Separator for electrochemical device, and electrochemical device comprising same
The separator's optimized coating layer with specific binder and particle ratios addresses the issue of uneven pressure and mechanical stress, improving breakdown voltage and reducing defect rates in electrochemical devices by ensuring uniform pressure distribution and enhanced porosity.
Patent Information
- Application Number
- PCT/KR2024/005850
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-26
- Filing Date
- 2024-04-30
- Publication Date
- 2024-12-05
AI Technical Summary
Existing electrochemical device separators face issues with uneven binder distribution and pressure concentration during lamination, leading to reduced breakdown voltage and increased short-circuit defect rates due to uneven coating layers and mechanical stress.
A separator with a porous polymer substrate and a coating layer containing a particulate first polymer binder, a second polymer binder, and inorganic particles, where the average particle diameter ratio and weight ratios are optimized to ensure uniform pressure distribution and improved porosity, reducing surface roughness and enhancing mechanical properties.
The solution effectively prevents damage to the separator during lamination, reduces short-circuit and low-voltage defect rates, and improves breakdown voltage by ensuring uniform pressure application and increased porosity, thereby enhancing the overall performance and reliability of electrochemical devices.
Smart Images

Figure KR2024005850_05122024_PF_FP_ABST
Abstract
Description
Separator for electrochemical devices and electrochemical devices containing the same
[0001] The present invention claims the benefit of Korean Patent Application No. 10-2023-0068199, filed with the Korean Intellectual Property Office on May 26, 2023, the entire contents of which are incorporated herein by reference. The present invention relates to a separator for an electrochemical device and an electrochemical device comprising the same, and more particularly, to a separator for an electrochemical device capable of reducing a short-circuit failure rate and a low-voltage failure rate by controlling the surface roughness of a coating layer and the size ratio of particles included in the coating layer, and to an electrochemical device comprising the same.
[0002] Among the components of electrochemical devices, the separator comprises a porous polymer substrate located between the anode and cathode. It isolates the anode and cathode, prevents electrical short-circuiting between the two electrodes, and allows the passage of electrolytes and ions. While the separator itself does not participate in electrochemical reactions, its physical properties, such as wettability with electrolyte, degree of porosity, and thermal shrinkage, influence the performance and safety of the electrochemical device.
[0003] Accordingly, various methods have been attempted to enhance the physical properties of membranes by adding a coating layer to a porous polymer substrate and by adding various substances to the coating layer to change the properties of the coating layer. For example, inorganic substances may be added to the coating layer to enhance the mechanical strength of the membrane, or inorganic substances or hydrates may be added to the coating layer to enhance the flame retardancy and heat resistance of the polymer substrate.
[0004] The separator can be bonded to the electrode through a lamination process, and a binder resin can be added to the coating layer composition of the separator to secure adhesion between the electrode and the separator.
[0005] Meanwhile, during the electrode assembly manufacturing process, a lamination process is required to bond the electrode and separator, applying high temperatures and pressures. This process has the problem of damaging the separator due to the pressure and temperature. In the case of separators formed using conventional phase inversion techniques, the binder is not evenly distributed on the surface, resulting in areas with high and low binder content, resulting in an uneven coating layer.
[0006] Furthermore, in the case of a separator with an uneven coating layer, when high pressure is applied, the pressure is not applied evenly across the entire separator, causing damage to the separator, which has the problem of reducing the insulation breakdown voltage.
[0007] Therefore, research was needed on a membrane that can evenly apply pressure to the entire membrane, including a uniform coating layer.
[0008] The technical problem to be achieved by the present invention is to provide a separator for an electrochemical device and an electrochemical device including the same, which can prevent damage to the separator due to excessive concentration of pressure applied to a certain area of the separator during the process of manufacturing a secondary battery by laminating an electrode and a separator, and prevent a decrease in the insulation breakdown voltage.
[0009] However, the problems to be solved by the present invention are not limited to the problems mentioned above, and other problems not mentioned can be clearly understood by those skilled in the art from the description below.
[0010] One embodiment of the present invention comprises a porous polymer substrate; and a coating layer provided on at least one surface of the porous polymer substrate, the coating layer including a first polymer binder in particle form, a second polymer binder, and inorganic particles, wherein the average particle diameter (D) of the first polymer binder 50 ) and the average particle diameter (D) of the above inorganic particles 50) is 1:0.5 to 1:5, and the weight of the first polymer binder included in the coating layer is greater than the weight of the second polymer binder.
[0011] According to one embodiment of the present invention, the roughness (Sa) of the surface opposite to the surface adjacent to the porous polymer substrate of the coating layer may be 0.20 ㎛ or less.
[0012] According to one embodiment of the present invention, the first polymer binder may include one selected from an acrylic binder, a polyvinylidene binder, and a combination thereof.
[0013] According to one embodiment of the present invention, the second polymer binder may be one selected from the group consisting of polyacrylic acid (PAA), polyvinyl alcohol (PVA), polyvinylpyrrolidone (PVP), polyacrylamide (PAM), and combinations thereof.
[0014] According to one embodiment of the present invention, the average particle diameter (D) of the first polymer binder 50 ) may be 200 nm or more and 450 nm or less.
[0015] According to one embodiment of the present invention, the average particle diameter (D) of the inorganic particles 50 ) may be 300 nm or more and 700 nm or less.
[0016] According to one embodiment of the present invention, the weight ratio of the first polymer binder and the second polymer binder may be 5.5:4.5 to 9.5:0.5.
[0017] According to one embodiment of the present invention, the total content of the first polymer binder and the second polymer binder may be 5 parts by weight or more and 30 parts by weight or less with respect to 100 parts by weight of the coating layer.
[0018] According to one embodiment of the present invention, when pressurized for 10 seconds under the conditions of 70°C and 5.2 MPa, the thickness change rate of the coating layer defined by the following mathematical formula 1 may be 10% or more and 25% or less.
[0019] [Mathematical Formula 1]
[0020] Thickness change rate = (thickness of coating layer before pressing - thickness of separator after pressing) / thickness of coating layer before pressing
[0021] According to one embodiment of the present invention, when impregnated in a solution containing 70 parts by volume of ethylene carbonate and 30 parts by volume of ethyl methyl carbonate under conditions of 25°C and 1 atm for 24 hours, the rate of change in porosity of the coating layer defined by the following mathematical formula 2 may be 10% or more and 20% or less.
[0022] [Equation 2]
[0023] Rate of change in porosity = (Porosity of coating layer after impregnation - Porosity of coating layer before impregnation) / Porosity of coating layer before impregnation
[0024] One embodiment of the present invention provides an electrochemical device including: an anode; a cathode; and a separator interposed between the anode and the cathode.
[0025] A separator for an electrochemical device according to one embodiment of the present invention can uniformly apply pressure to the separator during a lamination process for bonding an electrode and a separator, and can improve the insulation breakdown voltage.
[0026] A separator for an electrochemical device according to one embodiment of the present invention can prevent damage to a porous polymer substrate, reduce local changes in the separator, and reduce a short-circuit failure rate.
[0027] A separator for an electrochemical device according to one embodiment of the present invention includes a particle-type polymer binder to buffer the pressure applied in a lamination process, and includes a polymer binder that is dissolved by an electrolyte to increase the porosity of a coating layer, thereby buffering the pressure applied in a j / f (jig formation) process.
[0028] An electrochemical device according to one embodiment of the present invention can reduce a short-circuit failure rate and a low-voltage failure rate, and improve an insulation breakdown voltage.
[0029] Figure 1 is a schematic diagram of a separator for an electrochemical device according to one embodiment of the present invention.
[0030] Figure 2 is a schematic diagram of an electrochemical device according to one embodiment of the present invention.
[0031] In this specification, when a part is said to "include" a certain component, this does not mean that it excludes other components, but rather that it may include other components, unless otherwise specifically stated.
[0032] In this specification, “A and / or B” means “A and B, or A or B.”
[0033] In this specification, when it is said that a component is “provided on”, this does not exclude other components being placed in between, unless otherwise specifically stated, but rather means that other components may be placed thereon.
[0034] In this specification, the characteristic of “having pores” means that the object includes a plurality of pores and that the pores are interconnected with each other, thereby allowing gaseous and / or liquid fluids to pass from one side of the object to the other side.
[0035] In this specification, the separator has a porous characteristic including a large number of pores, and acts as a porous ion-conducting barrier that allows ions to pass while blocking electrical contact between the cathode and the anode in an electrochemical device.
[0036] Hereinafter, the present invention will be described in more detail.
[0037] One embodiment of the present invention comprises a porous polymer substrate (110); and a coating layer (130) provided on at least one surface of the porous polymer substrate (110) and including a first polymer binder in particle form, a second polymer binder, and inorganic particles, wherein the average particle diameter (D) of the first polymer binder 50 ) and the average particle diameter (D) of the above inorganic particles 50 ) is 1:0.5 to 1:5, and the weight of the first polymer binder included in the coating layer (130) is greater than the weight of the second polymer binder, thereby providing a separator (100) for an electrochemical device.
[0038] According to one embodiment of the present invention, a separator for an electrochemical device can uniformly apply pressure applied during a lamination process for bonding an electrode and a separator to the separator, thereby improving the breakdown voltage. Furthermore, according to one embodiment of the present invention, a separator for an electrochemical device can prevent damage to a porous polymer substrate, reduce local changes in the separator, and reduce a short-circuit defect rate. In addition, according to one embodiment of the present invention, a separator for an electrochemical device can buffer the pressure applied during the lamination process by including a particulate polymer binder, and can buffer the pressure applied during the j / f (jig formation) process by increasing the porosity of a coating layer by including a polymer binder that is dissolved by an electrolyte.
[0039] FIG. 1 is a schematic diagram of a separator (100) for an electrochemical device according to one embodiment of the present invention. Referring to FIG. 1, the separator for an electrochemical device according to one embodiment of the present invention will be described in detail.
[0040] According to one embodiment of the present invention, the separator for an electrochemical device includes a porous polymer substrate (110). As described above, the separator for an electrochemical device includes a porous polymer substrate, thereby allowing lithium ions to pass through while blocking electrical contact, and implementing a shutdown function at an appropriate temperature.
[0041] According to one embodiment of the present invention, the porous polymer substrate may be manufactured using a polyolefin resin as a base resin. Examples of polyolefin-based resins include polyethylene, polypropylene, and polypentene, and the substrate may include one or more of these. A porous membrane, i.e., a membrane having a large number of pores, manufactured using such a polyolefin resin as a base resin can provide a shutdown function at an appropriate temperature.
[0042] According to one embodiment of the present invention, the weight average molecular weight of the polyolefin resin may be 500,000 or more and 1,500,000 or less. By controlling the weight average molecular weight of the polyolefin resin within the above-described range, the compression resistance of the separator can be improved. Furthermore, when different types of polyolefin resins are mixed and used or the separator is formed with a multilayer structure made of different types of polyolefin resins, the weight average molecular weight of the polyolefin resin can be calculated by adding the weight average molecular weights according to the content ratio of each polyolefin resin.
[0043] In one embodiment of the present invention, the weight average molecular weight (Mw) can be measured by gel permeation chromatography (GPC: gel permeation chromatography, PL GPC220, Agilent Technologies), and the measurement conditions can be set as follows.
[0044] - Column: PL Olexis (Polymer Laboratories)
[0045] - Solvent: TCB (Trichlorobenzene)
[0046] - Flow rate: 1.0 ml / min
[0047] - Sample concentration: 1.0 mg / ml
[0048] - Injection volume: 200 ㎕
[0049] - Column temperature: 160 ℃
[0050] - Detector: Agilent High Temperature RI detector
[0051] - Standard: Polystyrene (corrected with a cubic function)
[0052] According to one embodiment of the present invention, the porous polymer substrate may be manufactured by a method (wet method) in which a polyolefin resin is mixed with a plasticizer at a high temperature to form a single phase, the polymer material and the plasticizer are phase-separated during a cooling process, the plasticizer is extracted to form pores, and then stretching and heat-setting are performed. In addition, the porous polymer substrate using the polyolefin resin may have a core portion made of a mixture of polyethylene and polypropylene and a polyethylene skin portion laminated on both sides of the core portion.
[0053] According to one embodiment of the present invention, the average size of the pores of the separation membrane and the maximum size of the pores can be easily manufactured by a person skilled in the art by controlling the mixing ratio of the plasticizer, the stretching ratio, the heat-setting treatment temperature, etc. to conform to the scope of the present invention.
[0054] According to one embodiment of the present invention, the separator (100) for an electrochemical device includes a coating layer (130) provided on at least one surface of the porous polymer substrate (110). Specifically, the separator for an electrochemical device includes a coating layer provided on one or both surfaces of the porous polymer substrate. As described above, by the separator for an electrochemical device including a coating layer provided on at least one surface of the porous polymer substrate, the heat resistance of the separator can be improved, mechanical properties can be improved, and the shrinkage of the separator at high temperatures can be prevented, resulting in an electrical short circuit of the electrode.
[0055] According to one embodiment of the present invention, the coating layer includes a first polymer binder in particle form, a second polymer binder, and inorganic particles. As described above, since the coating layer includes the first polymer binder in particle form, the second polymer binder, and the inorganic particles, the heat resistance of the separator is improved, the mechanical properties are improved, the separator shrinks at high temperatures, preventing an electrical short circuit of the electrode, and pores can be formed inside the coating layer.
[0056] According to one embodiment of the present invention, the coating layer may be formed by the inorganic particles being bound by the first polymer binder particles and the second polymer binder in particle form and being accumulated within the side. Alternatively, the coating layer may be formed by the inorganic particles being bound by the first polymer binder particles in particle form and being accumulated within the side. The pores within the coating layer may be derived from the interstitial volume, which is an empty space between the inorganic particles.
[0057] In one embodiment of the present invention, the porosity of the coating layer may be 30% to 70% by volume. If the porosity is 70% or less by volume, mechanical properties that can withstand the pressing process for bonding with the electrode can be secured, and the surface opening ratio is not too high, making it suitable for securing adhesive strength. On the other hand, if the porosity is 30% or more by volume, it is advantageous from the perspective of ion permeability.
[0058] In this specification, the porosity means the ratio of the volume occupied by pores to the total volume, and uses volume% as its unit, and can be used interchangeably with terms such as porosity and porosity.
[0059] In this specification, porosity corresponds to a value obtained by subtracting the volume converted into the weight and density of each component of the coating layer from the volume calculated in the thickness, width, and length of the coating layer.
[0060] In one embodiment of the present invention, the porosity and pore size of the coating layer can be measured by the BET 6-point method using a scanning electron microscope (SEM) image, a mercury porosimeter, a capillary flow porometer, or a porosimetry analyzer (Bell Japan Inc, Belsorp-II mini) using a nitrogen gas adsorption flow method. In this case, it may be advantageous to use a capillary flow porometer.
[0061] According to one embodiment of the present invention, the thickness of the coating layer may be formed to a thickness of 1 μm to 20 μm on either side of the porous high-branch substrate, but is not particularly limited thereto. The thickness can be adjusted to an appropriate range by those skilled in the art in terms of heat resistance or electrical resistance.
[0062] In one embodiment of the present invention, the thickness of the polymer substrate and / or the coating layer, etc., can be measured using a contact-type thickness measuring device. The contact-type thickness measuring device can be, for example, VL-50S-B from Mitutoyo.
[0063] According to one embodiment of the present invention, the average particle diameter (D) of the first polymer binder in the coating layer 50 ) and the average particle diameter (D) of the above inorganic particles 50 ) is 1:1.0 to 1:5. Specifically, the average particle diameter (D) of the first polymer binder in the coating layer 50 ) and the average particle diameter (D) of the above inorganic particles 50 ) may be 1:1.0 to 1:4.5, 1:1.5 to 1:4.0, 1:2.0 to 1:3.5 or 1:2.5 to 1:3.0. Preferably, the average particle diameter (D) of the first polymer binder in the coating layer 50 ) and the average particle diameter (D) of the above inorganic particles 50 ) may be 1:1.0 to 1:3.0. In the above-described range, the average particle diameter (D) of the first polymer binder of the coating layer 50 ) and the average particle diameter (D) of the above inorganic particles 50 ) can be adjusted to control the roughness (Sa) of the surface of the coating layer, and by reducing the surface roughness, even when pressure is applied, the breakdown voltage can be improved by preventing excessive pressure from being applied to a specific part. In addition, the average particle diameter (D) of the first polymer binder in the coating layer 50 ) and the average particle diameter (D) of the above inorganic particles 50 ) by controlling the ratio of the first polymer binder, the first polymer binder can migrate to the surface of the coating layer, thereby reducing the roughness of the surface.
[0064] In this specification, "D 50"Particle size" means the particle size at the 50% point of the cumulative distribution of the number of particles according to the particle size. The particle size can be measured using a laser diffraction method. Specifically, after the powder to be measured is dispersed in a dispersion medium, it is introduced into a commercially available laser diffraction particle size measuring device (e.g., Microtrac S3500) and the particle size distribution is calculated by measuring the difference in the diffraction pattern according to the particle size when the particles pass through the laser beam. By calculating the particle diameter at the point where the cumulative distribution of the number of particles according to the particle size in the measuring device becomes 50%, D 50 The mouth diameter can be measured.
[0065] According to one embodiment of the present invention, the second polymer binder may be a soluble polymer binder. Specifically, the soluble polymer binder may mean one that is dissolved by the electrolyte. That is, the soluble polymer binder may be dissolved and eluted by the electrolyte. As described above, by selecting the second polymer binder as a soluble polymer binder, the porosity of the coating layer in the electrochemical device injected with the electrolyte may increase from 10% to 20%, thereby buffering the pressure applied in the j / f (jig formation) process.
[0066] According to one embodiment of the present invention, the weight of the first polymer binder included in the coating layer is greater than the weight of the second polymer binder. As described above, by implementing the weight of the first polymer binder included in the coating layer to be greater than the weight of the second polymer binder, the porosity of the coating layer can be prevented from increasing excessively, and the bonding strength of the coating layer can be increased.
[0067] According to one embodiment of the present invention, the roughness (Sa) of the surface opposite to the surface adjacent to the porous polymer substrate of the coating layer may be 0.20 ㎛ or less. Specifically, the roughness (Sa) of the surface opposite to the surface adjacent to the porous polymer substrate of the coating layer may be 0 ㎛ or more and 0.20 ㎛ or less, more than 0 ㎛ and 0.19 ㎛ or less, 0.1 ㎛ or more and 0.18 ㎛ or less, 0.2 ㎛ or more and 0.17 ㎛ or less, 0.3 ㎛ or more and 0.16 ㎛ or less, 0.4 ㎛ or more and 0.15 ㎛ or less, 0.5 ㎛ or more and 0.14 ㎛ or less, 0.6 ㎛ or more and 0.13 ㎛ or less, 0.7 ㎛ or more and 0.12 ㎛ or less, 0.8 ㎛ or more and 0.11 ㎛ or less, or 0.9 ㎛ or more and 0.10 ㎛ or less. By controlling the surface roughness (Sa, area roughness) of the surface opposite to the surface adjacent to the porous polymer substrate of the coating layer within the above-described range, excessive pressure is prevented from being applied to a portion of the separator during the lamination process, which is a process for manufacturing an electrode, thereby preventing damage to the coating layer and improving the breakdown voltage of the separator. The surface roughness of the coating layer may be controlled by controlling the content of the first polymer binder and the average particle size ratio with the inorganic particles, and the first polymer binder may be positioned between the inorganic particles on the surface of the coating layer to reduce the surface roughness.
[0068]
[0069] In this specification, “surface roughness (Sa)” may mean that measured using an Optical Profiler NV 2700 from Nanosystem Co., Ltd.
[0070] According to one embodiment of the present invention, the first polymer binder may include one selected from an acrylic binder, a polyvinylidene binder, and a combination thereof. Furthermore, the first polymer binder may be a hybrid particle in which an acrylic binder and a polyvinylidene binder are hybridized into a single particle. By selecting the first polymer binder as described above, pores of the coating layer can be formed, the bonding strength of the coating layer can be improved, and the durability of the coating layer can be improved.
[0071] According to one embodiment of the present invention, the acrylic binder is a polymer containing a carboxylic acid ester as a repeating unit, and may preferably be a (meth)acrylic acid ester or an acrylic-styrene copolymer.
[0072] According to one embodiment of the present invention, the (meth)acrylic acid esters (methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, i-propyl (meth)acrylate, n-butyl (meth)acrylate, i-butyl (meth)acrylate, n-amyl (meth)acrylate, i-amyl (meth)acrylate, hexyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, hydroxymethyl (meth)acrylate, hydroxyethyl (meth)acrylate, ethylene glycol (meth)acrylate, di(meth)acrylate, propylene glycol (meth)acrylate, Examples thereof include trimethylolpropane tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, allyl (meth)acrylate, and ethylene di(meth)acrylate, and the like may be at least one selected from these. Among these, at least one selected from methyl (meth)acrylate, ethyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate is preferable, and methyl (meth)acrylate is particularly preferable.
[0073] According to one embodiment of the present invention, the acrylic-styrene copolymer may include an acrylic binder, and the acrylic binder may be a polyacrylate. For example, the binder may be at least one selected from the group consisting of styrenebutadiene rubber, nitrile-butadiene rubber, acrylonitrile-butadiene rubber, acrylonitrile-butadiene-styrene rubber, and acrylate polymers, and more specifically, may be a copolymer including acrylate.
[0074] According to one embodiment of the present invention, the polyvinylidene-based binder may be a polyvinylidene fluoride-based binder. As described above, by selecting the polyvinylidene fluoride-based binder as the polyvinylidene-based binder, the porosity of the separator can be maintained, thereby improving the resistance of the separator, enhancing wet adhesion, and reducing the resistance of the separator.
[0075] According to one embodiment of the present invention, the polyvinylidene-based binder may have a hexafluoropropylene content of 15 wt% or more. Specifically, the polyvinylidene-based binder included in the first polymer binder particle may have a hexafluoropropylene content of 10 wt% or more and 80 wt% or less, 15 wt% or more and 75 wt% or less, 20 wt% or more and 70 wt% or less, 25 wt% or more and 65 wt% or less, 30 wt% or more and 60 wt% or less, 35 wt% or more and 55 wt% or less, or 40 wt% or more and 50 wt% or less. By controlling the content of hexafluoropropylene included in the polyvinylidene-based binder in the first polymer binder particle within the above-described range, the resistance of the separator can be reduced. The content of the hexafluoropropylene (HFP) monomer 1 H-NMR and / or 19 It can be measured by F-NMR.
[0076] According to one embodiment of the present invention, the second polymer binder may be one selected from the group consisting of polyacrylic acid (PAA), polyvinyl alcohol (PVA), polyvinylpyrrolidone (PVP), polyacrylamide (PAM), and combinations thereof. By selecting the second polymer binder from the above, it is possible to improve the porosity of the coating layer by dissolving it in the electrolyte, and to implement a buffering action according to pressure in the lamination process, thereby preventing damage to the separator and improving the breakdown voltage.
[0077] According to one embodiment of the present invention, the average particle diameter (D) of the first polymer binder 50 ) may be 200 nm or more and 450 nm or less. Specifically, the average particle diameter (D) of the first polymer binder 50) may be 210 nm to 440 nm, 220 nm to 430 nm, 230 nm to 420 nm, 240 nm to 410 nm, 250 nm to 400 nm, 260 nm to 390 nm, 270 nm to 380 nm, 280 nm to 370 nm, 290 nm to 360 nm, 300 nm to 350 nm, 310 nm to 340 nm, or 320 nm to 330 nm. In the above-described range, the average particle diameter (D of the first polymer binder 50 ) by controlling the coating layer, the coating layer can prevent damage to the separator by providing a pressure-dependent buffering effect in the lamination process before electrolyte injection, thereby improving the insulation breakdown voltage and reducing the roughness of the coating layer surface.
[0078] According to one embodiment of the present invention, the average particle diameter (D) of the inorganic particles 50 ) may be 300 nm or more and 700 nm or less. Specifically, the average particle diameter (D) of the inorganic particles 50) is 310 nm to 690 nm, 320 nm to 680 nm, 330 nm to 670 nm, 340 nm to 660 nm, 350 nm to 650 nm, 360 nm to 640 nm, 370 nm to 630 nm, 380 nm to 620 nm, 390 nm to 610 nm, 400 nm to 600 nm, 410 nm to 590 nm, 420 nm to 580 nm, 430 nm to 570 nm, 440 nm to 560 nm, 450 nm to 550 nm, 460 nm to 540 nm, 470 nm to 530 nm, 480 nm to 520 nm or 490 nm or more It may be less than 510 nm. In the above-described range, the average particle diameter (D) of the inorganic particles 50 ) can be adjusted to lower the roughness of the surface of the coating layer and improve the insulation breakdown voltage.
[0079] According to one embodiment of the present invention, the weight ratio of the first polymer binder and the second polymer binder may be 5.5:4.5 to 9.5:0.5. Specifically, the weight ratio of the first polymer binder and the second polymer binder may be 5.5:4.5 to 9.5:0.5, 6.0:4.0 to 9.0:1.0, 6.5:3.5 to 8.5:1.5, or 7.0:3.0 to 8.0:2.0. By controlling the weight ratio of the first polymer binder and the second polymer binder within the above-described range, the coating layer can prevent damage to the separator by performing a pressure-dependent buffering action in the lamination process before electrolyte injection, thereby improving the breakdown voltage and reducing the roughness of the coating layer surface. In addition, by improving the porosity of the coating layer, the coating layer can prevent damage to the separator by performing a pressure-dependent buffering action in the lamination process after electrolyte injection, thereby improving the breakdown voltage.
[0080] According to one embodiment of the present invention, the total content of the first polymer binder and the second polymer binder may be 5 parts by weight or more and 30 parts by weight or less with respect to 100 parts by weight of the coating layer. Specifically, the total content of the first polymer binder and the second polymer binder may be 6 parts by weight or more and 29 parts by weight or less, 7 parts by weight or more and 28 parts by weight or less, 8 parts by weight or more and 27 parts by weight or less, 9 parts by weight or more and 26 parts by weight or less, 10 parts by weight or more and 25 parts by weight or less, 11 parts by weight or more and 24 parts by weight or less, 12 parts by weight or more and 23 parts by weight or less, 13 parts by weight or more and 22 parts by weight or less, 14 parts by weight or more and 21 parts by weight or less, 15 parts by weight or more and 20 parts by weight or less, 16 parts by weight or more and 19 parts by weight or less, or 17 parts by weight or more and 18 parts by weight or less with respect to 100 parts by weight of the coating layer. By controlling the total content of the first polymer binder and the second polymer binder within the above-described range, the bonding strength and porosity of the coating layer can be controlled.
[0081] According to one embodiment of the present invention, the content of the inorganic particles may be 70 parts by weight or more and 95 parts by weight or less with respect to 100 parts by weight of the coating layer. Specifically, the content of the inorganic particles may be 71 parts by weight or more and 94 parts by weight or less, 72 parts by weight or more and 93 parts by weight or less, 73 parts by weight or more and 92 parts by weight or less, 74 parts by weight or more and 91 parts by weight or less, 75 parts by weight or more and 90 parts by weight or less, 76 parts by weight or more and 89 parts by weight or less, 77 parts by weight or more and 88 parts by weight or less, 78 parts by weight or more and 87 parts by weight or less, 79 parts by weight or more and 86 parts by weight or less, 80 parts by weight or more and 85 parts by weight or less, 81 parts by weight or more and 84 parts by weight or less, or 82 parts by weight or more and 83 parts by weight or less with respect to 100 parts by weight of the coating layer. By controlling the content of the inorganic particles within the above-described range, the heat resistance of the separator can be improved.
[0082] According to one embodiment of the present invention, the inorganic particles that can be used in the coating layer are not particularly limited as long as they are electrochemically stable. That is, the inorganic particles that can be used in one embodiment of the present invention are those that can be used in the operating voltage range of the applied electrochemical device (e.g., Li / Li). + There are no particular limitations as long as no oxidation and / or reduction reaction occurs at a voltage of 0 V to 5 V (as a reference).
[0083] According to one embodiment of the present invention, non-limiting examples of the inorganic particles include BaTiO3, Pb(Zr,Ti)O3(PZT), Pb 1-x La x Zr 1-y Ti y O3(PLZT, 0 <x<1, 0<y<1), Pb(Mg 1 / 3 Nb 2 / 3 )O3-PbTiO3(PMN-PT), hafnia (HfO2), SrTiO3, SnO2, CeO2, MgO, Mg(OH)2, NiO, CaO, ZnO, ZrO2, SiO2, Y2O3, Al2O3, SiC, Al(OH)3, TiO2, aluminum peroxide, zinc tin hydroxide (ZnSn(OH)6), tin-zinc oxide (Zn2SnO4, ZnSnO3), antimony trioxide (Sb2O3), antimony tetroxide (Sb2O4), antimony pentoxide (Sb2O5), etc., and may include one or more of these.
[0084] According to one embodiment of the present invention, when pressurized for 10 seconds under the conditions of 70°C and 5.2 MPa, the thickness change rate of the coating layer defined by the following mathematical formula 1 may be 10% or more and 25% or less.
[0085] [Mathematical Formula 1]
[0086] Thickness change rate = (thickness of coating layer before pressing - thickness of separator after pressing) / thickness of coating layer before pressing
[0087] Specifically, when pressurized for 10 seconds under the conditions of 70 ℃ and 5.2 MPa, the thickness change rate of the coating layer defined by the above mathematical formula 1 may be 11% or more and 24% or less, 12% or more and 23% or less, 13% or more and 22% or less, 14% or more and 21% or less, 15% or more and 20% or less, 16% or more and 19% or less, or 17% or more and 18% or less. By controlling the thickness change rate of the coating layer within the above-described range, damage to the porous polymer substrate can be prevented, thereby improving the insulation breakdown voltage.
[0088] According to one embodiment of the present invention, when impregnated in a solution containing 70 parts by volume of ethylene carbonate and 30 parts by volume of ethyl methyl carbonate under conditions of 25°C and 1 atm for 24 hours, the rate of change in porosity of the coating layer defined by the following mathematical formula 2 may be 10% or more and 20% or less.
[0089] [Equation 2]
[0090] Rate of change in porosity = (Porosity of coating layer after impregnation - Porosity of coating layer before impregnation) / Porosity of coating layer before impregnation
[0091] Specifically, when impregnated in a solution containing 70 parts by volume of ethylene carbonate and 30 parts by volume of ethyl methyl carbonate at 25°C and 1 atm for 24 hours, the rate of change in the porosity of the coating layer defined by the above mathematical formula 2 may be 11% or more and 19% or less, 12% or more and 18% or less, 13% or more and 17% or less, or 14% or more and 16% or less. By controlling the rate of change in the porosity of the coating layer within the above-described range, the surface roughness of the coating layer can be reduced, the porosity of the coating layer can be improved, thereby preventing uneven application of pressure and improving the breakdown voltage.
[0092] One embodiment of the present invention provides a method for manufacturing a separator for an electrochemical device, comprising the steps of: mixing a slurry for a coating layer including a first polymer binder in particle form, a second polymer binder, and inorganic particles; applying the slurry for a coating layer on at least one surface of a porous polymer substrate; and drying the slurry for a coating layer to form a coating layer.
[0093] The method for manufacturing a separator for an electrochemical device according to one embodiment of the present invention can easily improve the breakdown voltage of the separator and prevent damage to the separator. In the description of the method for manufacturing a separator for an electrochemical device according to one embodiment of the present invention, any content that overlaps with the description of the separator for an electrochemical device will be omitted.
[0094] According to one embodiment of the present invention, the method for manufacturing a separator for an electrochemical device includes a step of mixing a slurry for a coating layer including a first polymer binder in particle form, a second polymer binder, and inorganic particles. By including the step of mixing a slurry for a coating layer including a first polymer binder in particle form, a second polymer binder, and inorganic particles as described above, a coating layer can be easily formed on the separator.
[0095] According to one embodiment of the present invention, a polymer binder resin, i.e., a first polymer binder and a second polymer binder, may be dispersed in an appropriate dispersion medium to prepare a polymer emulsion, thereby providing a slurry for a coating layer. The dispersion medium preferably has a low boiling point. This is to facilitate uniform mixing and subsequent removal of the dispersion medium. Non-limiting examples of usable dispersion mediums include acetone, tetrahydrofuran, methylene chloride, chloroform, dimethylformamide, N-methyl-2-pyrrolidone (NMP), cyclohexane, water, or a mixture thereof. Preferably, the dispersion medium may be water.
[0096] According to one embodiment of the present invention, a polymer binder resin, i.e., a first polymer binder and a second polymer binder, may be dissolved in an appropriate solvent to prepare a polymer solution, thereby preparing a slurry for a coating layer. The solvent is preferably one having a solubility index similar to that of the binder polymer to be used and a low boiling point. This is to facilitate uniform mixing and subsequent solvent removal. Non-limiting examples of usable solvents include acetone, tetrahydrofuran, methylene chloride, chloroform, dimethylformamide, N-methyl-2-pyrrolidone (NMP), cyclohexane, water, or a mixture thereof. Preferably, the solvent may be water.
[0097] According to one embodiment of the present invention, inorganic particles may be added and dispersed in the polymer emulsion or polymer solvent. The content ratio of the inorganic particles and the polymer binder is as described above, and is appropriately adjusted in consideration of the thickness, pore size, and porosity of the coating layer to be finally manufactured according to one embodiment of the present invention.
[0098] According to one embodiment of the present invention, the method for manufacturing a separator for an electrochemical device includes a step of applying the slurry for a coating layer on at least one surface of a porous polymer substrate. By including the step of applying the slurry for a coating layer on at least one surface of the porous polymer substrate as described above, a coating layer can be formed with a single application, and the slurry for a coating layer has an excess of inorganic particles in a portion close to the porous polymer substrate due to separation between the inorganic particles and the polymer binder, and an excess of polymer binder particles in a portion far from the porous polymer substrate, thereby improving adhesion to an electrode and improving the porosity of the separator.
[0099] According to one embodiment of the present invention, the method for applying the slurry for the coating layer to the surface of the porous polymer substrate is not particularly limited to any one method, and conventional methods known in the art may be used. For example, various methods such as dip coating, die coating, roll coating, comma coating, or a combination thereof may be used.
[0100] According to one embodiment of the present invention, the method for manufacturing the separator for the electrochemical device includes a step of drying the slurry for the coating layer to form a coating layer. By including the step of drying the slurry for the coating layer to form a coating layer as described above, damage to the coating layer can be minimized, and the dispersion medium or solvent contained in the slurry can be easily removed.
[0101] According to one embodiment of the present invention, the drying process appropriately sets time conditions to minimize the occurrence of surface defects in the coating layer. The drying may be performed using a drying assist device, such as a drying oven or hot air, within an appropriate range.
[0102] According to one embodiment of the present invention, the separator is interposed between the negative electrode and the positive electrode and is manufactured into an electrode assembly through a lamination process that applies heat and / or pressure to bond them. In one embodiment of the present invention, the lamination process can be performed by a roll press device including a pair of pressure rollers. That is, the negative electrode, the separator, and the positive electrode can be sequentially laminated and placed between the pressure rollers to achieve interlayer bonding. At this time, the lamination process can be performed by a hot press method.
[0103] One embodiment of the present invention provides an electrochemical device including: an anode (300); a cathode (500); and a separator (100) interposed between the anode (300) and the cathode (500).
[0104] An electrochemical device according to one embodiment of the present invention can reduce a short-circuit failure rate and a low-voltage failure rate, and improve an insulation breakdown voltage.
[0105] Figure 2 is a schematic diagram of an electrochemical device according to one embodiment of the present invention. Referring to Figure 2, the electrochemical device according to one embodiment of the present invention will be described in detail.
[0106] In the present invention, the electrochemical device is a device that converts chemical energy into electrical energy through an electrochemical reaction, and is a concept encompassing a primary battery and a secondary battery. In the present specification, the secondary battery is capable of charging and discharging, and refers to a lithium secondary battery, a nickel-cadmium battery, a nickel-hydrogen battery, etc. The lithium secondary battery uses lithium ions as an ion conductor, and examples thereof include, but are not limited to, a non-aqueous electrolyte secondary battery including a liquid electrolyte, an all-solid-state battery including a solid electrolyte, a lithium polymer battery including a gel polymer electrolyte, and a lithium metal battery using lithium metal as an anode.
[0107] According to one embodiment of the present invention, the positive electrode (300) has a positive electrode current collector and a positive electrode active material layer including a positive electrode active material, a conductive material, and a binder resin on at least one surface of the positive electrode current collector. The positive electrode active material is a layered compound such as lithium manganese oxide (LiMn2O4, LiMnO2, etc.), lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), or a compound substituted with one or more transition metals; chemical formula Li 1+x Mn 2-x Lithium manganese oxides such as O4 (where x is 0 to 0.33), LiMnO3, LiMn2O3, LiMnO2; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8, LiV3O4, V2O5, Cu2V2O7; chemical formula LiNi 1-x M x Ni-site type lithium nickel oxide represented by O2 (where M = Co, Mn, Al, Cu, Fe, Mg, B or Ga and x = 0.01 to 0.3); chemical formula LiMn1-xM xA lithium manganese composite oxide represented by O2 (wherein, M = Co, Ni, Fe, Cr, Zn or Ta, and x = 0.01 to 0.1) or Li2Mn3MO8 (wherein, M = Fe, Co, Ni, Cu or Zn); LiMn2O4 in which a portion of Li in the chemical formula is replaced by an alkaline earth metal ion; a disulfide compound; or a mixture of two or more of Fe2(MoO4)3.
[0108] According to one embodiment of the present invention, the negative electrode (500) has a negative electrode current collector and a negative electrode active material layer including a negative electrode active material, a conductive material, and a binder resin on at least one surface of the current collector. The negative electrode includes carbon such as lithium metal oxide, non-graphitizable carbon, and graphite carbon as the negative electrode active material; LixFe2O3(0≤x≤1), Li x WO2(0≤x≤1), Sn x Me 1-x Me' y O z (Me: Mn, Fe, Pb, Ge; Me': Al, B, P, Si, elements of group 1, 2, and 3 of the periodic table, halogens; 0 <x≤1; 1≤y≤3; 1≤z≤8) 등의 금속 복합 산화물; 리튬 금속; 리튬 합금; 규소계 합금; 주석계 합금; SnO, SnO2, PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O4, 및 Bi2O5등의 금속 산화물; 폴리아세틸렌 등의 도전성 고분자; Li-Co-Ni 계 재료; 티타늄 산화물 중 선택된 1종 또는 2종 이상의 혼합물을 포함할 수 있다.
[0109] According to one embodiment of the present invention, the conductive material may be, for example, one selected from the group consisting of graphite, carbon black, carbon fibers or metal fibers, metal powders, conductive whiskers, conductive metal oxides, activated carbon, and polyphenylene derivatives, or a mixture of two or more conductive materials among these. More specifically, the conductive material may be one selected from the group consisting of natural graphite, artificial graphite, super-p, acetylene black, Ketjen black, channel black, furnace black, lamp black, summer black, Denka black, aluminum powder, nickel powder, zinc oxide, potassium titanate, and titanium oxide, or a mixture of two or more conductive materials among these.
[0110] According to one embodiment of the present invention, the current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery, and for example, stainless steel, copper, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. can be used.
[0111] According to one embodiment of the present invention, the binder resin may be a polymer commonly used in electrodes in the art. Non-limiting examples of such binder resins include polyvinylidene fluoride-co-hexafluoropropylene, polyvinylidene fluoride-cotrichloroethylene, polymethylmethacrylate, polyethylhexyl acrylate, polybutylacrylate, polyacrylonitrile, polyvinylpyrrolidone, polyvinylacetate, polyethylene-co-vinyl acetate, polyethylene oxide, polyarylate, cellulose acetate, cellulose acetate butyrate, and cellulose acetate propionate. Examples thereof include, but are not limited to, cellulose acetatepropionate, cyanoethylpullulan, cyanoethylpolyvinylalcohol, cyanoethylcellulose, cyanoethylsucrose, pullulan, and carboxyl methyl cellulose.
[0112] In the present invention, the positive electrode slurry for manufacturing the positive electrode active material layer may include a dispersant, and the dispersant may be a pyrrolidone-based compound. Specifically, it may be N-methylpyrrolidone (ADC-01, LG Chemical).
[0113] According to one embodiment of the present invention, the content of the dispersant included in the positive electrode slurry may be more than 0 part by weight and less than or equal to 0.5 part by weight with respect to 100 parts by weight of the positive electrode slurry. Specifically, the content of the dispersant included in the positive electrode slurry may be more than 0.05 part by weight and less than or equal to 0.4 part by weight with respect to 100 parts by weight of the positive electrode slurry.
[0114] According to one embodiment of the present invention, the negative electrode slurry for producing the negative electrode active material layer may include a dispersant, and the dispersant may be a polypyrrolidone-based compound. Specifically, the dispersant may be polyvinylpyrrolidone (Polyvinylpyrrolidone, Junsei, Japan).
[0115] According to one embodiment of the present invention, the content of the dispersant included in the cathode slurry may be more than 0 part by weight and less than or equal to 0.5 part by weight with respect to 100 parts by weight of the cathode slurry. Specifically, the content of the dispersant included in the cathode slurry may be more than 0.05 part by weight and less than or equal to 0.4 part by weight with respect to 100 parts by weight of the cathode slurry.
[0116] According to one embodiment of the present invention, the electrode assembly prepared as described above can be loaded into an appropriate case and an electrolyte can be injected to manufacture an electrochemical device.
[0117] According to one embodiment of the present invention, the electrolyte is A + B - As a salt with the same structure, A + is Li + , Na + , K +B containing an ion composed of an alkali metal cation or a combination thereof, such as - is PF6 - , BF4 - , Cl - , Br - , I - , ClO4 - , AsF6 - , CH3CO2 - , CF3SO3 - , N(CF3SO2)2 - , C(CF2SO2)3 - Salts containing anions such as or combinations thereof are dissolved or dissociated in organic solvents such as propylene carbonate (PC), ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), dimethyl sulfoxide, acetonitrile, dimethoxyethane, diethoxyethane, tetrahydrofuran, N-methyl-2-pyrrolidone (NMP), ethyl methyl carbonate (EMC), gamma butyrolactone (γ-butyrolactone) or mixtures thereof, but are not limited thereto.
[0118] One embodiment of the present invention provides a battery module including a battery including the electrochemical element as a unit cell, a battery pack including the battery module, and a device including the battery pack as a power source. Specific examples of the device include, but are not limited to, a power tool that is powered by an electric motor; an electric vehicle including an electric vehicle (EV), a hybrid electric vehicle (HEV), a plug-in hybrid electric vehicle (PHEV), etc.; an electric two-wheeled vehicle including an electric bicycle (E-bike) and an electric scooter (E-scooter); an electric golf cart; and a power storage system.
[0119] Hereinafter, the present invention will be described in detail using examples. However, the examples according to the present invention may be modified in various ways, and the scope of the present invention is not limited to the examples described below. The examples in this specification are provided to more fully explain the present invention to those of ordinary skill in the art.
[0120] <Example 1>
[0121] Polyethylene resin (weight average molecular weight 900,000) was extruded and a porous polymer substrate (total thickness of approximately 9 ㎛, porosity of 40% by volume) was manufactured using a wet method.
[0122] As the first polymer binder, an acrylic binder, styrene-butyl acrylate (LG Chemical, particle size: 400 nm), and as a polyvinylidene binder, a copolymer of PVdF and HFP with a substitution degree (weight ratio of HFP in PVdF polymer) of 5 wt% (Arkema, particle size: 250 nm) were used. Acrylic acid (Lubrizol, Ck702) was used as the second polymer binder. The inorganic particles were Al2O 3( (Particle size 500 nm) was used.
[0123] The first polymer binder, the second polymer binder, and the inorganic particles were dispersed in water to prepare a slurry for a coating layer (solid concentration: 30 wt%). The weight ratio of the first polymer binder and the second polymer binder was added at 9:1, and the particle size (D) of the first polymer binder and the inorganic particles was 50 ) was 1:1. Furthermore, the weight of the first polymer binder and the second polymer binder was 20 wt% with respect to the total weight of the first polymer binder, the second polymer binder, and the inorganic particles.
[0124] The dispersion was applied to both sides of the porous polymer substrate using a doctor blade by bar coating, and the separation membrane was manufactured by drying with wind at 50°C using a heat gun.
[0125] <Example 2>
[0126] A separation membrane was manufactured in the same manner as in Example 1, except that the weight ratio of the first polymer binder and the second polymer binder was added in a 7:3 ratio to manufacture a slurry for the coating layer.
[0127] <Example 3>
[0128] In the above Example 1, the particle size (D) of the first polymer binder and the inorganic particles 50 ) was changed to 1:3, and the weight ratio of the first polymer binder and the second polymer binder was added to 7:3 to prepare a slurry for the coating layer, and a separation membrane was manufactured in the same manner as in Example 1.
[0129] <Comparative Example 1>
[0130] A separation membrane was manufactured in the same manner as in Example 1, except that a second polymer binder was used instead of the first polymer binder.
[0131] Comparative Example 2
[0132] In the above Example 1, the particle size (D) of the first polymer binder and the inorganic particles 50 ) was changed to 1:10, and the weight ratio of the first polymer binder and the second polymer binder was added at 5:5 to prepare a slurry for the coating layer, and a separation membrane was manufactured in the same manner as in Example 1.
[0133] <Comparative Example 3>
[0134] In the above Example 1, the particle size (D) of the first polymer binder and the inorganic particles 50) was changed to 1:10 and a separation membrane was manufactured in the same manner as in Example 1, except that the first polymer binder was used instead of the second polymer binder.
[0135] <Comparative Example 4>
[0136] A separation membrane was manufactured in the same manner as in Example 1, except that the weight ratio of the first polymer binder and the second polymer binder was added in a 5:5 ratio to manufacture a slurry for the coating layer.
[0137] Comparative Example 5
[0138] A separation membrane was manufactured in the same manner as in Example 1, except that the first polymer binder was used instead of the second polymer binder.
[0139] Comparative Example 6
[0140] A separation membrane was manufactured in the same manner as in Example 1, except that the weight ratio of the first polymer binder and the second polymer binder was added in a 3:7 ratio to manufacture a slurry for the coating layer.
[0141] <Comparative Example 7>
[0142] In the above Example 1, the particle size (D) of the first polymer binder and the inorganic particles 50 ) was changed to 1:0.5, and a separation membrane was manufactured in the same manner as in Example 1.
[0143]
[0144] Table 1 below is a table showing the particle size ratio of the first polymer binder and the second polymer binder of Examples 1 to 3 and Comparative Examples 1 to 7 and the weight ratio of the first polymer binder and the second polymer binder.
[0145] Ratio of particle sizes of the first polymer binder and the second polymer binder Weight ratio of the first polymer binder and the second polymer binder First polymer binder Inorganic particles First polymer binder Second polymer binder Example 11191 Example 21173 Example 31373 Comparative examples 1---10 Comparative example 211055 Comparative example 311010-Comparative example 41155 Comparative example 51110-Comparative example 61137 Comparative example 710.591
[0146] <Manufacturing of electrochemical devices>
[0147] 1) Manufacturing of the anode
[0148] Cathode active material (LiNi) 0.8 Mn 0.1 Co 0.1 O2), conductive agent (carbon black), dispersant (N-methylpyrrolidone, ADC-01, LG Chemical), and binder resin (PVDF-HFP and PVDF mixture) were mixed with water in a weight ratio of 97.5:0.7:0.14:1.66 to prepare a slurry for a positive electrode active material layer with a concentration of 50 wt% of the remaining components excluding water. Next, the slurry was applied to the surface of an aluminum thin film (thickness 10 μm) and dried to manufacture a positive electrode having a positive electrode active material layer (thickness 120 μm).
[0149] 2) Manufacturing of cathode
[0150] Graphite (natural graphite and artificial graphite blend), conductive agent (carbon black), dispersant (polyvinylpyrrolidone, Junsei, Japan), and binder resin (PVDF-HFP and PVDF blend) were mixed with water in a weight ratio of 97.5:0.7:0.14:1.66 to prepare a slurry for an anode active material layer with a concentration of 50 wt% of the remaining components excluding water. Next, the slurry was applied to the surface of a copper thin film (thickness 10 μm) and dried to manufacture an anode having an anode active material layer (thickness 120 μm).
[0151] 3) Lamination process
[0152] The separators of the examples and comparative examples were interposed between the manufactured cathodes and anodes, and a lamination process was performed to obtain an electrode assembly. The lamination process was performed using a hot press at 70°C and 5.2 MPa for 10 seconds.
[0153]
[0154] <Experimental Example 1: Measurement of roughness of the coating layer surface>
[0155] Measurements were made using the Optical Profiler NV 2700 from Nanosystem. The surface of the coating layer was set as the measurement surface on the sample stage, and the average value was calculated from four different measurement areas, and the conditions were set as follows.
[0156] Cutoff: 0.8 mm, Scan speed: 0.1 mm / s, Magnification: 500x
[0157] <Experimental Example 2: Measurement of the Thickness Change Rate of the Coating Layer>
[0158] The change in thickness of the membranes of Examples 1 to 3 and Comparative Examples 1 to 7 before and after pressurization for 10 seconds under the conditions of 70°C and 5.2 MPa was calculated using the following mathematical formula 1.
[0159] [Mathematical Formula 1]
[0160] Thickness change rate = (thickness of coating layer before pressing - thickness of coating layer after pressing) / thickness of coating layer before pressing
[0161] <Experimental Example 3: Measurement of Short-Circuit Defect Rate>
[0162] For the above Examples 1 to 3 and Comparative Examples 1 to 7, 100 specimens were prepared each, and their withstand voltage characteristics were evaluated. The breakdown voltage was measured using an AC / DC / IR Hi-Pot tester. The separator of each Example and Comparative Example was placed between the aluminum lower plate jig and the cylindrical electrode rod, and the DC current was set to 0.5 mA and the voltage was increased to 100 V / s (voltage 3 kV, ramp up time 30 s). When the experiment started, the voltage was increased, and the measurement was completed when a short circuit occurred, and the voltage at that time was measured as the breakdown voltage. The evaluation of the short-circuit failure rate (short-circuit occurrence rate or Hi-Pot failure rate) was based on 75 V, and the ratio (%) of the number of specimens in which a short circuit occurred under conditions of 75 V or less among the total number of specimens tested was calculated.
[0163] <Experimental Example 4: Specific change rate of porosity of coating layer>
[0164] The porosity of the membranes of Examples 1 to 3 and Comparative Examples 1 to 7 before and after impregnation in a solution containing 70 parts by volume of ethylene carbonate and 30 parts by volume of ethyl methyl carbonate at 25° C. and 1 atm for 24 hours was specified, and the rate of change in porosity of the coating layer was measured using the following mathematical formula 2.
[0165] [Equation 2]
[0166] Rate of change in porosity = (Porosity of coating layer after impregnation - Porosity of coating layer before impregnation) / Porosity of coating layer before impregnation
[0167] The above porosity was calculated using [Mathematical Formula 3] and [Mathematical Formula 4] below.
[0168] [Equation 3]
[0169] Porosity (volume %) = {1-(apparent density / true density)} × 100
[0170] [Equation 4]
[0171] Apparent density (g / cm) 3) = {Weight of coating layer [g] / Thickness of coating layer [cm] × Area of coating layer [cm 2 ])}
[0172] For each example and comparative example, three samples measuring 5 cm in MD / TD directions were obtained from the coating layer. The thickness of the coating layer was measured at five points for each sample, and the average value was used, and the weight of each sample was measured using a balance. The average value of the three samples was calculated and applied to Equations 3 and 4 to calculate the porosity. Meanwhile, the true density of each sample was applied based on theoretically confirmed values, such as the molecular weight for each component applied.
[0173] <Experimental Example 5: Wet Adhesion Measurement>
[0174] The separators of Examples 1 to 3 and Comparative Examples 1 to 7 were cut into 70 mm (length) x 20 mm (width), and the prepared electrodes and separators were laminated using a press under the conditions of 60°C, 6.5 MPa, and 1 sec to prepare specimens. The prepared specimens were loaded into a battery case together with the electrolyte and maintained for 4 hours to impregnate the specimens with the electrolyte. The electrolyte used was a mixture of ethylene carbonate and ethyl methylate in a volume ratio of 7:3 and prepared at a concentration of LiPF61M. After that, the specimens were taken out of the case and fixed by attaching them to a glass plate using double-sided tape, and at this time, the electrodes were positioned facing the glass plate. The separator portion of the specimen was peeled at a 90° angle at a speed of 200 mm / min at 25°C, and the strengths of each of the positive and negative electrodes at this time were measured.
[0175] <Experimental Example 6: Measurement of Low-Voltage Defect Rate>
[0176] After manufacturing, batteries undergo an activation process to ensure stable charging and discharging. This process involves charging and discharging the battery and storing it at high or room temperature for a specified period.
[0177] After a certain period of time, the voltage of a battery drops, and the standard deviation (σ) of the voltage distribution is calculated. Depending on the battery design, a battery that exceeds a constant * σ (the constant is 0.5 to 3) is considered defective.
[0178] The batteries including the separators of Examples 1 to 3 and Comparative Examples 1 to 7 were charged at a constant current (CC) of 0.05 C until the voltage reached 4.25 V, and then charged at a constant voltage until the voltage reached 0.01 C. Thereafter, the voltage of the batteries according to the activation process was measured.
[0179] The voltage dispersion of batteries produced at the same time was measured as the standard deviation multiplied by 0.5, and batteries that exceeded this value were judged to be defective.
[0180] Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Comparative Example 6 Comparative Example 7 Surface roughness (Sa, ㎛) 0.097 0.112 0.162 0.256 0.213 0.2210.1230.114 0.1210.085 Coating layer thickness change rate (%) 24 20 17 5 7 15 10 27 8 10 Short defect rate (%) 23 23 5 33 24 7 3 15 20 Porosity change rate (%) 10 14 15 37 25 5 13 4 20 4 Wet adhesion (gf / 20 mm) 7 6 7 15 21 21 23 7 Low voltage defect rate (%) 5 3 3 2 15 29 3 18 210
[0181] Referring to Table 2 above, it was confirmed that Examples 1 to 3 according to one embodiment of the present invention have a low surface roughness of the coating layer, a satisfactory particle size ratio, and a satisfactory weight ratio of the polymer binder, thereby achieving a low short-circuit failure rate and a low-voltage failure rate.
[0182] In this regard, it was confirmed that Comparative Examples 1 to 3, which had high surface roughness of the coating layer, showed an increase in the short-circuit failure rate and / or low-voltage failure rate, and Comparative Examples 4 and 5, which had a small content of the first polymer binder, showed a decrease in wet adhesion or an increase in low-voltage failure rate. Furthermore, it was confirmed that Comparative Example 6, which contained an excessive amount of the second polymer binder, showed an increase in the short-circuit failure rate, an increase in the porosity change rate, and a decrease in wet adhesion. In addition, it was confirmed that Comparative Example 7 showed an increase in the short-circuit failure rate and / or low-voltage failure rate.
[0183] Accordingly, the separator for an electrochemical device, which is an embodiment of the present invention, can reduce the surface roughness of the coating layer by controlling the average particle size ratio of the first polymer binder and the inorganic particles included in the coating layer, and by controlling the content ratio of the first polymer binder and the second polymer binder, while preventing damage occurring in the lamination process, which is a manufacturing process of the electrochemical device, and improving the breakdown voltage of the electrochemical device.
[0184] [Explanation of symbols]
[0185] 100: Separator for electrochemical devices
[0186] 110: Porous polymer substrate
[0187] 130: Coating layer
[0188] 300: Bipolar
[0189] 500: negative
Claims
1. Porous polymer substrate; and It is provided on at least one side of the porous polymer substrate, and includes a coating layer including a first polymer binder in particle form, a second polymer binder, and inorganic particles. The average particle diameter (D) of the first polymer binder 50 ) and the average particle diameter (D) of the above inorganic particles 50 ) is in the ratio of 1:1 to 1:5, A separator for an electrochemical device, wherein the weight of the first polymer binder included in the coating layer is greater than the weight of the second polymer binder.
2. In claim 1, A separator for an electrochemical device, wherein the roughness (Sa) of the surface opposite to the surface adjacent to the porous polymer substrate of the coating layer is 0.20 ㎛ or less.
3. In claim 1, A separator for an electrochemical device, wherein the first polymer binder comprises one selected from an acrylic binder, a polyvinylidene binder, and a combination thereof.
4. In claim 1, A separator for an electrochemical device, wherein the second polymer binder is one selected from the group consisting of polyacrylic acid (PAA), polyvinyl alcohol (PVA), polyvinylpyrrolidone (PVP), polyacrylamide (PAM), and combinations thereof.
5. In claim 1, The average particle diameter (D) of the first polymer binder 50 ) is a separator for an electrochemical device having a thickness of 200 nm or more and 450 nm or less.
6. In claim 1, The average particle diameter (D) of the above inorganic particles 50 ) is a separator for an electrochemical device having a thickness of 300 nm or more and 700 nm or less.
7. In claim 1, A separator for an electrochemical device, wherein the weight ratio of the first polymer binder and the second polymer binder is 5.5:4.5 to 9.5:0.
5.
8. In claim 1, A separator for an electrochemical device, wherein the total content of the first polymer binder and the second polymer binder is 10 parts by weight or more and 20 parts by weight or less with respect to 100 parts by weight of the coating layer.
9. In claim 1, A separator for an electrochemical device, wherein the thickness change rate of the coating layer defined by the following mathematical formula 1 is 10% or more and 25% or less when pressurized for 10 seconds under the conditions of 70 ℃ and 5.2 MPa: [Mathematical Formula 1] Thickness change rate = (thickness of coating layer before pressing - thickness of coating layer after pressing) / thickness of coating layer before pressing.
10. In claim 1, An electrochemical device separator, wherein when impregnated in a solution containing 70 parts by volume of ethylene carbonate and 30 parts by volume of ethyl methyl carbonate at 25°C and 1 atm for 24 hours, the porosity of the coating layer defined by the following mathematical formula 2 has a change rate of 10% or more and 20% or less: [Equation 2] Rate of change in porosity = (Porosity of coating layer after impregnation - Porosity of coating layer before impregnation) / Porosity of coating layer before impregnation.
11. An electrochemical device comprising: a positive electrode; a negative electrode; and a separator interposed between the positive electrode and the negative electrode, the separator being any one of claims 1 to 10.
Citation Information
Patent Citations
A coated porous separator and a secondary battery using the same
KR101298340B1
Opening and closing system for valve
KR1020230024769A
Charging station for personal mobility device
KR1020230152288A
Semiconductor wafer transfer device
KR1020240061757A