Method for manufacturing fe-ni-based alloy thin plate for metal mask, and fe-ni-based alloy thin plate for metal mask

The described manufacturing process for Fe-Ni alloy thin sheets addresses the issues of flatness and warping by using tensile stress correction and strain relief annealing, resulting in sheets with enhanced resistance to etching warping and improved dimensional stability for metal masks.

WO2026235053A1PCT designated stage Publication Date: 2026-11-12PROTERIAL LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2026/016749
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-07
Filing Date
2026-04-27
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing Fe-Ni alloy thin sheets used in metal masks and lead frames face challenges in maintaining flatness and resisting warping, particularly during deep etching processes, due to residual stress and processing strain, which conventional methods like strain relief annealing and shape correction with bending stress fail to adequately address.

Method used

A manufacturing process involving finishing cold rolling with a 5-50% reduction ratio, followed by recrystallization annealing at 800-1000°C, tensile stress application at 200-600 MPa, and strain relief annealing at 400-750°C, minimizes residual stress and warping by primarily using tensile stress for shape correction, ensuring sheets with 0.05-0.30 mm thickness and 800-1100 mm width.

Benefits of technology

The process achieves Fe-Ni alloy thin sheets with superior flatness and resistance to etching warping, suitable for high-precision metal mask applications, maintaining shape accuracy and dimensional stability even during deep etching.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
Patent Text Reader

Abstract

Provided is an Fe-Ni-based alloy thin plate which is suitable for use in a metal mask and with which both favorable flatness and etching warpage resistance can be achieved. This method for manufacturing an Fe-Ni-based alloy thin plate for a metal mask comprises: a finish cold rolling step for subjecting a cold rolling material, which contains, in terms of mass%, at most 0.01% of C, at most 0.5% of Si, at most 1.0% of Mn, and 28-52% of Ni, with the remainder consisting of Fe and inevitable impurities, to finish cold rolling to form a thin plate; a recrystallization annealing step for performing annealing on the thin plate, which has been subjected to the finish cold rolling; a tensile stress application step for performing shape correction on the thin plate, which has undergone the recrystallization annealing step, under the condition of a tension of 200-600 MPa and applying tensile stress; and a strain relieving annealing step for performing strain relieving annealing on the thin plate, which has undergone the tensile stress application step, at a temperature of 400-750ºC, wherein an Fe-Ni-based alloy thin plate for a metal mask, having a thickness of 0.05-0.30 mm and a width of 800-1,100 mm, is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Method for producing Fe-Ni alloy thin sheet for metal mask, and Fe-Ni alloy thin sheet for metal mask

[0001] The present invention relates to a method for producing an Fe-Ni alloy thin sheet for a metal mask, and an Fe-Ni alloy thin sheet for a metal mask.

[0002] Various studies have been conventionally conducted to improve the performance of Fe-Ni alloy thin sheets used for metal masks, lead frames and the like. As one of the methods for manufacturing such metal masks and lead frames, a method of subjecting an Fe-Ni alloy thin sheet to etching processing is known. Various studies have been conventionally conducted to improve this etching accuracy. For example, JP-A-10-204541 (Patent Document 1) discloses that an Fe-Ni alloy containing 32 to 38 wt% of Ni is subjected to cold rolling, then subjected to strain with an elongation of 0.4 to 3% to perform shape correction, followed by a thin sheet temperature of 550 to 690°C and a tension of 2 kgf / mm 2 There is an invention of a method for producing an Fe-Ni low thermal expansion alloy thin sheet excellent in sheet shape and heat shrinkage resistance, which performs strain relief annealing under the following conditions. In addition, JP-A-2003-253398 (Patent Document 2) discloses that in order to improve the etching rate and etching accuracy of an Fe-Ni-Co low thermal expansion alloy thin sheet, a hot-rolled material is subjected to cold rolling and annealing one or more times each, the cold rolling reduction of cold rolling before final recrystallization annealing is set to 90% or more, the annealing temperature of final recrystallization annealing is set to 850°C or more, and the final cold rolling reduction is set to 30% or less. There is an invention of a method for producing a low thermal expansion alloy thin sheet.

[0003] Furthermore, the applicant of the present application, in JP-A-2021-014639 (Patent Document 3), in order to achieve both good flatness and excellent etching warpage resistance in an Fe-Ni alloy thin sheet having a thickness of 0.5 mm or less, has proposed an Fe-Ni alloy thin sheet comprising: a finish cold rolling step of subjecting a material for cold rolling to finish cold rolling with a reduction ratio of 5% to 50% to obtain a thin sheet; a final annealing step of annealing the thin sheet after the finish cold rolling at a temperature of 800°C to 1000°C; and a tensile stress applying step of subjecting the thin sheet after the final annealing step to shape correction under a tension of 200 to 400 MPa to apply a tensile stress.

[0004] Japanese Patent Publication No. 10-204541, Japanese Patent Publication No. 2003-253398, Japanese Patent Publication No. 2021-014639

[0005] Due to the increasing complexity and precision of products in recent years, Fe-Ni based thin sheets, which are the materials used in these products, are required to be wide, have high flatness of the etched surface, and suppress warping after etching. In particular, as the width of the thin sheet increases, it tends to become more difficult to ensure flatness due to the effects of elongation differences in the width direction and variations in residual stress distribution. To improve flatness, shape correction using roller levelers and tension levelers has been effective since ancient times, but the residual stress applied to the thin sheet during shape correction is released during etching, causing warping, which is a problem. As a method to reduce warping due to residual stress as described above, strain relief annealing is known, in which the thin sheet is annealed at a temperature that does not reach the recrystallization temperature to remove the strain. However, with the diversification and complexity of product shapes, strain relief annealing alone cannot completely eliminate the effects of processing strain remaining in the thin sheet, and warping still tends to occur. The invention described in Patent Document 1 is expected to improve heat shrinkage resistance and flatness, but the study on suppressing warping that occurs when half-etching wide thin sheets is insufficient, leaving room for improvement. Similarly, the invention described in Patent Document 2 is expected to improve etching accuracy by increasing the (200) surface density of the rolled surface, but the study on suppressing warping that occurs when etching using etched material after finish rolling is insufficient, leaving room for improvement in suppressing warping during etching and improving flatness.

[0006] Furthermore, the invention described in Patent Document 3 is an excellent invention that can achieve both good flatness and excellent resistance to etching warping. However, in the case of metal masks, for example, high-precision pattern formation is required, so half-etching to various depths in the thickness direction is performed on the material for the metal mask. On the other hand, as the etching becomes deeper, there is a concern that warping may occur due to the influence of residual stress, so there is a need for a material that does not easily deform, such as warping, even with half-etching to various depths, and further investigation has been necessary.Therefore, the object of the present invention is to provide a method for manufacturing an Fe-Ni alloy thin sheet with a thickness of 0.05 to 0.30 mm and a width of 800 mm to 1100 mm that has even better flatness and resistance to etching warping and is suitable for metal mask applications, and to provide an Fe-Ni alloy thin sheet for metal masks obtained thereby.

[0007] One aspect of the present invention is a finishing cold rolling step in which a cold rolling material containing, by mass%, C: ≤0.01%, Si: ≤0.5%, Mn: ≤1.0%, Ni: 28-52%, with the remainder being Fe and unavoidable impurities is subjected to finishing cold rolling with a reduction ratio of 5-50% to form a thin sheet, and a recrystallization annealing step in which the thin sheet after finishing cold rolling is annealed at a temperature of 800-1000°C, and the recrystallization annealing step This method for manufacturing Fe-Ni alloy thin sheets for metal masks comprises a tensile stress application step, in which the thin sheet is subjected to shape correction under conditions of tension of 200 to 600 MPa to apply tensile stress, and a strain relief annealing step, in which the thin sheet after the tensile stress application step is subjected to strain relief annealing at a temperature of 400 to 750°C, thereby obtaining Fe-Ni alloy thin sheets for metal masks with a thickness of 0.05 to 0.30 mm and a width of 800 to 1100 mm. Another aspect of the present invention is an Fe-Ni alloy sheet for metal masks, having a thickness of 0.05 to 0.30 mm and a width of 800 to 1100 mm, containing, by mass%, C: ≤0.01%, Si: ≤0.5%, Mn: ≤1.0%, Ni: 28 to 52%, with the remainder being Fe and unavoidable impurities, wherein a sample of 150 mm in length and 30 mm in width is cut from the Fe-Ni alloy sheet, the sample is etched from one side, and when half the thickness of the sample is removed, the amount of warping is 10 mm or less, and the maximum floating height of the Fe-Ni alloy sheet over a length of 800 mm is 1.5 mm or less.

[0008] According to the present invention, it is possible to achieve both good flatness and resistance to etching warping, and a wide Fe-Ni alloy thin sheet suitable for metal mask applications can be provided.

[0009] Embodiments of the present invention will be described below. First, as mentioned above, the invention shown in Patent Document 3 proposed by the applicant of this application is capable of achieving both good flatness and excellent resistance to etching warpage. Based on this finding, the inventors conducted further studies and found optimal manufacturing conditions and process sequence that can achieve both good flatness and excellent resistance to etching warpage, which are required for wide thin sheets, particularly for metal mask applications. The method for manufacturing Fe-Ni alloy thin sheets for metal masks (hereinafter also simply referred to as Fe-Ni alloy thin sheets) of this embodiment will be described below. In this embodiment, a cold-rolled material obtained by hot rolling is prepared, having a composition in mass% of C: ≤0.01%, Si: ≤0.5%, Mn: ≤1.0%, Ni: 28-52%, with the remainder being Fe and unavoidable impurities. The composition specified in this embodiment ensures the thermal expansion characteristics and processability required for metal mask applications, and also allows the effects of each process described later to be stably exhibited. The reasons for specifying the above composition range are as follows.

[0010] [C: ≤0.01 mass%] Carbon (C) is an element that affects etching properties. Since excessive amounts of C inhibit etching, the upper limit for C is set to 0.01%. The lower limit for C can be 0%, but since it is inevitably present in some amount beyond 0% but below the impurity level during the manufacturing process, it is not particularly limited. [Si: ≤0.5 mass%, Mn: ≤1.0 mass%] Si and Mn are usually used for deoxidation purposes and are present in trace amounts in Fe-Ni alloys, but if they are present in excess, segregation is likely to occur, so Si: 0.5% or less, Mn: 1.0% or less. Preferred Si and Mn are Si: 0.1% or less, Mn: 0.5% or less. The lower limits for Si and Mn are not particularly limited, but for example, Si can be set to 0.01% and Mn to 0.05%.

[0011] [Ni: 28-52% by mass] Ni has the effect of adjusting the coefficient of thermal expansion and is an element that greatly affects low thermal expansion properties. If the content is less than 28% or more than 52%, the effect of reducing the coefficient of thermal expansion is lost, so the range of Ni is set to 28-52%. The lower limit of Ni that is preferable is 30%, the lower limit of Ni that is more preferable is 32%, and the lower limit of Ni that is even more preferable is 34%. The upper limit of Ni that is preferable is 50%, the upper limit of Ni that is more preferable is 45%, and the upper limit of Ni that is even more preferable is 38%. In addition, in this embodiment, a portion of Ni can be replaced with Co in order to adjust the thermal expansion properties and to provide high strength. When trying to impart the above effects to Fe-Ni alloy for metal masks, it is preferable to replace a portion of Ni with Co in the range of 20% or less. [Remainder] The remainder other than the above elements is Fe and unavoidable impurities. Examples of impurity elements include unavoidable impurities such as P, S, N, Al, and O, but they may be included as long as they do not hinder the effects of the present invention, within the ranges shown below: P ≤ 0.04%, S ≤ 0.03%, N ≤ 0.02%, Al ≤ 0.10%, and O ≤ 0.05%. In addition to the above unavoidable impurities, other elements may be included as impurities as long as they do not hinder the effects of the present invention. The elements included as impurities vary greatly depending on the raw materials such as alloys and recycled materials used in the manufacture of Fe-Ni alloys, so examples of elements are not given here, but the total content of elements included as impurities is preferably 0.5% or less.

[0012] <Material for Cold Rolling> In this embodiment, a strip-shaped material for cold rolling having the above-described composition is prepared. This material for cold rolling can be obtained, for example, by mechanically or chemically removing the oxide layer formed on the surface of a hot-rolled material having the above-described composition. In addition, in order to suppress the occurrence of defects such as cracks from the edges during cold rolling, the edges may be trimmed or otherwise smoothed as needed. Furthermore, if necessary, the steel ingot, slab, or forging material that will be the raw material for the hot-rolled material may be subjected to homogenization heat treatment at, for example, about 1200°C. This can mitigate component segregation. The thickness of the material for cold rolling is not particularly limited, but for example, it may be about 1.0 to 7.0 mm.

[0013] <Intermediate Cold Rolling, Intermediate Annealing> In this embodiment, one or more intermediate cold rollings may be performed to adjust the plate thickness prior to the finish cold rolling described later. In this embodiment, the case in which intermediate cold rolling is introduced will be described, but if the desired plate thickness can be adjusted after hot rolling, intermediate cold rolling may be omitted. After intermediate cold rolling, the intermediate cold-rolled material (hereinafter referred to as "intermediate sheet") may be subjected to intermediate annealing to soften the work-hardened intermediate sheet and remove processing distortion. The temperature for this intermediate annealing should be set to 800°C or higher, which promotes recrystallization. If the annealing temperature is less than 800°C, the material may not soften sufficiently, and the desired properties may not be obtained. There is no particular upper limit to the annealing temperature, but if the temperature is raised too high, there is a high possibility that the desired properties will not be obtained, so it can be set to around 1100°C. The heating and holding time at this time should be adjusted as appropriate according to the composition of the material and the plate thickness. Intermediate annealing can be performed by continuous annealing, where the intermediate sheet after intermediate cold rolling is continuously passed through a heating furnace set to a desired temperature. For example, the intermediate sheet after intermediate cold rolling can be pulled out from a rolled state, passed through a heating furnace, and then wound back into a roll. In this case, the method used for intermediate annealing does not have to be special; any conventional method is acceptable.

[0014] <Finishing Cold Rolling> In the manufacturing method of this embodiment, the intermediate sheet after the intermediate cold rolling or intermediate annealing described above is subjected to finishing cold rolling with a reduction ratio of 5% to 50% to obtain a sheet (hereinafter referred to as "finishing cold-rolled sheet"). By setting the reduction ratio of the finishing cold rolling within the above range, it is possible to reduce the difference in elongation between the center and the edges of the intermediate sheet during finishing cold rolling, thereby suppressing the generation of excessive wave shapes. As a result, it becomes easier to adjust to a flatter shape after the shape correction process described later. If the reduction ratio of the finishing cold rolling is less than 5%, elongation is likely to occur, and the flatness of the center of the sheet after shape correction tends to decrease. Also, if the reduction ratio of the finishing cold rolling is less than 5%, the recrystallization of the finishing cold-rolled sheet tends to be excessively promoted in the recrystallization annealing described later, so the hardness of the finishing cold-rolled sheet tends to decrease. On the other hand, when the reduction ratio exceeds 50%, the end wave becomes stronger, and the flatness tends to decrease after shape correction. For this reason, the reduction ratio for finish cold rolling should be between 5% and 50%. The lower limit of the preferred reduction ratio for finish cold rolling is 15%, and the lower limit is 20%. Furthermore, the upper limit of the preferred reduction ratio for finish cold rolling is 40%, and the upper limit is 30%.

[0015] The number of passes for this finish cold rolling is preferably one. If the finish cold rolling is performed in multiple passes, the effects of elongation differences in the width direction of the sheet and roll deflection in each pass tend to accumulate, which may exacerbate the difference in shape between the edges and the center. As a result, even if the shape correction process and strain relief annealing process described later are performed, non-uniformity in the residual stress distribution in the width direction of the sheet tends to remain, which may reduce flatness and resistance to etching warping. In contrast, performing the finish cold rolling in one pass simplifies the processing history and makes it easier to suppress the occurrence of shape defects and variations in residual stress distribution. The manufacturing method of Fe-Ni alloy thin sheets for metal masks in this embodiment can be applied to wide materials with a width of 800 to 1100 mm so that it can be applied to metal masks with a large area. In addition, the upper limit of the sheet thickness suitable for this embodiment is 0.30 mm so that a high-resolution metal mask can be made. The preferred upper limit of the sheet thickness is 0.20 mm. Furthermore, since plates that are too thin are unsuitable for half-etching, the lower limit of the plate thickness should be 0.05 mm. The preferred lower limit of the plate thickness is 0.08 mm.

[0016] <Recrystallization Annealing Process> In this embodiment, a recrystallization annealing process is performed on the finished cold-rolled sheet after finish cold rolling at a temperature of 800°C to 1000°C. It is preferable to apply continuous annealing in the recrystallization annealing process. This recrystallization annealing process recrystallizes the structure that has been work-hardened by cold rolling, removes the processing strain caused by cold rolling, and sufficiently reduces the yield strength of the sheet, making it easier to improve the flatness in the tensile stress application process described later. If the recrystallization annealing temperature is below 800°C, not only may a sufficient recrystallized structure not be obtained, but the processing strain may not be sufficiently removed. Also, if the recrystallization annealing temperature exceeds 1000°C, the hardness of the finished cold-rolled sheet tends to decrease too much, which is undesirable. The preferred lower limit of the recrystallization annealing temperature is 850°C, and the preferred upper limit of the recrystallization annealing temperature is 950°C.

[0017] <Tensile Stress Application Process> In the manufacturing method of Fe-Ni alloy thin sheets for metal masks according to this embodiment, a tensile stress application process is performed to correct the shape by applying tensile stress under conditions of 200 to 600 MPa tension. That is, a tensile stress application process is performed on the thin sheet that has completed the recrystallization annealing process (hereinafter referred to as "recrystallized annealed thin sheet") for the purpose of correcting the shape. This makes it possible to correct excessive edge waves and in-between elongation remaining in the recrystallized annealed thin sheet and to significantly improve the flatness. In particular, this embodiment is characterized by correcting mainly with tensile stress, while minimizing the application of bending stress applied by shape correction using a tension leveler. Conventionally, in order to remove such processing distortion, it was common to perform shape correction by applying bending stress using a tension leveler, etc., and then perform distortion-relieving annealing, in which the thin sheet is heat-treated at a temperature below the recrystallization temperature. However, in shape correction that applies bending stress, new processing distortion may be introduced into the thin sheet, and such processing distortion cannot be sufficiently removed even by distortion-relieving annealing, which may be a factor in reducing the flatness of the thin sheet. In contrast, the tensile stress application step of this embodiment allows for shape correction primarily using tensile stress on a recrystallized annealed thin sheet, which has had its work hardened state eliminated by the preceding recrystallized annealing step, while suppressing the application of processing strain due to new bending stress. This improves flatness while suppressing the introduction of new processing strain.

[0018] The device used for this shape correction can be a conventional shape correction device such as a stretcher, roller leveler, or tension leveler. In this embodiment, a tension leveler is used, but since the correction is mainly performed by tensile stress, even when using a tension leveler, it is not necessary to press in with a leveler roll (correction roll). Also, if pressing in with a leveler roll is performed, the amount of pressing may be less than or equal to the plate thickness. This makes it possible to effectively exhibit the shape correction effect by tension while suppressing the introduction of excessive processing distortion caused by bending deformation. The tension during shape correction in the tensile stress application process can be set to 200 to 600 MPa. If the tension is less than 200 MPa, the correction will be insufficient. If the tension exceeds 600 MPa, there is a possibility that new shape defects will occur due to excessive tension. The preferred lower limit of tension during shape correction is 250 MPa. On the other hand, the preferred upper limit of tension during shape correction is 500 MPa, more preferably 450 MPa, and even more preferably 400 MPa. Furthermore, in the manufacturing method of Fe-Ni alloy thin sheets for metal masks according to this embodiment, Fe-Ni alloy thin sheets for metal masks with excellent flatness and etching warp resistance can be manufactured without performing temper rolling (light reduction rolling) by the strain-relieving annealing process described later. Therefore, temper rolling can be omitted before and after the tensile stress application process.

[0019] <Strain Relief Annealing Process> In this embodiment, a strain relief annealing process is performed on the thin sheet (hereinafter referred to as "shape-corrected thin sheet") after the tensile stress application process at a temperature of 400°C to 750°C to obtain the Fe-Ni alloy thin sheet for metal masks of this embodiment. In this embodiment, a "strain relief annealing process" not disclosed in Patent Document 3 is essential. The tensile stress application process in this embodiment is a process that applies as little bending stress as possible to the sheet material, compared to conventional shape correction mainly using bending stress. However, even when shape correction is performed mainly using tensile stress, a stress difference remains between the surface layer and the center of the sheet thickness, so when deep etching is performed, the above-mentioned residual stress is released and there is a risk of excessive warping occurring. Therefore, in this embodiment, by performing a strain relief annealing process after the tensile stress application process, the residual stress difference in the sheet material generated by the tensile stress application process is mitigated, maintaining flatness while suppressing warping due to etching. This makes it possible to obtain Fe-Ni alloy thin sheets that have both good flatness and excellent resistance to etching warping, even in wide, thin sheets. In the stress relief annealing process of this embodiment, if the stress relief annealing temperature is less than 400°C, the relaxation of residual stress differences may be insufficient, and the warping suppression effect after etching may not be sufficiently obtained. On the other hand, if the stress relief annealing temperature exceeds 750°C, recrystallization is likely to occur, which may impair the flatness obtained by shape correction or prevent the desired mechanical properties from being obtained. For this reason, the stress relief annealing temperature should be between 400 and 750°C. The lower limit of the preferred stress relief annealing temperature is 500°C, and the upper limit of the preferred stress relief annealing temperature is 700°C.

[0020] <Fe-Ni alloy thin sheet for metal masks> Next, the Fe-Ni alloy thin sheet for metal masks of the present invention will be described. The Fe-Ni alloy thin sheet for metal masks of the present invention can be obtained by applying the aforementioned recrystallization annealing process, tensile stress application process, and strain relief annealing process in this order under appropriate conditions. This Fe-Ni alloy thin sheet of the present invention has the characteristics related to the amount of warping and the lift height described later, and is suitable for metal mask applications in which high-resolution patterns are formed by etching.

[0021] <Warpage Amount> The Fe-Ni alloy thin sheet for metal masks of this embodiment is characterized in that, when cut to a sample size of 150 mm in the length direction (rolling direction) and 30 mm in the width direction (direction perpendicular to rolling), the amount of warpage when 1 / 2 of the sheet thickness of the sample is removed is 10 mm or less. As a result, the residual stress at the center of the sheet thickness is reduced in the Fe-Ni alloy thin sheet for metal masks of this embodiment, and even when etching is performed to a depth in the center of the sheet thickness where the stress balance is more disrupted, deformation of the sheet material can be suppressed, and it is possible to ensure shape accuracy while the etching process proceeds smoothly. Furthermore, when 1 / 2 of the sheet thickness is removed, the stress balance in the thickness direction is more likely to be disrupted, and the effect of warpage is more likely to occur, compared to when 1 / 3 of the sheet thickness is removed as described in Patent Document 3. A more preferable upper limit for the amount of curvature is 7 mm, and an even more preferable upper limit for the amount of curvature is 5 mm.

[0022] In this embodiment, the amount of warpage is evaluated using a cut sample (warpage measurement sample) measuring 150 mm in length and 30 mm in width, obtained by cutting the sample so that the longitudinal direction is the rolling direction. Specifically, after etching away half of the plate thickness from one side of the sample, one end (upper end) in the longitudinal direction of the warpage measurement sample is suspended in contact with a vertical surface plate, and the horizontal distance between the other end (lower end) of the warpage measurement sample, which has moved away from the vertical surface plate due to warpage, and the vertical surface plate is measured as the amount of warpage. In this embodiment, a "+" warpage is defined as a case where the etched surface warps towards the concave side, and a "-" warpage is defined as a case where the etched surface warps towards the convex side, and the amount of warpage is evaluated by its absolute value. Therefore, a smaller absolute value of the amount of warpage is preferable. In this embodiment, it is preferable that the amount of warpage measured in a sample taken with a width of 150 mm (perpendicular to rolling) and a length of 30 mm (rolling direction) is 10 mm or less (more preferably 7 mm or less, and even more preferably 5 mm or less) when half of the plate thickness is removed. By having such warpage characteristics, the Fe-Ni alloy thin sheet of the present invention can easily ensure high dimensional accuracy and shape accuracy even in metal mask applications where half etching is performed.

[0023] <Floating Height> The Fe-Ni alloy thin sheet for metal masks of this embodiment is characterized by a low maximum floating height at a length of 800 mm and excellent flatness. Specifically, the maximum floating height when the length of the Fe-Ni alloy thin sheet is 800 mm is 1.5 mm or less. Thus, the Fe-Ni alloy thin sheet for metal masks obtained by carrying out the manufacturing method of this embodiment described above has excellent flatness even in wide thin sheet materials such as those with a thickness of 0.30 mm or less and a width of 800 mm or more (preferably 900 mm or more, more preferably 1000 mm or more). Therefore, it contributes to improved effects such as improved dimensional accuracy in etching. A more preferable value for the maximum floating height is 1.2 mm or less, and an even more preferable value for the maximum floating height is 1.0 mm or less. The lower limit of the maximum floating height is not particularly limited, but since it is extremely difficult to manufacture a completely flat shape, the lower limit of the maximum floating height may be set to, for example, about 0.1 mm. To measure the levitation height, cut an 800 mm length of Fe-Ni alloy sheet for metal masks, place it on a horizontal surface plate, and measure the levitation height of the sheet using a laser displacement meter or similar device. For example, the maximum distance between the bottom surface of the Fe-Ni alloy sheet for metal masks and the horizontal surface plate can be evaluated as the maximum levitation height.

[0024] <Steepness> In this embodiment, the Fe-Ni alloy sheet for metal masks preferably has a maximum steepness of 0.7% or less over a length of 800 mm. By setting the maximum steepness to be below this range, a Fe-Ni alloy sheet for metal masks with superior flatness can be obtained. A more preferable maximum steepness value is 0.5% or less, and an even more preferable maximum steepness value is 0.3% or less. There is no particular lower limit to the maximum steepness, but as with the rise height, it is extremely difficult to manufacture a perfectly flat shape, so for example, the lower limit of the maximum steepness may be set to about 0.01%. The steepness can be calculated by measuring the rise height at regular intervals (regular lengths) along the width and length directions of the sheet and recording the measured values ​​in a matrix. This makes it possible to evaluate the degree of shape change within the surface of the Fe-Ni alloy sheet for metal masks.

[0025] <Tensile Strength, 0.2% Yield Strength, Elongation> The Fe-Ni alloy sheet for metal masks in this embodiment preferably has a tensile strength of 400 MPa or more and a 0.2% yield strength of 200 MPa or more. Furthermore, if workability is important, the elongation may be set to 20-50%. As a result, the Fe-Ni alloy sheet of this embodiment can exhibit good plastic workability in addition to excellent flatness and resistance to etching warping, making it possible to more reliably suppress the occurrence of fracture and cracking during winding and plastic deformation. The preferred lower limit of the tensile strength is 450 MPa, and the preferred lower limit of the 0.2% yield strength is 250 MPa. The preferred lower limit of the elongation is 25%, and the preferred upper limit of the elongation is 45%. The tensile strength, 0.2% yield strength, and elongation characteristics can be determined by testing based on the method specified in JIS-Z2241.

[0026] For the Fe-Ni alloy having the composition shown in Table 1, hot pressing and hot rolling were performed to prepare a hot-rolled material with a thickness of 3.0 mm. The oxide layer formed on the surface of the hot-rolled material was removed by chemical polishing and mechanical polishing, and further, cracks from the hot rolling process at both ends in the width direction of the material were removed by trimming. Then, the material was divided into the present invention example and the comparative example, and each was subjected to intermediate cold rolling and intermediate annealing (approximately 900°C) once or more to produce intermediate cold-rolled material with a width of 1040 mm and a thickness of 0.2 mm. Next, both the present invention example and the comparative example were subjected to a one-pass finish cold rolling at a reduction ratio of 25% to produce a finish cold-rolled sheet. Then, the process shown in Table 2 was performed to produce wide-width Fe-Ni alloy sheets for metal masks, No. 1 of the present invention example and Nos. 11 and 12 of the comparative examples. Here, recrystallization annealing was performed at approximately 900°C for both the present invention example and the comparative examples. Furthermore, the tensile stress application process was carried out using a tension leveler, without pressing with leveler rolls, and shape correction was performed primarily with tensile stress under conditions of a corrective tension of approximately 300 MPa. In addition, in Example No. 1 of the present invention and Comparative Example No. 12, strain relief annealing was performed at approximately 630°C.

[0027] Various test pieces were taken from the Fe-Ni alloy thin sheet for wide metal masks of the fabricated Invention Example No. 1, and each was tested. The test results are shown in Table 2. To confirm the effect of etching warpage suppression, a warpage measurement sample with a length of 150 mm and a width of 30 mm was prepared. After removing half of the sheet thickness from one side by etching, the warpage measurement sample was suspended from a vertical surface plate, and the amount of warpage was measured and evaluated. The above warpage measurement sample was taken from the center of the width direction of the prepared warpage measurement sample so that the length direction was the rolling direction. A ferric chloride aqueous solution was used as the etching solution, and the etching of the warpage measurement sample was carried out by spraying the etching solution at a liquid temperature of 50°C. The effect of flatness was confirmed by evaluating the maximum floating height using a three-dimensional shape measuring instrument. The maximum floating height and maximum steepness were measured from a test piece cut to a length of 800 mm placed on a horizontal surface plate. The steepness was calculated from data recorded in a matrix format, showing the lift height at regular intervals (width: 21 mm, length: 8 mm). Tensile strength, 0.2% yield strength, and elongation were measured according to the test methods specified in JIS-Z2241.

[0028]

[0029]

[0030] As shown in Table 2, Example No. 1 of the present invention, in which the recrystallization annealing process, tensile stress application process, and strain relief annealing process were performed in this order after finish cold rolling, showed a warpage of 4 mm, indicating a good etching warpage of 5 mm or less. Furthermore, the tensile strength was 477 MPa (460 MPa or more), the 0.2% yield strength was 306 MPa (280 MPa or more), and the elongation was 34.4% (30% or more), showing good mechanical properties. In addition, the maximum lift height was 0.7 mm (0.8 mm or less) and the maximum steepness was 0.2% (0.3% or less), showing very excellent values. From this, it can be seen that the Fe-Ni alloy thin sheet obtained by applying the present invention is suitable for various etching processes. In contrast, Comparative Example No. 1, in which the recrystallization annealing process and tensile stress application process were performed after finish cold rolling, but strain relief annealing was not performed... Comparative example No. 11 showed a large amount of etching warp, with a maximum lift height of 0.9 mm and a maximum steepness of 0.4%, which was inferior to the example of the present invention. Furthermore, comparative example No. 12, which underwent only stress-relieving annealing after finish cold rolling, had a warp of 7 mm, a larger amount of etching warp than the example of the present invention, and excessive ear waves were generated in the thin sheet. As a result, the values ​​of the maximum lift height and maximum steepness were excessive, suggesting that it is unsuitable as a material for metal masks to be etched to form high-precision patterns.

Claims

1. A cold-rolling material containing, by mass%, C: ≤0.01%, Si: ≤0.5%, Mn: ≤1.0%, Ni: 28-52%, with the remainder being Fe and unavoidable impurities, is subjected to a finish cold-rolling process with a reduction ratio of 5% to 50% to form a thin sheet; a recrystallization annealing process in which the thin sheet after the finish cold-rolling is annealed at a temperature of 800°C to 1000°C; a tensile stress application process in which the thin sheet after the recrystallization annealing process is shaped and subjected to tensile stress under conditions of tension of 200 to 600 MPa; and a strain relief annealing process in which the thin sheet after the tensile stress application process is subjected to strain relief annealing at a temperature of 400°C to 750°C. A method for producing Fe-Ni alloy thin sheets for metal masks, comprising obtaining Fe-Ni alloy thin sheets with a thickness of 0.05 to 0.30 mm and a width of 800 mm to 1100 mm.

2. An Fe-Ni alloy sheet for metal masks, having a thickness of 0.05 to 0.30 mm and a width of 800 mm to 1100 mm, containing, by mass%, C: ≤0.01%, Si: ≤0.5%, Mn: ≤1.0%, Ni: 28 to 52%, with the remainder being Fe and unavoidable impurities, wherein a sample of 150 mm in length and 30 mm in width is cut from the Fe-Ni alloy sheet, the sample is etched from one side, and the amount of warping when half the thickness of the sample is removed is 10 mm or less, and the maximum floating height of the Fe-Ni alloy sheet at a length of 800 mm is 1.5 mm or less.