Stretchable film and multilayer body provided with same
A stretchable film with an uneven surface and high tensile elongation maintains functionality and anti-glare properties when stretched, addressing the issue of cracking in conventional films by ensuring comfort and visibility in wearable and display applications.
Patent Information
- Application Number
- PCT/JP2024/018241
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-19
- Filing Date
- 2024-05-16
- Publication Date
- 2024-11-28
AI Technical Summary
Conventional stretchable films used in skin sensors and deformable image display devices suffer from reduced functionality due to cracking or fractures when stretched, as their anti-glare, antireflection, and hard coat layers are not elastic, and incorporating particles into the resin can lead to haze and image distortion.
A stretchable film with an uneven surface shape, achieving tensile elongation at break of over 20% in multiple directions, combined with an adhesive or functional layer, maintains surface roughness and anti-glare properties even when stretched, preventing damage and maintaining functionality.
The film can be stretched without degrading its function, preventing cracks and maintaining anti-glare properties, ensuring comfort and visibility in wearable devices and image display applications.
Smart Images

Figure JP2024018241_28112024_PF_FP_ABST
Abstract
Description
Stretchable film and laminate including same
[0001] The present invention relates to a stretchable film and a laminate comprising the same.
[0002] In recent years, with the declining birthrate and aging population and growing health consciousness, interest in home healthcare, telemedicine, preventive medicine, etc. has increased, and the development of biosensors that are attached to the body and continuously monitor biological information is progressing. Examples of such biosensors include wearable devices, smart textiles, patch sensors, and skin sensors. Among these, skin sensors, which are films that can be directly attached to the body, are expected to become more widespread due to demands for miniaturization and reduced wearing comfort.
[0003] Skin sensors come in several forms, including a small sensor that is placed in contact with the living body and then covered with a film, a small sensor that is embedded in a film, and a film that has circuits, electrodes, etc. printed on it so that the film itself becomes the sensor. The film used in skin sensors must have the following functions: it must be able to be attached to the living body while stretching, it must be able to follow the movements of the living body, it must have stretchability that allows it to be worn comfortably, and it must have excellent adhesion to the sensor material.
[0004] In recent years, it has become desirable for image display devices equipped with touch panels, such as smartphones, to be foldable. Furthermore, development of image display devices that can be deformed, such as by stretching, bending, or twisting, is also underway. Optical laminates installed in such deformable image display devices may be provided with an antiglare layer for suppressing reflection of lighting and people in the background, an antireflection layer for suppressing surface reflection, a hard coat layer for suppressing surface damage, and the like. Optical laminates used in deformable image display devices are required to be durable against deformation.
[0005] Patent Document 1 proposes a resin film as a stretchable film that can be used in medical films such as skin sensors and in films for image display devices.
[0006] An antiglare film is formed by forming a layer having an uneven surface. Means for imparting an uneven surface include a method of forming an antiglare layer containing a binder resin and particles on one surface of a substrate, as exemplified in Patent Document 2, and a method of forming an antiglare layer by shaping, as exemplified in Patent Document 3.
[0007] JP 2021-116405 A JP 2015-210273 A JP 2023-048729 A
[0008] Various layers may be provided on extensible films to impart functions according to the application. The antiglare layer, antireflection layer, hard coat layer, and printed circuits and electrodes exemplified above are generally not stretchable layers themselves. Therefore, when the film is stretched during application or use, cracks or fractures occur in these layers, resulting in a decrease or loss of functionality, which has been a problem. Furthermore, incorporating particles into the resin constituting the film to impart antiglare properties to the extensible resin itself has also been considered. However, when the film is stretched, the thickness of the resin portion becomes thin, which raises concerns about particle detachment. Furthermore, when the film is applied to an image display device, there is a risk of increased haze, making images difficult to see. The present invention has been made in consideration of the above-mentioned problems. It is an object of the present invention to provide an extensible film that can be stretched and used without degrading the functionality of the film itself or layers formed on the film when attached to an adherend, and a laminate including the extensible film.
[0009] In order to solve the above problems, the present invention provides the following items <1> to <8>: <1> A film having an uneven shape on at least one surface, wherein the tensile elongation at break in a first direction that is an arbitrary direction within the plane of the film is more than 20%, and the tensile elongation at break in a second direction perpendicular to the first direction is more than 20%, and when a 0.44 mm square area of the uneven surface is observed with a white light interference microscope, the surface roughness measured in accordance with ISO 25178:2012 before elongation is Sa(0), and the surface roughness measured in accordance with ISO 25178:2012 after elongation by 20% in the first direction is Sa(1). 1 (20) When stretched 20% in the second direction, the surface roughness measured in accordance with ISO 25178: 2012 is Sa 2 When (20) is defined, the rate of change ΔSa of surface roughness in the first direction is expressed by the following formula (1): 1 is −15.0% or less, and the rate of change ΔSa of the surface roughness in the second direction is represented by the following formula (2): 2 An extensible film having a ΔSa of −15.0% or less. 1 (unit: %) = (Sa 1 (20)-Sa(0)) / Sa(0)×100 (1) ΔSa 2 (unit: %) = (Sa 2 (20) - Sa(0) / Sa(0) × 100 (2) <2> ΔSa 1 and the ΔSa 2 Absolute value of the difference |ΔSa 1 -ΔSa 2The stretchable film according to <1>, wherein | is 10.0% or less. <3> The stretchable film according to <1> or <2>, wherein Sa(0) is 0.05 μm or more and 5.0 μm or less. <4> The stretchable film according to any one of <1> to <3>, wherein 20 non-overlapping 0.06 mm square small regions are arbitrarily selected from a 0.44 mm square observation region using a white light interference microscope, and the average surface roughness measured in accordance with ISO 25178:2012 for each of the 20 small regions is defined as Sa'(0) and the standard deviation of the surface roughness of the 20 small regions is defined as σ, and the coefficient of variation calculated from the following formula (3) is 10.0% or less. Coefficient of variation = (σ / Sa'(0)) x 100 (3) <5> The stretchable film according to any one of <1> to <4>, wherein, with respect to the height of a 0.44 mm square observation area using a white light interference microscope, the maximum peak height is defined as P (μm), the surface having a height obtained by adding P / 6 to the average height is defined as a first reference plane, the number of convex portions exceeding the first reference plane is defined as N1, the surface having a height obtained by adding P / 3 to the average height is defined as a second reference plane, the number of convex portions exceeding the second reference plane is defined as N2, the surface having a height obtained by adding P / 2 to the average height is defined as a third reference plane, and the number of convex portions exceeding the third reference plane is defined as N3, and the stretchable film according to any one of <1> to <4>, wherein N1 is defined as 500 or more and 10,000 or less. <Condition 1> 0.50≦N2 / N1≦1.50 <Condition 2> 0.25≦N3 / N1≦1.00 <6> The stretchable film according to <5>, wherein N1 is 500 or more and 10,000 or less.
[0010] <7> A laminate comprising the stretchable film according to any one of <1> to <6> and an adhesive layer provided on the surface of the film opposite to the surface having the concave-convex shape. <8> A laminate comprising the stretchable film according to any one of <1> to <6> and a functional layer provided on the surface having the concave-convex shape of the stretchable film.
[0011] <9> A sanitary product having the stretchable film according to any one of <1> to <6>. <10> A cosmetic having the stretchable film according to any one of <1> to <6>. <11> An image display device having the stretchable film according to any one of <1> to <6>.
[0012] <12> A sanitary product having the laminate according to <7> or <8>. <13> A cosmetic having the laminate according to <7> or <8>. <14> An image display device having the laminate according to <7> or <8>.
[0013] When the stretchable film of the present invention is used by being attached to an adherend, it can be stretched without impairing the function of the film itself or the layer formed on the film.
[0014] FIG. 1 shows a schematic cross-sectional view of a stretchable film according to an embodiment of the present disclosure; FIG. 2 shows a scanning electron microscope photograph of a stretchable film of the present disclosure; FIG. 3 shows a white light interference microscope image of the stretchable film of Example 1 before stretching; FIG. 4 shows a white light interference microscope image of the stretchable film of Example 1 after stretching by 20%; FIG. 5 shows a schematic cross-sectional view of an example of a laminate of the present disclosure; FIG. 6 shows a schematic cross-sectional view of another example of a laminate of the present disclosure; FIG. 7 shows a schematic cross-sectional view of another example of a laminate of the present disclosure; FIG. 8 shows a photograph illustrating an example of use of a stretchable film of the present disclosure; FIG. 9 shows a schematic view of a stretching jig; FIG. 10 shows a schematic view illustrating a procedure for preparing a measurement sample in a stretched state; FIG. 11 shows a white light interference microscope image of the film of Comparative Example 1 before stretching; FIG. 12 shows a white light interference microscope image of the film of Comparative Example 1 after stretching by 20%; FIG. 13 shows a white light interference microscope image of the film of Comparative Example 2 before stretching; FIG. 14 shows a white light interference microscope image of the film of Comparative Example 2 after stretching by 20%.
[0015] Hereinafter, embodiments of the present disclosure will be described. In this specification, the numerical values relating to "greater than or equal to," "less than or equal to," and "to" in describing a numerical range can be arbitrarily combined, and the numerical values in the examples can be used as the upper and lower limits of the numerical range.
[0016] The stretchable film of the present disclosure is a film having an uneven shape on at least one surface, wherein the tensile breaking elongation in a first direction, which is any direction within the plane of the film, is greater than 20%, and the tensile breaking elongation in a second direction perpendicular to the first direction is greater than 20%. When a 0.44 mm square area of the uneven surface is observed with a white light interference microscope, the surface roughness measured in accordance with ISO 25178:2012 before elongation is Sa(0), and the surface roughness measured in accordance with ISO 25178:2012 after elongation by 20% in the first direction is Sa(0). 1 (20) When stretched 20% in the second direction, the surface roughness measured in accordance with ISO 25178: 2012 is Sa 2 When (20) is defined, the rate of change ΔSa of surface roughness in the first direction is expressed by the following formula (1): 1 is −15.0% or less, and the rate of change ΔSa of the surface roughness in the second direction is represented by the following formula (2): 2 is −15.0% or less. 1 (unit: %) = (Sa 1 (20)-Sa(0)) / Sa(0)×100 (1) ΔSa 2 (unit: %) = (Sa 2 (20)-Sa(0)) / Sa(0)×100 (2)
[0017] The stretchable film of the present disclosure has antiglare properties and extensibility due to the presence of a concave-convex shape on at least one surface. Figure 1 shows a cross-sectional schematic diagram of a stretchable film according to one embodiment of the present disclosure. The stretchable film 10 of Figure 1 has a single-layer structure of a resin layer 12, and one surface of the resin layer 12 has a concave-convex shape composed of a plurality of convex portions 14 and concave portions 16 between the convex portions 14. The resin layer may also have a structure in which a plurality of resin layers are laminated.
[0018] [Tensile Breaking Elongation] In the present disclosure, the shape of the stretchable film is not particularly limited and may be a polygon such as a triangle, rectangle, or pentagon, or a circle, ellipse, star, or the like. Regardless of the shape of the stretchable film, any direction selected within the plane of the textured surface of the stretchable film is defined as the first direction, and the direction perpendicular to the first direction is defined as the second direction. However, when the stretchable film is rectangular, the direction parallel to one of the two perpendicular sides is defined as the first direction, and the direction parallel to the other side is defined as the second direction. Here, "perpendicular" means that the angle between the first direction and the second direction is within the range of 85° to 95°. The angle between the first direction and the second direction is preferably within the range of 87° to 93°, more preferably within the range of 89° to 91°, and particularly preferably 90°.
[0019] The tensile elongation at break is measured according to the following procedure. According to JIS K 7127:1999, a sample with a tensile direction in the first direction and a sample with a tensile direction in the second direction are cut out from one extensible film. Five samples of each type are prepared. The sample shape is a type 2 test piece as described in JIS K 7127:1999. The sample width is 10 mm and the total length is 100 mm. A tensile test is performed on each sample using a tensile tester (e.g., a Tensilon universal testing machine RTC-1310A) under the following conditions: an initial chuck distance of 50 mm, a measurement ambient temperature of 23°C, and a test speed of 200 mm / min. The chuck distance (mm) at which the sample breaks is obtained from the elongation (mm) measured using software (e.g., MSAT0001V2 Ver. 1.3.6). The tensile elongation at break is calculated using the following formula: Tensile elongation at break (%) = (L - L 0 ) / L 0 × 100 L: Distance between chucks at break (mm) L 0 : initial distance between chucks (mm) The average of the measured values of five samples in each of the first direction and the second direction is defined as the tensile elongation at break in the first direction and the tensile elongation at break in the second direction.
[0020] The stretchable film of the present disclosure must have a tensile elongation at break of greater than 20% in the first direction and a tensile elongation at break of greater than 20% in the second direction. Having a tensile elongation at break of greater than 20% in both the first and second directions means that the stretchable film can be stretched not only in one direction but also in at least two directions that are perpendicular to each other in the plane of the film. If the tensile elongation at break is 20% or less in both the first and second directions, the stretchable film itself may be damaged when attached to an adherend or when used after being attached to an adherend. For example, when applied to a skin sensor, the stretchable film may feel lacking in stretchability, making it uncomfortable to use. Furthermore, when applied to a foldable image display device, the stretchable film may be damaged by bending. The tensile elongation at break in the first direction and the tensile elongation at break in the second direction are each preferably 30% or more, more preferably 40% or more, and even more preferably 50% or more. Taking into consideration productivity, handleability, and the like, the tensile elongation at break in the first direction and the tensile elongation at break in the second direction are each preferably 200% or less, more preferably 175% or less, and even more preferably 150% or less. That is, examples of the numerical range of the tensile elongation at break in the first direction include more than 20% to 200%, more than 20% to 175%, more than 20% to 150%, 30% to 200%, 30% to 175%, 30% to 150%, 40% to 200%, 40% to 175%, 40% to 150%, 50% to 200%, 50% to 175%, and 50% to 150%. Examples of numerical ranges for the tensile elongation at break in the second direction include more than 20% and not more than 200%, more than 20% and not more than 175%, more than 20% and not more than 150%, 30% to 200%, 30% to 175%, 30% to 150%, 40% to 200%, 40% to 175%, 40% to 150%, 50% to 200%, 50% to 175%, and 50% to 150%.
[0021] Furthermore, in the stretchable film of the present disclosure, when the direction rotated clockwise relative to the first direction is defined as "+" and the direction rotated counterclockwise relative to the first direction as "-", and the direction rotated approximately +45° relative to the first direction is defined as the third direction, the tensile elongation at break in the third direction is preferably greater than 20%. Furthermore, when the direction rotated approximately -45° relative to the first direction is defined as the fourth direction, the tensile elongation at break in the fourth direction is preferably greater than 20%. Here, "approximately +45°" means that the angle between the first direction and the third direction is within the range of 40° to 50°. The angle between the first direction and the third direction is preferably within the range of 42° to 47°, more preferably within the range of 44° to 46°, and particularly preferably 45°. Furthermore, "approximately -45°" here means that the angle between the first direction and the fourth direction is within the range of -40° to -50°. The angle between the first direction and the fourth direction is preferably within the range of -42° to -47°, more preferably within the range of -44° to -46°, and particularly preferably -45°.
[0022] In the third and fourth directions, the tensile elongation at break is greater than 20%, so that the stretchable film of the present disclosure can be stretched in any in-plane direction. Furthermore, the tensile elongation at break in the third direction and the tensile elongation at break in the fourth direction are each preferably 30% or more, more preferably 40% or more, and even more preferably 50% or more. Considering productivity, handleability, etc., the tensile elongation at break in the third direction and the tensile elongation at break in the fourth direction are each preferably 200% or less, more preferably 175% or less, and even more preferably 150% or less. That is, embodiments of the numerical range of the tensile elongation at break in the third direction include more than 20% and not more than 200%, more than 20% and not more than 175%, more than 20% and not more than 150%, 30% to 200%, 30% to 175%, 30% to 150%, 40% to 200%, 40% to 175%, 40% to 150%, 50% to 200%, 50% to 175%, and 50% to 150%. Examples of the numerical range of the tensile elongation at break in the fourth direction include more than 20% and not more than 200%, more than 20% and not more than 175%, more than 20% and not more than 150%, 30% to 200%, 30% to 175%, 30% to 150%, 40% to 200%, 40% to 175%, 40% to 150%, 50% to 200%, 50% to 175%, and 50% to 150%. The tensile elongation at break in the third and fourth directions can be measured in the same manner as the tensile elongation in the first and second directions.
[0023] [Uneven Profile] The stretchable film of the present disclosure has an uneven profile on at least one surface, and when the uneven profile is observed over a 0.44 mm square area using a white light interference microscope, the change rate of surface roughness in a first direction, ΔSa 1 is −15.0% or less, and the rate of change ΔSa of the surface roughness in the second direction 2 In this specification, the term "0.44 mm square area" means a "0.44 mm x 0.44 mm square area."
[0024] In the present disclosure, the rate of change ΔSa of surface roughness is determined by measuring the surface roughness Sa(0), Sa(1), Sa(2), Sa(3), Sa(4), Sa(5), Sa(6), Sa(7), Sa(8), Sa(9), Sa(10), Sa(11), Sa(12), Sa(13), Sa(14), Sa(15), Sa(16), Sa(17), Sa(18), Sa(19), Sa(20), Sa(21), Sa(2 1 (20), Sa 2 (20). A white light interference microscope is used to measure the surface roughness. The obtained surface roughness Sa value may vary depending on the field of view in which the microscope is observed. Therefore, in this disclosure, the surface roughness Sa(0), Sa(1) in a 0.44 mm square area is calculated. 1 (20), Sa 2 Evaluate (20).
[0025] Surface roughness change rate ΔSa 1 and ΔSa 2 A minus (-) value of ΔSa means that the surface roughness changes so that the convex portions that make up the uneven shape become lower. 1 is −15.0% or less, and ΔSa 2 By having a ΔSa of -15.0% or less, not only can the stretchable film be sufficiently stretched in the first and second directions that are perpendicular to each other, but also, by stretching the film so that the convex portions are lower, the occurrence of strain due to stretching inside the stretchable film is suppressed. Therefore, the stretchable film can be stretched while suppressing the occurrence of damage such as cracks in the stretchable film itself. Furthermore, even if other layers such as an anti-reflection layer, a hard coat layer, or a circuit are provided on the stretchable film, the occurrence of damage such as cracks in these layers when the stretchable film is stretched can be suppressed. In contrast, ΔSa 1 is more than -15.0%, and ΔSa 2 If the elongation ratio is greater than -15.0%, the film will be distorted when stretched. This makes the film more susceptible to damage and reduces its functionality. Furthermore, if other layers are provided on the film, these layers will be unable to follow the elongation of the film, making them more susceptible to damage and causing the loss of functionality of each layer.
[0026] ΔSa 1 is preferably −15.5% or less, and more preferably −16.0% or less. 2In order to suppress distortion occurring inside the stretchable film and to ensure the antiglare properties of the film itself even in a stretched state as will be described later, ΔSa 1 is preferably −25.0% or more, more preferably −24.5% or more, and even more preferably −24.0% or more. 2 is preferably −25.0% or more, more preferably −24.5% or more, and even more preferably −24.0% or more. 1 Examples of the numerical range of ΔSa include -25.0% or more and -15.0% or less, -24.5% or more and -15.0% or less, -24.0% or more and -15.0% or less, -25.0% or more and -15.5% or less, -24.5% or more and -15.5% or less, -24.0% or more and -15.5% or less, -25.0% or more and -16.0% or less, -24.5% or more and -16.0% or less, and -24.0% or more and -16.0% or less. 2 Examples of the numerical range include -25.0% or more and -15.0% or less, -24.5% or more and -15.0% or less, -24.0% or more and -15.0% or less, -25.0% or more and -15.5% or less, -24.5% or more and -15.5% or less, -24.0% or more and -15.5% or less, -25.0% or more and -16.0% or less, -24.5% or more and -16.0% or less, and -24.0% or more and -16.0% or less.
[0027] In addition, in the present disclosure, ΔSa 1 and ΔSa 2 Absolute value of the difference |ΔSa 1 -ΔSa 2 It is preferable that |ΔSa be 10.0% or less. When the absolute value of the difference is within the above range, the stretchable film of the present disclosure has small anisotropy in elongation and can stretch approximately uniformly in the first direction and the second direction. 1 -ΔSa 2 is more preferably 8.0% or less, even more preferably 6.0% or less, and particularly preferably 0%.
[0028] The stretchable film of the present disclosure has an uneven surface on at least one surface, thereby imparting antiglare properties to the film itself. To obtain good antiglare properties, the surface roughness Sa(0) is preferably 0.05 μm or more, more preferably 0.1 μm or more, and even more preferably 0.2 μm or more. Furthermore, in order to improve coverage when coating another layer on the uneven surface and to facilitate wiping off dirt and the like adhering to the uneven surface, the surface roughness Sa(0) is preferably 5.0 μm or less, more preferably 4.0 μm or less, and even more preferably 3.0 μm or less. That is, examples of the numerical range of the surface roughness Sa(0) include 0.05 μm or more and 5.0 μm or less, 0.1 μm or more and 5.0 μm or less, 0.2 μm or more and 5.0 μm or less, 0.05 μm or more and 4.0 μm or less, 0.1 μm or more and 4.0 μm or less, 0.2 μm or more and 4.0 μm or less, 0.05 μm or more and 3.0 μm or less, 0.1 μm or more and 3.0 μm or less, and 0.2 μm or more and 3.0 μm or less.
[0029] The stretchable film of the present disclosure preferably has antiglare properties even in a stretched state. In order to facilitate obtaining good antiglare properties even in a stretched state of the stretchable film, the surface roughness Sa 1 (20) is preferably 0.05 μm or more, more preferably 0.1 μm or more, and even more preferably 0.2 μm or more. 2 (20) is preferably 0.05 μm or more, more preferably 0.1 μm or more, and even more preferably 0.2 μm or more. In addition, in order to make it easier to wipe off dirt and the like that has adhered to the surface having an uneven shape, the surface roughness Sa 1 (20) is preferably 4.0 μm or less, more preferably 3.2 μm or less, and even more preferably 2.4 μm or less. 2 (20) is preferably 4.0 μm or less, more preferably 3.2 μm or less, and even more preferably 2.4 μm or less. That is, the surface roughness Sa 1Examples of the numerical range of (20) include 0.05 μm or more and 4.0 μm or less, 0.1 μm or more and 4.0 μm or less, 0.2 μm or more and 4.0 μm or less, 0.05 μm or more and 3.2 μm or less, 0.1 μm or more and 3.2 μm or less, 0.2 μm or more and 3.2 μm or less, 0.05 μm or more and 2.4 μm or less, 0.1 μm or more and 2.4 μm or less, and 0.2 μm or more and 2.4 μm or less. Surface roughness Sa 2 Examples of the numerical range of (20) include 0.05 μm or more and 4.0 μm or less, 0.1 μm or more and 4.0 μm or less, 0.2 μm or more and 4.0 μm or less, 0.05 μm or more and 3.2 μm or less, 0.1 μm or more and 3.2 μm or less, 0.2 μm or more and 3.2 μm or less, 0.05 μm or more and 2.4 μm or less, 0.1 μm or more and 2.4 μm or less, and 0.2 μm or more and 2.4 μm or less.
[0030] In the stretchable film of the present disclosure, 20 non-overlapping small regions of 0.06 mm square are arbitrarily selected from a 0.44 mm square observation area using a white light interference microscope, and the average surface roughness of each of the 20 small regions measured in accordance with ISO 25178:2012 is defined as Sa'(0) and the standard deviation of the surface roughness of the 20 small regions is defined as σ. The coefficient of variation calculated from the following formula (3) is preferably 10.0% or less. Coefficient of variation = (σ / Sa'(0)) × 100 (3)
[0031] The coefficient of variation σ / Sa'(0) is an index that indicates the degree of uneven distribution of the uneven surface. A small σ / Sa'(0) means that the unevenness is more uniformly distributed on the uneven surface. When σ / Sa'(0) is 10.0% or less, the unevenness is more uniformly distributed in the plane, making it easier for the stretchable film to stretch in the first direction and the second direction, and the tensile elongation at break in the first direction and the second direction, as well as ΔSa 1 , ΔSa 2However, the above-mentioned range is likely to be satisfied. As a result, the stretchable film can be easily stretched in the first direction and the second direction. σ / Sa'(0) is more preferably 9.0% or less, and even more preferably 8.5% or less. The lower limit of σ / Sa'(0) is preferably 1.0% or more in order to prevent the stretchable film from appearing glossy when observed at different angles.
[0032] The stretchable film of the present disclosure preferably satisfies the following conditions 1 and 2 for a surface having an uneven shape, where P (μm) is the maximum peak height, N1 is the surface having a height obtained by adding P / 6 to the average height, N2 is the number of convex portions exceeding the first reference plane, N3 is the surface having a height obtained by adding P / 3 to the average height, N4 is the number of convex portions exceeding the second reference plane, N5 is the surface having a height obtained by adding P / 2 to the average height, and N3 is the number of convex portions exceeding the third reference plane, as measured by a white light interference microscope. <Condition 1> 0.50≦N2 / N1≦1.50 <Condition 2> 0.25≦N3 / N1≦1.00 N2 / N1 and N3 / N1 are indicators of the variation in the height of the convex portions. N2 / N1 and N3 / N1 being 1 means that the height of the convex portions is not biased toward a predetermined height. By satisfying Conditions 1 and 2, a concave-convex shape with more uniform height of the convex portions is formed, which makes it easier to suppress the concentration of stress on convex portions of a specific height. Therefore, the tensile elongation at break in the first direction and the second direction and ΔSa 1 , ΔSa 2 However, it is easier to satisfy the above-mentioned range. As a result, the stretchable film can be easily stretched in the first direction and the second direction. Furthermore, by satisfying condition 1 and condition 2, the anti-glare properties are easily improved. Furthermore, when the stretchable film of the present disclosure is used by being attached to a living body, the glossiness of the stretchable film is suppressed, making it less noticeable. The lower limit of N2 / N1 is more preferably 0.60 or more, and even more preferably 0.80 or more. Furthermore, the lower limit of N3 / N1 is more preferably 0.30 or more, and even more preferably 0.35 or more.
[0033] In the stretchable film of the present disclosure, the N1 is preferably 500 or more and 10,000 or less. When N1 satisfies the above range, a sufficient number of convex portions are present in a predetermined region, and the tensile elongation at break in the first direction and the second direction is more likely to satisfy the above-mentioned range. Furthermore, when N1 satisfies the above range, the antiglare properties are more likely to be good. N1 is more preferably 1,000 or more and 8,000 or less, more preferably 1,000 or more and 6,000 or less, even more preferably 2,000 or more and 6,000 or less, and even more preferably 2,000 or more and 5,000 or less. Furthermore, in the stretchable film of the present disclosure, the N2 is preferably 500 or more and 10,000 or less, more preferably 1,000 or more and 8,000 or less, even more preferably 1,500 or more and 5,000 or less, and even more preferably 2,000 or more and 5,000 or less. Furthermore, the above N3 is preferably 300 or more and 5,000 or less, more preferably 500 or more and 4,000 or less, and even more preferably 1,000 or more and 3,000 or less.
[0034] [Surface Unevenness] Figure 2 shows a scanning electron microscope photograph of a surface having an unevenness in one embodiment of the stretchable film of the present disclosure. Figure 2 is an image of the surface having an unevenness captured from diagonally above. The observation sample was obtained by attaching and fixing the surface opposite the observation surface of the stretchable film to a resin plate (made of polyvinyl chloride) using an adhesive (an adhesive containing α-cyanoacrylate), and then cutting the cross section of the sample. Figure 2 shows the unevenness of the surface of the stretchable film, as well as the cross section of the film, the adhesive layer, and the resin plate. Figures 3 and 4 show white light interference microscope photographs of the surface having an unevenness in one embodiment (Example 1) of the stretchable film of the present disclosure. Figure 3 shows the image before stretching, and Figure 4 shows the image after 20% stretching in the vertical direction of the image. Note that Figures 3 and 4 are 0.44 mm square images observed under the conditions described in the Examples below.
[0035] The stretchable film of the present disclosure preferably has an uneven shape caused by minute wrinkles. The wrinkles are composed of multiple convex portions and concave portions located between the multiple convex portions. When viewed in a planar view (i.e., when observed from a direction approximately perpendicular to the surface having the uneven shape), the convex portions are curved or meandering linear stripes. When viewed in a planar view, the shapes of the individual convex portions are different from each other. Furthermore, the convex portions are not parallel to each other, but are arranged in an intricate manner, such that, for example, a portion of an adjacent convex portion is inserted into the curved portion of one convex portion, and multiple convex portions are folded. Therefore, it cannot be said that the convex portions have a shape with a fixed rule or are arranged according to a fixed rule. Similarly, it cannot be said that the concave portions located between the convex portions have a shape with a fixed rule. The surface of the stretchable film of the present disclosure preferably has a shape in which multiple linear convex portions are arranged irregularly and densely. Comparing Figures 3 and 4, it can be seen that the number of convex portions decreases before and after stretching.
[0036] Here, "curved" means that, in plan view, there is one or more portions where the extension direction of the continuous linear convex portions reverses from one side to the other. Examples of portions where the extension direction reverses from one side to the other include, for example, a form having an inflection point when the linear convex portions are approximated by a continuous curve when the width of the plan view shape is ignored (when the width of the plan view shape is considered to be 0). Also, examples include a form having a portion that is approximated by a V-shaped folded line or two sides of a triangle that sandwich one vertex when the linear convex portions are approximated by a straight line when the width of the plan view shape is ignored.
[0037] Furthermore, "meandering" means that, in plan view, there are at least two or more portions where the extension direction of the continuous linear convex portions is reversed from one side to the other (hereinafter also referred to as "reversed portions"), and when proceeding along the extension direction of the linear convex portions, there are portions where the extension direction of the linear convex portions is reversed alternately in opposite directions at two adjacent portions. For example, when the width of the planar shape of the linear convex portions is approximated by a continuous curve, ignoring the width of the planar shape, there is an example of a form having a portion approximated by the Roman letter "S." Furthermore, when the width of the planar shape of the linear convex portions is approximated by a straight line, ignoring the width of the planar shape, there is an example of a form having a portion approximated by the Roman letter "W."
[0038] Furthermore, the convex portions in the present disclosure may have a branched portion. Such a form can be considered as a form in which two or more filamentary convex portions are connected and integrated. For example, a form in which the end or middle portion of one filamentary convex portion is connected to the middle portion of another filamentary convex portion and integrated is exemplified. Examples of branched forms include shapes approximated by the Roman letters "T" and "Y" and dendritic shapes such as dendrimers.
[0039] In addition, a convex portion is defined as a region having a height equal to or greater than the first reference plane defined above, i.e., a plane having a height equal to or greater than the average height plus P / 6 (P is the maximum peak height (μm)), in an image obtained by a white light interference microscope. A concave portion is defined as a region below the first reference plane.
[0040] When a stretchable film having wrinkles of the above-described shape is pulled in the surface direction (the first direction and the second direction described above), not only does the material itself stretch, but the wrinkles also unfold, reducing the height of the convex portions, making it more easily stretchable. The shape in which the multiple linear convex portions are irregularly and densely arranged provides ample room for the wrinkles to unfold in the surface direction. Therefore, the stretchable film having the above-described surface shape has a tensile elongation at break, ΔSa, within the above-described range. 1 , ΔSa 2This makes it easier to satisfy the above requirement. Since the wrinkles are expanded to facilitate stretching, the occurrence of large distortion in the stretchable film can be suppressed compared to when wrinkles are not formed. This suppresses the occurrence of damage such as cracks during stretching, and furthermore, the functionality of the stretchable film itself can be maintained. For example, by having an uneven shape as shown in FIG. 2, the stretchable film itself has anti-glare properties, and the uneven shape is maintained to a certain extent even after the stretchable film is stretched, so the anti-glare properties can be maintained. Furthermore, even if other layers are provided on the stretchable film, damage such as cracks can be suppressed in these layers when the stretchable film is stretched. This allows the performance of these layers to be maintained even after the stretchable film is stretched.
[0041] By forming a plate or a shaped sheet using a sandblasting method, a solvent treatment method, or the like, it is possible to form a film having a surface with a plurality of irregularly and densely arranged convex portions. However, in a film having a convex-concave shape imparted by the above method, the convex portions do not expand and the degree of elongation is mainly due to the material of the film. Furthermore, since the concave portions corresponding to the thin portions of the film are more likely to elongate than the convex portions, the height of the convex portions is less likely to decrease due to elongation, and ΔSa 1 , ΔSa 2 It is difficult to satisfy the above requirement. Furthermore, the film itself is significantly distorted by stretching. Even if the film does not break due to stretching, damage occurs to the surface of the film or other layers formed on the film, making it more likely to lose function. Therefore, it can be said that the stretchable film of the present disclosure has a different effect from a film whose surface is provided with an uneven shape using a shaping sheet produced by sandblasting or the like.
[0042] When particles are added to the resin, it is also possible to form a film having a surface with a plurality of irregularly and densely arranged convex portions. However, in such a film, the resin portion stretches when pulled, but the particles cannot. That is, in such a film, the extension is not caused by the spreading of the convex portions, and the magnitude of the extension is mainly contributed by the material of the film, so the tensile breaking elongation and ΔSa 1 , ΔSa 2 It is difficult to satisfy the numerical range of . In particular, the resin part stretches due to tension, but the particles do not stretch, so the particles become apparent. For this reason, the surface roughness Sa after stretching is smaller than the surface roughness S(0) before stretching. 1 (20) and Sa 2 (20) tends to become large, resulting in ΔSa 1 , ΔSa 2 tends to have a "+" value. Furthermore, since the film itself is significantly distorted by stretching, even if the film does not break due to stretching, damage occurs to the surface of the film and other layers formed on the film, making it more likely to lose function. Therefore, it can be said that the stretchable film of the present disclosure has a different effect from a film having an uneven surface formed by adding particles.
[0043] Also, an accordion-folded structure is known as an example of an uneven shape having fold wrinkles. In the accordion-folded structure, the peaks are spaced apart to form a surface shape with densely packed convex portions. However, in the accordion-folded structure, the peaks and valleys are arranged in one direction with regularity. Therefore, the accordion-folded structure can be easily stretched in the direction in which the peaks and valleys are arranged, but is difficult to stretch in the direction in which the ridges of the peaks extend. In other words, the accordion-folded structure causes directional dependency in the degree of stretching. In a film having a accordion-folded structure, if the arrangement direction of the peaks and valleys is defined as a first direction, the tensile breaking elongation and ΔSa in the first direction are 1 may satisfy the above-mentioned numerical range, but the tensile breaking elongation and ΔSa in the second direction 2Therefore, the uneven shape of the stretchable film of the present disclosure is different from that of a bellows-folded structure, and it can be said that the stretchable film of the present disclosure exhibits effects different from those of a film having a surface with a bellows-folded structure.
[0044] As mentioned above, the convex portions and concave portions of the stretchable film of the present disclosure do not have a shape and arrangement that follow a fixed rule, so it is difficult to define their sizes in general. As an example, the width of the convex portions is 1 μm or more and 50 μm or less, and the length of the convex portions is 10 μm or more and 300 μm or less. The width of the concave portions is 1 μm or more and 100 μm or less. The length of the convex portions is defined as the length when the curved filamentary convex portions are stretched linearly. When the sizes of the convex portions and concave portions are within the above ranges, the tensile breaking elongation and ΔSa described above can be achieved. 1 , ΔSa 2 This makes it easier to satisfy the numerical range of
[0045] When viewed in plan, the area ratio of the convex portions is preferably 10% or more, more preferably 12.5% or more, and even more preferably 15% or more, with the upper limit being preferably 70% or less, more preferably 60% or less, and even more preferably 50% or less. When the area ratio of the convex portions is within the above range, the above-mentioned tensile breaking elongation is easily satisfied. Here, in order to determine the area ratio of the convex portions, a first reference plane having a height obtained by adding P / 6 to the average height is identified in an image of an observation area of 0.44 mm square obtained by a white light interference microscope, and the area A (mm 2 The area ratio of the convex portions was calculated using the obtained area A according to the following formula: Area ratio of convex portions (%) = A / (0.44 x 0.44) x 100
[0046] [Film size and physical properties] <Thickness> The thickness of the stretchable film of the present disclosure is not particularly limited and can be set appropriately depending on the application. Considering the strength, handleability, stretchability, etc. of the film, the lower limit of the thickness of the stretchable film in an unstretched state is preferably 0.5 μm, more preferably 0.8 μm, and even more preferably 1.0 μm, and the upper limit is preferably 100 μm, more preferably 50 μm, and even more preferably 30 μm. The thickness of the stretchable film is measured by observing the cross section of the film in an unstretched state using a scanning electron microscope (SEM) and measuring the average thickness at 10 randomly selected locations in the cross-sectional image.
[0047] <Haze> The stretchable film of the present disclosure preferably has a haze (H(0)) according to JIS K7136:2000 of 50% or more, more preferably 60% or more, and even more preferably 70% or more, when unstretched. Furthermore, the stretchable film of the present disclosure preferably has a haze (H(20)) according to JIS K7136:2000 of 50% or more, more preferably 60% or more, and even more preferably 70% or more, when stretched by 20%. By ensuring that the haze H(0) and H(20) satisfy the above ranges, when the stretchable film is attached to a living body, the glossiness of the stretchable film is suppressed by light scattering, making it less noticeable. Furthermore, by ensuring that the haze H(0) and H(20) satisfy the above ranges, high antiglare properties can be obtained when used in an image display device. On the other hand, the higher the haze (0) and haze (20), the whitish the stretchable film appears due to light scattering. In order to make the stretchable film less noticeable when attached to a living body, the stretchable film of the present disclosure preferably has a haze (H(0)) according to JIS K7136:2000 in an unstretched state of 99% or less, more preferably 95% or less, and even more preferably 90% or less. For the same reason, the stretchable film of the present disclosure preferably has a haze (H(20)) according to JIS K7136:2000 in an unstretched state of 99% or less, more preferably 95% or less, and even more preferably 90% or less. The upper limit of the rate of change in haze according to JIS K7136:2000 (ΔH = (H(20) - H(0)) / H(0) x 100) before and after stretching of the stretchable film of the present disclosure is preferably 10% or less, more preferably 5% or less, and even more preferably 3% or less. Furthermore, the haze change rate ΔH is preferably −10% or more, more preferably −5% or more, and even more preferably −3% or more. When the haze change rate ΔH is within the above range, when the stretchable film is stretched, the whiteness due to light scattering becomes uniform throughout the film, and visual changes in the stretched portions can be suppressed.
[0048] <Total Light Transmittance> The stretchable film of the present disclosure, when unstretched, preferably has a total light transmittance (T(0)) according to JIS K7361-1:1997 of 80% or more, more preferably 85% or more, and even more preferably 90% or more. Furthermore, the stretchable film of the present disclosure, when stretched 20%, preferably has a total light transmittance (T(20)) according to JIS K7361-1:1997 of 80% or more, more preferably 85% or more, and even more preferably 90% or more. When the total light transmittances T(0) and T(20) satisfy the above ranges, the stretchable film can be made less noticeable when attached to a living body. Furthermore, when the total light transmittances T(0) and T(20) satisfy the above ranges, high brightness can be obtained when used in an image display device. There are no particular restrictions on the upper limits of the total light transmittances T(0) and T(20), but the upper limit is preferably 99% for both so that the attached location can be visually confirmed when peeling off the stretchable film. The stretchable film of the present disclosure has a rate of change in total light transmittance (ΔT = (T(20) - T(0)) / T(0) x 100) according to JIS K7361-1:1997 before and after stretching of preferably 3% or less, more preferably 1% or less, and even more preferably 0.5% or less. Furthermore, the rate of change in total light transmittance ΔT is preferably -3% or more, more preferably -1% or more, and even more preferably -0.5% or more. When the rate of change in total light transmittance ΔT is within the above range, the stretchable film can be made less noticeable when attached to a living body. Furthermore, when the rate of change ΔT of total light transmittance is within the above range, when the film is used in an image display device and a portion of the film is stretched, it is possible to easily suppress uneven brightness within the surface of the stretchable film.
[0049] <Luminous reflectance> The stretchable film of the present disclosure preferably has a luminous reflectance Y value (Y(0)) of 6.0% or less, more preferably 5.5% or less, and even more preferably 5.0% or less, measured at a light incidence angle of 5 degrees from a surface having a textured shape when not stretched. The stretchable film of the present disclosure preferably has a luminous reflectance Y value (Y(20)) of 6.0% or less, more preferably 5.5% or less, and even more preferably 5.0% or less, measured at a light incidence angle of 5 degrees from a surface having a textured shape when stretched 20%. By having the luminous reflectances Y(0) and Y(20) within the above ranges, the stretchable film can be made less noticeable when attached to a living body. Furthermore, by having the luminous reflectances Y(0) and Y(20) within the above ranges, reflection can be suppressed when used in an image display device. Although there are no particular restrictions on the lower limit values of the luminous reflectances Y(0) and Y(20), it is preferable that the lower limit value for both is 0.1% so that, for example, when peeling off the stretchable film, the attached location can be visually confirmed. In the stretchable film of the present disclosure, the rate of change in the luminous reflectance Y value before and after stretching (ΔY = (Y(20) - Y(0)) / Y(0) x 100) is preferably 10% or less, more preferably 5% or less, and even more preferably 3% or less. Furthermore, the rate of change in luminous reflectance ΔY is preferably -10% or more, more preferably -5% or more, and even more preferably -3% or more. When the rate of change in luminous reflectance ΔY is within the above range, uneven reflection within the surface of the stretchable film can be suppressed when the stretchable film is stretched. In particular, when attached to a living body, the stretchable film can be made less noticeable. In the present disclosure, the luminous reflectance Y value is measured by preparing a sample in which a black PET film is attached to the surface opposite to the uneven surface of the stretchable film via a transparent adhesive layer, and irradiating the sample with light at an incident angle of 5° from the uneven surface side.The luminous reflectance Y value at 20% elongation is measured using a sample obtained by laminating a black PET film to the surface opposite the textured surface of the stretchable film via a transparent adhesive layer using a stretching tool described in the Examples, and then removing the stretchable film from the stretching tool. The light source conditions for calculating reflectance are D65 light source. The refractive index difference between the transparent adhesive layer and the member in contact with the sample's transparent adhesive layer is within 0.15. The refractive index difference is preferably within 0.10, and more preferably within 0.05. The member in contact with the sample's transparent adhesive layer is, for example, a resin layer. The black plate has a total light transmittance of 1% or less according to JIS K7361-1:1997. The total light transmittance of black PET is preferably 0%. The refractive index difference between the resin constituting the black plate and the transparent adhesive layer is within 0.15. The refractive index difference is preferably within 0.10, and more preferably within 0.05.
[0050] <60° Gloss Value> The stretchable film of the present disclosure preferably has a 60° gloss value (G(0)) of 30% or less, more preferably 20% or less, and even more preferably 10% or less, measured from a surface having an uneven shape in accordance with JIS Z8741:1997 when not stretched. Furthermore, the stretchable film of the present disclosure preferably has a 60° gloss value (G(20)) of 30% or less, more preferably 20% or less, and even more preferably 10% or less, measured from a surface having an uneven shape in accordance with JIS Z8741:1997 when stretched 20%. Having the 60° gloss values G(0) and G(20) within the above ranges makes the stretchable film less noticeable when attached to a living body. Furthermore, having the 60° gloss values G(0) and G(20) within the above ranges makes it possible to obtain high antiglare properties when used in an image display device. The lower limits of the 60° gloss values G(0) and G(2) are not particularly limited, but preferably the lower limit is 0.1% for both, so that the attached portion can be visually confirmed when peeling off the stretchable film, for example. In the stretchable film of the present disclosure, the rate of change in the 60° gloss value before and after stretching (ΔG = (G(20) - G(0)) / G(0) x 100) is preferably 50% or less, more preferably 40% or less, and even more preferably 30% or less. Furthermore, the rate of change in the 60° gloss value ΔG is preferably -50% or more, more preferably -40% or more, and even more preferably -30% or more. When the rate of change in 60° gloss ΔG is within the above range, when the stretchable film is stretched, the glossiness becomes uniform throughout the film, and visual changes in the stretched portion can be suppressed. The 60° gloss value is measured according to Method 3 described in Table 2 of JIS Z8741:1997. The sample used for measuring the 60° gloss value is prepared by the same process as that used for measuring the luminous reflectance.
[0051] In this specification, unless otherwise specified, haze, total light transmittance, luminous reflectance, and 60° gloss value refer to the average value of 14 measured values obtained by excluding the maximum and minimum values from the measured values at 16 locations.
[0052] [Resin Composition] Each component of the resin composition used to obtain the resin layer of the stretchable film of the present disclosure will be described in detail below. (Resin) As described in the manufacturing method below, the resin constituting the stretchable film of the present disclosure includes an ionizing radiation-curable resin that can be cured by ultraviolet irradiation. The ionizing radiation-curable resin is a resin having an ionizing radiation-curable functional group. The ionizing radiation-curable functional group is a group that crosslinks and hardens upon irradiation with ionizing radiation, and preferred examples include functional groups having an ethylenic double bond such as a (meth)acryloyl group, a vinyl group, or an allyl group. In the present disclosure, the ionizing radiation-curable functional group is preferably a (meth)acrylate. In this specification, a (meth)acryloyl group refers to an acryloyl group or a methcroyl group. In addition, in this specification, a (meth)acrylate refers to an acrylate or a methacrylate. Furthermore, ionizing radiation refers to electromagnetic waves or charged particle beams that have an energy quantum capable of polymerizing and / or crosslinking molecules. Typically, ultraviolet rays (UV) or electron beams (EB) are used, but other examples include electromagnetic waves such as X-rays and gamma rays, and charged particle beams such as alpha rays and ion beams.
[0053] The stretchable film of the present disclosure has the above-mentioned tensile breaking elongation, ΔSa 1 , ΔSa 2 In order to easily satisfy the numerical range of (1), it is preferable to contain a resin having elasticity. Furthermore, depending on the application of the stretchable film of the present disclosure, it is preferable to use a resin having strength such as scratch resistance, weather resistance, etc. Examples of such resins include urethane-based ionizing radiation curable resins. Among them, it is preferable to contain a urethane (meth)acrylate oligomer.
[0054] The urethane (meth)acrylate oligomer used in the present disclosure has an isocyanate unit, a polyol unit, and a (meth)acrylate unit. The isocyanate unit is derived from a polyfunctional isocyanate. The (meth)acrylate unit is derived from a hydroxyl group-containing (meth)acrylate monomer. Therefore, the urethane (meth)acrylate oligomer used in the present disclosure is a resin obtained by polymerizing a polyfunctional isocyanate compound, a polyol compound, and a hydroxyl group-containing (meth)acrylate monomer. Only one type of the polyfunctional isocyanate compound, the polyol compound, and the hydroxyl group-containing (meth)acrylate monomer may be used, or multiple types may be used.
[0055] Examples of polyfunctional isocyanate compounds include aromatic polyisocyanates such as tolylene diisocyanate, diphenylmethane diisocyanate, xylylene diisocyanate, and polymethylene polyphenylene polyisocyanate; and aliphatic polyisocyanates such as hexamethylene diisocyanate and isophorone diisocyanate. Among these, isophorone diisocyanate is preferred. The polyol compound is a segment that imparts stretchability to the film. Examples of polyol compounds include polyether polyols, polyester polyols, and polyoxyalkylene polyols, with polyoxyalkylene polyols being preferred. Examples of polyoxyalkylene polyols include polyoxyethylene polyols and polyoxypropylene polyols. The number of repeating oxyalkylene units in the polyoxyalkylene polyol is preferably 2 to 8, more preferably 2 to 5, even more preferably 2 or 3, and particularly preferably 2. Examples of the hydroxyl group-containing (meth)acrylate monomer include hydroxyethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, pentaerythritol triacrylate, etc. The hydroxyl group-containing (meth)acrylate monomer can be appropriately selected depending on the number of functional groups of the urethane (meth)acrylate oligomer.
[0056] Considering the stretchability, strength after curing, etc., the proportion of isocyanate units in the urethane (meth)acrylate oligomer is preferably 5% by mass or more and 80% by mass or less, and more preferably 5% by mass or more and 70% by mass or less. The proportion of polyol units in the urethane (meth)acrylate oligomer is preferably 10% by mass or more and 90% by mass or less, and more preferably 20% by mass or more and 90% by mass or less. The proportion of (meth)acrylate units in the urethane (meth)acrylate oligomer is preferably 0.1% by mass or more and 10% by mass or less, and more preferably 0.1% by mass or more and 5% by mass or less.
[0057] The number of functional groups of the urethane (meth)acrylate oligomer is more preferably 2 or 3, particularly preferably 2, taking into consideration elasticity, strength after curing, and viscosity. The weight average molecular weight of the urethane (meth)acrylate oligomer is preferably 8,000 or more and 100,000 or less, more preferably 8,300 or more and 80,000 or less, and even more preferably 8,500 or more and 50,000 or less. The weight average molecular weight in the present disclosure is the average molecular weight measured by GPC analysis and converted into standard polystyrene. By using a urethane (meth)acrylate oligomer with a small number of functional groups and a large molecular weight, elasticity can be improved.
[0058] The above-mentioned wrinkles are stably formed, and the above-mentioned tensile breaking elongation, ΔSa 1 , ΔSa 2In order to facilitate satisfying the numerical range of (1), it is preferable that the ionizing radiation curable resin further contains a polymerizable monomer. The polymerizable monomer is preferably a (meth)acrylate monomer. The (meth)acrylate monomer may be a monofunctional (meth)acrylate monomer or a polyfunctional (meth)acrylate monomer. As the number of functional groups in the (meth)acrylic group increases, wrinkles tend to form more easily, while stretchability tends to decrease. In order to achieve a good balance between stretchability and ease of wrinkle formation, suitable (meth)acrylate monomers include monofunctional (meth)acrylate monomers and bifunctional (meth)acrylate monomers, with bifunctional (meth)acrylate monomers being more preferred. Examples of monofunctional (meth)acrylate monomers include acryloylmorpholine, isobornyl (meth)acrylate, tetrahydrofurfuryl alcohol, β-carboxyethyl (meth)acrylate, and phenoxyethyl (meth)acrylate. Examples of the bifunctional (meth)acrylate monomer include triethylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, tripropylene glycol di(meth)acrylate, etc. Only one type of (meth)acrylate monomer may be used, or multiple types may be used.
[0059] The compounding ratio of the urethane (meth)acrylate oligomer and the polymerizable monomer (urethane (meth)acrylate oligomer / polymerizable monomer) can be adjusted taking into consideration factors such as elasticity, strength after curing, and ease of wrinkle formation. The higher the compounding ratio of the polymerizable monomer, the more easily wrinkles form, but the lower the compounding ratio of the bifunctional urethane acrylate oligomer, the lower the elasticity tends to be. Furthermore, if an excessive amount of polymerizable monomer is compounded, the number of bonds between the polymerizable monomers increases, which acts as a plasticizer in the cured resin, potentially reducing the strength after curing. The compounding ratio of the urethane (meth)acrylate oligomer and the polymerizable monomer is preferably in the range of 95 / 5 to 50 / 50, more preferably in the range of 90 / 10 to 60 / 40, and even more preferably in the range of 85 / 15 to 70 / 30.
[0060] (Photopolymerization initiator) Since the resin is an ultraviolet-curable resin that is cured by ultraviolet light, it is preferable that the resin composition contains a photopolymerization initiator. By containing a photopolymerization initiator in the resin composition, the resin can be cured by ultraviolet light irradiation, and surface properties useful for practical use can be obtained. Examples of the photopolymerization initiator include one or more selected from acetophenone, benzophenone, α-hydroxyalkylphenone, 1-hydroxycyclohexyl phenyl ketone, Michler's ketone, benzoin, benzyl dimethyl ketal, benzoyl benzoate, α-acyloxime ester, thioxanthones, etc.
[0061] (Other Components) The resin composition may contain a photopolymerization accelerator, a solvent, an ultraviolet absorber, a light stabilizer, a leveling agent, a colorant, etc. depending on the properties of the resin composition, the performance required of the stretchable film, etc.
[0062] The photopolymerization accelerator can reduce polymerization inhibition caused by air during curing and increase the curing rate. Examples of the photopolymerization accelerator include one or more selected from p-dimethylaminobenzoic acid isoamyl ester, p-dimethylaminobenzoic acid ethyl ester, etc.
[0063] A solvent is added as needed for the purpose of adjusting the viscosity and solid content of the resin composition. If there is no problem in the manufacturing process, such as coating, a solvent need not be used. There are no particular limitations on the solvent used, and a commonly used solvent can be appropriately selected and used. Examples of solvents include ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone (MIBK), and cyclohexanone; ethers such as dioxane and tetrahydrofuran; aliphatic hydrocarbons such as hexane; alicyclic hydrocarbons such as cyclohexane; aromatic hydrocarbons such as toluene and xylene; halogenated carbons such as dichloromethane and dichloroethane; esters such as methyl acetate, ethyl acetate, and butyl acetate; alcohols such as isopropanol, butanol, and cyclohexanol; cellosolves such as methyl cellosolve and ethyl cellosolve; glycol ethers such as propylene glycol monomethyl ether acetate; cellosolve acetates; sulfoxides such as dimethyl sulfoxide; and amides such as dimethylformamide and dimethylacetamide. These solvents may be used alone or in combination.
[0064] Examples of the ultraviolet absorber include a benzotriazole-based ultraviolet absorber, a benzophenone-based ultraviolet absorber, a triazine-based ultraviolet absorber, a hydroxyphenyltriazine-based ultraviolet absorber, etc. Examples of the light stabilizer include a hindered amine-based light stabilizer such as a piperidinyl sebacate-based light stabilizer, etc.
[0065] The leveling agent is added to improve the wettability of the resin composition to the releasable substrate when the resin composition is applied to the releasable substrate in the production method described below, and to adjust the surface condition of the coating film, thereby reducing variation in the surface condition of the coating film. Examples of the leveling agent include silicone-based leveling agents and fluorine-based leveling agents.
[0066] [Method for manufacturing stretchable film] The method for manufacturing a stretchable film of the present disclosure includes a step of applying a resin composition to a releasable substrate to form a coating layer, a step of irradiating the coating layer with light having a wavelength of at least 100 nm or more and 380 nm or less, and a step of peeling off the releasable substrate.
[0067] <Process for forming coating layer> The release substrate may be a support sheet alone or a laminate in which a release layer is formed on a support sheet. The support sheet is not particularly limited, and various materials such as resins, metals, non-metallic inorganic materials, paper materials, and wood-based materials can be appropriately selected depending on the application. The support sheet can be used as a single layer selected from these, or as a multi-layer combination of two or more layers of materials selected from these. The support sheet is preferably a resin or fibrous material, more preferably a resin, because it is easy to peel, easy to handle, and economical.
[0068] Resins that can be used for the support sheet include various synthetic resins, natural resins, etc. Examples of synthetic resins include thermoplastic resins and curable resins, and thermoplastic resins are preferred in consideration of suitability for manufacturing matte articles, suitability for handling, suitability for post-processing, etc.
[0069] Preferred examples of the thermoplastic resin include olefin resins such as polyethylene, polypropylene, polymethylpentene, ionomers, and various olefin-based thermoplastic elastomers; vinyl chloride resins such as polyvinyl chloride, polyvinylidene chloride, and vinyl chloride-vinyl acetate copolymers; polyester resins such as polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, ethylene glycol-terephthalic acid-isophthalic acid copolymers, and polyester-based thermoplastic elastomers; acrylic resins such as polymethyl (meth)acrylate, polyethyl (meth)acrylate, polybutyl (meth)acrylate, and methyl (meth)acrylate-butyl (meth)acrylate copolymers; polyamide resins typified by nylon 6 and nylon 66; cellulose resins such as cellulose triacetate, cellophane, and celluloid; styrene resins such as polystyrene, acrylonitrile-styrene copolymers, and acrylonitrile-butadiene-styrene copolymers (ABS resins); polyvinyl alcohol, ethylene-vinyl acetate copolymers, ethylene-vinyl alcohol copolymers, polycarbonate resins, polyarylate resins, and polyimide resins.
[0070] Preferred examples of paper materials include tissue paper, kraft paper, fine paper, Japanese paper, titanium paper, linter paper, sulfate paper, paraffin paper, parchment paper, glassine paper, backing paper for wallpaper, paperboard, base paper for gypsum board, reinforced paper between papers, and resin-impregnated paper.
[0071] The release layer is a layer that is provided as needed to facilitate the release of the releasable substrate from the film after the resin composition has been cured to form a film. Examples of release layers include those containing polyvinyl alcohol, acrylic resin, vinyl chloride-vinyl acetate, olefin resin, silicone resin, fluororesin, and various resins modified with silicone or fluorine. If necessary, wax can be mixed with these resins. Preferred examples of wax include microcrystalline wax, carnauba wax, paraffin wax, Fischer-Tropsch wax, various low-molecular-weight polyethylenes, Japan wax, beeswax, whale wax, ivory wax, wool wax, shellac wax, candelilla wax, petrolactam, partially modified wax, fatty acid esters, fatty acid amides, and various other waxes.
[0072] The resin composition contains the above-mentioned urethane (meth)acrylate oligomer, and is prepared by adding a polymerizable monomer, a photopolymerization initiator, a solvent, etc. as necessary.
[0073] The resin composition can be applied by known methods such as gravure printing, bar coating, roll coating, reverse roll coating, and comma coating. The thickness of the coating layer is not particularly limited and may be determined according to the thickness required for the stretchable film. The lower limit of the dried thickness of the coating layer is preferably 0.5 μm, more preferably 0.8 μm, and even more preferably 1.0 μm, and the upper limit is preferably 100 μm, more preferably 50 μm, and even more preferably 30 μm.
[0074] <Light Irradiation Step> In the manufacturing method of the present disclosure, the resin composition is irradiated with light having a wavelength of at least 100 nm or more and 380 nm or less. This irradiation allows the ultraviolet energy to penetrate only the surface portion, and the energy does not reach the layers below, so that only the surface portion of the resin composition begins to harden. As a result, curing shrinkage occurs only on the surface, forming wrinkles, and the surface layer of the resin composition becomes a cured product. Subsequently, curing progresses from the surface-near portion, where curing progresses slowly, to portions further away in the depth direction, and the layer of the resin composition becomes a cured product. As a result, the resin composition hardens throughout its entire thickness, forming a resin layer with an uneven surface caused by wrinkles.
[0075] As the light having a wavelength of at least 100 nm or more and 380 nm or less, for example, a dimer in an excited state formed by discharge of a rare gas such as Ar, Kr, Xe, Ne, a halide of a rare gas such as F, Cl, I, Br, or a mixed gas of these, that is, "excimer light" including light in the ultraviolet wavelength region from an excimer, is preferable. The wavelength of the excimer light and the excimer as a light source are, for example, Ar 2 Light with a wavelength of 126 nm (hereinafter referred to as "126 nm (Ar)") emitted from the excimer 2 ), 146 nm (Kr 2 ), 157 nm (F 2 ), 172 nm (Xe 2Wavelengths such as 193 nm (ArF), 222 nm (KrCl), 247 nm (KrF), 308 nm (XeCl), and 351 nm (XeF) can be preferably used. As the excimer light, either spontaneous emission or laser light with high coherence due to stimulated emission can be used, but spontaneous emission is usually sufficient. Discharge lamps that emit light (ultraviolet light) are also called "excimer lamps." Excimer light is characterized by a single wavelength peak and a narrower half-width wavelength than ordinary ultraviolet light (e.g., ultraviolet light emitted from metal halide lamps, mercury lamps, etc.). The use of such excimer light allows for stable formation of wrinkles. Furthermore, wrinkles formed using excimer light have relatively uniform depths, narrow widths, and narrow spacing between adjacent wrinkles, as shown in FIG. 3 . Therefore, forming wrinkles using excimer light can easily prevent high-altitude or low-altitude areas from concentrating locally. That is, forming wrinkles using excimer light can easily reduce σ / Sa′(0) and can easily satisfy Condition 1 and Condition 2.
[0076] In order to stably form wrinkles, the wavelength is preferably 120 nm or more, more preferably 140 nm or more, even more preferably 150 nm or more, and even more preferably 155 nm or more, and the upper limit is preferably 320 nm or less, more preferably 300 nm or less, even more preferably 250 nm or less, and even more preferably 200 nm or less, and most preferably 172 nm (Xe 2 ) In this way, in the present disclosure, it is preferable to use light with a shorter wavelength, and it can be said that medium-wavelength ultraviolet light (wavelength: 280 to 320 nm) and short-wavelength ultraviolet light (wavelength: 280 nm or less) are more preferable, and short-wavelength ultraviolet light is even more preferable.
[0077] In the present disclosure, the integrated light amount of light of the above wavelengths is preferably 1 mJ / cm from the viewpoint of stably forming wrinkles. 2 More preferably, 10 mJ / cm 2 More preferably, 30 mJ / cm 2More preferably, 50 mJ / cm 2 There is no particular upper limit, but in consideration of reducing the number of lamps required for irradiation and improving production efficiency, it is preferably 1,000 mJ / cm. 2 or less, more preferably 500 mJ / cm 2 More preferably, 300 mJ / cm or less 2 or less. For the same reason, the ultraviolet light output density is preferably 0.001 W / cm or more, more preferably 0.01 W / cm or more, even more preferably 0.03 W / cm, with the upper limit being preferably 10 W / cm or less, more preferably 5 W / cm or less, and even more preferably 3 W / cm or less. Furthermore, the oxygen concentration when irradiating with light of the above wavelengths is preferably lower, and is preferably 1,000 ppm or less, more preferably 750 ppm or less, even more preferably 500 ppm or less, and still more preferably 300 ppm or less.
[0078] In this process, in addition to the irradiation with light having a wavelength of at least 100 nm or more and 380 nm or less, other treatments that contribute to the curing of the resin composition may be performed. For example, in order to stabilize wrinkle formation and promote the progression of curing from the surface vicinity to the depth direction, the resin composition may be pre-irradiated with light having a wavelength exceeding 380 nm, preferably light having a wavelength of about 385 nm or more and 400 nm or less, to pre-cure the entire resin composition, and then irradiated with light having a wavelength of 100 nm or more and 380 nm or less. Alternatively, after irradiation with light having a wavelength of 100 nm or more and 380 nm or less, post-curing may be performed to further cure the resin composition. The necessity of pre-curing and post-curing can be determined appropriately depending on the productivity, the performance required for the stretchable film, etc. In addition to ultraviolet light, other ionizing radiation, such as electron beams, can also be used. For example, electron beams may be used in post-curing to improve surface properties.
[0079] <Peeling Step> After the resin layer is formed, the releasable substrate is peeled off, thereby obtaining the stretchable film of the present disclosure having an uneven shape on one surface.
[0080] Another method for producing the stretchable film of the present disclosure includes the steps of obtaining a shaped sheet or embossing plate using the stretchable film obtained by the above method, applying a resin composition to a releasable substrate to form a coating layer, curing the resin composition while contacting the shaped sheet or embossing plate with the surface of the coating layer to form a resin layer, and peeling the resin layer from the shaped sheet or embossing plate. In this way, by using a shaped sheet or embossing plate made from the stretchable film of the present disclosure, a film having a concave-convex shape on one surface can be obtained.
[0081] [Uses] The stretchable film of the present disclosure is applicable to medical components such as skin sensors, film dressings, and transdermal absorption preparations; cosmetics used by being attached to a living body such as makeup products, sun care products, and fragrances; sanitary products used by being attached to a living body such as deodorant products and cooling sheets; etc. The stretchable film of the present disclosure is also applicable to components constituting image display devices such as polarizing plates and anti-reflection films.
[0082] In the present disclosure, the resin layer alone (film) as exemplified in FIG. 1 can be applied to the above applications. Alternatively, a laminate of the resin layer and other layers can be applied to the above applications. Examples of the layer configuration of the laminate include the following. FIG. 5 is a cross-sectional schematic diagram of an example of a laminate of the present disclosure. The laminate 20 of FIG. 5 has a resin layer 22 and an adhesive layer 24 formed on the side of the resin layer 22 opposite the uneven surface. Known adhesives can be used for the adhesive layer. The adhesive layer preferably has extensibility. As a variation of the laminate shown in FIG. 5, a substrate layer having releasability may be provided on the side of the adhesive layer 24 opposite the resin layer 22. Examples of the substrate layer include various films and paper substrates. FIG. 6 is a cross-sectional schematic diagram of another example of a laminate of the present disclosure. The laminate 30 of FIG. 6 has a resin layer 32 and a functional layer 36 formed on the uneven surface of the resin layer 32. Examples of functional layers include an anti-reflection layer, a hard coat layer, an electrode layer, an ultraviolet absorbing layer, a drug layer, a fragrance layer, and a deodorizing layer, and are appropriately provided depending on the intended use of the laminate. These layers can be formed by known methods. The electrode layer may be patterned. FIG. 7 is a cross-sectional schematic diagram of another example of a laminate of the present disclosure. The laminate 40 of FIG. 7 includes a resin layer 42, an adhesive layer 44 formed on the side opposite the uneven surface of the resin layer 42, and a functional layer 46 formed on the uneven surface of the resin layer 42. As a modification of the laminate shown in FIG. 7, a substrate layer having releasability may be provided on the side of the adhesive layer 44 opposite the resin layer 42, similar to the modification of the laminate shown in FIG. 5.
[0083] FIG. 8 is a photograph illustrating an example of the use of the stretchable film of the present disclosure, showing it adhered to a human body. The area surrounded by a dotted line on the right side of the photograph is the area where the stretchable film of the present disclosure is adhered. The area surrounded by a solid line on the left side of the photograph is the area where a film made of the same material as the stretchable film of the present disclosure but without an uneven surface is adhered. The stretchable film of the present disclosure is less susceptible to reflections of light and has anti-glare properties. Therefore, it is not noticeable when adhered to a human body. On the other hand, a film without an uneven surface reflects and shines with illuminating light, making the area where it is adhered easy to see.
[0084] FIG. 9 is a photograph illustrating an example of use of the stretchable film of the present disclosure. FIG. 9 shows a laminate in which an adhesive layer is formed on a resin layer, and a stretchable film is provided on the surface of the adhesive layer opposite the resin layer. The laminate of FIG. 9 is freely deformable, such as by stretching, bending, twisting, and folding. Even after repeated deformation of the laminate of FIG. 9, damage such as cracking and tearing can be suppressed. It also has excellent handleability. Because of this repeated stretchability, it can be said that the stretchable film of the present disclosure can be used on the surface of a deformable image display device. The stretchable film of the present disclosure has the above-described uneven shape on its surface, and therefore can suppress reflection of illumination light and the like when applied to an image display device. Furthermore, an image display device using the stretchable film of the present disclosure has various deformabilities, such as stretching, bending, twisting, and folding.
[0085] Next, the present invention will be described in more detail by way of examples, but the present invention is not limited to these examples in any way.
[0086] 1. Measurement and Evaluation The atmosphere for the measurements and evaluations in 1-1 to 1-3 below shall be a temperature of 23°C ± 5°C and a relative humidity of 40% to 65%. Furthermore, prior to measurement and evaluation, the measurement sample shall be exposed to the above atmosphere for 30 to 60 minutes. The measurement sample shall be taken from a clean and undamaged location. Measurement and evaluation shall be carried out when the sample has good flatness.
[0087] 1-1. Observation with a White Light Interference Microscope (1) Sample Preparation The sheets of Examples 1 to 4 and Comparative Examples 1 to 5 were visually inspected to ensure there were no abnormalities such as dust or scratches. Then, with the long side of each sheet set as a first direction and the short side set as a second direction, a 50 mm x 50 mm sample was cut out so that the sides of the sample were parallel to the first direction and the second direction, respectively.
[0088] (2) Measurement Preparation <Measurement Sample Before Stretching> When observing without stretching, the measurement sample was prepared according to the following procedure. The release substrate or cover film was slowly peeled off from each sample. A black PET sheet (PET75NBPET38, manufactured by Lintec Corporation) with an adhesive layer formed on one side was placed on the release surface of the sample so that the release surface and the adhesive layer were in contact. Then, an AZPURE Hand Cleaner II (manufactured by AS ONE Corporation) was brought into contact with the black PET sheet and moved once. This resulted in a measurement sample.
[0089] <Measurement Sample After Stretching> When observing in a stretched state, a measurement sample was prepared using the following procedure. An extension jig as shown in FIG. 10 was prepared. FIG. 10 is a schematic diagram of the extension jig, viewed from above (+Z direction). The extension jig 100 includes a pair of support parts 102-1 and 102-2, male screws 104a to 104c, and nuts 106-1 to 106-3. The support parts 102-1 and 102-2 each have a rectangular cross section measuring 13 mm in length, 13 mm in width, and 80 mm in length. The cross sections of the support parts 102-1 and 102-2 correspond to the XZ cross sections in FIG. 10, and their lengths coincide with the Y direction. When viewed from the +X direction, each of the support parts 102-1 and 102-2 has three cylindrical through-holes 102a to 102c formed on its side surface in the longitudinal direction (Y direction). The diameter of the through-holes 102a to 102c is 6 mm. The centers of the through-holes 102a to 102c are aligned with the longitudinal centerlines of the side surfaces of the support parts 102-1 and 102-2. Therefore, when viewed from the +X direction, the through-holes 102a to 102c are each spaced 3.5 mm apart from the long sides of the side surfaces of the support parts 102-1 and 102-2. When viewed from the +X direction, the through-holes 102a and 102c are each spaced 2 mm apart from the short sides of the side surfaces of the support parts 102-1 and 102-2. The distance between the through-holes 102a and 102b is 7.5 mm. The support parts 102-1 and 102-2 were manufactured using a 3D printer from ultraviolet curing resin (ELEGOO Standard LCD UV-Curing Photopolymer Rapid Resign (Green) manufactured by ELEGOO).
[0090] Male screws (80 mm long M5 metric coarse threads) 104a to 104c are inserted into the through holes 102a to 102c of the support parts 102-1 and 102-2. Each of the male screws 104a to 104c is inserted from one of the support parts. The positions of the support parts 102-1 and 102-2 are fixed by nuts 106-1 to 106-3 (hexagonal nuts, M5, type 1). Three nuts 106-1 to 106-3 are placed on the male screws 104a and 104c, as shown in FIG. 10 . A nut 106-3 is placed only on the tip of the male screw 104b.
[0091] The procedure for preparing the measurement sample in the stretched state is shown in FIG. 11. As shown in FIG. 11(a), the support part 102-1 was fixed with nut 106-1 so that the distance between the support parts 102-1 and 102-2 (the distance between the opposing sides of the support parts 102-1 and 102-2) was 30 mm, and the support part 102-2 was fixed with nuts 106-2 and 106-3 on the male screws 104a and 104c. The nut 106-3 on the male screw 104b was loosened. Double-sided tape (Teraoka Seisakusho Co., Ltd., No. 775) was cut into 10 mm x 60 mm pieces and attached to the top surface (sample mounting surface) of each support part 102. At this time, as shown in FIG. 11(a), the long sides of the double-sided tape 108 were arranged along the opposing sides of the support parts 102-1 and 102-2. The double-sided tape 108 was placed so that the areas up to 10 mm from both ends of the support parts 102-1 and 102-2 in the longitudinal direction were free of the double-sided tape.
[0092] Next, as shown in FIG. 11(b), the sample was attached to double-sided tape 108 so that the resin layer was facing the support part and so that the sample would not bend. At this time, the sample was positioned so that the longitudinal (Y-direction) edges of the support parts 102-1 and 102-2 and the edges of the film were approximately parallel. The sample was also positioned so that the distance d1 between the edges of the support parts 102-1 and 102-2 on the tip side of the male screws 104a to 104c and the edges of the film was within a range of 0 mm to 6 mm, and the distance d2 from both ends of the short sides of the support parts 102-1 and 102-2 was within a range of 10 mm to 20 mm. After attaching the sample, the release substrate or cover film was slowly peeled off to prevent the resin layer from stretching. This fixed the resin layer 110 to the support parts 102-1 and 102-2.
[0093] Next, as shown in FIG. 11(c), the nuts 106-3 were each moved toward the tip of the male screw (-X direction). Thereafter, the support part 102-2 was moved by moving the nut 106-2 toward the tip of the male screw. At this time, the two nuts 106-2 were moved alternately so that the difference between the spacing of the support parts on the male screw 104a side and the spacing of the support parts on the male screw 104c side was not more than 1 mm. After moving the nut 106-2 by 6 mm, the support 102-2 was fixed by tightening the nut 106-3. This operation stretched the resin layer 110.
[0094] Next, black PET (PET75NBPET38, manufactured by Lintec Corporation) with an adhesive layer formed on one side was placed on the resin layer from the +Z direction in Figure 11(c). In this state, an AZPURE Hand Cleaner II (manufactured by AS ONE Corporation) was brought into contact with the black PET and moved once along the longitudinal direction of the support parts 102-1 and 102-2 (the Y direction in Figure 11(c)). This caused the black PET to adhere to the resin layer. The resin layer was then peeled off from the double-sided tape. Using the above procedure, a measurement sample in a 20% elongated state was obtained. Note that for resin layers that could not be elongated by 20%, the adhesion of the black PET, the acquisition of images described below, and the various evaluations were not performed.
[0095] (3) Image Acquisition The resin layer was placed on the measurement stage of a white light interference microscope (New View 7300, manufactured by Zygo) with the resin layer facing up, and the measurement sample was set so that it was fixed and in close contact with the sample. Then, a white light microscope image of the film surface was acquired under the following measurement conditions. Note that, for the observation, a 50x objective lens was used, the magnification was set to 0.5x, and the measurement range was set to 0.44 mm x 0.44 mm. <Measurement conditions> Objective lens: 50x Mirau [manufactured by Measurement Controls] Acquisition Mode: Scan Scan Type: Bipolar Camera Mode: 992 x 992, 48 Hz SubtractSysErr: Off AGC: Off PhaseRes: High ConnectionOrder: Location DisconAction: Filter MinMod (%): 0.001 MinAreaSize: 7 Scan Direction: Downward Image Zoom: 0.5x Remove Fringes: Off Number of Averages: 0 FDA Noise Threshold: 10 Scan Length: 10 umbipolar Extended Scan Length: 1000 μm FDA Res: High 2G Camera resolution (spacing per point): 0.219
[0096] (4) Analysis of surface roughness The images obtained in (3) were analyzed using the Microscope Application and Advanced Texture Application of MetroPro ver. 9.0.10 under the following analysis conditions: Sa(0), Sa 1 (20), Sa 2 (20) and P were measured. The obtained Sa(0), Sa 1 (20), Sa 2 From (20), ΔSa 1 , ΔSa 2was calculated. <Analysis conditions> <<Microscope Application>> Removed: None Trim: 0 DataFill: On DataFillMax: 100 Filter: HighPass FilterLowWavelen: 150μm FilterType: GaussSpline FilterTrim: Off Removespikes: on SpikeHeight (xRMS): 2.5 <<AdvancedTextureApplication>> HighFFTFilter:Off LowFFTFilter:Off Removespikes:Off NoiseFilterSize:0 NoiseFilterType:2Sigma FillData:Off Trim:0 Remove:Plane
[0097] Analysis of σ / Sa'(0) was performed according to the following procedure. In the image acquired of the measurement sample before elongation, "Square" was selected in "Mask Editor," a mask was applied with a size of 0.06 mm, and a square mask of 0.06 mm x 0.06 mm was created by removing the background using "BG Excl." Then, the mode was set to "Move," and the mask was manually moved arbitrarily to measure Sa(0) in 20 areas within the image. The 20 areas within the image were selected so that they did not overlap. The average value Sa'(0) and standard deviation σ of Sa(0) at 20 locations were calculated. σ / Sa'(0) was calculated from the obtained Sa'(0) and σ.
[0098] (5) Evaluation of convexity height The image of the measurement sample before elongation was analyzed using Advanced Texture Application under the above analysis conditions in (3). In the "Peaks / Vallesys" window, when "Peak Lower Limit" was set to P / 6, the "Peaks" (number of convexities) were N1, when set to P / 3, the "Peaks" (number of convexities) were N2, and when set to P / 2, the "Peaks" (number of convexities) were N3.
[0099] The above measurements and analyses were performed at nine points for each measurement sample. The maximum and minimum values of the nine measurements were excluded, and the average of seven measurements was calculated. The obtained average values are shown in Tables 1 and 2.
[0100] 1-2. Tensile elongation at break According to JIS K 7127:1999, five samples were cut out from the sheets of Examples 1 to 4 and Comparative Examples 1 to 5, one in which the tensile direction was the first direction, and one in which the tensile direction was the second direction. The sample shape was test piece type 2, with a width of 10 mm and a total length of 100 mm. Then, the release substrate or cover film was peeled off from each sample to obtain a measurement sample. Each measurement sample was measured at an initial distance between chucks (L 0 The sample was set to a 50 mm gap and attached to a tensile testing machine (Tensilon universal material testing machine RTC-1310A). Then, a tensile test was carried out under the conditions of a measurement ambient temperature of 23°C and a test speed of 200 mm / min. The distance L (mm) between the chucks when the sample broke was measured. 0 The tensile elongation at break was calculated from L and . The average values of the five measurement samples were taken as the tensile elongation at break in the first direction and the tensile elongation at break in the second direction, respectively. The results are shown in Tables 1 and 2.
[0101] 1-3. Total Light Transmittance, Luminous Reflectance, Haze, and 60° Gloss Value <Measurement Samples Before Stretching> 50 mm x 50 mm samples were cut from the sheets of Examples 1 to 4 and Comparative Examples 1 to 5. The release substrate or cover film was peeled off from each sample. For measuring the luminous reflectance and 60° gloss value, a black PET sheet was attached to the sample in the same manner as in 1-1(1) to prepare a measurement sample. For measuring the total light transmittance and haze, a sample without the black PET sheet attached was used as the measurement sample. <Measurement After Stretching> 50 mm x 50 mm samples were cut from the sheets of Examples 1 to 4 and Comparative Examples 1 to 5. The measurement samples stretched by 20% were prepared using the method described in 1-1(2). For measuring the luminous reflectance and 60° gloss value, the sample removed from the stretching jig after the black PET sheet was attached was used as the measurement sample. When measuring total luminous transmittance and haze, the measurement samples were prepared by the method described in 1-1(2), except that the black PET was not attached after stretching. <Measurement> Using a haze meter (HM-150, manufactured by Murakami Color Research Laboratory), the total luminous transmittance of each measurement sample according to JIS K7361-1:1997 and the haze according to JIS K7136:2000 were measured. The light incident surface during measurement was the surface with the uneven shape. A spectral reflectance meter (manufactured by Shimadzu Corporation, product name: UV-2600) was used to measure luminous reflectance. The light incident surface during measurement was the surface with the uneven shape. The measuring device measures reflectance in wavelengths ranging from 380 nm to 780 nm at 0.5 nm intervals, and then converts the measured values into brightness perceived by the human eye using software. The software is built into the measuring device. The software calculates reflectance under the conditions of a D65 light source and a viewing angle of 2 degrees. A gloss meter (GM-26PRO, manufactured by Murakami Color Research Laboratory) was used to measure the 60° gloss of each measurement sample according to JIS Z8741:1997. The light incident surface during measurement was the surface with the uneven shape. Measurements of total luminous transmittance and haze after stretching were performed while the measurement sample was still attached to the stretching jig. Total luminous transmittance, luminous reflectance, haze, and 60° gloss values were measured at 16 locations within the surface of the measurement sample.The maximum and minimum values were excluded from the 14 measured values, and the average values were calculated to determine the total light transmittance, luminous reflectance, haze, and 60° gloss value of the films of the Examples and Comparative Examples. The results are shown in Tables 1 and 2.
[0102] 2. Film Preparation [Example 1] 5 parts by weight of polyvinyl alcohol (manufactured by Wako Pure Chemical Industries, Ltd., partially saponified type, molecular weight: 3,500) and 95 parts by weight of pure water were mixed to prepare a release layer coating liquid. The release layer coating liquid was applied to the flat surface of a polyethylene terephthalate film (product name "Cosmoshine A4160", manufactured by Toyobo Co., Ltd., thickness 50 μm, size: 21.0 cm × 29.7 cm) using a bar coater. Thereafter, by heating at 110 ° C. for 2 minutes, a release substrate having a release layer made of polyvinyl alcohol with a thickness of 4 μm was produced.
[0103] Resin composition 1 having the following formulation was prepared. [Resin composition 1] Bifunctional urethane acrylate oligomer (weight average molecular weight (Mw): 8,900): 80 parts by mass Triethylene glycol diacrylate (product name "Light Acrylate 3EG-A", manufactured by Kyoeisha Chemical Co., Ltd.): 20 parts by mass Polymerization initiator (1-hydroxycyclohexyl phenyl ketone, product name "Irgacure (registered trademark) 184", manufactured by BASF Japan Ltd.): 3 parts by mass Solvent (methyl isobutyl ketone): 400 parts by mass Leveling agent (polyether-modified polydimethylsiloxane, product name "BYK-302", manufactured by BYK Corporation): 0.1 parts by mass
[0104] Resin composition 1 used a bifunctional urethane acrylate oligomer obtained from the following three components: Isocyanate unit: isophorone diisocyanate, 20% by mass; Polyol unit: polyoxypropylene polyol (weight average molecular weight (Mw): 1000), 78% by mass; Acrylate unit: hydroxyethyl acrylate, 2% by mass.
[0105] The resin composition was applied to the release layer of a releasable substrate (21.0 cm x 29.7 cm: A4 size) using a bar coater to form a coating film. The coating film was then heated at 70°C for 1 minute to evaporate the solvent in the coating film and dry it. Next, using an excimer irradiation device (manufactured by MDCOM Corporation, MEIRA-MS-1-152-H2, wavelength: 172 nm), the coating film was irradiated once with ultraviolet light at a conveying speed of 70 mm / sec, a voltage of 5.6 V, and an oxygen concentration of 200 ppm or less. The irradiation area was 15 cm x 15 cm square. This allowed only the coating film surface to harden, forming wrinkles on the surface. Next, using an ultraviolet irradiation device (manufactured by Fusion UV Systems Japan Co., Ltd., light source: H bulb), the coating film was irradiated once with ultraviolet light at an integrated light dose of 600 mJ / cm. 2 The coating was cured by irradiating it with ultraviolet light so that the thickness of the resin layer was 3 μm.
[0106] [Example 2] A sheet of Example 2 having a resin layer with a thickness of 3 μm was obtained in the same process as in Example 1, except that resin composition 2 having the following formulation was used. [Resin composition 2] Bifunctional urethane acrylate oligomer (weight average molecular weight (Mw): 34,500): 60 parts by mass Triethylene glycol diacrylate (product name "Light Acrylate 3EG-A", manufactured by Kyoeisha Chemical Co., Ltd.): 40 parts by mass Polymerization initiator (1-hydroxycyclohexyl phenyl ketone, product name "Irgacure (registered trademark) 184", manufactured by BASF Japan Ltd.): 3 parts by mass Solvent (methyl isobutyl ketone): 400 parts by mass Leveling agent (polyether-modified polydimethylsiloxane, product name "BYK-302", manufactured by BYK Corporation): 0.1 parts by mass
[0107] Resin composition 2 used a bifunctional urethane acrylate oligomer obtained from the following three components: Isocyanate unit: isophorone diisocyanate, 5% by mass; Polyol unit: polyoxypropylene polyol (weight average molecular weight (Mw): 4,650), 94% by mass; Acrylate unit: hydroxyethyl acrylate, 1% by mass.
[0108] [Example 3] A sheet of Example 3 having a resin layer with a thickness of 15 μm was obtained using the same process as in Example 1, except that resin composition 3 having the following formulation was used and the drying process of the coating film was not performed. [Resin composition 3] Bifunctional urethane acrylate oligomer (same as resin composition 1): 50 parts by mass Acryloyl morpholine (product name "ACMO", manufactured by KJ Chemicals Co., Ltd.): 50 parts by mass Polymerization initiator (1-hydroxycyclohexyl phenyl ketone, product name "Irgacure (registered trademark) 184", manufactured by BASF Japan Ltd.): 3 parts by mass Leveling agent (polyether-modified polydimethylsiloxane, product name "BYK-302", manufactured by BYK Corporation): 0.1 parts by mass
[0109] [Example 4] A sheet of Example 4 having a resin layer with a thickness of 3 μm was obtained in the same process as in Example 1, except that resin composition 4 having the following formulation was used. [Resin composition 4] Bifunctional urethane acrylate oligomer (weight average molecular weight (Mw): 11,000): 95 parts by mass Acryloyl morpholine (product name "ACMO", manufactured by KJ Chemicals Co., Ltd.): 5 parts by mass Polymerization initiator (1-hydroxycyclohexyl phenyl ketone, product name "Irgacure (registered trademark) 184", manufactured by BASF Japan Ltd.): 3 parts by mass Solvent (methyl isobutyl ketone): 400 parts by mass Leveling agent (perfluoropolyether-containing acrylate, product name "X-71-1203M", manufactured by Shin-Etsu Chemical Co., Ltd.): 0.1 parts by mass
[0110] Resin composition 4 used a bifunctional urethane acrylate oligomer obtained from the following three components: Isocyanate unit: isophorone diisocyanate, 19% by mass; Polyol unit: polyoxypropylene polyol (weight average molecular weight (Mw): 1,000), 79% by mass; Acrylate unit: hydroxyethyl acrylate, 2% by mass.
[0111] [Comparative Example 1] A thin film dressing (product name "Yuhada Permiroll Lite", manufactured by Nitoms Corporation, size: 10.0 cm x 30.0 cm) was prepared, and the cover film was peeled off. The cover film was a shaped sheet. Resin composition 1 was applied to the thin film dressing surface of the cover film using a bar coater to form a coating film. Thereafter, the coating film was heated at 70°C for 1 minute to evaporate the solvent in the coating film. Next, an ultraviolet irradiation device (manufactured by Fusion UV System Japan Co., Ltd., light source: H bulb) was used to evaporate the coating film at an integrated light dose of 600 mJ / cm. 2 The coating was cured by irradiating it with ultraviolet light so that the thickness of the resin layer was 28 μm. As a result, a sheet of Comparative Example 1 having a resin layer with a thickness of 28 μm was obtained.
[0112] [Comparative Example 2] Resin composition 5 was prepared according to the following formulation. [Resin composition 5] Bifunctional urethane acrylate oligomer (same as resin composition 1): 80 parts by mass Triethylene glycol diacrylate (product name "Light Acrylate 3EG-A", manufactured by Kyoeisha Chemical Co., Ltd.): 20 parts by mass Silica particles (gel-method amorphous silica, average particle size: 2.7 μm, manufactured by Fuji Silysia Chemical Ltd.): 80 parts by mass Polymerization initiator (1-hydroxycyclohexyl phenyl ketone, product name "Irgacure (registered trademark) 184", manufactured by BASF Japan Ltd.): 3 parts by mass Methyl isobutyl ketone: 400 parts by mass Leveling agent (polyether-modified polydimethylsiloxane, product name "BYK-302", manufactured by BYK Corporation): 0.1 parts by mass
[0113] Resin composition 5 was applied to the flat surface of a polyethylene terephthalate film (product name "Cosmoshine A4160", manufactured by Toyobo Co., Ltd., thickness 50 μm, size: 21.0 cm × 29.7 cm: A4 size) as a release substrate using a bar coater to form a coating film. Thereafter, the solvent in the coating film was evaporated by heating at 70°C for 1 minute. Next, an ultraviolet irradiation device (manufactured by Fusion UV System Japan Co., Ltd., light source: H bulb) was used to evaporate the coating film with an accumulated light dose of 600 mJ / cm. 2 The coating was cured by irradiating it with ultraviolet light so that the thickness of the resin layer was 5.5 μm. As a result, a sheet of Comparative Example 2 having a resin layer with a thickness of 5.5 μm was obtained.
[0114] [Comparative Example 3] A sheet of Comparative Example 3 having a resin layer with a thickness of 3 μm was obtained in the same process as in Example 1, except that Resin Composition 6 having the following formulation was used. [Resin Composition 6] Bifunctional urethane acrylate oligomer (weight average molecular weight (Mw): 3,500): 80 parts by mass Triethylene glycol diacrylate (product name "Light Acrylate 3EG-A", manufactured by Kyoeisha Chemical Co., Ltd.): 20 parts by mass Polymerization initiator (1-hydroxycyclohexyl phenyl ketone, product name "Irgacure (registered trademark) 184", manufactured by BASF Japan Ltd.): 3 parts by mass Solvent (methyl isobutyl ketone): 400 parts by mass Leveling agent (polyether-modified polydimethylsiloxane, product name "BYK-302", manufactured by BYK Corporation): 0.1 parts by mass
[0115] Resin composition 6 used a bifunctional urethane acrylate oligomer obtained from the following three components: Isocyanate unit: isophorone diisocyanate, 37% by mass; Polyol unit: polyoxypropylene polyol (weight average molecular weight (Mw): 400), 56% by mass; Acrylate unit: hydroxyethyl acrylate, 7% by mass.
[0116] [Comparative Example 4] A sheet of Comparative Example 4 having a resin layer with a thickness of 3 μm was obtained in the same process as in Example 1, except that Resin Composition 7 having the following formulation was used. [Resin Composition 7] Bifunctional urethane acrylate oligomer (same as Resin Composition 1): 70 parts by mass Pentaerythritol triacrylate (product name "KAYARAD PET-30", manufactured by Nippon Kayaku Co., Ltd.): 30 parts by mass Polymerization initiator (1-hydroxycyclohexyl phenyl ketone, product name "Irgacure (registered trademark) 184", manufactured by BASF Japan Ltd.): 3 parts by mass Solvent (methyl isobutyl ketone): 400 parts by mass Leveling agent (polyether-modified polydimethylsiloxane, product name "BYK-302", manufactured by BYK Corporation): 0.1 parts by mass
[0117] [Comparative Example 5] A sheet of Comparative Example 5 having a resin layer having a thickness of 3 μm was obtained in the same process as in Example 1, except that Resin Composition 8 having the following formulation was used. [Resin Composition 8] Bifunctional urethane acrylate oligomer (same as Resin Composition 1): 40 parts by mass Triethylene glycol diacrylate (product name "Light Acrylate 3EG-A", manufactured by Kyoeisha Chemical Co., Ltd.): 60 parts by mass Polymerization initiator (1-hydroxycyclohexyl phenyl ketone, product name "Irgacure (registered trademark) 184", manufactured by BASF Japan Ltd.): 3 parts by mass Solvent (methyl isobutyl ketone): 400 parts by mass Leveling agent (polyether-modified polydimethylsiloxane, product name "BYK-302", manufactured by BYK Corporation): 0.1 parts by mass
[0118] 3. Results Figures 12 and 13 show white light interference microscope photographs of the surface having a concave-convex shape in Comparative Example 1. Figure 12 shows the image before stretching, and Figure 13 shows the image after stretching 20% in the vertical direction of the image. Figures 14 and 15 show white light interference microscope photographs of the surface having a concave-convex shape in Comparative Example 2. Figure 14 shows the image before stretching, and Figure 15 shows the image after stretching 20% in the vertical direction of the image.
[0119]
[0120]
[0121] As described above, it can be seen that Example 1 has an uneven surface caused by minute wrinkles. It can be seen that dot-shaped convex portions are formed on the surface of Comparative Example 1 and Comparative Example 2. The size and density of the individual dot-shaped convex portions tended to be larger in Comparative Example 1 than in Comparative Example 2.
[0122] In Example 1, ΔSa 1 , ΔSa 2 In Example 1, the tensile elongation at break was 98% in the first direction and 82% in the second direction, which indicated excellent extensibility. 1 -ΔSa 23 and 4, a change in the distribution of the convex portions was observed in Example 1.
[0123] In contrast, in Comparative Example 1, ΔSa 1 , ΔSa 2 12 and 13, almost no change was observed in the distribution of the convex portions. 1 was a positive (+) value. This is thought to be because the silica particles became apparent due to tension, increasing the undulations caused by the silica particles. Referring also to the images in Figures 14 and 15, the convex portions appear to have become larger. Furthermore, although the resin portion of Comparative Example 2 uses the same material as Example 1, the tensile breaking elongation was low. From these results, it is thought that the film of Example 1 elongates due to the material of the resin layer, and the unfolding of the convex portions of the wrinkles also contributed to the extensibility.
[0124] In Example 1, σ / Sa′(0) is smaller than in Comparative Examples 1 and 2. From this, it can be understood that in Example 1, wrinkles (protrusions) are uniformly distributed within the surface.
[0125] In Example 1, N2 / N1 and N3 / N1 satisfy conditions 1 and 2, and therefore it can be seen that the height of the convex portions is more uniform. On the other hand, in Comparative Example 1, although N2 / N1 is high, N3 / N1 is very low, and therefore it can be said that the uniformity of the height of the convex portions is inferior to that of Example 1. In Comparative Example 2, N1 exceeded the detection limit (10,000 particles), and an accurate value could not be obtained. For this reason, calculations of N2 / N1 and N3 / N1 were not performed. A large N1 means that there are many convex portions present in a region of the same area. Since the convex portions are caused by silica particles, in Comparative Example 2, ΔSa is lower due to the influence of the silica particles. 1 , ΔSa 2 It can be seen that the tensile elongation at break is reduced.
[0126] Similarly, in Examples 2 to 4, ΔSa 1 , ΔSa 2In Examples 2 to 4, |ΔSa was −15.0% or less, and the tensile elongation at break in the first direction and the second direction was high. 1 -ΔSa 2 | was small, and the specimens could be stretched approximately uniformly in the first and second directions. It can be seen that Examples 2 to 4 also had small σ / Sa'(0), and wrinkles (protrusions) were uniformly distributed within the surface. Furthermore, in all of Examples 2 to 4, N2 / N1 and N3 / N1 satisfied Conditions 1 and 2, and it can be seen that the height of the protrusions was more uniform.
[0127] In all of Comparative Examples 3 to 5, the tensile elongation at break was 20% or less. Therefore, evaluation at 20% elongation was not possible. In Comparative Example 3, compared to Example 1, the polyol units in the bifunctional urethane acrylate oligomer were shorter and the ratio of polyol units to isocyanate units was lower. This is thought to have prevented the resin layer from being imparted with sufficient flexibility, resulting in the low tensile elongation at break. In Comparative Example 4, the addition of a trifunctional acrylate (polymerizable monomer) to the resin composition hardened the resin layer, preventing it from being imparted with sufficient flexibility, resulting in the low tensile elongation at break. In Comparative Example 5, compared to Example 1, the ratio of bifunctional urethane acrylate oligomer was lower, and a large amount of (polymerizable monomer) was blended, preventing it from being imparted with sufficient flexibility, resulting in the low tensile elongation at break.
[0128] A 50 mm x 50 mm sample was cut from the sheet of each example. The release substrate was peeled off from each sample and attached to a Bioskin plate (small size) (manufactured by Viewlux Co., Ltd., No. 64, #Biocolor (BCB)). At this time, the release surface of each sample was brought into contact with the Bioskin plate. Ten subjects evaluated the visibility of the samples under illumination (illuminance: 750 lx) with a white LED (color temperature: 5000 K). As a result, for each example, eight or more subjects evaluated that the boundary between the Bioskin plate and the sample was inconspicuous.
[0129] REFERENCE SIGNS LIST 10 Stretchable film 12, 22, 32, 42 Resin layer 14 Convex portion 16 Concave portion 20, 30, 40 Laminate 24, 44 Adhesive layer 36, 46 Functional layer 100 Stretching jig 102-1, 102-2 Support part 104a, 104b, 104c Male screw 106-1, 106-2, 106-3 Nut 108 Double-sided tape 110 Resin layer
Claims
1. A film having an uneven shape on at least one surface, the film having a tensile breaking elongation of more than 20% in a first direction that is any direction within the plane of the film, and a tensile breaking elongation of more than 20% in a second direction perpendicular to the first direction, the uneven surface having a surface roughness measured in accordance with ISO 25178:2012 before elongation when observed with a white light interference microscope in an area of 0.44 mm square is Sa(0), and the surface roughness measured in accordance with ISO 25178:2012 after elongation by 20% in the first direction is Sa(1). 1 (20) When stretched 20% in the second direction, the surface roughness measured in accordance with ISO 25178:2012 is Sa 2 (20), the rate of change ΔSa of surface roughness in the first direction is expressed by the following formula (1): 1 is −15.0% or less, and the rate of change ΔSa of the surface roughness in the second direction represented by the following formula (2) 2 A stretchable film having a stretchability of -15.0% or less. 1 (Unit:%) = (Sa 1 (20)-Sa(0)) / Sa(0)×100 (1) ΔSa 2 (Unit:%) = (Sa 2 (20)-Sa(0)) / Sa(0)×100 (2) 2. The above ΔSa 1 and the ΔSa 2 Absolute value of the difference |ΔSa 1 -ΔSa 2 2. The stretchable film of claim 1, wherein | is 10.0% or less.
3. The stretchable film according to claim 1 or 2, wherein Sa(0) is 0.05 μm or more and 5.0 μm or less.
4. The stretchable film according to claim 1 or 2, wherein 20 non-overlapping small areas of 0.06 mm square are arbitrarily selected from an observation area of 0.44 mm square using a white light interference microscope, and the average surface roughness of each of the 20 small areas measured in accordance with ISO 25178:2012 is defined as Sa'(0) and the standard deviation of the surface roughness of the 20 small areas is defined as σ, the coefficient of variation calculated from the following formula (3) is 10.0% or less. Coefficient of variation = (σ / Sa'(0)) x 100 (3) 5. The stretchable film according to claim 1 or 2, wherein the surface having the uneven shape satisfies the following conditions 1 and 2, when the maximum peak height is defined as P (μm), the surface having a height obtained by adding P / 6 to the average height as a first reference surface, the number of convex portions exceeding the first reference surface as N1, the surface having a height obtained by adding P / 3 to the average height as a second reference surface, the number of convex portions exceeding the second reference surface as N2, the surface having a height obtained by adding P / 2 to the average height as a third reference surface, and the number of convex portions exceeding the third reference surface as N3, in relation to the height of a 0.44 mm square observation area observed by a white light interference microscope. <Condition 1> 0.50≦N2 / N1≦1.50 <Condition 2> 0.25≦N3 / N1≦1.00 6. The stretchable film according to claim 5, wherein N1 is 500 or more and 10,000 or less.
7. A laminate comprising the stretchable film according to claim 1 or 2 and an adhesive layer provided on the surface of said film opposite to the surface having said uneven shape.
8. A laminate comprising the stretchable film according to claim 1 or 2 and a functional layer provided on the uneven surface of the stretchable film.
9. A sanitary product comprising the stretchable film according to claim 1 or 2.
10. A cosmetic comprising the stretchable film according to claim 1 or 2.
11. An image display device comprising the stretchable film according to claim 1 or 2.
12. A sanitary article comprising the laminate according to claim 7.
13. A cosmetic comprising the laminate according to claim 7.
14. An image display device comprising the laminate according to claim 7.
Citation Information
Patent Citations
Method for manufacturing laminate, laminate, polarizer, and image display device
JP2015210273A
Resin film, method for manufacturing resin film, resin film / adhesive layer laminate, method for manufacturing resin film / adhesive layer laminate, electric circuit body, healthcare sensor, wearable sensor, and method for manufacturing resin film processed product
JP2021116405A
Transfer film and Anti-glare molded body
JP2023048729A
Stretchable conductive elastomer with wrinkle structure, preparation and application thereof
CN113808780A
Stretchable film, method for forming the same, method for manufacturing wiring coated substrate, stretchable wiring film, and method for manufacturing the same
JP2017206626A