and the second epoxy resin.

[0062] Specific examples of the (D) curing accelerator include phthalic anhydride, trimellitic anhydride, pyromellitic anhydride, maleic anhydride, tetrahydrophthalic anhydride, and methyltetrahydroanhydride. Acid anhydrides such as phthalic acid, hexahydrophthalic anhydride, methylhexahydrophthalic anhydride, and succinic anhydride; imidazoles such as imidazole, 2-methylimidazole, 2-ethyl-4-methylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 1-benzyl-2-methylimidazole, 2-phenyl-4-methylimidazole, 1-cyanoethyl-2-methylimidazole, 1-aminoethyl-2-methylimidazole, 1-methylimidazole, and 2-ethylimidazole; dimethyloctylamine, dimethyldecylamine, dimethyllaurylamine, dimethylmyristylamine, dimethylpalmitylamine, dimethylstearylamine, dimethylbehenylamine, dilaurylmonoethylamine, methyldidecylamine, methyldioleylamine, triallylamine, and triisopropanol. tertiary amines such as boron trifluoride ethyl ether, boron trifluoride phenol, boron trifluoride piperidine, boron trifluoride acetate, boron trifluoride monoethylamine, boron trifluoride triethanolamine, and boron trifluoride monoethanolamine; Lewis acids or compounds thereof containing boron fluoride such as Amicure series PN-23 or MY-24 commercially available from Ajinomoto Fine-Techno Co., Ltd., and Fujicure series FXR-1020 or FXR-1030 commercially available from Fuji Chemical Industry Co., Ltd.; dicyandiamide; and the like.

[0063] These curing accelerators (D) may be used alone or in combination of two or more. The amount or conditions of use of the curing accelerator (D) are not particularly limited, and it may be used in a known amount or under known conditions.

[0064] In the examples described below, Examples 1 to 14 and Comparative Examples 1 to 7 all use 2-ethyl-4-methylimidazole as the curing accelerator (D).

[0065] [Method for producing conductive paste composition and its use] The method for producing the conductive paste composition according to the present disclosure is not particularly limited, and known methods can be suitably used. As a typical example, the components (A) to (D) described above, as well as other components that are added or mixed as needed, are mixed in a predetermined mixing ratio (by mass) and then made into a paste using a known kneading device. Examples of the kneading device include a three-roll mill.

[0066] The blending amount (content) of each of the components (A) to (D) in the conductive paste composition according to the present disclosure is not particularly limited, provided that the blending amount of the conductive powder (A) is within a range of 70 to 99 mass%, or may be within a range of 80 to 98 mass%, or may be within a range of 85 to 95 mass%, when the total amount of the conductive powder (A) and the resin component is taken as 100 mass%.

[0067] If the blending amount of the (A) conductive powder is less than 70% by mass, the contact density between the (A) conductive powder particles in the cured conductive paste composition (cured product) will be small, and poor contact between the (A) conductive powder particles will result in insufficient conductivity, which may lead to an increase in volume resistivity. On the other hand, if the content of the (A) conductive powder is more than 99% by mass, the amount of the resin component will be small, and the (A) conductive powder may not be able to be uniformly dispersed.

[0068] The conductive paste composition according to the present disclosure may contain, as necessary, a solvent known in the field of conductive paste compositions, as well as various additives, in addition to the aforementioned (A) conductive powder and resin components ((B) epoxy resin, (C) curing agent, and (D) curing accelerator). While the additives are not particularly limited, specific examples include leveling agents, antioxidants, ultraviolet absorbers, silane coupling agents, antifoaming agents, and viscosity adjusters. These additives may be added within a range that does not impair the effects of the present invention.

[0069] The solvent is added to adjust the physical properties, such as the viscosity or fluidity, of the conductive paste composition according to the present disclosure. The physical properties of the conductive paste composition according to the present disclosure are not particularly limited, but the viscosity thereof can be, for example, within a range of 75 to 100 Pa·s, from the viewpoint of convenience in forming patterns of electrodes, electrical wiring, etc., particularly the efficiency of screen printing. If the viscosity of the conductive paste composition is within this range, pattern formation by screen printing can be carried out satisfactorily.

[0070] The specific type of solvent is not particularly limited, and examples thereof include saturated hydrocarbons such as hexane; aromatic hydrocarbons such as toluene; glycol ethers (cellosolves) such as ethyl cellosolve, butyl cellosolve, and butyl cellosolve acetate; glycol ethers such as diethylene glycol diethyl ether and butyl diglycol (butyl carbitol and diethylene glycol monobutyl ether); acetate esters of glycol ethers such as butyl diglycol acetate and butyl carbitol acetate; alcohols such as diacetone alcohol, terpineol, and benzyl alcohol; ketones such as cyclohexanone and methyl ethyl ketone; esters such as DBE, 2,2,4-trimethyl-1,3-pentanediol monoisobutyrate, and 2,2,4-trimethyl-1,3-pentanediol diisobutyrate; etc. These solvents may be used alone or in appropriate combinations of two or more.

[0071] The amount of solvent to be added is not particularly limited, and can be an amount that can adjust the viscosity or fluidity of the conductive paste composition according to the present disclosure within a suitable range. If the content of the solvent exceeds 40 mass% with respect to the entire conductive paste composition, fluidity suitable for printing may not be obtained, and printability may be reduced, although this depends on the types of other components or the composition of the conductive paste composition.

[0072] The method for forming a predetermined pattern on a substrate using the conductive paste composition according to the present disclosure is not particularly limited, and various known forming methods can be suitably used. A representative example is a method using a printer that employs a screen printing method, but other printing methods such as gravure printing, offset printing, inkjet printing, dispenser printing, and dipping can also be applied.

[0073] Furthermore, the method for forming a pattern that will become a cured product using the conductive paste composition according to the present disclosure is not particularly limited, and various known forming methods can be suitably used. Representative examples include printing methods such as screen printing, gravure printing, offset printing, inkjet printing, dispenser printing, and dipping. Therefore, the conductive paste composition according to the present disclosure may be used by being applied to a substrate using a printer, a dispenser, or dipping.

[0074] The method for curing the conductive paste composition according to the present disclosure is not particularly limited, and known heating methods can be suitably used depending on the types of epoxy resin (B) and curing agent (C) that constitute the resin components. In the examples described below, when preparing an evaluation sample, the conductive paste composition is applied to a substrate and heated in a hot air dryer at 200°C for 60 minutes, but it goes without saying that the present disclosure is not limited to this heating method. In the present disclosure, the method for measuring or evaluating various physical properties of the cured product of the conductive paste composition is not particularly limited, and the methods exemplified in the examples described below can be suitably used.

[0075] The conductive paste composition according to the present disclosure can be suitably used in a wide range of applications in which a conductive cured product is formed by curing with heat. A typical example is the formation of patterned electrodes or electrical wiring on a substrate. Specific examples include external electrodes of chip-type electronic components; electrodes or electrical wiring of components used in RFID (Radio Frequency Identification), electromagnetic wave shielding, vibrator bonding, membrane switches, or electroluminescence; and collecting electrodes of solar cells. The conductive paste composition according to the present disclosure can be particularly suitably used in applications in which it is applied to electrodes of electronic components.

[0076] As described above, the conductive paste composition according to the present disclosure may be configured as follows: (A) a conductive powder and a resin component; the resin component contains (B) an epoxy resin, (C) a curing agent, and (D) a curing accelerator; the (B) epoxy resin contains at least one epoxy resin having an epoxy equivalent of 500 g / eq or more; and the (C) curing agent is a phenolic ester compound having a structure represented by the general formula (1) described above.

[0077] According to the above configuration, the (B) epoxy resin contained as the resin component is one or more epoxy resins having an epoxy equivalent of 500 g / eq or more, and the (C) curing agent is a phenolic ester compound of the general formula (1). This allows the resulting cured product of the conductive paste composition to have good thermal shock resistance and good moist heat resistance while maintaining good electrical properties. Therefore, a conductive paste composition containing an epoxy resin as a resin component can be obtained that can achieve good thermal shock resistance and good moist heat resistance after curing.

[0078] The present disclosure will be described in more detail based on examples and comparative examples, but the present invention is not limited thereto. Those skilled in the art can make various changes, modifications, and alterations without departing from the scope of the present invention. In the following examples, the evaluation method of (A) the conductive powder, the synthesis method of (C) the phenolic ester compound as a curing agent, and the evaluation method of the cured product were as follows.

[0079] [Method for evaluating (A) conductive powder] (1) Average particle size D50 The average particle size D50 of the (A) conductive powder shown in Table 1 was evaluated by laser diffraction. 0.3 g of a sample of the (A) conductive powder was weighed into a 50 ml beaker, 30 ml of isopropyl alcohol was added, and the powder was dispersed by treating it for 5 minutes in an ultrasonic cleaner (manufactured by AS ONE Corporation, product name: USM-1), and the average particle size D50 was measured and evaluated using a Microtrac particle size distribution analyzer (manufactured by Nikkiso Co., Ltd., product name: Microtrac particle size distribution analyzer 9320-HRA X-100).

[0080] (2) Evaluation of BET Specific Surface Area The BET specific surface area of ​​the (A) conductive powder shown in Table 1 was evaluated using a surface area analyzer (product name: Monosorb, manufactured by Quanta Chrome). 1 g of a sample of the (A) conductive powder was subjected to the surface area analyzer, and the specific surface area was measured and evaluated by the BET single-point method using nitrogen adsorption. In the BET specific surface area measurement, the degassing conditions before the measurement were 60°C for 10 minutes.

[0081] (3) Evaluation of Tap Density The tap density of the (A) conductive powder shown in Table 1 was evaluated using a tap density measuring device (Shibayama Scientific Instruments Manufacturing Co., Ltd., product name: bulk specific gravity measuring device SS-DA-2) according to the following calculation formula (3). A 15 g sample of the (A) conductive powder was weighed and placed in a 20 ml test tube, and tapped 1,000 times at a drop of 20 mm. The sample volume (cm) after tapping was measured using the tap density measuring device. 3 ) was measured, and the tap density was calculated and evaluated using the following formula (3): Tap density = sample mass / sample volume after tapping (3)

[0082] [Method for Evaluating Cured Products] (1) Evaluation of Conductive Resistance Using the conductive paste composition according to the Examples or Comparative Examples, a conductor pattern 11 shown in FIG. 1 was screen-printed on the surface of an alumina substrate, which served as a base material. As shown in FIG. 1, the conductor pattern 11 had rectangular terminals 11a and 11b located at both ends, and a zigzag wiring portion 11c connecting these terminals 11a and 11b. The alumina substrate on which the conductor pattern 11 had been formed was heated in a hot air dryer at 200°C for 60 minutes, thereby curing the conductor pattern 11 (conductive paste composition). This produced a sample for evaluating conductor resistance.

[0083] For the evaluation samples of each Example or Comparative Example, the film thickness of the cured conductive pattern 11 (cured product) was measured using a surface roughness meter (manufactured by Tokyo Seimitsu Co., Ltd., product name Surfcom 480A), and the electrical resistance was measured using a digital multimeter (manufactured by Advantest Corporation, product name R6551). Based on the measured film thickness and electrical resistance and the aspect ratio of the conductive pattern 11, the volume resistivity (μΩ cm) of the cured product of the conductive paste composition of each Example, Comparative Example, or Reference Example was calculated and evaluated.

[0084] (2) Method for Evaluating Connection Resistance As shown in FIG. 2 , the conductive paste composition of the example or comparative example was applied to a tin (Sn)-plated substrate 21 using a dispenser to form a paste layer 22 with a diameter of 2.5 mm. Then, a gold-plated rivet 23 having a circular fixing surface with a diameter of 5 mm was laminated on the paste layer 22. A 200 μm-thick polyimide film was used as a spacer to set the thickness of the paste layer 22 to 200 μm. Next, the tin-plated substrate 21 was heated in a hot air dryer at 200° C. for 60 minutes to harden the paste layer 22 and form a hardened layer. This produced a sample 20 for evaluating connection resistance.

[0085] The electrical resistance between the tin-plated substrate 21 and the gold-plated rivet 23 in the evaluation sample 20 was measured with an electrical resistance meter 24 (digital multimeter, manufactured by Advantest Corporation, product name: R6551) and was taken as the connection resistance of the cured layer. Measured connection resistance of less than 0.05 Ω was evaluated as "A," and that of 0.05 Ω or more was evaluated as "B."

[0086] (3) Evaluation Method of Moisture and Heat Resistance The aforementioned connection resistance evaluation sample was stored for 1000 hours in a thermo-hygrostat (manufactured by Espec Corporation, product name: SH-262) set to conditions of a temperature of 85°C and a humidity of 85% RH. The connection resistance of the connection resistance evaluation specimen before and after storage was measured in the same manner as in the evaluation of connection resistance described above. A case in which the rate of change in resistance value after storage relative to the initial resistance value before storage was less than 10% was rated "A," a case in which it was 10% or more but less than 20% was rated "B," and a case in which it was 20% or more was rated "C."

[0087] (4) Evaluation method for thermal shock resistance The above-mentioned sample for evaluation of connection resistance was subjected to 1000 heat cycles in which temperatures were held at -55°C and +125°C for 30 minutes each using a thermal shock device (manufactured by Espec Corporation, product name: TSE-11-A). The connection resistance of the test piece for connection resistance evaluation before and after the heat cycle was measured in the same manner as in the above-mentioned evaluation of connection resistance. When the rate of change in resistance value after storage relative to the initial resistance value before storage was less than 10%, it was rated as "A", when it was 10% or more but less than 20%, it was rated as "B", and when it was 20% or more, it was rated as "C".

[0088] [(A) Conductive Powder] In the conductive paste compositions according to the Examples and Comparative Examples, the (A) conductive powder was used in appropriate combination with three types of powder shown in Table 1. In each Example or Comparative Example, the (A) conductive powder is represented by the abbreviations shown in Table 1.

[0089]

[0090] [Resin Component] In the conductive paste compositions according to the Examples or Comparative Examples, the resin components were appropriately combined with five types of (B) epoxy resins and four types of (C) curing agents shown in Table 2. In addition, to cure these resins, (D) curing accelerators shown in Table 2 were used. In each Example or Comparative Example, the respective resins, curing catalysts, or initiators are represented by the abbreviations shown in Table 2, as with the (A) conductive powder.

[0091]

[0092] [Synthesis of Phenol Ester Compounds] Among the (C) curing agents shown in Table 2, the phenol ester compounds, acetylated phenol novolak resin designated by the abbreviation C-01 and propionated cresol novolak resin designated by the abbreviation C-02, were synthesized (produced) by the method described below.

[0093] (1) Synthesis of Acetylated Phenol Novolac Resin (C-01): 212 g of phenol novolac resin (manufactured by DIC Corporation, product name: PHENOLITE TD-2106 (C-03 in Table 2), hydroxyl equivalent: 106 g / eq) was placed in a 3-liter four-neck flask equipped with a thermometer, a condenser, a nitrogen inlet tube, and a stirrer, and 500 g of methyl isobutyl ketone was added and dissolved by stirring under a nitrogen atmosphere. 210 g of acetic anhydride and 200 g of pyridine were then added to the solution and dissolved. The solution was then reacted at 50°C for 4 hours. The resulting reaction solution was then diluted with 500 g of methyl isobutyl ketone and cooled. The cooled, diluted reaction solution was then thoroughly washed with distilled water and concentrated under reduced pressure to obtain an acetylated phenol novolac resin (esterification rate 95%) designated C-01.

[0094] (2) Synthesis of propionated cresol novolac resin (abbreviated as C-02): 238 g of cresol novolac resin (manufactured by DIC Corporation, product name: PHENOLITE KA-1165 (abbreviated as C-04 in Table 2), hydroxyl equivalent: 119 g / eq) was placed in a 3-liter four-neck flask equipped with a thermometer, a condenser, a nitrogen inlet tube, and a stirrer, and 500 g of methyl isobutyl ketone was added and dissolved by stirring under a nitrogen atmosphere. 267 g of propionic anhydride and 200 g of pyridine were then added to the solution and dissolved. The solution was then reacted at 50°C for 4 hours. The resulting reaction solution was then diluted with 500 g of methyl isobutyl ketone and cooled. The cooled, diluted reaction solution was then thoroughly washed with distilled water and concentrated under reduced pressure to obtain a propionated cresol novolac resin (esterification rate 93%) designated as C-02.

[0095] Example 1 (A) As the conductive powders, the flake silver powder designated A-01 and the spherical silver powder designated A-02 in Table 1 were selected.

[0096] Among the resin components, two types of epoxy resin (B) were used: a first epoxy resin having an epoxy equivalent of 500 g / eq or more, and a second epoxy resin having an epoxy equivalent of less than 500 g / eq. As the first epoxy resin, the epoxy resin designated by the abbreviation B-01 (epoxy equivalent: 3,000 g / eq) in Table 2 was selected, and as the second epoxy resin, the epoxy resin designated by the abbreviation B-03 (epoxy equivalent: 190 g / eq) was selected.

[0097] Of the resin components, a phenol ester compound (acetylated phenol novolak resin) designated C-01 in Table 2 was selected as the (C) curing agent, and an imidazole designated D-01 in Table 2 was used as the (D) curing accelerator.

[0098] These components (A) to (D) were blended in the composition (blending ratio) shown in Table 3. In Table 3 (and Tables 4 and 5 described below), the blending ratios of the two types of (A) conductive powders total 100 mass %. In Example 1, the mass ratio (A-01 / A-02) of the flaky silver powder designated A-01 to the spherical silver powder designated A-02 was 50 / 50.

[0099] In Table 3 (and Tables 4 and 5 described below), the resin component composition is such that the blending ratio of the epoxy resin (B) and the curing agent (C) totals 100% by mass. In Example 1, the mass ratio (B-01 / B-03 / C-01) of the first epoxy resin (abbreviated as B-01), the second epoxy resin (abbreviated as B-03), and the curing agent (abbreviated as C-01) is 25 / 50 / 25.

[0100] The content of the first epoxy resin in the (B) epoxy resin was 33.3 mass% (25 / (25+75)), and the amount of the (C) curing agent used was 33.3 mass parts per 100 mass parts of the (B) epoxy resin. In Table 3 (and Tables 4 and 5 described below), the amount of the (D) curing accelerator blended was 1 mass part per 100 mass parts of the resin components in total.

[0101] Furthermore, in Table 3 (and Tables 4 and 5 described below), the blending ratio of (A) conductive powder to the resin component is shown as a mass ratio. In Example 1, the mass ratio of the total amount of (A) conductive powder to the total amount of the resin components (B) epoxy resin and (C) curing agent (solid content mass ratio (A) / (B)+(C)) was 93 / 7. This also applies to each of the following Examples and Comparative Examples.

[0102] The components (A) to (D) blended according to the composition shown in Table 3 were kneaded in a three-roll mill to prepare (manufacture) the conductive paste composition according to Example 1.

[0103] Using the obtained conductive paste composition of Example 1, samples for evaluating conductor resistance and connection resistance (as well as moist heat resistance and thermal shock resistance) were prepared (manufactured) as described above. Using these evaluation samples, the properties of the cured product of the conductive paste composition (conductor resistance, connection resistance, moist heat resistance, and thermal shock resistance) were evaluated by the evaluation methods described above. The results are shown in Table 3.

[0104] Examples 2 and 3 A conductive paste composition according to Example 2 or Example 3 was prepared (manufactured) in the same manner as Example 1, except that either a phenolic ester compound (propionated cresol novolak resin) designated by the abbreviation C-02 in Table 2 was selected as the (C) curing agent (Example 2), or an epoxy resin designated by the abbreviation B-02 in Table 2 (epoxy equivalent: 8,000 g / eq) was selected as the first epoxy resin among the (B) epoxy resins, and an epoxy resin designated by the abbreviation B-04 in Table 2 (epoxy equivalent: 170 g / eq) was selected as the second epoxy resin (Example 3).

[0105] As described above, evaluation samples were prepared (manufactured) using the obtained conductive paste compositions of Examples 2 and 3. Using these evaluation samples, the properties of the cured products of the conductive paste compositions were evaluated by the evaluation methods described above. The results are shown in Table 3.

[0106] Examples 4 to 6 Conductive paste compositions according to Examples 4 to 6 were prepared (manufactured) in the same manner as in Example 3, except that (A) the compounding ratio of the conductive powders was A-01 / A-02 = 30 / 70 (Example 4), (B) the epoxy resin with the abbreviation B-03 was selected as the second epoxy resin among the epoxy resins, and the solid content mass ratio was (A) / (B) + (C) = 90 / 10 (Example 5), or the epoxy resin with the abbreviation B-03 was selected as the second epoxy resin, and (C) the phenol ester compound with the abbreviation C-02 was selected as the curing agent (Example 6).

[0107] The obtained conductive paste compositions according to Examples 4 to 6 were used to prepare (manufacture) evaluation samples as described above. Using these evaluation samples, the properties of the cured products of the conductive paste compositions were evaluated according to the evaluation methods described above. The results are shown in Table 3.

[0108] Example 7 A conductive paste composition according to Example 7 was prepared (manufactured) in the same manner as in Example 1, except that the epoxy resin (epoxy equivalent: 190 g / eq) abbreviated as B-05 in Table 2 was selected as the second epoxy resin among the (B) epoxy resins, and the solid content mass ratio was set to (A) / (B)+(C)=95 / 5.

[0109] As described above, evaluation samples were prepared (manufactured) using the obtained conductive paste composition of Example 7. Using these evaluation samples, the properties of the cured products of the conductive paste compositions were evaluated by the evaluation methods described above. The results are shown in Table 3.

[0110]

[0111] (Examples 8 to 10) An epoxy resin designated by the abbreviation B-05 was selected as the second epoxy resin from among the (B) epoxy resins, and the mass ratio of the first epoxy resin, the second epoxy resin, and the (C) curing agent was set to B-02 / B-05 / C-01) = 30 / 50 / 20 (Example 8), or an epoxy resin designated by the abbreviation B-03 was selected as the second epoxy resin, and the mass ratio of the first epoxy resin, the second epoxy resin, and the (C) curing agent was set to B-02 / B-03 / C-01) = 25 / 55 / 20, and further, the solid content mass The ratio was (A) / (B) + (C) = 85 / 15 (Example 9), or as the (A) conductive powder, in addition to the flaky silver powder of abbreviation A-01 and the spherical silver powder of abbreviation A-02, the silver-coated copper powder of abbreviation A-03 shown in Table 1 (silver coating amount relative to copper powder: 10 mass%) was used, and the mass ratio (compounding ratio) of these (A) conductive powders was A-01 / A-02 / A-03 = 30 / 30 / 40 (Example 10). Except for this, the conductive paste compositions according to Examples 8 to 10 were prepared (manufactured) in the same manner as in Example 3.

[0112] In Example 8, the content of the first epoxy resin in the epoxy resin (B) was 37.5 mass % (30 / (30+50)), and the amount of the curing agent (C) used was 25 parts by mass per 100 parts by mass of the epoxy resin (B).

[0113] As described above, evaluation samples were prepared (manufactured) using the obtained conductive paste composition of Example 8. Using these evaluation samples, the properties of the cured products of the conductive paste compositions were evaluated by the evaluation methods described above. The results are shown in Table 4.

[0114] Example 9 A conductive paste composition according to Example 9 was prepared (manufactured) in the same manner as in Example 4, except that an epoxy resin designated by the abbreviation B-03 was selected as the second epoxy resin, the mass ratio of the first epoxy resin, the second epoxy resin, and the (C) curing agent was set to B-02 / B-03 / C-01 (25 / 55 / 20), and the mass ratio of the solid contents was set to (A) / (B)+(C)=85 / 15. In Example 9, the amount of the (C) curing agent used was 26.6 parts by mass relative to 100 parts by mass of the (B) epoxy resin.

[0115] The obtained conductive paste composition of Example 9 was used to prepare (manufacture) evaluation samples as described above. Using these evaluation samples, the properties of the cured products of the conductive paste compositions were evaluated by the evaluation methods described above. The results are shown in Table 4.

[0116] (Example 10) As the (A) conductive powder, in addition to the flaky silver powder with the abbreviation A-01 and the spherical silver powder with the abbreviation A-02, a silver-coated copper powder with the abbreviation A-03 shown in Table 1 (amount of silver coated on copper powder: 10% by mass) was used, and the mass ratio (blending ratio) of these (A) conductive powders was A-01 / A-02 / A-03 = 30 / 30 / 40 (Example 10). Except for this, the conductive paste compositions according to Examples 8 to 10 were prepared (manufactured) in the same manner as in Example 3.

[0117] The obtained conductive paste composition according to Example 10 was used to prepare (manufacture) evaluation samples as described above. Using these evaluation samples, the properties of the cured products of the conductive paste compositions were evaluated by the evaluation methods described above. The results are shown in Table 4.

[0118] Example 11 A conductive paste composition according to Example 11 was prepared (manufactured) in the same manner as in Example 1, except that only the epoxy resin designated B-01, which is the first epoxy resin, was used as the (B) epoxy resin, and the mass ratio of the first epoxy resin to the (C) curing agent was B-01 / C-01=95 / 5. In Example 11, the content of the first epoxy resin in the (B) epoxy resin was 100 mass %, and the amount of the (C) curing agent used was 5.2 parts by mass per 100 parts by mass of the (B) epoxy resin.

[0119] The obtained conductive paste composition of Example 11 was used to prepare (manufacture) evaluation samples as described above. Using these evaluation samples, the properties of the cured products of the conductive paste compositions were evaluated by the evaluation methods described above. The results are shown in Table 4.

[0120] Example 12 A conductive paste composition according to Example 12 was prepared (manufactured) in the same manner as in Example 11, except that the epoxy resin (B) was a combination of the epoxy resin designated by the abbreviation B-01 and the epoxy resin designated by the abbreviation B-02 in a mass ratio of B-01 / B-02 = 50 / 45. In Example 12, the content of the first epoxy resin in the epoxy resin (B) was 52.6 mass% (50 / (50+45)), and the amount of the curing agent (C) used was 5.2 parts by mass per 100 parts by mass of the epoxy resin (B).

[0121] The obtained conductive paste composition of Example 12 was used to prepare (manufacture) evaluation samples as described above. Using these evaluation samples, the properties of the cured products of the conductive paste compositions were evaluated by the evaluation methods described above. The results are shown in Table 4.

[0122] (Examples 13 and 14) (A) The compounding ratio of the conductive powder was A-01 / A-02 = 70 / 30, the mass ratio of the first epoxy resin was B-01 / B-02 = 48 / 48, and the solid mass ratio was (A) / (B)+(C) = 87 / 13 (Example 13), or (A) The compounding ratio of the conductive powder was A-01 / A-02 = 20 / 80, the mass ratio of the first epoxy resin was B-01 / B-02 = 70 / 25, and the solid mass ratio was (A) / (B)+(C) = 91 / 9 (Example 14). Except for this, the conductive paste compositions according to Example 13 or Example 14 were prepared (manufactured) in the same manner as in Example 11.

[0123] In Example 13, the content of the first epoxy resin in the (B) epoxy resin was 50 mass % (48 / (48+48)), and the amount of the (C) curing agent used was 4.1 mass parts per 100 mass parts of the (B) epoxy resin. In Example 14, the content of the first epoxy resin in the (B) epoxy resin was 73.6 mass % (70 / (70+25)), and the amount of the (C) curing agent used was 5.2 mass parts per 100 mass parts of the (B) epoxy resin.

[0124] The conductive paste compositions of Examples 13 and 14 were used to prepare (manufacture) evaluation samples as described above. Using these evaluation samples, the properties of the cured products of the conductive paste compositions were evaluated according to the evaluation methods described above. The results are shown in Table 4.

[0125]

[0126] (Comparative Examples 1 and 2) A conductive paste composition according to Comparative Example 1 or Comparative Example 2 was prepared (manufactured) in the same manner as in Example 1, except that a phenol novolak resin (hydroxyl equivalent: 104 g / eq, Comparative Example 1) designated by the abbreviation C-03 in Table 2 or a cresol novolak resin (hydroxyl equivalent: 119 g / eq, Comparative Example 2) designated by the abbreviation C-04 in Table 2 was selected as the (C) curing agent without using a phenol ester compound.

[0127] As described above, evaluation samples were prepared (manufactured) using the obtained conductive paste compositions according to Comparative Examples 1 and 2. Using these evaluation samples, the properties of the cured products of the conductive paste compositions were evaluated according to the evaluation methods described above. The results are shown in Table 5.

[0128] Comparative Example 3 A conductive paste composition according to Comparative Example 3 was prepared (manufactured) in the same manner as in Example 5, except that a phenol novolak resin designated C-03 was selected as the (C) curing agent without using a phenolic ester compound.

[0129] As described above, evaluation samples were prepared (manufactured) using the obtained conductive paste composition according to Comparative Example 3. Using these evaluation samples, the properties of the cured products of the conductive paste compositions were evaluated according to the evaluation methods described above. The results are shown in Table 5.

[0130] Comparative Example 4 A conductive paste composition according to Comparative Example 4 was prepared (manufactured) in the same manner as in Example 1, except that, as the (B) epoxy resin, a first epoxy resin having an epoxy equivalent of 500 g / eq or more was not used, and only a second epoxy resin designated by the abbreviation B-03 was selected, and, as the (C) curing agent, an acetylated phenol novolak resin designated by the abbreviation C-01, which is a phenolic ester compound, was used, and the mass ratio of the second epoxy resin to the (C) curing agent was set to B-03 / C-01 = 65 / 35.

[0131] As described above, evaluation samples were prepared (manufactured) using the obtained conductive paste composition according to Comparative Example 4. Using these evaluation samples, the properties of the cured products of the conductive paste compositions were evaluated according to the evaluation methods described above. The results are shown in Table 5.

[0132] Comparative Examples 5 and 6 A conductive paste composition according to Comparative Example 5 or Comparative Example 6 was prepared (manufactured) in the same manner as in Comparative Example 4, except that either an epoxy resin designated by the abbreviation B-05 was selected as the second epoxy resin, and a propionated cresol novolak resin designated by the abbreviation C-02, which is a phenolic ester compound, was used as the (C) curing agent (Comparative Example 5), or an epoxy resin designated by the abbreviation B-05 was selected, and a phenol novolak resin designated by the abbreviation C-03, which is not a phenolic ester compound, was used as the (C) curing agent (Comparative Example 6).

[0133] The obtained conductive paste compositions according to Comparative Examples 5 and 6 were used to prepare (manufacture) evaluation samples as described above. Using these evaluation samples, the properties of the cured products of the conductive paste compositions were evaluated according to the evaluation methods described above. The results are shown in Table 5.

[0134] Comparative Example 7 A conductive paste composition according to Comparative Example 7 was prepared (manufactured) in the same manner as in Example 11, except that a phenol novolak resin designated C-03, which is not a phenol ester compound, was selected as the (C) curing agent.

[0135] As described above, evaluation samples were prepared (manufactured) using the obtained conductive paste composition according to Comparative Example 7. Using these evaluation samples, the properties of the cured products of the conductive paste compositions were evaluated according to the evaluation methods described above. The results are shown in Table 5.

[0136]

[0137] (Comparison of Examples and Comparative Examples) As is clear from the results of Examples 1 to 14, by containing a first epoxy resin having an epoxy equivalent of 500 g / eq or more as the epoxy resin (B) and using a phenolic ester compound represented by the general formula (1) as the curing agent (C), the obtained cured product can achieve good electrical properties (conductor resistance and connection resistance) and can also achieve good moist heat resistance and good thermal shock resistance.

[0138] Furthermore, as is clear from the results of Examples 1 to 10, by using a second epoxy resin having an epoxy equivalent of less than 500 g / eq together with a first epoxy resin as the epoxy resin (B), it is possible to improve all of the electrical properties, moist heat resistance, and thermal shock resistance. Alternatively, as is clear from the results of Examples 11 to 14, even when only the first epoxy resin is used as the epoxy resin (B), it is possible to improve all of the electrical properties, moist heat resistance, and thermal shock resistance.

[0139] In contrast, good thermal shock resistance cannot be achieved when the phenol ester compound represented by general formula (1) is not used as the (C) curing agent, as is clear from the results of Comparative Examples 1 to 3. Furthermore, as is clear from the results of Comparative Examples 4 and 5, even when the phenol ester compound having the structure represented by general formula (1) is used as the (C) curing agent, good moist heat resistance cannot be achieved when a first epoxy resin having an epoxy equivalent of 500 g / eq or more is not used.

[0140] Furthermore, as is clear from the results of Comparative Example 6, when the phenolic ester compound represented by general formula (1) is not used as the curing agent (C) and the first epoxy resin is not used, good thermal shock resistance cannot be achieved. Moreover, as is clear from the results of Comparative Example 7, even when only the first epoxy resin is used, good moist heat resistance cannot be achieved unless the phenolic ester compound represented by general formula (1) is used as the curing agent (C).

[0141] Based on the results of Comparative Examples 1 to 7, it can be seen that when the first epoxy resin is not used as the epoxy resin (B) or the phenolic ester compound represented by general formula (1) is not used as the curing agent (C), good electrical properties can be achieved, but either the moist heat resistance or the thermal shock resistance cannot be made good.

[0142] The present invention is not limited to the description of the above-described embodiments, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in different embodiments or multiple modified examples are also included in the technical scope of the present invention.

[0143] The present invention can be suitably used widely in the fields of electrical and electronic equipment, where a conductive cured product is formed, typically in the fields of forming a conductive layer on an electrode of an electronic component by application with a printer, a dispenser, or dipping.

[0144] 11: Conductive pattern 11a, 11b: Terminal 11c: Wiring portion 20: Evaluation sample 21: Tin-plated substrate 22: Paste layer (or hardened layer) 23: Gold-plated rivet 24: Electrical resistance meter

Claims

1. A conductive powder and a resin component (A), the resin component includes an epoxy resin (B), a curing agent (C), and a curing accelerator (D), the epoxy resin (B) includes at least one epoxy resin having an epoxy equivalent of 500 g / eq or more, and the curing agent (C) is represented by the following general formula (1): (In the formula (1), R is an alkyl group having 1 to 10 carbon atoms, a substituted or unsubstituted phenyl group, a substituted or unsubstituted aralkyl group, an alkoxyl group, or a halogen atom; X in the formula (1) is a hydrogen atom or an ester structure represented by the following general formula (2); A in the formula (2) is an alkyl group having 1 to 6 carbon atoms; wherein Z in formula (1) is a divalent hydrocarbon group having 1 to 15 carbon atoms, m in formula (1) is an integer of 0 to 4, n in formula (1) is a number of 0 to 2 on average, R, X, Z, and A included in formula (1) may be the same substituent or atom or different substituents or atoms, and m in formula (1) may be the same integer or different integers.

2. The conductive paste composition according to claim 1, wherein the epoxy resin (B) contains 30 mass % or more of an epoxy resin having an epoxy equivalent of 500 g / eq or more.

3. The conductive paste composition according to claim 1, wherein the esterification rate of the curing agent (C) is 70% or more.

4. The conductive paste composition according to claim 1, wherein the (C) hardener is blended in an amount within the range of 3 to 150 parts by mass per 100 parts by mass of the (B) epoxy resin.

5. The conductive paste composition according to claim 1, wherein the (A) conductive powder is at least one selected from the group consisting of silver powder, copper powder, silver-coated copper powder, silver-coated nickel powder, silver-coated aluminum powder, and silver-coated glass powder.

6. The conductive paste composition according to any one of claims 1 to 5, which is used by being applied onto a substrate by a printer, a dispenser, or by dipping.

7. The conductive paste composition according to any one of claims 1 to 5, which is used by being applied to an electrode of an electronic component.

Citation Information

Patent Citations

  • Conductive resin composition and conductive paste

    JP2005264095A

  • Epoxy resin, curable resin composition, and cured product thereof

    JP2020176189A

  • Epoxy resin, epoxy resin cured product, method for producing epoxy resin cured product, and epoxy resin composition

    JP2022135942A