Polar monomer grafted polypropylene resin and preparation method and application thereof

Polar monomer grafting in polypropylene resin is carried out through microwave initiation technology, which solves the problems of molecular weight decrease and initiator residue during graft modification of polypropylene, achieves high grafting rate and low-cost production, and ensures the stability of the material. Mechanical properties and environmental protection.

CN112055721BActive Publication Date: 2024-10-22CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201980026153.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-04-27
Filing Date
2019-04-26
Publication Date
2024-10-22
Estimated Expiration
2039-04-26

Smart Images

  • Figure CN112055721B_ABST
    Figure CN112055721B_ABST
Patent Text Reader

Abstract

The invention relates to the field of polypropylene graft modification, and provides a polar monomer grafted polypropylene resin and a preparation method and application thereof. The grafted polypropylene resin according to the invention is prepared by grafting a polar monomer capable of absorbing microwaves so as to increase its temperature in a microwave field to above 200°C with a solid polypropylene resin under microwave irradiation without adding an initiator. According to the invention, a polar grafted polypropylene resin is obtained which does not contain initiator residues and has a molecular weight that is not significantly reduced compared with the resin before grafting. The preparation process of the invention is simple, easy to operate, has simple production equipment, is low in cost, and is easy to industrialize.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of graft modification of polypropylene, and in particular to a polar monomer grafted polypropylene resin, a preparation method and application thereof, and granules, products, composite materials, coatable film materials and adhesive materials prepared from the grafted polypropylene resin. Background Art

[0002] Polypropylene is a widely used general polymer material with excellent physical and mechanical properties. However, due to the non-polarity and low surface energy of polypropylene, it has poor compatibility with most polymers and fillers, is not easy to wet and bond, and has poor printing and coating properties. It is also difficult to obtain materials with good performance when blended with polar materials. Therefore, some methods are needed to improve the polarity of polypropylene. A common method is to graft polar monomers such as maleic anhydride onto the main chain of polypropylene to increase its polarity. The main methods of grafting modification are solvent method, melt method and solid phase method.

[0003] The solvent method achieves a high grafting rate and a relatively low reaction temperature. However, the organic solvent is usually toluene or xylene, so the post-processing is complicated, the cost is high, and the environmental friendliness is poor, and it has gradually been eliminated in industrial practice.

[0004] Melt grafting is the most reasonable method currently and is suitable for industrial production. For example, Chinese patent application CN104804143A reported the use of a twin-screw extruder with an aspect ratio greater than 48:1, adding a mixed solution of styrene and initiator at multiple positions of different barrel sections of the extruder, and obtaining maleic anhydride grafted polypropylene with a high grafting rate and no significant decrease in molecular weight compared with the raw polypropylene. U.S. Patent US6,228,948B1 reported the use of different process parameters and conditions in each section of the twin-screw extruder, adding polypropylene and maleic anhydride into the extruder, adding an initiator after it is melted, and the maleic anhydride reaction is grafted onto the polypropylene molecular chain to obtain a polypropylene with a grafting rate of more than 2% and excellent comprehensive performance. Chinese patent application CN102924661A reports that the use of auxiliary monomers can increase the grafting rate of polypropylene and inhibit the degradation of polypropylene. At the same time, a new initiator is used to reduce the pungent odor of maleic anhydride grafted polypropylene. The initiator can also enhance the degree of grafting reaction and the degree of copolymerization with the auxiliary monomer to obtain maleic anhydride grafted polypropylene with high grafting rate and low pungent odor.

[0005] However, the β-chain scission reaction during the melt grafting of polypropylene is an unavoidable side reaction during the grafting process. Therefore, the melt index of maleic anhydride grafted polypropylene products prepared by the melt grafting method is usually very high, that is, the molecular weight is greatly reduced, which will lead to poor mechanical properties of polypropylene products. Therefore, the main problem faced by the melt grafting method is how to maintain the mechanical properties of the polypropylene matrix while obtaining a sufficiently high maleic anhydride grafting rate, that is, to keep the molecular weight basically unchanged, so that when blended with other materials, it will not affect the final overall mechanical properties of the material. The traditional solid phase method refers to the graft copolymerization reaction after mixing polypropylene with monomers, initiators, and interfacial agents. The reaction temperature is relatively low (100-140°C). Polypropylene (melting point is about 164-171°C) is still a solid particle at the reaction temperature, so this method is called solid phase grafting. In the solid phase method, the reaction takes place on the exposed surface of polypropylene. Chinese patent application CN1283642A discloses a preparation method and application of a solid phase graft copolymer of polypropylene and three monomers, which is to put polypropylene, initiator and three monomers into a reactor in proportion, add surfactant xylene, and carry out solid phase graft reaction under nitrogen atmosphere. Chinese patent application CN103102455A discloses a grafting method of polypropylene, which is to add polypropylene, organic acid (or salt) and surfactant into a reactor with stirring, add initiator after reaching the reaction temperature, and carry out solid phase graft reaction, wherein the initiator is wax-coated peroxide microcapsule. Chinese patent application CN1704436A discloses a continuous solid phase grafting production method and device for polypropylene. US patent application US5,585,435A discloses a production method for solid phase grafting modification of polypropylene on a fluidized bed. Both technologies achieve high grafting rate by improving the contact efficiency of reactants and initiators.

[0006] The above-mentioned existing polypropylene graft modification methods all have the following disadvantages: graft modification leads to a decrease in molecular weight, monomer residues exist in the product, initiators need to be used in the modification process, the product has an odor or requires special equipment, etc. Due to the wide application and huge market demand of polar polypropylene, a grafted polypropylene that is cheap, has a simple preparation method and does not have the above disadvantages has become an urgent problem to be solved. In order to solve the above problems, the present invention is proposed. Summary of the invention

[0007] The purpose of the present invention is to provide a polar monomer grafted polypropylene resin prepared by microwave initiation and a preparation method thereof, which does not have the shortcomings of existing grafted polypropylene resins and polypropylene grafting modification methods. The grafted polypropylene resin product should have no initiator residues, the molecular weight should not be significantly reduced after grafting, and the occurrence of β-chain scission reaction should be greatly reduced during its preparation process.

[0008] Another object of the present invention is to provide a polar monomer grafted polypropylene resin, which can achieve a higher grafting rate.

[0009] Another object of the present invention is to provide an odorless polar monomer grafted polypropylene resin which does not contain residual unreacted monomers or auxiliary grafted monomers.

[0010] Another object of the present invention is to provide a method for preparing a polar grafted polypropylene resin, which has a simple process, is easy to operate, has simple production equipment, is low in cost, and is easy to industrialize.

[0011] According to the present invention, it was unexpectedly found that the above-mentioned object was achieved by utilizing the selective heating property of microwaves, by grafting a polar monomer that can absorb microwaves so that its temperature in the microwave field is increased to above 200°C with a solid polypropylene resin under microwave irradiation without adding an initiator.

[0012] Therefore, in a first aspect, the present invention provides a polar monomer grafted polypropylene resin, wherein the grafted polypropylene resin does not contain initiator residues, and the polar monomer can absorb microwaves so that its temperature in the microwave field increases to above 200°C.

[0013] The term "microwave" as used herein refers to electromagnetic waves having a frequency of 300 MHz-300 GHz.

[0014] The term "polar monomer" used herein refers to a monomer containing heteroatoms such as oxygen, sulfur, nitrogen, halogen, etc. or their substituents. The polar monomers that can be used in the present invention can absorb microwaves so that their temperature in the microwave field increases to more than 200°C.

[0015] The polar monomers that can be used can be determined by the following test method:

[0016] The polar monomer is loaded into a 10 ml glass medicine bottle until the volume of the polar monomer occupies 2 / 3 of the volume of the glass medicine bottle. Then, a thermocouple is inserted into the glass medicine bottle containing the polar monomer, and the glass medicine bottle together with the thermocouple is placed in a microwave oven, and the microwave is turned on to test the temperature of the polar monomer under microwave irradiation. The polar monomer with a temperature exceeding 200° C. at any power and time can be used as the polar monomer of the present invention. Specifically, for example, under the condition of microwave irradiation with a power of 700 W for 30 minutes, the polar monomer that is tested to be heated to a temperature exceeding 200° C. can be used in the present invention.

[0017] For example, the polar monomer may be selected from those containing a carbon-carbon double bond, such as polar monomers containing heteroatoms or substituents thereof selected from oxygen, sulfur, nitrogen and halogens and combinations thereof and containing a carbon-carbon double bond.

[0018] Preferably, the polar monomer can be selected from organic acids, derivatives of organic acids (such as anhydrides, esters, salts) and combinations thereof, preferably selected from maleic anhydride, maleic anhydride derivatives, (meth) acrylic acid, (meth) acrylic acid derivatives (such as glycidyl methacrylate), vinyl acetate, olefin sulfonic acid and its derivatives, p-phenylene formic acid, p-phenylene acetic acid, itaconic acid, oleic acid, arachidonic acid and combinations thereof and their salt forms. The (meth) acrylic acid includes acrylic acid, methacrylic acid and mixtures thereof.

[0019] The polar monomer is preferably selected from one or more of maleic anhydride, maleic anhydride derivatives, (meth)acrylic acid, (meth)acrylic acid derivatives (e.g. glycidyl methacrylate), and vinyl acetate, preferably maleic anhydride, maleic anhydride derivatives, (meth)acrylic acid, (meth)acrylic acid derivatives, more preferably maleic anhydride, and salt forms thereof.

[0020] Herein, the term "initiator" refers to a substance commonly used in the art to initiate polymerization reactions (including grafting reactions) of monomers, such as free radical initiators, including peroxide initiators, azo initiators, and redox initiators, etc. Peroxide initiators can be further divided into organic peroxide initiators (such as diisopropylbenzene peroxide) and inorganic peroxide initiators.

[0021] In the grafted polypropylene resin according to the present invention, the grafting rate can be 0.01%-8%, preferably 0.01%-6%. There are side groups of polar monomers on the main chain of the polypropylene molecule, such as side groups of organic acids or their salts, and the grafting rate of the organic acid side groups can be 0.01%-8%, preferably 0.01%-6%, more preferably 0.01%-3%, and most preferably 0.01%-1.2%. For organic acid salt grafted polypropylene resin, there are organic acid salt side groups on the main chain of the polypropylene molecule, and the grafting rate of the organic acid side groups of the organic acid salt side groups can be 0.01%-8%, preferably 0.01%-6%, more preferably 0.01%-3%, and most preferably 0.01%-1.2%.

[0022] The organic acid salt side groups may include at least one of salified maleic anhydride side groups, maleic anhydride derivative side groups, (meth)acrylic acid side groups, (meth)acrylic acid derivative side groups (eg, glycidyl methacrylate side groups), and vinyl acetate side groups.

[0023] In this paper, the grafting rate of polar monomers was characterized by infrared spectroscopy.

[0024] The water contact angle value of the grafted polypropylene resin according to the present invention can be less than 90°, preferably less than 65°, measured for a film prepared by a solution method from the grafted polypropylene resin. For example, for an organic acid grafted polypropylene resin, the water contact angle value of the side of the film containing the organic acid group after the film is prepared by the solution method is less than 90°, preferably less than 65°. For an organic acid salt grafted polypropylene resin, the water contact angle value of the side of the film containing the organic acid salt group after the film is prepared by the solution method is less than 90°, preferably 50°-0°, and more preferably 0°.

[0025] Herein, the water contact angle is measured in the following manner: a grafted polypropylene resin is prepared into a film by a solution method, and the side of the obtained film containing the polar monomer side group is subjected to water contact angle measurement using a water contact angle measuring instrument.

[0026] The melt index of the grafted polypropylene resin according to the present invention is preferably less than or equal to the melt index of the polypropylene resin used as the graft base, that is, its melt index is less than or equal to the melt index of the raw material itself before the grafting of the polypropylene resin. During the preparation process of the polar monomer grafted polypropylene resin of the present invention, the β-chain scission reaction of the polypropylene is controlled, and the phenomenon of molecular weight reduction of the polypropylene will not occur. The melt index of the grafted polypropylene can be consistent with that of the raw polypropylene, or even lower.

[0027] In this article, the melt index is measured according to the standard GB / T3682-2000.

[0028] As used herein, the term "polypropylene" or "polypropylene resin" includes homopolymers and copolymers of propylene and mixtures thereof.

[0029] The polypropylene resin as the graft base can be selected from propylene homopolymers and propylene copolymers and mixtures thereof, preferably random copolymers of propylene. For example, the comonomer in the random copolymer of propylene can be selected from ethylene, α-olefins other than propylene and combinations thereof, preferably ethylene, C4, C5, C6 to C8-α-olefins and combinations thereof. More preferably, the random copolymer of propylene contains only ethylene or an α-olefin other than propylene as a comonomer.

[0030] The polypropylene resin used as the graft base may also be an impact polypropylene resin, which contains a rubber phase in addition to a propylene homopolymer. The rubber phase may be a copolymer formed by propylene and a comonomer selected from at least one of ethylene and α-olefins, preferably ethylene, C4, C5, C6 to C8 α-olefins. Preferably, the rubber phase of the impact polypropylene resin is formed by polymerization of propylene and ethylene or an α-olefin other than propylene.

[0031] The polypropylene resin used as the graft base may be in the form of a solid including powder, pellets or products, preferably a polypropylene powder obtained by polymerization using a spherical catalyst.

[0032] Preparation method of polar monomer grafted polypropylene resin

[0033] In a second aspect, the present invention also provides a method for preparing a polar monomer grafted polypropylene resin according to the present invention, comprising the step of grafting the polar monomer with a solid polypropylene resin using microwave irradiation without adding an initiator. No auxiliary grafting monomer may be used during the grafting reaction.

[0034] In the method of the present invention, the polar monomer may be used in an amount of 0.1-10% by weight based on the weight of the solid polypropylene resin as a raw material; preferably 1-8% by weight.

[0035] The polar monomer may be in the form of a liquid or a solution. If the polar monomer itself is a liquid at ambient temperature, the polar monomer itself may be used; in other cases, the polar monomer may be dissolved in a solvent to obtain a solution for use. The solvent may be selected from an organic solvent, such as at least one of an alcohol, a ketone, an ester, and water, preferably acetone or ethanol.

[0036] The solid polypropylene resin used as the graft base can be used in the form of powder, pellets or products.

[0037] Specifically, the method may include the following steps:

[0038] 1) Fully mixing the polar monomer and the solid polypropylene resin;

[0039] 2) subjecting the mixture obtained in step 1) to microwave irradiation, preferably under an inert gas atmosphere.

[0040] In step 1), the polar monomer and the solid polypropylene resin can be fully mixed under vacuum conditions. For example, the solid polypropylene resin can be fully mixed with the polar monomer solution under vacuum conditions. Vacuum is conducive to more complete mixing of the polar monomer and the polypropylene resin, especially for polypropylene resin with pores, which promotes the grafting monomer to enter the pores of the polypropylene resin, which is more conducive to the grafting reaction.

[0041] The inert gas in step 2) can be selected from one or more of nitrogen, helium and argon.

[0042] If the polar monomer is in the form of a solution dissolved in a solvent, the mixture obtained in step 1) is dried to remove the solvent before step 2).

[0043] If necessary, the irradiated mixture obtained in step 2) is washed to remove unreacted polar monomers and dried. The solvent used for washing can be selected from organic solvents, such as alcohols, ketones, esters, and at least one of water, preferably water.

[0044] More specifically, the method of the present invention may include the following steps:

[0045] 1') dissolving a polar monomer in a solvent to obtain a polar monomer solution;

[0046] 1) fully mixing the solid polypropylene resin with the polar monomer solution obtained in step 1'), and then drying it;

[0047] 2) subjecting the mixture obtained in step 1) to microwave irradiation, preferably under an inert gas atmosphere;

[0048] 3) The irradiated mixture obtained in step 2) is washed with a solvent to remove unreacted polar monomers and dried to obtain a polar monomer grafted polypropylene resin. The solvents in the above steps 1') and 3) can be selected from at least one of water and an organic solvent, and the two can be the same or different from each other.

[0049] The amount of solvent used in the above step 1') is sufficient as long as it can dissolve the polar monomer to form a solution. Preferably, the amount of the obtained polar monomer solution can be enough to completely immerse the solid polypropylene resin as the raw material, so as to facilitate the full mixing of the two. Usually, the weight ratio of the polar monomer to the solvent can be in the range of (0.1-100):100, preferably (0.5-50):100, and more preferably (1-30):100.

[0050] Furthermore, the method of the present invention may further include step 4) based on the above steps:

[0051] The product obtained in step 3) is subjected to melt extrusion granulation with optional addition of additives to obtain pellets of grafted polypropylene resin.

[0052] In the method according to the present invention, the solid polypropylene resin used as the raw material preferably does not contain an antioxidant. The solid polypropylene resin described in step 1) is preferably a polypropylene resin without adding an antioxidant, such as a powder. Usually, the polypropylene resin raw materials in the prior art contain a certain antioxidant, and the antioxidant is added when the polypropylene powder obtained after the polymerization reaction is melt-extruded and granulated. The solid polypropylene resin or powder of the present invention is preferably a solid polypropylene resin or powder obtained by polymerization and not yet melt-extruded and granulated, and the solid resin or powder at this time does not contain an antioxidant. Antioxidants easily consume free radicals in the subsequent grafting modification, so the use of polypropylene resin without adding an antioxidant achieves a better grafting effect.

[0053] The solid polypropylene resin used in the method according to the present invention can be various types of solid polypropylene resins or powders commonly used in the prior art, such as at least one of homopolymer polypropylene, random copolymer polypropylene, and impact copolymer polypropylene.

[0054] The polymerization process of the solid polypropylene resin of the present invention is known in the prior art. The solid polypropylene resin of the present invention is preferably a polypropylene powder obtained by polymerization using a spherical catalyst. The particles of the polypropylene powder obtained by polymerization using a spherical catalyst are spherical and have many pores on the particle surface. Therefore, the polypropylene powder has a large specific surface area and a large area in contact with the polar monomer, which helps to obtain a grafted product with a higher grafting rate.

[0055] When the polypropylene resin of the present invention is a random copolymer polypropylene, the comonomer of the random copolymer polypropylene contains at least one of ethylene or α-olefin comonomers other than propylene; preferably ethylene, C4α-olefin, C5α-olefin, C6α-olefin to C8α-olefin, more preferably ethylene, 1-butene, 1-heptene, 1-hexene and 1-octene, more preferably ethylene and C4α-olefin, more preferably ethylene and 1-butene, most preferably ethylene. The comonomer may contain a mixture of the above-mentioned ethylene and / or α-olefin comonomers other than propylene, preferably only ethylene or one α-olefin monomer; in the most preferred embodiment, the random copolymer polypropylene contains only propylene and ethylene.

[0056] When the solid polypropylene resin of the present invention is an impact copolymer polypropylene, the impact copolymer polypropylene contains a rubber phase in addition to a propylene homopolymer. The rubber phase is polymerized from propylene and a comonomer, and the comonomer is at least one of ethylene or an α-olefin other than propylene; preferably ethylene, C4α-olefin, C5α-olefin, C6α-olefin to C8α-olefin, more preferably ethylene, 1-butene, 1-heptene, 1-hexene and 1-octene, even more preferably ethylene and C4α-olefin, even more preferably ethylene and 1-butene, and most preferably ethylene. The rubber phase of the impact copolymer polypropylene is preferably polymerized from propylene and ethylene or an α-olefin other than propylene; in the most preferred embodiment, the rubber phase contains only a copolymer of propylene and ethylene.

[0057] The polar monomers that can be used in step 1) are as described above.

[0058] In step 1), various mixing methods known in the prior art can be used to fully mix the polar monomer and the solid polypropylene resin, preferably using a common stirring method and stirring equipment. The stirring equipment can be a conventional stirring device such as a magnetic stirring device or a mechanical stirring device.

[0059] The drying in step 1) above can be carried out by various conventional drying methods known in the prior art, including but not limited to forced air drying, room temperature drying, etc. The preferred drying temperature is a temperature that does not cause the polypropylene to melt, for example, not exceeding 160°C.

[0060] The irradiation power of the microwave irradiation in step 2) can be 100w-2000w, preferably 500-1000w, more preferably 600w-800w; the irradiation time can be 1s-120min, preferably 1min-30min, more preferably 3min-10min. The microwave irradiation can be carried out in various microwave reactors available in the prior art.

[0061] The inert gas in step 2) may include one or more of nitrogen, helium, and argon, preferably nitrogen.

[0062] The solvent in step 3) may include at least one of alcohol, ketone, ester and water, preferably water.

[0063] There is no special limitation on the washing of the irradiated mixture in step 3), and the residual polar monomers (such as organic acids) can be removed, and the usual washing method can be used. For example, immediately after microwave irradiation, the solid polypropylene resin is soaked in a solvent with a volume exceeding that of the solid polypropylene resin for a certain period of time (such as 5-15 minutes) at high temperature, and then the excess solvent or water is removed using a filtering device; the soaking and filtering are repeated for multiple times (such as 2-6 times) to obtain a clean solid polypropylene resin. Step 3) Drying is the same as step 1), and various conventional drying methods in the prior art can be used, including but not limited to forced air drying, room temperature drying, etc. The preferred drying temperature is a temperature that does not cause the polypropylene to melt, for example, not exceeding 160°C.

[0064] In step 4), the melt extrusion granulation is carried out by using a conventional melt extrusion device in plastic processing to melt-extrude the polar monomer grafted polypropylene resin through a conventional melt extrusion device to obtain pellets of the polar monomer grafted polypropylene resin. The additives that can be used are additives commonly used in the field of rubber and plastic processing, such as antioxidants, plasticizers, lubricants, release agents (calcium stearate), etc.

[0065] During the preparation process, the blending temperature of the materials is the usual processing temperature of the polypropylene resin, and is selected within a range that ensures that the polypropylene resin is completely melted but does not decompose. In addition, according to processing requirements, commonly used additives for polypropylene, such as antioxidants, plasticizers, etc., can be added to the polar monomer grafted polypropylene resin in usual amounts.

[0066] Preparation method of organic acid salt grafted polypropylene resin

[0067] In order to prepare the polypropylene resin grafted with an organic acid salt, an organic acid or its derivative (e.g., anhydride or ester) can be subjected to a grafting reaction with a solid polypropylene resin (e.g., powder) using microwave irradiation to obtain a grafted product, and then the grafted product is reacted with an alkali (e.g., hydroxide). The term "organic acid grafted polypropylene" or "organic acid grafted solid polypropylene resin" herein includes polypropylene or solid polypropylene resin grafted with an organic acid or its anhydride or ester.

[0068] Preferably, the organic acid grafted polypropylene powder is fully mixed with an aqueous alkali solution under vacuum for reaction, and optionally washed with a solvent to remove unreacted alkali and dried to obtain an organic acid salt grafted polypropylene resin.

[0069] The base can be a hydroxide, preferably selected from ammonia water and metal hydroxides, such as sodium hydroxide, potassium hydroxide, barium hydroxide, lithium hydroxide, strontium hydroxide, calcium hydroxide, ferric hydroxide, ferrous hydroxide, zinc hydroxide, magnesium hydroxide, cobalt hydroxide, gold hydroxide, aluminum hydroxide, copper hydroxide, beryllium hydroxide, rare earth hydroxides, preferably selected from sodium hydroxide, potassium hydroxide, barium hydroxide, lithium hydroxide, strontium hydroxide, calcium hydroxide, and combinations thereof.

[0070] Specifically, the preparation method of organic acid salt grafted polypropylene resin may include the following steps:

[0071] 1') dissolving an organic acid or its derivative monomer in a solvent to obtain an organic acid or its derivative monomer solution; dissolving a base (such as a hydroxide) in a solvent (such as water) to obtain a base solution (preferably an aqueous solution);

[0072] 1) fully mixing a solid polypropylene resin (such as powder) with the organic acid or its derivative monomer solution obtained in step 1'), and then drying the mixture;

[0073] 2) subjecting the mixture obtained in step 1) to microwave irradiation, preferably under an inert gas atmosphere;

[0074] 3) washing the irradiated mixture obtained in step 2) with a solvent to remove unreacted organic acid or its derivative monomers and drying the mixture to obtain an organic acid grafted solid polypropylene resin;

[0075] 4) fully mixing the organic acid grafted solid polypropylene resin obtained in step 3) with the alkaline solution prepared in step 1') under vacuum to react;

[0076] 5) The reaction mixture obtained in step 4) is washed with a solvent to remove the alkali that has not reacted with the organic acid grafted solid polypropylene resin and dried to obtain an organic acid salt grafted solid polypropylene resin.

[0077] The solvent mentioned above is at least one of water and an organic solvent, and at least two of the solvents in step 1'), step 3) and step 5) are the same or different.

[0078] The hydroxide in step 1') may be ammonia water or a metal hydroxide, preferably one or more of sodium hydroxide, potassium hydroxide, barium hydroxide, lithium hydroxide, strontium hydroxide, calcium hydroxide, ferric hydroxide, ferrous hydroxide, zinc hydroxide, magnesium hydroxide, cobalt hydroxide, gold hydroxide, aluminum hydroxide, copper hydroxide, beryllium hydroxide, and rare earth hydroxides, more preferably sodium hydroxide, potassium hydroxide, barium hydroxide, lithium hydroxide, strontium hydroxide, and calcium hydroxide, and most preferably sodium hydroxide, potassium hydroxide, and calcium hydroxide. Sodium hydroxide is most preferred.

[0079] The amount of the solvent for the organic acid or its derivative monomer in step 1') is the same as that described above for the solvent for the polar monomer.

[0080] The amount of solvent (preferably water) used to dissolve the alkali in step 1') is also sufficient as long as it can dissolve the alkali, such as hydroxide, to form a solution. Preferably, the amount of the obtained alkali solution can completely immerse the organic acid-grafted solid polypropylene resin, which is more convenient for the full mixing and reaction of the two. Generally, the weight ratio of the solvent (preferably water) to the alkali (such as hydroxide) can be (0.1-100):100, preferably (0.5-50):100, and more preferably (1-30):100. The amount of the alkali (such as hydroxide) can be 0.1-10% by weight based on the weight of the raw material polypropylene resin used; preferably 1-8% by weight.

[0081] In this method, the drying treatment in step 1), step 3) and step 5) can adopt various conventional drying methods in the prior art, including but not limited to forced air drying, room temperature drying, etc. The preferred drying temperature is a temperature that does not cause the polypropylene to melt, for example, not exceeding 160°C.

[0082] In step 4), various mixing methods in the prior art can be used to fully mix the organic acid grafted solid polypropylene resin and the alkaline solution, preferably using a common stirring method and stirring equipment. The stirring equipment can be a conventional stirring device such as a magnetic stirring device or a mechanical stirring device.

[0083] In step 4), the alkaline solution and the organic acid grafted solid polypropylene resin are fully mixed and reacted simultaneously. There is no special requirement for the reaction time, and the reaction time is sufficient. Generally, after the addition of the alkaline solution is completed, further mixing and reacting for a period of time is sufficient, for example, 1-20 minutes, preferably 2-8 minutes. The reaction temperature and pressure are not limited, and are generally normal temperature and pressure.

[0084] The solvent in step 5) is the same as or different from the solvent in step 3), and includes at least one of alcohol, ketone, ester, and water, preferably water. There is no special limitation on the cleaning of the reaction mixture after the mixed reaction in step 5), and the residual alkali can be removed, and a common cleaning method can be used. For example, after microwave irradiation, immediately use the solvent with a volume exceeding that of the solid polypropylene resin (such as polypropylene powder) to soak for a certain time (such as 5-15 minutes) at high temperature, and then use a filtering device to remove excess solvent or water; repeat soaking and filtering for multiple times (such as 2-6 times) to obtain a clean solid polypropylene resin.

[0085] The method preferably further comprises: melt extrusion granulation of the powder obtained in the above step 5) with optional addition of additives to obtain pellets of organic acid salt grafted polypropylene resin. Here, melt extrusion granulation is to use a common melt extrusion equipment in plastic processing to melt extrusion granulate the organic acid salt grafted polypropylene powder through a conventional melt extrusion equipment to obtain organic acid salt grafted polypropylene resin pellets. The additives that can be used are additives commonly used in the field of rubber and plastic processing, such as antioxidants, plasticizers, lubricants, release agents (calcium stearate), etc.

[0086] During the preparation process, the blending temperature of the materials is the usual processing temperature of the polypropylene resin, and is selected within a range that ensures that the polypropylene resin is completely melted but does not decompose. In addition, according to processing requirements, commonly used additives for polypropylene, such as antioxidants, plasticizers, etc., can be added to the organic acid salt grafted polypropylene powder in usual amounts.

[0087] Preparation method using inorganic microwave absorbing medium

[0088] In one embodiment of the preparation method according to the present invention, an inorganic microwave absorbing medium may be used.

[0089] The inorganic microwave absorbing medium may be added before microwave irradiation. The amount of the inorganic microwave absorbing medium may be 0.1-10% by weight based on the weight of the solid polypropylene resin; preferably 1-8% by weight.

[0090] The inorganic microwave absorbing medium can be various inorganic substances that can absorb microwaves in the prior art. For example, the inorganic microwave absorbing medium can be selected from metal hydroxides, preferably potassium hydroxide, barium hydroxide, sodium hydroxide, lithium hydroxide, strontium hydroxide, calcium hydroxide, ferric hydroxide, ferrous hydroxide, zinc hydroxide, magnesium hydroxide, cobalt hydroxide, gold hydroxide, aluminum hydroxide, copper hydroxide, beryllium hydroxide, and rare earth hydroxides; metal salts, preferably ammonium nitrate, potassium nitrate, sodium nitrate, barium nitrate, calcium nitrate, magnesium nitrate, aluminum nitrate, manganese nitrate, zinc nitrate, ferric nitrate, ferrous nitrate, copper nitrate, silver nitrate, ammonium chloride, potassium chloride, sodium chloride, barium chloride, calcium chloride, magnesium chloride, aluminum chloride, manganese chloride, chloride zinc chloride, ferric chloride, ferrous chloride, cupric chloride, ammonium sulfate, potassium sulfate, sodium sulfate, calcium sulfate, magnesium sulfate, aluminum sulfate, manganese sulfate, zinc sulfate, ferric sulfate, ferrous sulfate, cupric sulfate, silver sulfate, ammonium carbonate, potassium carbonate, sodium carbonate, magnesium carbonate, calcium carbonate, barium carbonate, potassium dihydrogen phosphate, barium titanate, strontium titanate, calcium copper titanate; metal oxides, preferably ferric oxide and ferroferric oxide; graphite materials, preferably carbon black, graphite powder, graphene oxide and its reduction products (reducing agent such as ascorbic acid), graphene, carbon nanotubes, activated carbon; ferroelectric materials; electrolytic stone; chalcopyrite; and combinations thereof.

[0091] The polar monomer (optionally dissolved in a solvent), the inorganic microwave absorbing medium (optionally dissolved or dispersed in a solvent) and the solid polypropylene resin may be fully mixed before microwave irradiation. Two of the polar monomer, the inorganic microwave absorbing medium and the solid polypropylene resin may be mixed first, and then mixed with the other, or the three may be mixed together. The mixing process is preferably carried out under vacuum conditions.

[0092] The mixing process can be carried out by various mixing methods commonly used in the prior art, using common stirring methods and stirring equipment, such as mechanical stirring mixing, centrifugal mixing, magnetic stirring mixing, etc., so that the polar monomer is fully dissolved in the solvent, the microwave absorbing medium can be fully and stably dissolved or dispersed in the solvent, and the mixed substances are fully mixed.

[0093] In one embodiment, the polypropylene resin is first mixed with a polar monomer optionally dissolved in a solvent, and the resulting mixture is then mixed with an inorganic microwave absorbing medium optionally dissolved or dispersed in the solvent.

[0094] The solvent for dissolving the polar monomers may be the same as or different from the solvent for dissolving or dispersing the inorganic microwave absorbing medium, and is preferably selected from water and an organic solvent (e.g., alcohol, ketone, ester). The solvent for dissolving the polar monomers may be selected from at least one of alcohol, ketone, ester, and water, preferably acetone or ethanol. The solvent for dissolving or dispersing the inorganic microwave absorbing medium may be selected from at least one of alcohol, ketone, ester, and water, preferably water.

[0095] The amount of solvent used to dissolve or disperse the microwave absorbing medium is sufficient as long as it can dissolve the microwave absorbing medium to form a microwave absorbing medium solution, or can make the microwave absorbing medium fully and evenly dispersed. Preferably, the amount of the obtained microwave absorbing medium solution or dispersion can completely immerse the mixture of the polar monomer and the polypropylene resin, which is more convenient for the full mixing and reaction of the three. Generally, the weight ratio of the solvent to the microwave absorbing medium in the microwave absorbing medium solution or dispersion can be (0.1-100):100, preferably (0.5-50):100, and more preferably (1-30):100.

[0096] In order to ensure that the microwave absorbing medium can form a fully dispersed and stable dispersion with the solvent, a conventional surfactant in the prior art can be added to the microwave absorbing medium dispersion. Generally, a surfactant of polyoxyethylene type or polyol type can be selected, and the amount used is usually 0.1-100% by weight of the inorganic microwave absorbing medium.

[0097] Preferably, a drying treatment may be performed after the above mixing to remove the solvent in the mixture before microwave irradiation. The microwave absorbing medium may be removed by washing with a solvent after irradiation grafting. The washing solvent is selected from at least one of water and an organic solvent, preferably at least one of alcohol, ketone, ester and water, preferably water.

[0098] Further products and applications

[0099] In a third aspect of the present invention, the present invention also provides pellets or products, which are obtained by melt extrusion granulation or further molding process with the optional addition of additives according to the grafted polypropylene resin of the present invention. Available additives are additives commonly used in the field of rubber and plastic processing, such as antioxidants, plasticizers, lubricants, release agents (calcium stearate), etc.

[0100] In a fourth aspect of the present invention, the present invention provides a composite material, a coatable film material and an adhesive material, which can be obtained by blending the grafted polypropylene resin of the present invention with other polymers. The composite material is, for example, an inorganic-filled polyolefin composite material and a glass fiber-reinforced polyolefin composite material.

[0101] In the fifth aspect of the present invention, the present invention also provides use of the grafted polypropylene resin of the present invention for modifying plastics.

[0102] The polar monomer grafted polypropylene resin of the present invention can be widely used in plastic modification, including but not limited to blending the polar monomer grafted polypropylene resin (granules or powders) with other polymers to prepare composite materials, coatable film materials and adhesive materials. Specifically, the polar monomer grafted polypropylene resin of the present invention can be used as a compatibilizer when polypropylene is blended with other polymers in plastic modification; for example, in inorganic-filled polyolefin composite materials, glass fiber-reinforced polyolefin composite materials, coatable film materials and adhesive materials, the interface interaction between inorganic materials or other components and polypropylene resin is improved, so that the obtained material has excellent comprehensive performance and can be applied to the fields of automobiles, tools and construction engineering.

[0103] The present invention utilizes the characteristic of microwave selective heating, and uses microwave irradiation to graft polar monomers with solid polypropylene resin without adding initiator, so as to prepare polar monomer grafted polypropylene resin without initiator residue and without significantly reducing molecular weight. Without being bound by any theory, the applicant believes that solid polypropylene resin (such as powder) is microwave transparent in a microwave environment (little or no microwave absorption under microwave irradiation, so no heat is generated under microwave irradiation), and the polar monomer used in the present invention can absorb microwaves so that its temperature in the microwave field is increased to above 200°C, such temperature increase can cause tertiary carbon atoms in the polypropylene molecular chain near the polar monomer to dehydrogenate, thereby generating free radicals, and such free radicals further trigger the reaction of polar monomers, thereby grafting onto the polypropylene chain; the increased temperature is near the melting point of polypropylene, which will not cause chain scission of polypropylene, so that grafting reaction will occur but chain scission reaction of polypropylene will not be caused; such microwave grafting reaction can greatly avoid the β-chain scission reaction of polypropylene during melt grafting, does not reduce the molecular weight of polypropylene, and maintains excellent mechanical properties of the product. Since no initiator is added in the method of the present invention, the obtained grafted polypropylene resin will not contain any initiator residue, thereby avoiding the adverse effects of the initiator residue on product performance and subsequent processing; in addition, a large number of β-chain scission reactions of polypropylene caused by adding an initiator and the resulting increase in the polypropylene melt index and corresponding decrease in molecular weight are avoided, and the competition between the grafting reaction and the self-polymerization reaction that may occur when an initiator is added is avoided, thereby improving the grafting rate.

[0104] In the case of organic acid grafted polypropylene, further reacting it with a base (such as metal hydroxide) can convert the organic acid grafted polypropylene into organic acid salt grafted polypropylene, which will further increase the polarity of the grafted polypropylene.

[0105] In the preferred case of adding a microwave absorbing medium, the grafting rate of the polar monomer can be increased. Due to the selective heating of microwaves, the inorganic microwave absorbing medium is heated, so that it heats up in the microwave environment, and then the temperature of the polar monomer near it is quickly increased to above 200°C, thereby more effectively initiating the grafting reaction without causing a chain breaking reaction, so that an efficient grafting reaction can be achieved in a short time and polar polypropylene with a high grafting rate can be obtained.

[0106] In addition, since no auxiliary grafting monomer is added in the preferred case and unreacted polar monomers and alkali (such as hydroxide) can be fully removed, a highly polar grafted polypropylene with no significant decrease in molecular weight, no residual monomers, no initiator residues, and no color or odor can be obtained.

[0107] The invention has simple preparation process, easy operation, simple production equipment, low cost and easy industrialization. BRIEF DESCRIPTION OF THE DRAWINGS

[0108] Figure 1 The infrared spectra of the maleic anhydride grafted polypropylene samples prepared in Examples 1 and 2 of the present invention are shown. Curve a is the curve of pure polypropylene powder, curve b is the curve of maleic anhydride grafted polypropylene obtained after microwave irradiation for 3 minutes in Example 1, and curve c is the curve of maleic anhydride grafted polypropylene obtained after microwave irradiation for 5 minutes in Example 2.

[0109] For the organic acid grafted polypropylene, the monomer is grafted onto the polypropylene molecular chain in the form of anhydride. After washing with water, part of the anhydride group opens to become acid, while part of it remains anhydride. Figure 1 It can be seen that the grafted polypropylene samples all have anhydride groups and carboxylic acid groups, and the extension of microwave time is helpful to improve the grafting rate.

[0110] Figure 2 The infrared spectra of the organic acid salt grafted polypropylene samples prepared in Examples S1 and S2 of the present invention are shown, wherein curve a is the curve of pure polypropylene powder, curve b is the curve of the organic acid salt grafted polypropylene obtained after microwave irradiation for 3 minutes in Example S1, and curve c is the curve of the organic acid salt grafted polypropylene obtained after microwave irradiation for 5 minutes in Example S2.

[0111] For the organic acid salt grafted polypropylene, there is only one acid salt peak. This is because the anhydride or acid grafted on the polypropylene molecular chain is salified and can become an acid salt peak. Figure 2 It can be seen from the infrared spectrum that the grafted polypropylene samples after grafting and reaction with hydroxide all have carboxylic acid groups, and the extension of microwave time is helpful to improve the grafting rate. DETAILED DESCRIPTION

[0112] The present invention is further described below in conjunction with the embodiments. However, the scope of the present invention is not intended to be limited by these embodiments, but the scope of the present invention is set forth in the appended claims.

[0113] The experimental data in the embodiments and comparative examples were measured using the following instruments and methods:

[0114] (1) The melt index of the resin in the examples and comparative examples was measured with reference to the standard GB / T3682-2000.

[0115] (2) The water contact angle measuring instrument in the embodiments and comparative examples is: German EASYDROP contact angle tester.

[0116] The preparation method of the resin contact angle measurement sample is as follows: dissolve 4g of resin in 40ml of xylene (analytical grade AR), and fully dissolve the resin in xylene at 120°C; then pour the xylene solution of the resin into a 100mm diameter watch glass to make a film, and place the watch glass in a 110°C oven to fully evaporate the solvent to obtain a resin film sample; then wash the resin film sample in ethanol and dry it to obtain the resin contact angle measurement sample. The sample will produce phase separation after the solution method film making process, and the dispersed phase is one side containing polar monomers (organic acids or organic acid salts), and the other side is only polypropylene. The water contact angle of the obtained contact angle measurement sample containing the side group of the polar monomer is measured using the above-mentioned water contact angle measuring instrument.

[0117] (3) The grafting rate of the polar monomer (organic acid or organic acid salt) in the examples and comparative examples was characterized by infrared spectroscopy as follows:

[0118] First, a standard curve was established. The mixed samples of high temperature resistant dodecenyl succinic anhydride (DDSA) and pure polypropylene resin in different proportions were used as standard samples to determine the anhydride carbonyl group (C=O group) in dodecenyl succinic anhydride at 1818-1755 cm -1 (The peak position is about 1782cm -1 ) has an infrared absorption peak area similar to the internal standard peak of polypropylene at 484-435 cm -1 (The peak position is about 460cm -1 )'s absorption area, and by plotting the ratio of the two against the content of maleic anhydride, a standard curve of the maleic anhydride grafting rate in grafted polypropylene can be obtained.

[0119] The specific test process of the grafting rate of the grafted sample is:

[0120] A. For the microwave grafted samples used in the examples and comparative examples, since deionized water has been used to fully remove the unreacted MAH monomer after the grafting is completed, the samples only need to be pressed on a flat vulcanizer (temperature 200°C) into a transparent film with a thickness of about 100 μm, and then the characteristic absorption peak is measured using an infrared spectrometer (model Nicolet iS 50, Nicolet Corporation), and then the grafting rate is calculated using the above standard curve.

[0121] B. The sample grafted by the melt method in the comparative example is tested as follows: weigh about 1g of the grafted polypropylene sample obtained in the comparative example, put it into 20ml of xylene, heat it to completely dissolve, and immediately pour it into 150ml of acetone. The unreacted small molecules and the monomers not grafted on the polypropylene molecules are dissolved in acetone, and the precipitated white floccules are pure grafted products. Filter it, dry it, and then press it into a transparent film with a thickness of about 100μm on a flat vulcanizer (temperature 200℃), measure the characteristic absorption peak with an infrared spectrometer, and then calculate the grafting rate through the above standard curve. The grafting rate of the organic acid salt grafted polypropylene of the present invention can be equivalent to the grafting rate of the organic acid grafted polypropylene obtained in the organic acid grafted polypropylene step.

[0122] (4) The microwave reactor used was: SINEO (Xinyi) multifunctional microwave synthesis extraction instrument, model: UWave-2000.

[0123] The raw materials and their manufacturers used in the embodiments and comparative examples are as follows:

[0124] Homopolymer polypropylene powder (Zhenhai Refining and Chemical M60, MI=60g / 10min, obtained by polymerization using a spherical catalyst), random copolymer polypropylene powder (Zhenhai Refining and Chemical M60ET, MI=60g / 10min, obtained by polymerization using a spherical catalyst), impact copolymer polypropylene powder (Zhenhai Refining and Chemical M30RH, MI=30g / 10min, obtained by polymerization using a spherical catalyst), maleic anhydride (Xilong Science Co., Ltd.), acrylic acid (Sinopharm Chemical Reagent Co., Ltd.), methacrylic acid (Sinopharm Chemical Reagent Co., Ltd.), sodium chloride (Sinopharm Chemical Reagent Co., Ltd.), graphene oxide (Nanjing Jicang Nanotechnology Co., Ltd.), ascorbic acid (B&K Company), (sodium hydroxide (Xilong Science Co., Ltd.), potassium hydroxide (Xilong Science Co., Ltd.), calcium hydroxide (Xilong Science Co., Ltd.), acetone (Xilong Science Co., Ltd.), diisopropylbenzene peroxide (Tianjin Guangfu Fine Chemical Research Institute), antioxidant 1010 (BASF), antioxidant 168 (BASF), calcium stearate (Tianjin Jinke Fine Chemical Research Institute).

[0125] Embodiment 1:

[0126] Based on 100 parts by mass of homopolymerized polypropylene powder, maleic anhydride (5 parts by mass) is dissolved in acetone (50 parts by mass) to obtain a maleic anhydride acetone solution; the maleic anhydride acetone solution is added to the polypropylene powder under vacuum and mechanical stirring to fully mix, and then the mixture is dried (dried in a forced air drying oven at 80°C). The dried polypropylene / maleic anhydride mixture powder is irradiated with microwaves (power 700W) for 3 minutes under a nitrogen atmosphere; the powder after microwave irradiation is soaked in deionized water for 10 minutes and the deionized water is replaced and repeated 3 times to ensure that the maleic anhydride monomer that does not participate in the grafting reaction is removed, and then the powder is placed in a forced air drying oven at 80°C for drying. Finally, the powder was melt-extruded and granulated with 0.1 parts by mass (based on 100 parts by mass of homopolymer polypropylene powder) of antioxidant 1010, 0.1 parts by mass of antioxidant 168 and 0.1 parts by mass of calcium stearate in a twin-screw extruder. The temperature of the feeding section of the extruder was 190-200°C, the temperature of the mixing section was 200-210°C, and the temperature of the die was 190-200°C. After extrusion granulation, the melt index, contact angle and grafting rate were tested. The test results are shown in Table 1.

[0127] Embodiment 1 ':

[0128] Based on 100 parts by mass of homopolymerized polypropylene powder, maleic anhydride (5 parts by mass) is dissolved in acetone (50 parts by mass) to obtain a maleic anhydride acetone solution; sodium chloride (3 parts by mass) is dissolved in deionized water (50 parts by mass) to obtain a sodium chloride aqueous solution; the maleic anhydride acetone solution is added to the polypropylene powder under vacuum and mechanical stirring to fully mix, and then the mixture is dried (dried in a blast drying oven at 80°C). The dried polypropylene / maleic anhydride mixture powder is fully mixed with the sodium chloride aqueous solution, and then the mixture is dried (dried in a blast drying oven at 80°C); the dried polypropylene / maleic anhydride / sodium chloride mixture powder is irradiated with microwaves (power 700W) for 2 minutes under a nitrogen atmosphere; the powder after microwave irradiation is soaked in deionized water for 10 minutes and the deionized water is replaced and repeated 3 times to ensure that the maleic anhydride monomer and sodium chloride that are not involved in the grafting reaction are removed, and then the powder is placed in a blast drying oven at 80°C for drying. Finally, the powder was melt-extruded and granulated with 0.1 parts by mass (based on 100 parts by mass of homopolymer polypropylene powder) of antioxidant 1010, 0.1 parts by mass of antioxidant 168 and 0.1 parts by mass of calcium stearate in a twin-screw extruder. The temperature of the feeding section of the extruder was 190-200°C, the temperature of the mixing section was 200-210°C, and the temperature of the die was 190-200°C. After extrusion granulation, the melt index, contact angle and grafting rate were tested. The test results are shown in Table 1.

[0129] Example 1

[0130] Except that the dried polypropylene / maleic anhydride / sodium chloride mixture powder was irradiated with microwave (power 700 W) for 3 min under nitrogen atmosphere, the rest was the same as Example 1'. The samples were tested for melt index, contact angle and grafting rate. The test results are shown in Table 1.

[0131] Comparative Example 1:

[0132] Based on 100 parts by mass of homopolymerized polypropylene powder (same as in Example 1), maleic anhydride (5 parts by mass) and dicumyl peroxide (0.005 parts by mass) were dissolved in acetone (50 parts by mass) to obtain a maleic anhydride acetone solution; the maleic anhydride acetone solution was added to the polypropylene powder under vacuum accompanied by mechanical stirring and fully mixed, and then the mixture was dried (dried in a forced air drying oven at 80 degrees Celsius). The powder of the dried polypropylene / maleic anhydride mixture was irradiated with microwave (power 700 W) for 3 min under a nitrogen atmosphere; the powder after microwave irradiation was soaked in deionized water for 10 minutes and the deionized water was replaced and repeated 3 times to ensure that the maleic anhydride monomer not involved in the grafting reaction was removed, and then the powder was placed in an 80°C forced air drying oven for drying; finally, the powder was melt-extruded and granulated with 0.1 parts by mass of antioxidant 1010, 0.1 parts by mass of antioxidant 168 and 0.1 parts by mass of calcium stearate in a twin-screw extruder, the extruder feeding section temperature was 190-200°C, the mixing section temperature was 200-210°C, and the head temperature was 190-200°C. After extrusion granulation, the melt index, contact angle and grafting rate were tested. The test results are shown in Table 1.

[0133] Embodiment 2:

[0134] Except that the dried polypropylene / maleic anhydride mixture powder was irradiated with microwave (power 700 W) for 5 min under nitrogen atmosphere, the rest was the same as Example 1. The samples were tested for melt index, contact angle and grafting rate. The test results are shown in Table 1.

[0135] Comparative Example 2:

[0136] Except that the dried polypropylene / maleic anhydride mixture powder was irradiated with microwave (power 700 W) for 5 min under nitrogen atmosphere, the rest was the same as comparative example 1. The samples were tested for melt index, contact angle and grafting rate. The test results are shown in Table 1.

[0137] Embodiment 3:

[0138] Except that the dried polypropylene / maleic anhydride mixture powder was irradiated with microwave (power 700 W) for 7 min under nitrogen atmosphere, the rest was the same as Example 1. The samples were tested for melt index, contact angle and grafting rate. The test results are shown in Table 1.

[0139] Comparative Example 3:

[0140] Except that the dried polypropylene / maleic anhydride mixture powder was irradiated with microwave (power 700 W) for 7 min under nitrogen atmosphere, the rest was the same as comparative example 1. The samples were tested for melt index, contact angle and grafting rate. The test results are shown in Table 1.

[0141] Embodiment 4:

[0142] Except that the dried polypropylene / maleic anhydride mixture powder was irradiated with microwave (power 700 W) for 10 min under nitrogen atmosphere, the rest was the same as Example 1. The samples were tested for melt index, contact angle and grafting rate. The test results are shown in Table 1.

[0143] Comparative Example 4:

[0144] Except that the dried polypropylene / maleic anhydride mixture powder was irradiated with microwave (power 700 W) for 10 min under nitrogen atmosphere, the rest was the same as comparative example 1. The samples were tested for melt index, contact angle and grafting rate. The test results are shown in Table 1.

[0145] Comparative Example 5:

[0146] According to 100 parts by mass of homopolymerized polypropylene powder (same as in Example 1), dicumyl peroxide (0.005 parts by mass) was dissolved in acetone (20 parts by mass) to obtain an initiator solution; maleic anhydride (5 parts by mass) and polypropylene powder were solid-phase dry mixed in a metal cup using a stirring paddle, and the dissolved peroxide initiator solution was added during the mixing process. Finally, the mixed reactants were melt-extruded and granulated with 0.1 parts by mass of antioxidant 1010, 0.1 parts by mass of antioxidant 168 and 0.1 parts by mass of calcium stearate in a twin-screw extruder, the extruder feeding section temperature was 190-200°C, the mixing section temperature was 200-210°C, and the head temperature was 190-200°C. After extrusion granulation, the melt index, contact angle and grafting rate were tested, and the test results are shown in Table 1.

[0147] Embodiment 5:

[0148] Except that maleic anhydride (1 part by mass) was dissolved in acetone (50 parts by mass) to obtain a maleic anhydride acetone solution, the powder of the dried polypropylene / maleic anhydride mixture was irradiated with microwave (power 700 W) for 7 min under a nitrogen atmosphere, and the rest was the same as in Example 1. The samples were tested for melt index, contact angle and grafting rate, and the test results are shown in Table 1.

[0149] Comparative Example 6:

[0150] Except that maleic anhydride (1 part by mass) was dissolved in acetone (50 parts by mass) to obtain a maleic anhydride acetone solution, the powder of the dried polypropylene / maleic anhydride mixture was irradiated with microwave (power 700 W) for 7 min under a nitrogen atmosphere, and the rest was the same as Comparative Example 1. The samples were tested for melt index, contact angle and grafting rate, and the test results are shown in Table 1.

[0151] Embodiment 6:

[0152] Except that maleic anhydride (8 parts by mass) was dissolved in acetone (50 parts by mass) to obtain a maleic anhydride acetone solution, and the powder of the dried polypropylene / maleic anhydride mixture was irradiated with microwave (power 700 W) for 7 min under a nitrogen atmosphere, the rest was the same as in Example 1. The samples were tested for melt index, contact angle and grafting rate, and the test results are shown in Table 1.

[0153] Comparative Example 7:

[0154] Except that maleic anhydride (8 parts by mass) was dissolved in acetone (50 parts by mass) to obtain a maleic anhydride acetone solution, the powder of the dried polypropylene / maleic anhydride mixture was irradiated with microwave (power 700 W) for 7 min under a nitrogen atmosphere, and the rest was the same as Comparative Example 1. The samples were tested for melt index, contact angle and grafting rate, and the test results are shown in Table 1.

[0155] Embodiment 7:

[0156] Except that maleic anhydride (10 parts by mass) was dissolved in acetone (50 parts by mass) to obtain a maleic anhydride acetone solution, the powder of the dried polypropylene / maleic anhydride mixture was irradiated with microwave (power 700 W) for 7 min under a nitrogen atmosphere, and the rest was the same as in Example 1. The samples were tested for melt index, contact angle and grafting rate, and the test results are shown in Table 1.

[0157] Comparative Example 8:

[0158] Except that maleic anhydride (10 parts by mass) was dissolved in acetone (50 parts by mass) to obtain a maleic anhydride acetone solution, the powder of the dried polypropylene / maleic anhydride mixture was irradiated with microwave (power 700 W) for 7 min under a nitrogen atmosphere, and the rest was the same as Comparative Example 1. The samples were tested for melt index, contact angle and grafting rate, and the test results are shown in Table 1.

[0159] Embodiment 8:

[0160] Except that acrylic acid (5 parts by mass) was dissolved in acetone (50 parts by mass) to obtain an acrylic acid acetone solution, and the powder of the dried polypropylene / acrylic acid mixture was irradiated with microwave (power 700 W) for 5 min under a nitrogen atmosphere, the rest was the same as in Example 1. The samples were tested for melt index, contact angle and grafting rate, and the test results are shown in Table 1.

[0161] Comparative Example 9:

[0162] Except that acrylic acid (5 parts by mass) was dissolved in acetone (50 parts by mass) to obtain an acrylic acid acetone solution, and the powder of the dried polypropylene / acrylic acid mixture was irradiated with microwave (power 700 W) for 5 min under a nitrogen atmosphere, the rest was the same as in Comparative Example 1. The samples were tested for melt index, contact angle and grafting rate, and the test results are shown in Table 1.

[0163] Embodiment 9:

[0164] Except that acrylic acid (5 parts by mass) was dissolved in acetone (50 parts by mass) to obtain an acrylic acid acetone solution, and the powder of the dried polypropylene / acrylic acid mixture was irradiated with microwave (power 700 W) for 7 min under a nitrogen atmosphere, the rest was the same as in Example 1. The samples were tested for melt index, contact angle and grafting rate, and the test results are shown in Table 1.

[0165] Comparative Example 10:

[0166] Except that acrylic acid (5 parts by mass) was dissolved in acetone (50 parts by mass) to obtain an acrylic acid acetone solution, and the powder of the dried polypropylene / acrylic acid mixture was irradiated with microwave (power 700 W) for 7 min under a nitrogen atmosphere, the rest was the same as in Comparative Example 1. The samples were tested for melt index, contact angle and grafting rate, and the test results are shown in Table 1.

[0167] Embodiment 10:

[0168] Except that methacrylic acid (5 parts by mass) was dissolved in acetone (50 parts by mass) to obtain a methacrylic acid acetone solution, and the powder of the dried polypropylene / methacrylic acid mixture was irradiated with microwave (power 700 W) for 5 min under a nitrogen atmosphere, the rest was the same as Example 1. The samples were tested for melt index, contact angle and grafting rate, and the test results are shown in Table 1.

[0169] Comparative Example 11:

[0170] Except that methacrylic acid (5 parts by mass) was dissolved in acetone (50 parts by mass) to obtain a methacrylic acid acetone solution, and the powder of the dried polypropylene / methacrylic acid mixture was irradiated with microwave (power 700 W) for 5 min under a nitrogen atmosphere, the rest was the same as in Comparative Example 1. The samples were tested for melt index, contact angle and grafting rate, and the test results are shown in Table 1.

[0171] Embodiment 11:

[0172] Except that the powder of the dried polypropylene / maleic anhydride mixture was irradiated with microwave (power 700 W) for 5 min under nitrogen atmosphere, the other procedures were the same as in Example 1. The samples were tested for melt index, contact angle and grafting rate, and the test results are shown in Table 1.

[0173] Embodiment 11 ':

[0174] Except that, based on 100 parts by mass of impact copolymer polypropylene powder, graphene oxide (0.5 parts by mass) and ascorbic acid (0.5 parts by mass) are dissolved in deionized water (50 parts by mass) to obtain a graphene oxide aqueous solution; the dried polypropylene / maleic anhydride mixture powder is fully mixed with the graphene oxide aqueous solution, and then the mixture is dried (dried in a forced air drying oven at 80°C); the dried polypropylene / maleic anhydride / graphene oxide mixture powder is irradiated with microwaves (power 700W) for 1 min under a nitrogen atmosphere, and the rest is the same as in Example 1. The samples were tested for melt index, contact angle and grafting rate, and the test results are shown in Table 1.

[0175] Example 11

[0176] Except that the dried polypropylene / maleic anhydride / graphene oxide mixture powder was irradiated with microwave (power 700 W) for 2 min under nitrogen atmosphere, the rest was the same as Example 11'. The samples were tested for melt index, contact angle and grafting rate. The test results are shown in Table 1.

[0177] Comparative Example 12:

[0178] Except that the powder of the dried polypropylene / maleic anhydride mixture was irradiated with microwave (power 700 W) for 5 min under nitrogen atmosphere, the other procedures were the same as those in Comparative Example 1. The samples were tested for melt index, contact angle and grafting rate, and the test results are shown in Table 1.

[0179] Embodiment 12:

[0180] Except that acrylic acid (5 parts by mass) is dissolved in acetone (50 parts by mass) to obtain an acrylic acid acetone solution based on 100 parts by mass of the impact copolymer polypropylene powder, and the dried polypropylene / acrylic acid mixture powder is irradiated with microwave (power 700 W) for 5 minutes under a nitrogen atmosphere, the rest is the same as Example 1. The samples were tested for melt index, contact angle and grafting rate, and the test results are shown in Table 1.

[0181] Comparative Example 13:

[0182] Except that acrylic acid (5 parts by mass) was dissolved in acetone (50 parts by mass) to obtain an acrylic acid acetone solution based on 100 parts by mass of the impact copolymer polypropylene powder, and the dried polypropylene / acrylic acid mixture powder was irradiated with microwave (power 700 W) for 5 minutes under a nitrogen atmosphere, the rest was the same as Comparative Example 1. The samples were tested for melt index, contact angle and grafting rate, and the test results are shown in Table 1.

[0183] Embodiment 13:

[0184] Except that the powder of the dried polypropylene / maleic anhydride mixture was irradiated with microwave (power 700 W) for 5 min under nitrogen atmosphere, the other conditions were the same as Example 1. The samples were tested for melt index, contact angle and grafting rate. The test results are shown in Table 1.

[0185] Comparative Example 14:

[0186] Except that the powder of the polypropylene / maleic anhydride mixture dried after drying was irradiated with microwave (power 700 W) for 5 min under nitrogen atmosphere, the rest was the same as Comparative Example 1. The samples were tested for melt index, contact angle and grafting rate, and the test results are shown in Table 1.

[0187] Embodiment 14:

[0188] The same procedures as in Example 1 were followed except that 100 parts by mass of the random copolymerized polypropylene powder was used to dissolve acrylic acid (5 parts by mass) in acetone (50 parts by mass) to obtain an acrylic acid acetone solution, and the dried polypropylene / acrylic acid mixture powder was irradiated with microwaves (power 700 W) for 5 min under a nitrogen atmosphere. The samples were tested for melt index, contact angle, and grafting rate, and the test results are shown in Table 1.

[0189] Comparative Example 15:

[0190] Except that acrylic acid (5 parts by mass) was dissolved in acetone (50 parts by mass) to obtain an acrylic acid acetone solution based on 100 parts by mass of the random copolymer polypropylene powder, and the dried polypropylene / acrylic acid mixture powder was irradiated with microwave (power 700 W) for 5 minutes under a nitrogen atmosphere, the rest was the same as Comparative Example 1. The samples were tested for melt index, contact angle and grafting rate, and the test results are shown in Table 1.

[0191] Table 1

[0192]

[0193] As can be seen from Table 1, the embodiment of the present invention of grafting polypropylene under microwave irradiation without adding initiator has a higher grafting rate than the comparative example of polypropylene grafted by melt blending with adding initiator, and the melt index of polypropylene after grafting does not increase, that is, the molecular weight does not decrease. It can be seen that the main chain breakage phenomenon of the polar monomer grafted polypropylene resin obtained in the embodiment of the present invention is controlled, ensuring that the mechanical properties of the resin are not lost. In addition, it can be seen that in the comparative example of microwave irradiation grafting with peroxide added, even under the condition of microwave irradiation grafting, the polypropylene melt index increases sharply due to the addition of peroxide; and due to the competition between the grafting reaction and the self-polymerization reaction, under the same microwave irradiation time, the grafting rate of the sample obtained without adding peroxide is always higher than the grafting rate of the sample obtained with the addition of peroxide. The higher the grafting rate, the lower the water contact angle after film making. The grafted polypropylene according to the present invention changes from the non-hydrophilicity (contact angle greater than 90°) of the raw polypropylene to hydrophilicity.

[0194] In addition, it can be seen that when the inorganic microwave absorbing medium is additionally added, the grafting rate of the grafted polypropylene can be further increased, the water contact angle can be reduced, and the melt index can be reduced. In addition, compared with the case where the inorganic microwave absorbing medium is not added, the use of the inorganic microwave absorbing medium can achieve a grafted polypropylene resin with similar properties using a shorter microwave irradiation time, thereby improving production efficiency.

[0195] Example S1:

[0196] Based on 100 parts by mass of homopolymerized polypropylene powder, maleic anhydride (5 parts by mass) is dissolved in acetone (50 parts by mass) to obtain a maleic anhydride acetone solution; sodium hydroxide (5 parts by mass) is dissolved in deionized water (50 parts by mass) to obtain a sodium hydroxide aqueous solution; the maleic anhydride acetone solution is added to the polypropylene powder under vacuum and mechanical stirring to fully mix, and then the mixture is dried (dried in an 80°C forced air drying oven). The dried polypropylene / maleic anhydride mixture powder is irradiated with microwaves (power 700W) for 3 minutes under a nitrogen atmosphere; the powder after microwave irradiation is soaked in deionized water for 10 minutes and the deionized water is replaced and repeated 3 times to ensure that the maleic anhydride monomer that does not participate in the grafting reaction is removed, and then the powder is placed in an 80°C forced air drying oven for drying; the sodium hydroxide aqueous solution is added to the dried maleic anhydride grafted polypropylene powder under vacuum stirring and fully mixed, and the sodium hydroxide aqueous solution is stirred and mixed after the addition and reacted for 5 minutes. After the reaction is completed, the powder is washed with deionized water according to the above washing steps and then placed in an 80°C blast drying oven for drying. Finally, the powder is melt-extruded and granulated with 0.1 parts by mass (based on 100 parts by mass of homopolymerized polypropylene powder) of antioxidant 1010, 0.1 parts by mass of antioxidant 168 and 0.1 parts by mass of calcium stearate in a twin-screw extruder. The temperature of the feeding section of the extruder is 190-200°C, the temperature of the mixing section is 200-210°C, and the temperature of the die head is 190-200°C. After extrusion granulation, the melt index, contact angle and grafting rate are tested. The test results are shown in Table 2.

[0197] Comparative Example S1:

[0198] Based on 100 parts by mass of homopolymerized polypropylene powder (same as in Example S1), maleic anhydride (5 parts by mass) and dicumyl peroxide (0.005 parts by mass) were dissolved in acetone (50 parts by mass) to obtain a maleic anhydride acetone solution; sodium hydroxide (5 parts by mass) was dissolved in deionized water (50 parts by mass) to obtain an aqueous sodium hydroxide solution; the maleic anhydride acetone solution was added to the polypropylene powder under vacuum accompanied by mechanical stirring and fully mixed, and then the mixture was dried (dried in a forced air drying oven at 80°C). The dried polypropylene / maleic anhydride mixture powder was irradiated with microwave (power 700W) for 3 minutes under nitrogen atmosphere; the microwave irradiated powder was soaked in deionized water for 10 minutes and the deionized water was replaced and repeated 3 times to ensure that the maleic anhydride monomer that did not participate in the grafting reaction was removed, and then the powder was placed in an 80°C forced air drying oven for drying; sodium hydroxide aqueous solution was added to the dried maleic anhydride grafted polypropylene powder under vacuum stirring conditions and fully mixed, and the sodium hydroxide aqueous solution was added and stirred and reacted for 5 minutes. After the reaction was completed, the powder was washed with deionized water according to the same washing steps as above, and then the powder was placed in an 80°C forced air drying oven for drying. Finally, the powder was melt-extruded and granulated with 0.1 parts by mass of antioxidant 1010, 0.1 parts by mass of antioxidant 168 and 0.1 parts by mass of calcium stearate in a twin-screw extruder. The temperature of the feeding section of the extruder was 190-200°C, the temperature of the mixing section was 200-210°C, and the temperature of the die was 190-200°C. After extrusion granulation, the melt index, contact angle and grafting rate were tested. The test results are shown in Table 2.

[0199] Example S2:

[0200] Except that the dried polypropylene / maleic anhydride mixture powder was irradiated with microwave (power 700 W) for 5 min under nitrogen atmosphere, the rest was the same as Example S1. The samples were tested for melt index, contact angle and grafting rate. The test results are shown in Table 2.

[0201] Comparative Example S2:

[0202] Except that the dried polypropylene / maleic anhydride mixture powder was irradiated with microwave (power 700 W) for 5 min under nitrogen atmosphere, the rest was the same as comparative example S1. The samples were tested for melt index, contact angle and grafting rate. The test results are shown in Table 2.

[0203] Example S3:

[0204] Except that the dried polypropylene / maleic anhydride mixture powder was irradiated with microwave (power 700 W) for 7 min under nitrogen atmosphere, the rest was the same as Example S1. The samples were tested for melt index, contact angle and grafting rate. The test results are shown in Table 2.

[0205] Comparative Example S3:

[0206] Except that the dried polypropylene / maleic anhydride mixture powder was irradiated with microwave (power 700 W) for 7 min under nitrogen atmosphere, the rest was the same as comparative example S1. The samples were tested for melt index, contact angle and grafting rate. The test results are shown in Table 2.

[0207] Example S4:

[0208] Except that the dried polypropylene maleic anhydride mixture powder was irradiated with microwave (power 700 W) for 10 min under nitrogen atmosphere, the rest was the same as Example S1. The samples were tested for melt index, contact angle and grafting rate. The test results are shown in Table 2.

[0209] Comparative Example S4:

[0210] Except that the dried polypropylene / maleic anhydride mixture powder was irradiated with microwave (power 700 W) for 10 min under nitrogen atmosphere, the rest was the same as comparative example S1. The samples were tested for melt index, contact angle and grafting rate. The test results are shown in Table 2.

[0211] Example S5:

[0212] Except that sodium hydroxide (1 part by mass) was dissolved in deionized water (50 parts by mass) to obtain a sodium hydroxide aqueous solution, the powder of the dried polypropylene / maleic anhydride mixture was irradiated with microwave (power 700 W) for 5 min under a nitrogen atmosphere, and the rest was the same as Example S1. The samples were tested for melt index, contact angle and grafting rate, and the test results are shown in Table 2.

[0213] Comparative Example S5:

[0214] Except that sodium hydroxide (1 part by mass) was dissolved in deionized water (50 parts by mass) to obtain a sodium hydroxide aqueous solution, the powder of the dried polypropylene / maleic anhydride mixture was irradiated with microwave (power 700 W) for 5 min under a nitrogen atmosphere, and the rest was the same as Comparative Example S1. The samples were tested for melt index, contact angle and grafting rate, and the test results are shown in Table 2.

[0215] Example S6:

[0216] Except that sodium hydroxide (8 parts by mass) was dissolved in deionized water (50 parts by mass) to obtain a sodium hydroxide aqueous solution, the powder of the dried polypropylene / maleic anhydride mixture was irradiated with microwaves (power 700 W) for 5 min under a nitrogen atmosphere, and the rest was the same as Example S1. The samples were tested for melt index, contact angle and grafting rate, and the test results are shown in Table 2.

[0217] Comparative Example S6:

[0218] Except that sodium hydroxide (8 parts by mass) was dissolved in deionized water (50 parts by mass) to obtain a sodium hydroxide aqueous solution, the powder of the dried polypropylene / maleic anhydride mixture was irradiated with microwave (power 700 W) for 5 min under a nitrogen atmosphere, and the rest was the same as Comparative Example S1. The samples were tested for melt index, contact angle and grafting rate, and the test results are shown in Table 2.

[0219] Example S7:

[0220] Except that sodium hydroxide (10 parts by mass) was dissolved in deionized water (50 parts by mass) to obtain a sodium hydroxide aqueous solution, the powder of the dried polypropylene / maleic anhydride mixture was irradiated with microwaves (power 700 W) for 5 min under a nitrogen atmosphere, and the rest was the same as Example S1. The samples were tested for melt index, contact angle and grafting rate, and the test results are shown in Table 2.

[0221] Comparative Example S7:

[0222] Except that sodium hydroxide (10 parts by mass) was dissolved in deionized water (50 parts by mass) to obtain a sodium hydroxide aqueous solution, the powder of the dried polypropylene / maleic anhydride mixture was irradiated with microwave (power 700 W) for 5 minutes under a nitrogen atmosphere, and the rest was the same as Comparative Example S1. The samples were tested for melt index, contact angle and grafting rate, and the test results are shown in Table 2.

[0223] Example S8:

[0224] The potassium hydroxide aqueous solution was obtained by dissolving potassium hydroxide (5 parts by mass) in deionized water (50 parts by mass), and the powder of the dried polypropylene / maleic anhydride mixture was irradiated with microwave (power 700 W) for 5 min under a nitrogen atmosphere, and the rest was the same as Example S1. The samples were tested for melt index, contact angle and grafting rate, and the test results are shown in Table 2.

[0225] Comparative Example S8:

[0226] The potassium hydroxide aqueous solution was obtained by dissolving potassium hydroxide (5 parts by mass) in deionized water (50 parts by mass), and the powder of the dried polypropylene / maleic anhydride mixture was irradiated with microwave (power 700 W) for 5 min under a nitrogen atmosphere, and the rest was the same as that of Comparative Example S1. The samples were tested for melt index, contact angle and grafting rate, and the test results are shown in Table 2.

[0227] Embodiment S9:

[0228] Except that calcium hydroxide (5 parts by mass) was dissolved in deionized water (50 parts by mass) to obtain a calcium hydroxide aqueous solution, the powder of the dried polypropylene / maleic anhydride mixture was irradiated with microwaves (power 700 W) for 5 min under a nitrogen atmosphere, and the rest was the same as Example S1. The samples were tested for melt index, contact angle and grafting rate, and the test results are shown in Table 2.

[0229] Comparative Example S9:

[0230] Except that calcium hydroxide (5 parts by mass) was dissolved in deionized water (50 parts by mass) to obtain a calcium hydroxide aqueous solution, the powder of the dried polypropylene / maleic anhydride mixture was irradiated with microwave (power 700 W) for 5 min under a nitrogen atmosphere, and the rest was the same as Comparative Example S1. The samples were tested for melt index, contact angle and grafting rate, and the test results are shown in Table 2.

[0231] Embodiment S10:

[0232] Except that maleic anhydride (1 part by mass) was dissolved in acetone (50 parts by mass) to obtain a maleic anhydride acetone solution, the powder of the dried polypropylene / maleic anhydride mixture was irradiated with microwave (power 700 W) for 7 min under a nitrogen atmosphere, and the rest was the same as Example S1. The samples were tested for melt index, contact angle and grafting rate, and the test results are shown in Table 2.

[0233] Embodiment S11:

[0234] Except that maleic anhydride (8 parts by mass) was dissolved in acetone (50 parts by mass) to obtain a maleic anhydride acetone solution, the powder of the dried polypropylene / maleic anhydride mixture was irradiated with microwave (power 700 W) for 7 min under a nitrogen atmosphere, and the rest was the same as Example S1. The samples were tested for melt index, contact angle and grafting rate, and the test results are shown in Table 2.

[0235] Embodiment S12:

[0236] Except that maleic anhydride (10 parts by mass) was dissolved in acetone (50 parts by mass) to obtain a maleic anhydride acetone solution, the powder of the dried polypropylene / maleic anhydride mixture was irradiated with microwave (power 700 W) for 7 min under a nitrogen atmosphere, and the rest was the same as Example S1. The samples were tested for melt index, contact angle and grafting rate, and the test results are shown in Table 2.

[0237] Embodiment S13:

[0238] Except that the dried polypropylene / maleic anhydride mixture powder was irradiated with microwave (power 700 W) for 5 min under nitrogen atmosphere, the other aspects were the same as Example S1. The samples were tested for melt index, contact angle and grafting rate, and the test results are shown in Table 2.

[0239] Embodiment S14:

[0240] Except that acrylic acid (5 parts by mass) was dissolved in acetone (50 parts by mass) to obtain an acrylic acid acetone solution based on 100 parts by mass of the impact copolymer polypropylene powder, and the dried polypropylene / acrylic acid mixture powder was irradiated with microwave (power 700 W) for 5 minutes under a nitrogen atmosphere, the rest was the same as Example S1. The samples were tested for melt index, contact angle and grafting rate, and the test results are shown in Table 2.

[0241] Embodiment S15:

[0242] Except that the powder of the polypropylene / maleic anhydride mixture dried after drying was irradiated with microwave (power 700 W) for 5 min under nitrogen atmosphere, the rest was the same as Example S1. The samples were tested for melt index, contact angle and grafting rate, and the test results are shown in Table 2.

[0243] Embodiment S16:

[0244] The same procedures as in Example S1 were followed except that 100 parts by mass of random copolymerized polypropylene powder was used to dissolve acrylic acid (5 parts by mass) in acetone (50 parts by mass) to obtain an acrylic acid acetone solution, and the dried polypropylene / acrylic acid mixture powder was irradiated with microwaves (power 700 W) for 5 min under a nitrogen atmosphere. The samples were tested for melt index, contact angle, and grafting rate, and the test results are shown in Table 2.

[0245] Embodiment S17:

[0246] The same method as in Example S1 was used except that acrylic acid (5 parts by mass) was dissolved in acetone (50 parts by mass) to obtain an acrylic acid acetone solution, and the dried polypropylene / acrylic acid mixture powder was irradiated with microwave (power 700 W) for 5 min under a nitrogen atmosphere. The samples were tested for melt index, contact angle and grafting rate, and the test results are shown in Table 2.

[0247] Embodiment S18:

[0248] Except that methacrylic acid (5 parts by mass) was dissolved in acetone (50 parts by mass) to obtain a methacrylic acid acetone solution, the powder of the dried polypropylene methacrylic acid mixture was irradiated with microwave (power 700 W) for 5 min under a nitrogen atmosphere, and the rest was the same as Example S1. The samples were tested for melt index, contact angle and grafting rate, and the test results are shown in Table 2.

[0249] Table 2

[0250]

[0251] As can be seen from Table 2, the embodiment of the present invention in which organic acid salt grafted polypropylene under microwave irradiation without adding initiator has a higher grafting rate than the comparative example of polypropylene grafted by melt blending with adding initiator, and the melt index of polypropylene after grafting does not increase, that is, the molecular weight does not decrease, which shows that the main chain breakage phenomenon of the organic acid salt grafted polypropylene resin obtained in the embodiment of the present invention is controlled, ensuring that the mechanical properties of the resin are not lost. In addition, it can be seen that in the comparative example of microwave irradiation grafting with peroxide, even under the condition of microwave irradiation grafting, the melt index of polypropylene increases sharply due to the addition of peroxide; and due to the competition between grafting reaction and self-polymerization reaction, under the same microwave irradiation time, the grafting rate of the sample obtained without adding peroxide is always higher than the grafting rate of the sample obtained with adding peroxide.

[0252] It can also be seen from Table 2 that for the organic acid salt grafted polypropylene according to the embodiment of the present invention, the higher the grafting rate, the lower the water contact angle after film formation. The organic acid salt grafted polypropylene of the present invention changes from the non-hydrophilicity (contact angle greater than 90°) of the raw material polypropylene to hydrophilicity, and the contact angle can even reach 0°.

[0253] In addition, from the comparison of Tables 1 and 2, it can be seen that after adding hydroxide, the water contact angle of organic acid salt grafted polypropylene with the same grafting rate is significantly smaller than the water contact angle of organic acid grafted polypropylene. Therefore, the addition of hydroxide can further improve the polarity of grafted polypropylene.

Claims

1. A polar monomer grafted polypropylene resin, wherein the grafted polypropylene resin does not contain initiator residues, There are side groups of polar monomers on the main chain of the polypropylene molecule, and the grafting rate of the polar monomers is 0.01%-8%; wherein the melt index of the grafted polypropylene resin is less than or equal to the melt index of the polypropylene resin as the graft base; The polypropylene resin used as the graft base is selected from propylene homopolymers and random copolymers of propylene and mixtures thereof, and wherein the polar monomer is selected from maleic anhydride, acids and esters of maleic anhydride, (meth)acrylic acid, anhydrides and esters of (meth)acrylic acid, vinyl acetate, olefin sulfonic acid and anhydrides and esters thereof, p-styrene formic acid, p-styrene acetic acid, itaconic acid, oleic acid, arachidonic acid, combinations thereof, and salt forms thereof; The grafted polypropylene resin is obtained by grafting the polar monomer with the solid polypropylene resin by microwave irradiation without adding an initiator.

2. The grafted polypropylene resin according to claim 1, characterized in that The ester of (meth)acrylic acid is glycidyl methacrylate.

3. The grafted polypropylene resin according to claim 1, characterized in that The grafting rate is 0.01%-6%.

4. The grafted polypropylene resin according to any one of claims 1 to 3, characterized in that The water contact angle value of the grafted polypropylene resin is less than 90 o , measured for a film prepared from the grafted polypropylene resin by a solution process.

5. The grafted polypropylene resin according to claim 4, characterized in that The water contact angle value of the grafted polypropylene resin is less than 65 o , measured for a film prepared from the grafted polypropylene resin by a solution process.

6. The grafted polypropylene resin according to claim 4, characterized in that The water contact angle value of the grafted polypropylene resin is 50 o -0 o , measured for a film prepared from the grafted polypropylene resin by a solution process.

7. The grafted polypropylene resin according to any one of claims 1 to 3, characterized in that The comonomer in the random copolymer of propylene is selected from ethylene, α-olefins other than propylene, and combinations thereof.

8. The grafted polypropylene resin according to any one of claims 1 to 3, characterized in that The comonomer in the random copolymer of propylene is selected from ethylene, C4, C5, C6 to C8-α-olefins and combinations thereof.

9. The grafted polypropylene resin according to any one of claims 1 to 3, characterized in that The polypropylene resin as the graft base is in the form of a solid including powder, pellets or a product.

10. The grafted polypropylene resin according to claim 9, characterized in that The polypropylene resin used as the graft base is a polypropylene powder obtained by polymerization using a spherical catalyst.

11. The grafted polypropylene resin according to claim 1, characterized in that The polar monomer used is not in the form of a salt, and the product obtained after the grafting reaction is further salted.

12. A method for preparing a grafted polypropylene resin according to any one of claims 1 to 11, comprising the step of grafting the polar monomer with a solid polypropylene resin using microwave irradiation without adding an initiator.

13. The method according to claim 12, characterized in that The polar monomer is used in an amount of 0.1-10% by weight based on the weight of the solid polypropylene resin.

14. A method according to claim 13, characterised in that The polar monomer is used in an amount of 1-8% by weight based on the weight of the solid polypropylene resin.

15. A method according to any one of claims 12 to 14, characterised in that The polar monomer is in the form of a liquid or a solution.

16. A method according to any one of claims 12 to 14, characterised in that The irradiation power of the microwave irradiation is 100w-2000w; the irradiation time is 1s-120min.

17. The method according to claim 16, characterized in that The irradiation power of the microwave irradiation is 500w-1000w.

18. The method according to claim 16, characterized in that The microwave irradiation has an irradiation time of 1 min to 30 min.

19. A method according to any one of claims 12 to 14, characterised in that The method comprises the following steps: 1) Thoroughly mix the polar monomer and solid polypropylene resin; 2) The mixture obtained in step 1) is subjected to microwave irradiation.

20. The method according to claim 19, characterized in that Step 2) is carried out under an inert gas atmosphere.

21. The method according to claim 19, characterized in that In step 1), the polar monomer and the solid polypropylene resin are fully mixed under vacuum conditions.

22. The method according to claim 20, characterized in that The inert gas in step 2) is selected from one or more of nitrogen, helium and argon.

23. The method according to claim 19, characterized in that The polar monomer is in the form of a solution dissolved in a solvent, and the mixture obtained in step 1) is dried to remove the solvent before step 2).

24. The method according to claim 23, characterized in that The solvent is selected from at least one of alcohol, ketone, ester and water.

25. The method according to claim 24, characterized in that The solvent is acetone or ethanol.

26. The method according to claim 19, characterized in that The irradiated mixture obtained in step 2) is washed to remove unreacted polar monomers, and then dried, wherein the washing solvent is selected from at least one of alcohol, ketone, ester and water.

27. A method according to any one of claims 12 to 14, characterised in that The solid polypropylene resin used does not contain antioxidants.

28. A method according to any one of claims 12 to 14, characterised in that The polar monomer used is not in a salt form, and the product obtained after the grafting reaction under microwave irradiation is further reacted with a base.

29. The method according to claim 28, characterized in that The organic acid grafted polypropylene powder and the alkali aqueous solution are fully mixed and reacted under vacuum.

30. The method according to claim 28, characterized in that The method further comprises washing with a solvent to remove unreacted alkali and performing a drying process to obtain an organic acid salt grafted polypropylene resin.

31. The method according to claim 28, characterized in that The base is selected from ammonia and metal hydroxides.

32. The method according to claim 31, characterized in that The base is selected from sodium hydroxide, potassium hydroxide, barium hydroxide, lithium hydroxide, strontium hydroxide, calcium hydroxide, ferric hydroxide, ferrous hydroxide, zinc hydroxide, magnesium hydroxide, cobalt hydroxide, gold hydroxide, aluminum hydroxide, copper hydroxide, beryllium hydroxide, rare earth hydroxides, and combinations thereof.

33. The method according to claim 28, characterized in that The base is used in an amount of 0.1-10% by weight based on the weight of the polypropylene resin used.

34. A method according to claim 33, characterised in that The base is used in an amount of 1-8% by weight based on the weight of the polypropylene resin used.

35. A method according to any one of claims 12 to 14, characterised in that No auxiliary grafting monomer is used during the grafting reaction.

36. A method according to any one of claims 12 to 14, characterised in that Add inorganic microwave absorbing medium.

37. The method according to claim 36, characterized in that The inorganic microwave absorbing medium is used in an amount of 0.1-10% by weight based on the weight of the solid polypropylene resin.

38. The method according to claim 37, characterized in that The inorganic microwave absorbing medium is used in an amount of 1-8% by weight based on the weight of the solid polypropylene resin.

39. The method according to claim 36, characterized in that The inorganic microwave absorbing medium is selected from metal hydroxides; metal salts; metal oxides; graphite materials; ferroelectric materials; electrolytic stones; chalcopyrite; and combinations thereof.

40. The method according to claim 39, characterized in that The inorganic microwave absorbing medium is selected from potassium hydroxide, barium hydroxide, sodium hydroxide, lithium hydroxide, strontium hydroxide, calcium hydroxide, ferric hydroxide, ferrous hydroxide, zinc hydroxide, magnesium hydroxide, cobalt hydroxide, gold hydroxide, aluminum hydroxide, copper hydroxide, beryllium hydroxide, rare earth hydroxides, ammonium nitrate, potassium nitrate, sodium nitrate, barium nitrate, calcium nitrate, magnesium nitrate, aluminum nitrate, manganese nitrate, zinc nitrate, ferric nitrate, ferrous nitrate, copper nitrate, silver nitrate, ammonium chloride, potassium chloride, sodium chloride, barium chloride, calcium chloride, magnesium chloride, aluminum chloride, chloride Manganese sulfate, zinc chloride, ferric chloride, ferrous chloride, cupric chloride, ammonium sulfate, potassium sulfate, sodium sulfate, calcium sulfate, magnesium sulfate, aluminum sulfate, manganese sulfate, zinc sulfate, ferric sulfate, ferrous sulfate, cupric sulfate, silver sulfate, ammonium carbonate, potassium carbonate, sodium carbonate, magnesium carbonate, calcium carbonate, barium carbonate, potassium dihydrogen phosphate, barium titanate, strontium titanate, calcium copper titanate, ferric oxide, ferroferric oxide, carbon black, graphite powder, graphene oxide and its reduction products, graphene, carbon nanotubes, activated carbon, ferroelectric materials, electrolytic stone, chalcopyrite and combinations thereof.

41. The method according to claim 36, characterized in that Before microwave irradiation, the polar monomer, the inorganic microwave absorbing medium and the solid polypropylene resin are fully mixed.

42. The method according to claim 41, characterized in that The mixing is performed under vacuum conditions.

43. The method according to claim 41, characterized in that The polar monomer is dissolved in a solvent.

44. The method according to claim 41, characterized in that The inorganic microwave absorbing medium is dissolved or dispersed in the solvent.

45. The method according to claim 41, characterized in that In the case where a surfactant is added, the inorganic microwave absorbing medium is dissolved or dispersed in the solvent.

46. ​​A method according to any one of claims 43 to 45, characterised in that The solvent used to dissolve the polar monomer is the same as or different from the solvent used to dissolve or disperse the inorganic microwave absorbing medium, and is selected from water, alcohol, ketone, and ester.

47. A method according to any one of claims 43 to 45, characterised in that After mixing, a drying process is performed to remove the solvent.

48. A method according to any one of claims 41 to 45, characterised in that The polypropylene resin is first mixed with a polar monomer, and then the resulting mixture is mixed with an inorganic microwave absorbing medium.

49. The method according to claim 36, characterized in that The irradiated mixture is washed to remove unreacted polar monomers and dried.

50. The method according to claim 49, characterized in that The irradiated mixture is washed to remove unreacted polar monomers and inorganic microwave absorbing medium, and then dried.

51. A pellet or article obtained from the grafted polypropylene resin according to any one of claims 1 to 11 or the grafted polypropylene resin prepared by the method according to any one of claims 12 to 50 by melt extrusion pelletization or further shaping process.

52. A granular material or article according to claim 51, characterised in that The grafted polypropylene resin is added with additives.

53. A composite material, a coatable film material or an adhesive material obtained by blending a grafted polypropylene resin according to any one of claims 1 to 11 or a grafted polypropylene resin prepared by a process according to any one of claims 12 to 50 with other polymers.

54. Use of a grafted polypropylene resin according to any one of claims 1 to 11 or prepared by a process according to any one of claims 12 to 50 for the modification of plastics.