Method of manufacturing graphite material
The method of preliminary carbonization and graphitization of graphite materials addresses the challenge of maintaining packing density during rapid charging, resulting in enhanced performance and lifespan for lithium secondary batteries.
Patent Information
- Application Number
- PCT/KR2024/007024
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-31
- Filing Date
- 2024-05-23
- Publication Date
- 2024-12-05
AI Technical Summary
The challenge in manufacturing graphite materials for lithium secondary batteries is to enhance rapid charging performance while maintaining or increasing packing density, as reducing particle size or improving coarseness can lead to decreased packing density.
A method involving preliminary carbonization of graphite raw materials and a coating material at specific temperature ranges (1,050 to 1,300 °C) followed by graphitization, which includes steps like pulverizing, disintegrating, and controlling the rotation speed and air inflow to achieve a higher packing density and improved particle size distribution.
This approach results in graphite materials with enhanced rapid charging performance and increased packing density, leading to improved battery lifespan and output characteristics.
Smart Images

Figure KR2024007024_05122024_PF_FP_ABST
Abstract
Description
Method for producing graphite material
[0001] The present invention relates to a lithium secondary battery, and more particularly, to a method for producing a graphite material used as an anode active material for a lithium secondary battery.
[0002] As technological development and demand for mobile devices increase, the demand for secondary batteries as an energy source is rapidly increasing. Among secondary batteries, lithium secondary batteries, which exhibit high energy density and operating potential, long cycle life, and low self-discharge rate, are being commercialized and widely used.
[0003] In addition, as interest in environmental issues grows, interest in electric vehicles and hybrid electric vehicles that can replace vehicles that use fossil fuels, such as gasoline vehicles and diesel vehicles, which are one of the main causes of air pollution, is increasing, and research is actively being conducted to use lithium secondary batteries as a power source for the electric vehicles and hybrid electric vehicles.
[0004] Lithium secondary batteries generally consist of a positive electrode containing positive active material, a negative electrode containing negative active material, a separator, and an electrolyte, and charge and discharge are performed by the intercalation and decalation of lithium ions. The lithium secondary batteries have the advantages of high energy density, high electromotive force, and high capacity, and are therefore applied in various fields.
[0005] Materials such as metallic lithium anode active materials, carbon-based anode active materials, or silicon oxide (SiOx) are used as the above-mentioned anode active materials. The carbon-based anode active materials exhibit excellent capacity retention characteristics and efficiency. Since the carbon-based anode active materials used as the anodes of lithium secondary batteries have an electrode potential close to that of lithium metal, the change in crystal structure during the insertion and deintercalation process of ionic lithium is small. In addition, the carbon-based anode active materials enable continuous and repeated oxidation and reduction reactions at the electrode, thereby enabling lithium secondary batteries to exhibit high capacity and excellent lifespan.
[0006] As the above carbon-based negative electrode active material, various types of materials are used, such as crystalline carbon-based materials such as natural graphite and artificial graphite, or amorphous carbon-based materials such as hard carbon and soft carbon. Among the above carbon-based negative electrode active materials, graphite-based negative electrode active materials are the most widely used because they have excellent reversibility and can improve the life characteristics of lithium secondary batteries. Since the graphite-based negative electrode active material has a low discharge voltage of -0.2 V compared to lithium, a battery using the graphite-based active material can exhibit a high discharge voltage of 3.6 V, which has an excellent advantage in terms of energy density of lithium secondary batteries.
[0007] The above-mentioned crystalline carbon-based material, artificial graphite, has a more stable crystal structure than the natural graphite because it forms a graphite crystal structure by applying high heat energy of 2,700℃ or more, and the change in the crystal structure is small even with repeated charging and discharging of lithium ions, so the artificial graphite has an advantage of a lifespan that is about 2 to 3 times longer than the natural graphite. The above-mentioned amorphous carbon-based materials, soft carbon and hard carbon, whose crystal structures are not stabilized, have the characteristic of smoother entry and exit of lithium ions, and can increase the charging and discharging speeds, so they can be used in electrodes that require high-speed charging. Therefore, it is common to mix and use the above-mentioned carbon-based materials at a certain ratio in consideration of the lifespan characteristics and output characteristics of the lithium secondary battery to be used.
[0008] Among the graphite-based materials, which are the above-mentioned negative active materials, artificial graphite is also used as a negative active material for rapid charging, but there is a problem that the filling density decreases when the particle size is reduced or the degree of assembly is improved to improve the rapid charging performance.
[0009] According to one embodiment of the present invention, a method for manufacturing a graphite material provides a method for manufacturing a graphite material having a reduced particle size or an improved granulation degree while simultaneously increasing a packing density to improve rapid charging performance when artificial graphite is used as a negative electrode active material for rapid charging.
[0010] According to one embodiment of the present invention, a method for manufacturing a graphite material may include a step of pre-carbonizing a result obtained from a graphite raw material and a coating material at a temperature ranging from 1,050 to 1,300° C., and a step of graphitizing the pre-carbonized result. In one embodiment, the pre-carbonizing step includes a step of assembling the graphite raw material and the coating material, and the coating material may be included in an amount of 5 to 20 wt% based on 100 wt% of the obtained result.
[0011] In one embodiment, the pre-carbonizing step may be performed for 3.0 hours or more. In one embodiment, the pre-carbonizing step may be performed at a heating rate in the range of 5 to 20° C. / min.
[0012] In one embodiment, the pre-carbonization step may include a step of crushing the graphite raw material and the coating material. In one embodiment, the step of crushing the graphite raw material and the coating material may be performed under conditions where the rotation speed of the crushing blade is 35 to 40 [Hz].
[0013] In one embodiment, the step of crushing the graphite raw material and the coating material may be performed under conditions where the air inflow is less than 35 to 50 [Hz]. In one embodiment, the step of crushing the graphite raw material and the coating material may be performed under conditions where the classification (rotational speed of the classifier blade) is 15 or more.
[0014] In one embodiment, the step of crushing the graphite raw material and the coating material may be performed so that the average particle diameter (D50) of the obtained result is 12 to 17 μm. In one embodiment, the coating material may include a coke-based raw material.
[0015] In one embodiment, the coke-based raw material may include coal-based needle-like green coke. In one embodiment, before the pre-carbonization step, the volatile content of the coating material may be 4.0 to 5.0%, and after the pre-carbonization step, the volatile content of the coating material may be 0.1 to 0.5%.
[0016] In one embodiment, the apparent density of the pre-carbonized result may be greater than or equal to 0.65 g / cc. In one embodiment, the tap density of the pre-carbonized result may be from 1.04 to 1.09 g / cc. In one embodiment, the weight reduction rate of the pre-carbonized result may be from 4.0 to 7.0%.
[0017] According to one embodiment of the present invention, a method for producing a graphite material includes a preliminary carbonization step prior to a graphitization step, thereby providing a method for producing a graphite material having a reduced particle size or an improved granularity while simultaneously increasing a packing density to improve rapid charging performance.
[0018] FIGS. 1A to 1D illustrate SEM photographs of graphite materials manufactured according to a method for manufacturing graphite materials according to one embodiment of the present invention.
[0019] The terms first, second, and third, etc., are used to describe, but are not limited to, various parts, components, regions, layers, and / or sections. These terms are used only to distinguish one part, component, region, layer, or section from another part, component, region, layer, or section. Accordingly, a first part, component, region, layer, or section described below may be referred to as a second part, component, region, layer, or section without departing from the scope of the present invention.
[0020] The terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the present invention. As used herein, the singular forms "singular" and "comprising" include plural forms as well, unless the context clearly dictates otherwise. The word "comprising" as used herein specifies a particular feature, region, integer, step, operation, element, and / or component, but does not exclude the presence or addition of other features, regions, integers, steps, operations, elements, and / or components.
[0021] When a part is referred to as being "on" or "over" another part, it can be directly on or over the other part, or there may be other parts intervening. Conversely, when a part is referred to as being "directly on" another part, there are no other parts intervening.
[0022] Although not defined otherwise, all terms, including technical and scientific terms, used herein have the same meaning as commonly understood by those of ordinary skill in the technical field to which the present invention pertains. Terms defined in commonly used dictionaries are further interpreted to have meanings consistent with the relevant technical literature and the present disclosure, and are not to be construed as ideal or overly formal unless otherwise defined.
[0023] Hereinafter, embodiments of the present invention will be described in detail. However, these are presented as examples and the present invention is not limited thereto, and the present invention is defined solely by the scope of the claims set forth below.
[0024] According to one embodiment of the present invention, a method for producing a graphite material comprises a step of pre-carbonizing a result obtained from a graphite raw material and a coating material, and a step of graphitizing the pre-carbonized result. Specifically, the method for producing a graphite material of the present invention may further comprise a step of preliminarily heat-treating the graphite material prior to the step of graphitizing the graphite material.
[0025] In the step of pre-carbonizing the result obtained from the graphite raw material and the coating material, the graphite raw material may be a coke-based material. The coke-based material may be at least one of coal-based coke, metallurgical coke, and pitch coke.
[0026] In one embodiment, the coke-based material may be, for example, coal-based coke. Specifically, the coal-based coke may be coal-based needle coke. The coal-based needle coke may be coal-based needle coke. The coal-based needle coke may contain less moisture and volatile matter compared to petroleum-based general green coke. Since the coal-based needle coke contains less moisture and volatile matter, the density of the coal-based needle coke may be significantly improved when going through a preliminary carbonization or graphitization process compared to the petroleum-based coke.
[0027] In one embodiment, the result obtained from the graphite raw material and the coating material may include a moisture content of 0.28 to 0.42%. Specifically, the result obtained from the graphite raw material and the coating material may include a moisture content of 0.30 to 0.40%.
[0028] In one embodiment, the result obtained from the graphite raw material and the coating material may include a volatile matter content of 4.0 to 5.0%. Specifically, the result obtained from the graphite raw material and the coating material may include a volatile matter content of 4.2 to 4.6%. By satisfying the above-described range, the result obtained from the graphite raw material and the coating material may have high self-adhesiveness during the assembly process, may improve the bonding strength between primary particles in the artificial graphite, may enable the artificial graphite to have high structural strength, and may have the advantage of being able to manufacture high-density artificial graphite through a preliminary carbonization or graphitization process. The volatile matter content may be measured using a method known in the art.
[0029] The coating material may be a pitch. Specifically, the pitch may include at least one of coal tar, tar light oil, tar heavy oil, tar heavy oil, naphthalene oil, anthracene oil, coal tar pitch, pitch oil, oxygen-crosslinked petroleum pitch, and heavy oil. Specifically, the pitch may be, for example, coal tar pitch.
[0030] In one embodiment, the pre-carbonization step may include assembling the graphite raw material and the coating material. The assembling of the graphite raw material and the coating material may be a step of uniformly mixing the graphite raw material and the coating material. The assembling step may utilize a known mixer, such as a stirring, rotary, or wind-driven mixer, for example.
[0031] In one embodiment, in the step of assembling the graphite raw material and the coating material, the coating material may comprise 5 to 20 wt% based on 100 wt% of the result obtained by assembling the graphite raw material and the coating material. Specifically, the coating material may comprise 13 to 15%. By satisfying the above-described range, the coating material can be uniformly mixed with the graphite raw material.
[0032] If the content of the coating material exceeds the upper limit, there is a problem of the capacity per unit weight of the graphite product being reduced. If the content of the coating material exceeds the lower limit, there is a problem of the output characteristics of the graphite product being poor due to the low degree of assembly.
[0033] The step of pre-carbonizing the result obtained from the graphite raw material and the coating material may include a step of heat-treating the result obtained by assembling the graphite raw material and the coating material prior to the graphitization step. In one embodiment, the pre-carbonization step may be performed at a lower temperature than the graphitization step.
[0034] In one embodiment, the pre-carbonization step may be performed at a temperature range of 1,050 to 1,300°C. Specifically, the pre-carbonization step may be performed at a temperature of 1,050 to 1,200°C, more specifically, 1,050 to 1,150°C. By performing the pre-carbonization step within the aforementioned range, moisture and volatile matter in the graphite raw material and the coating material are removed, thereby improving particle flowability and thereby improving density.
[0035] If the temperature range of the above-mentioned preliminary carbonization step exceeds the upper limit, there is a problem that the process time is prolonged and productivity is reduced. If the temperature range of the above-mentioned preliminary carbonization step exceeds the lower limit, there is a problem that the specific surface area increases and the tap density decreases.
[0036] In one embodiment, the pre-carbonization step may be performed for 3.0 hours or longer. Specifically, the pre-carbonization step may be performed for 3.42 hours or longer, and more specifically, for 5.0 hours or longer. The time may refer to the maintenance time of the pre-carbonization. By satisfying the above-mentioned range for the maintenance time, the apparent density and the tap density are advantageously improved. If the time exceeds the above-mentioned range, there is a problem of the apparent density and the tap density being reduced.
[0037] In one embodiment, the pre-carbonization step may be performed at a temperature increase rate of 5 to 20°C / min. Specifically, the pre-carbonization step may be performed at a temperature increase rate of 5 to 10°C / min. More specifically, the pre-carbonization step may be performed at a temperature increase rate of 5 to 8°C / min.
[0038] When the above-mentioned temperature increase rate range satisfies the aforementioned range, there is an advantage of a reduced specific surface area. When the above-mentioned temperature increase rate range does not satisfy the aforementioned range, there is a problem of an increased specific surface area, resulting in a decrease in powder flowability between processes and an increase in process time.
[0039] In one embodiment, after the pre-carbonization step, the result obtained from the pre-carbonized graphite raw material and coating material may have a moisture content of 0.01 to 0.1%. Specifically, the moisture content may be 0.01 to 0.03%.
[0040] In one embodiment, after the pre-carbonization step, the result obtained from the graphite raw material and the coating material may have a volatile content of 0.1 to 1.5%. Specifically, the volatile content may be 0.1 to 0.5%.
[0041] The result obtained from the above graphite raw material and coating material has the advantage of improved productivity due to greatly improved density caused by shrinkage and volatilization of volatile matter by going through a preliminary carbonization step.
[0042] In one embodiment, the apparent density of the pre-carbonized result may be greater than or equal to 0.65 g / cc. Specifically, the apparent density of the pre-carbonized result may be from 0.65 to 0.69 g / cc. It can be confirmed that the density of the pre-carbonized result increases as it undergoes shrinkage and volatile matter evaporation processes during the pre-carbonization process.
[0043] In one embodiment, the tap density of the pre-carbonized result may be from 1.04 to 1.09 g / cc. In one embodiment, the weight reduction of the pre-carbonized result may be from 4.0 to 7.0%, specifically from 4.5 to 6.5%.
[0044] As described above, the above tap density and weight reduction rate may be expressed according to the shrinkage and evaporation of volatile matter during the preliminary carbonization process.
[0045] In one embodiment, the pre-carbonization step may include a step of crushing the graphite raw material and the coating material. The crushing step refers to a step of crushing the graphite raw material and the coating material so that the resulting product has an average particle diameter (D50) of 12 to 17 μm.
[0046] The above-described disintegrating step may be a step performed to prevent the material obtained by assembly from being excessively fused. The above-described disintegrating method may utilize a known crusher, such as a hammer mill, a stirring mill, a jet mill, a ball mill, or a bead mill. Preferably, a method utilizing a mechanochemical processor (shear compression processor) such as Hybridization System (Nara Kikai Seisakusho Co., Ltd.), Mechanofusion System (Hosokawa Micron Co., Ltd.), Novirta (Hosokawa Micron Co., Ltd.), or Dry Attritor (Nippon Coke Kogyo Co., Ltd.) is exemplified.
[0047] In one embodiment, the step of crushing the graphite raw material and the coating material may be performed under conditions where the rotation speed of the blade is 35 to 45 [HZ]. Specifically, the rotation speed may be 38 to 42 [HZ].
[0048] In one embodiment, the step of crushing the graphite raw material and the coating material may be performed under conditions where the air inflow rate is 35 to 50 [Hz]. Specifically, the air inflow rate may be 38 to 45 [Hz].
[0049] In one embodiment, the step of crushing the graphite raw material and the coating material may be performed under conditions where the classification (the speed at which the blade rotates to classify the powder according to its size) is 15 [Hz] or higher. Specifically, the classification may be 18 [Hz] or higher.
[0050] The step of crushing the graphite raw material and coating material is performed within the aforementioned conditions, thereby enhancing tap density and thus productivity. However, the step of crushing the graphite raw material and coating material, when performed outside the aforementioned conditions, presents the problem of lowering density and thus productivity.
[0051] The step of graphitizing the pre-carbonized result may be a step of graphitizing the result that has undergone the pre-carbonization step at a temperature higher than the pre-carbonization temperature. In one embodiment, the graphitizing step may be performed in a range of 2,800 to 3,200°C. Specifically, the graphitizing step may be performed in a range of 2,900 to 3,100°C. By performing the graphitizing step in the above range, the manufactured artificial graphite can obtain an appropriate degree of graphitization, and the artificial graphite can obtain high structural stability and capacity per gram.
[0052] The above graphitization can be performed by heat treatment using a known high-temperature furnace, such as an Acheson furnace. After the graphitization process is complete, the small amount of oversized particles formed by agglomeration of the assembled product during the high-temperature graphitization process can be removed by sieving. By separating the oversized particles, it is possible to prevent them from affecting the processing performance of the material, such as slurry stability and coating performance.
[0053]
[0054] Hereinafter, preferred embodiments and comparative examples of the present invention are described. However, the following examples are only preferred embodiments of the present invention, and the present invention is not limited to the following examples.
[0055] <Experimental Example>
[0056] Assembly material manufacturing steps
[0057] Coal-based coke was coarsely pulverized using a pin mill and then finely pulverized using a crusher to produce coke fines. Pitch was then pulverized using a jet mill to produce pitch powder. The coke fines and pitch powder were mixed and fed into a granulator, where they were heated to 700°C under a nitrogen atmosphere to produce granules. The granules were then crushed using an ACM.
[0058] Pre-carbonization stage
[0059] Table 1 below shows the results of metal foreign matter production by crushing the granulated material produced through the above-described granulated material production step under crushing conditions of high rotational speed of the crushing blade and high air inflow and low classifier. Subsequently, subsequent steps were performed as in Example 1 and Comparative Example 1 below.
[0060] In Table 1 below, ash was measured after drying sample 5 at 120°C, cooling it in a desiccator, placing it in an electric furnace, heating it at 1200°C for 12 hours, allowing it to cool, and then cooling it in a desiccator for 30 minutes. Metal foreign matter was measured using an ICAP-7000 device.
[0061] <Example 1>: Preliminary carbonization
[0062] The crushed granulated material was subjected to preliminary carbonization at a temperature of 1,200°C, a heating rate of 5.7°C / min, and a holding time of 3.42 h, and then subjected to a graphitization step at 3,000°C.
[0063]
[0064] <Comparative Example 1>
[0065] The graphitization step was performed at 3000 ℃ without a preliminary carbonization step of the crushed assembly material.
[0066] ashFeNiZnCrAlCaCuSSiCoOther Examples 10.02411.215.70.30.40.634.50.21.31.20.70.4Comparative Example 10.03215.919.10.30.61.365.70.31.81.30.91.9
[0067] Looking at Table 1 above, Example 1, which underwent preliminary carbonization prior to the graphitization step, was confirmed to have a lower content of ash and metal foreign substances compared to Comparative Example 1, which did not undergo the preliminary carbonization step. Specifically, Example 1 has a lower content of metal foreign substances such as Fe, Ni, and Ca, and thus has the advantage of less side reactions during electrochemical evaluation.
[0068] Condition control of the pre-carbonization stage: maximum temperature
[0069] Looking at Table 2 below, when the maximum pre-carbonization temperature was controlled in the pre-carbonization stage, the weight change rate [%], average particle size [D50], apparent density [g / cc], tap density before and after carbonization [g / cc], and specific surface area (BET-SSA) [m 2 / g], and the measurement methods for each are as follows.
[0070] (Weight change rate [%]): Weight after pre-carbonization / Weight before pre-carbonization
[0071] (Average particle size [D50]): 0.04 g of sample was mixed with distilled water and Triton X100, dispersed in an ultrasonic disperser for 1 minute, and then the particle size was measured using a Microtac particle size analyzer. D50 is the particle size when the cumulative percentage reaches 50%.
[0072] (Apparent density [g / cc]): After weighing the sample, pour it into the flowmeter funnel. When the density cup is sufficiently filled with the sample, remove the sample from the top of the density cup and check the weight to obtain the apparent density.
[0073] (Tap density before and after carbonization [g / cc]): The tap density was measured by tapping 10 g of the sample in a 25 ml cylinder at 250 rpm, 3000 times using a Bettersize tap density meter.
[0074] (Specific surface area (BET-SSA)[m 2 / g]): 2g of the sample was placed in a cylinder, pretreated at 300℃ for 1 hour in a vacuum, cooled to room temperature for 30 minutes, and then measured using Tristar equipment.
[0075]
[0076] Number Carbonization Conditions Weight change rate after carbonization [%] Average particle size [D50] Apparent density [g / cc] Tap density [g / cc] BET [m 2 / g]Maximum temperature [℃]Duration time [h]Heating rate [℃ / min]CarbonizationPre-carbonizationAfter carbonizationExample 2-112003.425.7-5.512.90.650.680.962.5Example 2-211503.425.7-5.313.70.670.680.962.2Example 2-311003.425.7-5.213.60.690.680.973.2Example 2-410503.425.7-5.113.90.650.680.962.4Comparative example 210003.425.7-5.013.40.620.680.931.2
[0077] Looking at Table 2 above, it was confirmed that Examples 2-1 to 2-4, in which preliminary carbonization was performed at a maximum temperature in the range of 1,050 to 1,200°C, had higher tap density and specific surface area compared to Comparative Example 2, in which preliminary carbonization was performed at a maximum temperature of 1,000°C.
[0078] Condition control of the pre-carbonization stage: holding time
[0079] Looking at Table 3 below, when the holding time was adjusted in the preliminary carbonization stage, the weight change rate [%], average particle size [D50], apparent density [g / cc], tap density before and after carbonization [g / cc], and specific surface area (BET-SSA) [m 2 / g] is displayed.
[0080]
[0081] Number Carbonization Conditions Weight change rate after carbonization [%] Average particle size [D50] Apparent density [g / cc] Tap density [g / cc] BET [m 2 / g]Maximum temperature [℃]Duration time [h]Heating rate [℃ / min]CarbonizationPre-carbonizationAfter carbonizationComparative Example 3-11200015-5.213.00.610.680.951.4Example 3-112003.4215-5.613.90.690.700.952.8Example 3-21200515-5.513.40.650.680.981.7Comparative Example 3-21200010-5.413.70.620.700.932.2Example 3-31200210-5.413.80.620.700.922.9Example 3-412003.4210-5.313.20.670.700.952.0Comparative Example 3-3120005.7-5.013.50.680.700.931.4Example 3-512003.425.7-5.014.00.680.700.961.6Example 3-6120055.7-5.813.60.680.700.952.3
[0082] Looking at Table 3 above, it was confirmed that the apparent density increased as the holding time increased under the pre-carbonization conditions. In addition, it was confirmed that the tap density increased as the holding time increased.
[0083] Condition control in the pre-carbonization stage: heating rate
[0084] Looking at Table 4 below, when the heating rate was controlled in the preliminary carbonization stage, the weight change rate [%], average particle size [D50], apparent density [g / cc], tap density before and after carbonization [g / cc], and specific surface area (BET-SSA) [m 2 / g] is displayed.
[0085]
[0086] Number Carbonization Conditions Weight change rate after carbonization [%] Average particle size [D50] Apparent density [g / cc] Tap density [g / cc] BET [m 2 / g]Maximum temperature [℃]Duration time [h]Heating rate [℃ / min]CarbonizationPre-carbonizationAfter carbonizationExample 4-112003.425.7-5.014.00.680.700.961.6Example 4-212003.4210-5.313.20.670.700.952.0Example 4-312003.4215-5.613.90.690.700.952.8
[0087] Looking at Table 4 above, it was confirmed that the tap density increased and the specific surface area decreased as the heating rate decreased under the preliminary carbonization conditions.
[0088] Control of the disintegration stage
[0089] As shown in Table 5 below, the content of coarse pitch in coal-based coke raw materials was adjusted to 8 wt%, 13 wt%, and 15 wt% of the weight of the coarse pitch based on the input amount, respectively, and the coarse pitch was granulated, and then the coarse pitch was crushed under the crushing conditions of high rotation speed of the crushing blade and high air inflow and low classifier, and then preliminary carbonization was performed at 1200 ℃ and graphitization was performed at 3000 ℃. The average particle diameter (D50), tap density, BET specific surface area, graphitization degree, capacity, and efficiency of the graphitized product were as follows. The average particle diameter (D50), tap density, BET specific surface area, graphitization degree, capacity, and efficiency of the graphitized product were measured by the following methods.
[0090] (Average particle size of graphite product (D50)): 0.04 g of sample was mixed with distilled water and Triton X100, dispersed in an ultrasonic disperser for 1 minute, and then the particle size was measured using a Microtac particle size analyzer.
[0091] (Tap density [g / cc]): The tap density was measured by tapping 15 g of the sample into a 25 ml cylinder at 250 rpm, 3000 times using a Bettersize tap density meter.
[0092] (Specific surface area (BET) [m 2 / g]): 2g of the sample was placed in a cylinder, pretreated at 300℃ for 1 hour in a vacuum, cooled to room temperature for 30 minutes, and then measured using Tristar equipment.
[0093] (Graphitization degree [%]): After mixing graphite and silicon in a 5:1 ratio, the mixed powder is placed in the sample holder and measured using XRD equipment (Bruker AXS, D8 Discover with GADDS). The measurement conditions are as follows: Scan range: 10~80˚ / Scan rate: 1˚ / min, Step size: 0.02˚
[0094] (Capacity [mAh / g]): The third discharge capacity when charging and discharging in 0.1CC / CV, 0.1CC mode at a C-rate of 0.1C after a 30-hour rest time after cell manufacturing.
[0095] (Efficiency [%]): After 30 hours of rest time after cell manufacturing, discharge capacity / charge capacity in the first cycle when charging and discharging in 0.1CC / CV, 0.1CC mode at a C-rate of 0.1C
[0096] Number of assembly pitch content [wt%] Graphite product D50 [㎛] Tap density [g / cc] BET [m 2 / g]Graphitization degree[%]Capacity[mAh / g]Efficiency[%]Comparative example 5512..01.071.892.2352.193.8Example 5-11315.11.051.291.8350.593.6Example 5-21514.21.091.591.1349.193.6
[0097] Looking at Table 5 above, when manufacturing an assembly, if the assembly pitch content is excessively low, there is a problem of low tap density and charging output characteristics, and within the scope of the present invention, it can be confirmed that the assembly degree is increased, resulting in excellent tap density and charging output characteristics. It is believed that if the assembly pitch content is excessively high, the capacity will decrease.
[0098] Control of disintegration conditions
[0099] Looking at Table 6 and Table 7 below, the content of metal foreign matter is shown after the assembly is dismantled under the dismantling conditions of Table 6 below.
[0100] The disintegration conditions in Table 6 are as follows.
[0101] Main Machine = Rotation speed of the shredding blade
[0102] Air Blower = Air intake (wind volume) for transporting powder
[0103] Classification = Rotation speed of classifier blades
[0104] The Y12 condition was carried out with the purpose of disintegrating the clumped assembly by rapidly rotating the disintegrator blade, and corresponds to the disintegration condition with high rotation speed of the disintegrator blade and air inflow and low classifier. The X1 condition was carried out with the purpose of passing the clumped assembly through the assembly disintegrator by gently rotating the disintegrator blade so that it does not break apart, and corresponds to the disintegration condition with low rotation speed of the disintegrator blade and classifier and high air inflow.
[0105]
[0106] <Example 6-1>
[0107] It is characterized by Y12 disintegration conditions and a pitch content of 13 wt%.
[0108]
[0109] <Example 6-2>
[0110] It is characterized by Y12 disintegration conditions and a pitch content of 15 wt%.
[0111]
[0112] <Comparative Example 6-1>
[0113] It is characterized by the fact that the X1 disintegration condition and the pitch content are disintegrated at 13 wt%.
[0114]
[0115] <Comparative Example 6-2>
[0116] It is characterized by the fact that the X1 disintegration condition and the pitch content are disintegrated at 15 wt%.
[0117]
[0118] Shredding TypeMain Machine[HZ]Air Blower[HZ]Classification[HZ]Y12Strong Shredding404020X1Weak Shredding105010
[0119] Number of crushing conditions, assembly pitch content [wt%], assembly product, pre-carbonized product, graphitized product, average particle size D50 [㎛], tap density [g / cc], average particle size D50 [㎛], tap density [g / cc], BET specific surface area [m 2 / g]Average particle size D50 [㎛]Tap density [g / cc]BET specific surface area [m 2 / g]Graphitization degree[%]Capacity[mAh / g]Efficiency[%]Example 6-1Y121316.50.6414.90.971.0515.11.051.291.8350.593.6Comparative example 6-1X11316.50.6115.10.950.8514.91.041.391.5348.793.8Example 6-2Y121516.30.6514.40.980.8414.21.091.591.1349.193.6Comparative example 6-2X11517.70.6515.50.950.7315.21.071.791.7346.993.1
[0120] Looking at Tables 6 and 7 above, it was confirmed that when the assembly was disintegrated under the disintegration conditions of the present invention, there was a difference in the specific surface area of the pre-carbonized product that had undergone pre-carbonization, and there was a difference in the tap density and capacity of the graphitized product. FIGS. 1A to 1D illustrate SEM photographs of graphite materials manufactured according to a method for manufacturing graphite materials according to one embodiment of the present invention.
[0121] Figures 1a to 1d respectively show SEM photographs of graphite materials manufactured according to a method for manufacturing graphite materials at magnifications of 1 K, 3 K, 5 K, and 10 K using FE-SEM. Referring to Figures 1a to 1d, it can be confirmed that the graphite material that has undergone a preliminary carbonization step as in the present invention has a dense density.
[0122]
[0123] Although the preferred embodiments have been described in detail above, the scope of the present invention is not limited thereto, and various modifications and improvements made by those skilled in the art using the basic concepts defined in the following claims also fall within the scope of the present invention.
Claims
1. A step of pre-carbonizing the result obtained from the graphite raw material and the coating material in the range of 1,050 to 1,300 ℃; and A method for producing a graphite material comprising a step of graphitizing a pre-carbonized resultant.
2. In paragraph 1, The above preliminary carbonization step Comprising a step of assembling the graphite raw material and the coating material, A method for producing a graphite material, wherein the coating material comprises 5 to 20 wt% based on 100 wt% of the obtained result.
3. In paragraph 1, A method for producing a graphite material, wherein the above preliminary carbonization step is performed for 3.0 hours or more.
4. In paragraph 1, A method for producing a graphite material, wherein the above preliminary carbonization step is performed at a heating rate range of 5 to 20 ℃ / min.
5. In paragraph 1, The above preliminary carbonization step A method for producing a graphite material, comprising the step of crushing a graphite raw material and a coating material.
6. In paragraph 5, A method for producing a graphite material, wherein the step of crushing the graphite raw material and the coating material is performed under conditions where the rotation speed of the crushing blade is 35 to 40 [HZ].
7. In paragraph 5, A method for producing a graphite material, wherein the step of crushing the graphite raw material and the coating material is performed under conditions where the air inflow is less than 35 to 50 [HZ].
8. In paragraph 5, A method for manufacturing a graphite material, wherein the step of crushing the above graphite raw material and coating material is performed under conditions where the classification (rotation speed of the classifier blade) is 15 or higher.
9. In paragraph 5, A method for producing a graphite material, wherein the step of crushing the graphite raw material and the coating material is performed so that the average particle diameter (D50) of the obtained result is 12 to 17 ㎛.
10. In paragraph 1, The above coating material is a method for producing a graphite material including a coke-based raw material.
11. In paragraph 10, The above coke-based raw material is a method for producing a graphite material including coal-based needle-like green coke.
12. In paragraph 1, Before the above preliminary carbonization step, the volatile content of the coating material is 4.0 to 5.0%, A method for producing a graphite material, wherein the volatile content of the coating material is 0.1 to 0.5% after the above preliminary carbonization step.
13. In paragraph 1, A method for producing a graphite material having an apparent density of 0.65 g / cc or more of the above-mentioned pre-carbonized result.
14. In paragraph 1, A method for producing a graphite material, wherein the tap density of the above-mentioned pre-carbonized resultant is 1.04 to 1.09 g / cc.
15. In paragraph 1, A method for producing a graphite material, wherein the weight reduction rate of the above-mentioned pre-carbonized result is 4.0 to 7.0%.
Citation Information
Patent Citations
Graphite particle, method for producing the same, negative electrode for lithium secondary battery and lithium secondary battery
JP2001089118A
Active material for negative electrode for lithium secondary battery and manufacturing method of the same
JP2004214192A
Anode active material with high electrical conductivity and manufacturing method thereof
KR101417588B1
Method of preparing artificial graphite negative electrode material for rechargeable lithium battery and artificial graphite negative electrode material for rechargeable lithium battery prepared from the same
KR1020150074295A
Atherosclerosis swine model using nicotine and induction method thereof
KR102206274B1