A low-resistivity, low-temperature solar silver paste and preparation method thereof
Through silver powder combinations and resin systems of different shapes and sizes, combined with dual curing agents, the problem of high resistivity of silver paste in HIT batteries is solved, low resistivity and improved stability are achieved, and it is suitable for low-temperature processes.
Patent Information
- Application Number
- CN202210065061.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-01-20
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-01-20
AI Technical Summary
The resistivity of existing HIT battery silver paste is high, which affects its conversion rate, and the production process temperature is high, making it difficult to achieve low-temperature curing.
Using a combination of silver powders with different shapes and sizes, combined with epoxy resin and auxiliary resin, using dual curing agents and catalysts, a low-temperature solar silver paste with low resistivity is achieved through a specific preparation method.
It achieves close accumulation of silver powder, reduces resistivity, improves conductivity, ensures the stability and low volume resistivity of silver paste, and is suitable for low-temperature process conditions.
Smart Images

Figure CN114464342B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of conductive silver paste preparation, and in particular to a low-resistivity, low-temperature solar silver paste and a preparation method thereof. Background Art
[0002] With the depletion of non-renewable resources such as oil and natural gas, new energy sources such as wind energy, tidal energy, and solar energy are becoming more and more important. Solar energy is an inexhaustible new energy source, and the time and cost of building a solar power station are lower than those of a traditional power station. Therefore, in the long-term energy strategy, photovoltaic power generation is an ideal solution to the energy crisis.
[0003] In recent years, solar cell technology has entered a rapid development stage, forming a variety of technical products, such as crystalline silicon solar cells, inorganic semiconductor thin film cells, dye-sensitized solar cells, perovskite solar cells, organic polymer solar cells, etc. At present, traditional crystalline silicon is still the mainstream. Inorganic semiconductor thin film cells have problems such as high production cost and low conversion rate, and only occupy a small part of the market. Dye-sensitized solar cells, perovskite solar cells, and organic polymer solar cells are still in the laboratory. HIT cells, commonly known as heterojunction cells, combine the advantages of crystalline silicon cells and thin film cells, and are a popular direction for improving the conversion rate of silicon-based solar cells. This technology effectively prevents the recombination of light-generated carriers and increases the life of carriers by passivating the front and back surfaces of the crystalline silicon substrate, thereby improving the conversion rate. Due to the design of this structure, the production process temperature of HIT cells is below 250°C, so the silver paste of the metallized grid formed on its surface must be cured at low temperature, so silver paste is its important key raw material. Usually, the factors affecting the conversion rate of HIT silver paste include resistivity, lap impedance, meshing amount, etc. The resistivity of the current mainstream HIT silver paste is 5*10 -6 Ω·cm, and as an important factor affecting the conversion rate, the preparation of <5*10 -6 Ω·cm resistivity helps to improve the conversion rate of HIT silver paste. Therefore, it is of great significance to prepare HIT silver paste with low resistivity. Summary of the invention
[0004] In view of the shortcomings of the prior art, the present invention provides a low-resistivity low-temperature solar silver paste and a preparation method thereof. The silver paste prepared by the present invention has good stability, good fine line meshing, and low volume resistivity and excellent contact resistance performance.
[0005] The technical solution of the present invention is as follows:
[0006] The invention discloses a low-resistivity, low-temperature solar silver paste. The raw materials of the silver paste include the following components by mass percentage: 87-93% silver powder, 2-5% resin, 1-2% diluent, 0.5-2% curing agent, 0.01-1% thixotropic agent, 0.01-1% catalyst and 2-5% organic solvent.
[0007] Furthermore, the silver powder is flaky powder or spherical powder; the mass ratio of the flaky powder to the spherical powder is 0.01 to 0.3:1, preferably 0.02 to 0.1.
[0008] Furthermore, the D50 of the flaky powder is 2 to 8 μm, and the tap density is 4 to 6 g / mL.
[0009] Furthermore, the spherical powder is spherical powder I or spherical powder II; the spherical powder I, in terms of weight percentage, includes spherical powders of the following particle sizes: 5-15% D50 is 0.05-0.8 μm, and the tap density is 3-5 g / mL; 65-80% D50 is 2-4 μm, and the tap density is 5-8 g / mL; 14-30% D50 is 1-1.8 μm, and the tap density is 4-6 g / mL.
[0010] Furthermore, the particle size distribution of the spherical powder II satisfies: D50 is 0.8-1.5 μm, the tap density is 4-7 g / mL, D10 is 0.05-0.5 μm, and D100 is 2-5 μm, preferably D10 is 0.1-0.5 μm, and D100 is 2.5-3.5 μm.
[0011] Furthermore, the resin is composed of epoxy resin and auxiliary resin; the epoxy resin is two or more of bisphenol A epoxy resin, phenoxy resin, bisphenol F epoxy resin, aliphatic epoxy resin, silicone modified epoxy, polyether modified epoxy resin, epoxidized rubber; the bisphenol A epoxy resin is JER 827, JER828, JER834, JER1007 or JER1001; the phenoxy resin is PKHB, PKHH, PKHJ or PKFE; the bisphenol F epoxy resin is 4007P, 4010P, 7787, 835 or 830S; the aliphatic epoxy resin is 2021P, EHPE3150, HE200 or HE2025; the silicone modified epoxy is ERS-Si1700, YH600 or EPS-231; the polyether modified epoxy resin is EP4000, EP4010S or EP1307; the epoxidized rubber is JP100, JP200 or XP1740; the auxiliary resin is polyether polyol, acrylate polyol, polyester polyol At least one of polyols, polyurethane resins, polyester resins, and acrylic resins; the auxiliary resin is a resin containing a hydroxyl group and a hydroxyl value greater than 5 or a resin containing a carboxyl group and a carboxyl value greater than 5, and the Tg of the auxiliary resin is less than 100°C; the polyether polyol is CP450, 2070A, 2000ML, or 3003LM; the acrylic ester polyol is Q850M, Q519, BM666, or BM261; the polyester polyol is 4073, 4009, 4010, or 4040; the polyurethane resin is 5836, 5778, 5715, or 5703; the polyester resin is Toyobo220, 280, 296, or GK888; the acrylic resin is AC169, AC166, AC166B, or BM52.
[0012] The mass ratio of the epoxy resin to the auxiliary resin is 1 to 10:1, and the mass ratio of the epoxy resin to the auxiliary resin is preferably 2 to 5:1.
[0013] Furthermore, the diluent is epoxy glycidyl ether, and the diluent is one or more of ethylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, 1,4-butanediol diglycidyl ether, glycerol triglycidyl ether, pentaerythritol glycidyl ether, resorcinol diglycidyl ether, trimethylolpropane triglycidyl ether, hexahydrobisphenol A diglycidyl ether, terephthalic acid diglycidyl ether, and sorbitol glycidyl ether; the thixotropic agent is one or more of fumed silica, organic bentonite, hydrogenated castor oil, and polyamide wax.
[0014] Furthermore, the curing agent consists of a main curing agent and an auxiliary curing agent; the main curing agent is a blocked isocyanate curing agent, and the deblocking temperature is 80 to 150° C., preferably 90 to 120° C.; the auxiliary curing agent is one or more of an imidazole curing agent, an acid anhydride curing agent, and a dicyandiamide curing agent; the imidazole curing agent is one or more of benzimidazole, DBU, dimethyltetraethylimidazole, PN23, PN23J, and PN40; the acid anhydride curing agent is one or more of methyl hexadecene, DDSA, and methyl nadic anhydride; the dicyandiamide curing agent is DICY; the mass ratio of the main curing agent to the auxiliary curing agent is 1.5 to 5:1, preferably 2 to 5:1.
[0015] Furthermore, the thixotropic agent is one or more of fumed silica, organic bentonite, modified hydrogenated castor oil, and polyamide wax.
[0016] Furthermore, the catalyst is an epoxy catalyst, and the catalyst is one or more of CXC1612, CXC1614, XC9206, XC258, CXC1756, XC2007, Vicbase TC3630, Vicbase TC3633, and ICAM-8409; the organic solvent is one or more of propylene carbonate, ethylene glycol ethyl ether acetate, ethylene glycol butyl ether acetate, diethylene glycol butyl ether acetate, dimethyl adipate, diethyl adipate, propylene glycol methyl ether acetate, and terpineol.
[0017] A low resistivity, low temperature solar silver paste, when the spherical powder used is spherical powder II, its preparation method comprises the following steps, in terms of mass percentage:
[0018] (1) adding 2-5% of an organic solvent into a reaction kettle and mixing, then adding 2-5% of a resin, heating and stirring, cooling to room temperature, and filtering to obtain a resin solution;
[0019] (2) adding 0.01-1% of a catalyst, 0.01-1% of a thixotropic agent, 0.5-2% of a curing agent, and 1-2% of a diluent to the resin solution prepared in step (1), and centrifugally dispersing the mixture to obtain an organic carrier;
[0020] (3) adding 87-93% of silver powder to the organic carrier prepared in step (2), centrifugally dispersing, shearing and dispersing by a three-roll mill until the slurry fineness is less than 5 μm, filtering, and obtaining a finished silver paste;
[0021] In step (1), the heating temperature is 70-95° C.; the stirring speed is 200-300 r / min, and the time is 1-2 h;
[0022] In step (2), the centrifugal dispersion speed is 800-850 rpm and the time is 2-4 min;
[0023] In step (3), the specific process of the centrifugal dispersion is: dispersing at 800 rpm, 1000 rpm, 1200 rpm, and 1600 rpm, respectively, for 1 to 3 minutes.
[0024] A low resistivity, low temperature solar silver paste, when the spherical powder used is spherical powder I, its preparation method comprises the following steps, in terms of mass percentage:
[0025] (1) adding 2-5% of an organic solvent into a reaction kettle and mixing, then adding 2-5% of a resin, heating and stirring, cooling to room temperature, and filtering to obtain a resin solution;
[0026] (2) adding 0.01-1% of a catalyst, 0.01-1% of a thixotropic agent, 0.5-2% of a curing agent, and 1-2% of a diluent to the resin solution prepared in step (1), and centrifugally dispersing the mixture to obtain an organic carrier;
[0027] (3) adding spherical powder accounting for 5-15% of spherical powder I and having a D50 of 0.05-0.8 μm to the organic carrier prepared in step (2), centrifugally dispersing, adding the remaining silver powder and centrifugally dispersing, shearing and dispersing by a three-roll mill until the slurry fineness is less than 5 μm, filtering, and obtaining a finished silver paste;
[0028] In step (1), the heating temperature is 70-95° C.; the stirring speed is 200-300 r / min, and the time is 1-2 h;
[0029] In step (2), the centrifugal dispersion speed is 800-850 rpm and the time is 2-4 min;
[0030] In step (3), the specific process of the centrifugal dispersion is: dispersing at 800 rpm, 1000 rpm, 1200 rpm, and 1600 rpm, respectively, for 1 to 3 minutes.
[0031] The beneficial technical effects of the present invention are:
[0032] (1) The present invention achieves close packing of silver powders by combining silver powders of different morphologies, different sizes, and different tap densities, thereby increasing the contact points between silver powder particles, reducing silver powder voids, reducing the slurry resistivity and intrinsic resistance, and optimizing the conductive properties of the silver powder. The silver paste prepared by the present invention has good stability, good fine line meshing, and excellent contact resistance performance with low volume resistivity.
[0033] (2) The resin used in the present invention is composed of a main resin and an auxiliary resin. The main resin is an epoxy resin, which is mainly responsible for the adhesion, heat resistance and stability of the slurry. The addition of the auxiliary resin improves the flexibility of the slurry resin and promotes the improvement of the electrical properties of the slurry.
[0034] (3) The present invention uses a dual curing agent, which is introduced together with a catalyst to jointly deepen the curing degree of the slurry and improve the slurry performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 This is a SEM image of the low-resistivity, low-temperature solar silver paste prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0036] The present invention is described in detail below in conjunction with the accompanying drawings and embodiments.
[0037] Example 1
[0038] A low-resistivity, low-temperature solar silver paste comprises the following components in percentage by mass: 93% silver powder, 1.5% resin, 1% diluent, 1.2% curing agent, 0.2% thixotropic agent, 0.1% catalyst and 3% organic solvent.
[0039] The silver powder is composed of flaky powder with a D50 of 3.0 μm and a tap density of 4.5 g / mL, which accounts for 5% of the slurry; spherical powder with a D50 of 0.6 μm and a tap density of 4.8 g / mL, 55% spherical powder with a D50 of 2 μm and a tap density of 6 g / mL, and 23% spherical powder with a D50 of 1 μm and a tap density of 5.8 g / mL. The spherical powder is spherical powder and quasi-spherical powder.
[0040] Epoxy resin is the main resin: 0.5% of phenoxy resin PKHH and 0.7% of bisphenol A epoxy resin JER827, auxiliary resin: 0.3% of 2000ML.
[0041] Diluent: 1% resorcinol diglycidyl ether.
[0042] Curing agent: It includes isocyanate curing agent and auxiliary curing agent, specifically 1% G282 isocyanate curing agent, the unblocking temperature is 80°C, and the auxiliary curing agent is 0.2% benzimidazole.
[0043] Thixotropic agent: 0.2% polyamide wax.
[0044] Catalyst: 0.1% XC2007.
[0045] Organic solvent: 3% diethylene glycol butyl ether acetate.
[0046] A method for preparing low-resistivity low-temperature solar silver paste comprises the following steps:
[0047] (1) 3% of diethylene glycol butyl ether acetate organic solvent was mixed in a reaction kettle, 1.5% of resin was gradually added, heated to 85° C., stirred at a speed of 260 r / min for 1 hour until the resin was completely dissolved, allowed to stand, cooled to room temperature, and filtered with a 300-400 mesh cloth to obtain a resin solution;
[0048] (2) taking the prepared resin solution, gradually adding 0.1% XC2007 catalyst, 0.2% polyamide wax thixotropic agent, 1% resorcinol diglycidyl ether, 1% G282 isocyanate curing agent and 0.2% benzimidazole auxiliary curing agent, centrifugally dispersing at 800 rpm for 2 minutes, and fully mixing to obtain an organic carrier;
[0049] (3) Take the prepared organic carrier, add 10% D50 0.6 μm spherical powder and stir, then disperse by centrifugation at 800 rpm, 1000 rpm, 1200 rpm and 1600 rpm for 1 min respectively.
[0050] (4) Slowly add the remaining silver powder and stir it manually. After all the silver powder is evenly mixed, centrifuge and stir it at 800 rpm, 1000 rpm, 1200 rpm, and 1600 rpm for 1 min respectively. After centrifugation, use a three-roll mill to shear and disperse the slurry until the slurry fineness reaches less than 2 μm, and then stop the three rollers.
[0051] (5) Use a 500-mesh sieve to filter out impurities and uneven large particles in the slurry to obtain a low-resistivity, low-temperature solar silver paste.
[0052] Example 2
[0053] A low-resistivity, low-temperature solar silver paste comprises the following components by mass percentage: 93% silver powder, 1.5% resin, 1% diluent, 1.2% curing agent, 0.2% thixotropic agent, 0.1% catalyst and 3% organic solvent.
[0054] The silver powder is composed of flaky powder with a D50 of 3.0 μm and a tap density of 4.5 g / mL, which accounts for 5% of the slurry; spherical powder with a D50 of 0.6 μm and a tap density of 4.8 g / mL, spherical powder with a D50 of 55% and a tap density of 6 g / mL, and spherical powder with a D50 of 1 μm and a tap density of 5.8 g / mL, which accounts for 23% of the slurry. The spherical powder includes spherical powder and spherical-like powder.
[0055] The epoxy resin is the main resin: 0.4% of phenoxy resin PKFE and 0.7% of bisphenol A epoxy resin JER830S, and the auxiliary resin is 0.4% of 220.
[0056] Diluent: 1% resorcinol diglycidyl ether.
[0057] Curing agent: It includes isocyanate curing agent and auxiliary curing agent, specifically 1% G282 isocyanate curing agent, the unblocking temperature is 80° C., and the auxiliary curing agent is 0.2% dimethyltetraethylimidazole.
[0058] Thixotropic agent: 0.2% polyamide wax.
[0059] Catalyst: 0.1% XC2007.
[0060] Organic solvent: 3% diethylene glycol butyl ether acetate.
[0061] A method for preparing low-resistivity low-temperature solar silver paste comprises the following steps:
[0062] (1) 3% of diethylene glycol butyl ether acetate organic solvent was mixed in a reaction kettle, 1.5% of polymer resin was gradually added, heated to 85° C., stirred at a speed of 260 r / min for 2 h until the resin was completely dissolved, allowed to stand, cooled to room temperature, and filtered with a 300-400 mesh cloth to obtain a resin solution;
[0063] (2) taking the prepared resin solution, gradually adding 0.1% XC2007 catalyst, 0.2% polyamide wax thixotropic agent, 1% resorcinol diglycidyl ether, 1% G282 isocyanate curing agent and 0.2% dimethyltetraethylimidazole as an auxiliary curing agent, centrifugally dispersing at 800 rpm for 2 minutes, and fully mixing to obtain an organic carrier;
[0064] (3) Take the prepared organic carrier, add 10% D50 0.6 μm spherical powder and stir, then centrifuge and disperse at speeds of 800 rpm, 1000 rpm, 1200 rpm, and 1600 rpm for 1 min respectively.
[0065] (4) Slowly add silver powder and stir manually. After all the silver powder is evenly mixed, centrifuge at 800 rpm, 1000 rpm, 1200 rpm, and 1600 rpm for 1 min respectively. After centrifugation, use a three-roll mill to shear and disperse the slurry until the slurry fineness reaches less than 2 μm, and then stop the three rollers.
[0066] (4) Using a 500-mesh sieve to filter out impurities and uneven large particles in the slurry, a low-resistivity, low-temperature solar silver paste is obtained.
[0067] Example 3
[0068] A low-resistivity, low-temperature solar silver paste comprises the following components by mass percentage: 93% silver powder, 1.5% resin, 1% diluent, 1.2% curing agent, 0.2% thixotropic agent, 0.1% catalyst and 3% organic solvent.
[0069] The silver powder is composed of flake powder with D50 of 3.0 μm and tap density of 4.5 g / mL, which accounts for 5% of the slurry; and spherical powder with D50 of 1 μm, tap density of 5.8 g / mL, D10 of 0.1 μm, D100 of 3 μm and wide particle size distribution, which accounts for 88% of the slurry.
[0070] Epoxy resin is the main resin: 0.5% of phenoxy resin PKHH and 0.7% of bisphenol A epoxy resin JER827, auxiliary resin: 0.3% of 2000ML.
[0071] Diluent: 1% resorcinol diglycidyl ether.
[0072] Curing agent: It includes isocyanate curing agent and auxiliary curing agent, specifically 1% G282 isocyanate curing agent, the unblocking temperature is 80°C, and the auxiliary curing agent is 0.2% benzimidazole.
[0073] Thixotropic agent: 0.2% polyamide wax.
[0074] Catalyst: 0.1% XC2007.
[0075] Organic solvent: 3% diethylene glycol butyl ether acetate.
[0076] A method for preparing low-resistivity low-temperature solar silver paste comprises the following steps:
[0077] (1) 3% of diethylene glycol butyl ether acetate organic solvent is mixed in a reaction kettle, 1.5% of a polymer resin is gradually added, the mixture is heated to 85° C., stirred at a speed of 260 r / min until the resin is completely dissolved, allowed to stand, cooled to room temperature, and filtered through a 300-400 mesh cloth to obtain a resin solution;
[0078] (2) taking the prepared resin solution, gradually adding 0.1% XC2007, 0.2% polyamide wax thixotropic agent, 1% resorcinol diglycidyl ether, 1% G282 isocyanate curing agent and 0.2% benzimidazole auxiliary curing agent, centrifugally dispersed at 800 rpm for 2 minutes, and fully mixed to obtain an organic carrier;
[0079] (3) Take the prepared organic carrier, add 93% silver powder, and stir manually. After all the silver powder is evenly stirred, put it into a centrifugal disperser and centrifuge it at 800 rpm, 1000 rpm, 1200 rpm, and 1600 rpm for 1 min respectively. After centrifugation, use a three-roller mill to shear and disperse the slurry until the slurry fineness reaches less than 2 μm, and then stop the three rollers.
[0080] (4) Using a 500-mesh sieve to filter out impurities and uneven large particles in the slurry, a low-resistivity, low-temperature solar silver paste is obtained.
[0081] Example 4
[0082] A low-resistivity, low-temperature solar silver paste comprises the following components by mass percentage: 93% silver powder, 0.5% resin, 2% diluent, 1.2% curing agent, 0.2% thixotropic agent, 0.1% catalyst and 3% organic solvent.
[0083] The silver powder is composed of flaky powder with a D50 of 3.0 μm and a tap density of 4.5 g / mL, spherical powder with a D50 of 0.6 μm and a tap density of 4.8 g / mL, spherical powder with a D50 of 55% and a tap density of 6 g / mL, and spherical powder with a D50 of 1 μm and a tap density of 5.8 g / mL, which accounts for 5% of the slurry. The spherical powder is ball powder.
[0084] Epoxy resin is the main resin: 0.4% of phenoxy resin PKHH, and the auxiliary resin is 0.1% of GK888.
[0085] Diluent: 2% hexahydrobisphenol A diglycidyl ether.
[0086] Curing agent: comprising isocyanate curing agent and auxiliary curing agent, specifically 1% B-897N isocyanate curing agent, the unblocking temperature is 120° C., and the auxiliary curing agent is 0.2% benzimidazole.
[0087] Thixotropic agent: 0.2% polyamide wax.
[0088] Catalyst: 0.1% XC2007.
[0089] Organic solvent: 3% diethylene glycol butyl ether acetate.
[0090] A method for preparing low-resistivity low-temperature solar silver paste comprises the following steps:
[0091] (1) 3% of diethylene glycol butyl ether acetate organic solvent is mixed in a reaction kettle, 0.5% of a polymer resin is gradually added, the mixture is heated to 85° C., stirred at a speed of 260 r / min until the resin is completely dissolved, allowed to stand, cooled to room temperature, and filtered through a 300-400 mesh cloth to obtain a resin solution;
[0092] (2) taking the prepared resin solution, gradually adding 0.1% XC2007, 0.2% polyamide wax thixotropic agent, 2% hexahydrobisphenol A diglycidyl ether, 1% B-897N isocyanate curing agent and 0.2% benzimidazole auxiliary curing agent, centrifugally dispersed at 800 rpm for 2 minutes, and fully mixed to obtain an organic carrier;
[0093] (3) Take the prepared organic carrier, add spherical powder with a D50 of 0.6 μm, stir, and then put it into a centrifugal disperser, and centrifuge and stir at speeds of 800 rpm, 1000 rpm, and 1200 rpm for 1 minute respectively.
[0094] (4) Slowly add the remaining silver powder and stir it manually. After all the silver powder is evenly mixed, put it into the centrifugal disperser and centrifuge it at 800 rpm, 1000 rpm, 1200 rpm, and 1600 rpm for 1 min respectively. After centrifugation, use a three-roller mill to shear and disperse the slurry until the slurry fineness reaches less than 2 μm, and then stop the three rollers.
[0095] (5) Use a 500-mesh sieve to filter out impurities and uneven large particles in the slurry to obtain a low-resistivity, low-temperature solar silver paste.
[0096] Example 5
[0097] A low-resistivity, low-temperature solar silver paste comprises the following components by mass percentage: 87% silver powder, 5% resin, 1% diluent, 2% curing agent, 0.2% thixotropic agent, 0.2% catalyst and 4.6% organic solvent.
[0098] The silver powder is a flaky powder with a D50 of 3.0 μm and a tap density of 4.5 g / mL, which accounts for 10% of the slurry; and a spherical powder with a D50 of 1 μm, a tap density of 5.8 g / mL, a D10 of 0.1 μm, a D100 of 3 μm, and a wide particle size distribution, which accounts for 77% of the slurry. The spherical powder is a ball powder.
[0099] The epoxy resin is the main resin: 3% of phenoxy resin PKFE and 1.5% of bisphenol A epoxy resin JER 828, and the auxiliary resin is 0.5% of AC166B.
[0100] Diluent: 1% hexahydrobisphenol A diglycidyl ether.
[0101] Curing agent: It includes isocyanate curing agent and auxiliary curing agent, specifically 1.5% G282 isocyanate curing agent, the unblocking temperature is 80°C, and the auxiliary curing agent is 0.5% benzimidazole.
[0102] Thixotropic agent: 0.2% polyamide wax.
[0103] Catalyst: 0.1% XC2007.
[0104] Organic solvent: 3% diethylene glycol butyl ether acetate.
[0105] A method for preparing low-resistivity low-temperature solar silver paste comprises the following steps:
[0106] (1) 4.6% of diethylene glycol butyl ether acetate organic solvent is mixed in a reaction kettle, 5% of a polymer resin is gradually added, the mixture is heated to 90° C., stirred at a speed of 260 r / min until the resin is completely dissolved, allowed to stand, cooled to room temperature, and filtered through a 300-400 mesh cloth to obtain a resin solution;
[0107] (2) taking the prepared resin solution, gradually adding 0.1% XC2007, 0.2% polyamide wax thixotropic agent, 1% hexahydrobisphenol A diglycidyl ether, 1.5% G282 isocyanate curing agent and 0.5% benzimidazole auxiliary curing agent, centrifugally dispersed at 800 rpm for 2 minutes, and fully mixed to obtain an organic carrier;
[0108] (3) Slowly add silver powder and stir it manually. After all the silver powder is evenly mixed, put it into the centrifugal disperser and centrifuge it at 800 rpm, 1000 rpm, 1200 rpm, and 1600 rpm for 1 min respectively. After centrifugation, use a three-roller mill to shear and disperse the slurry until the slurry fineness reaches less than 2 μm, and then stop the three rollers.
[0109] (4) Using a 500-mesh sieve to filter out impurities and uneven large particles in the slurry, a low-resistivity, low-temperature solar silver paste is obtained.
[0110] Comparative Example 1
[0111] A solar silver paste comprises the following components by mass percentage: 93% silver powder, 1.5% resin, 1% epoxy diluent, 1.3% curing agent, 0.2% thixotropic agent, 0% catalyst and 3% organic solvent.
[0112] The silver powder is composed of flaky powder accounting for 5% of the slurry, with a D50 of 3.0 μm and a tap density of 4.5 g / mL, and spherical powder accounting for 85% of the slurry, with a D50 of 2 μm and a tap density of 6 g / mL.
[0113] Epoxy resin as main resin: 0.5% phenoxy resin PKHH and 1.3% bisphenol A epoxy resin JER827, auxiliary resin: none.
[0114] Epoxy diluent: 1% resorcinol diglycidyl ether.
[0115] Curing agent: comprising isocyanate curing agent and auxiliary curing agent, specifically 1% G282 isocyanate curing agent, auxiliary curing agent: none.
[0116] Thixotropic agent: 0.2% polyamide wax.
[0117] Catalyst: None.
[0118] Organic solvent: 3% diethylene glycol butyl ether acetate.
[0119] A method for preparing solar silver paste comprises the following steps:
[0120] (1) 3% of diethylene glycol butyl ether acetate organic solvent is mixed in a reaction kettle, 1.5% of a polymer resin is gradually added, the mixture is heated to 85° C., stirred at a speed of 260 r / min until the resin is completely dissolved, allowed to stand, cooled to room temperature, and filtered through a 300-400 mesh cloth to obtain a resin solution;
[0121] (2) taking the prepared resin solution, gradually adding 0.2% polyamide wax thixotropic agent, 1% resorcinol diglycidyl ether, and 1% G282 isocyanate curing agent, centrifugally dispersing at 800 rpm for 2 minutes, and fully mixing to obtain an organic carrier;
[0122] (3) Take the prepared organic carrier, add 93% silver powder, and stir manually. After all the silver powder is evenly stirred, centrifuge and disperse it at 800 rpm, 1000 rpm, 1200 rpm, and 1600 rpm for 1 min respectively. After centrifugation, use a three-roller mill to shear and disperse the slurry until the slurry fineness reaches less than 2 μm, and then stop the three rollers.
[0123] (4) Use a 500-mesh sieve to filter out impurities and uneven large particles in the slurry to obtain a finished silver paste.
[0124] Comparative Example 2
[0125] A solar silver paste comprises the following components by mass percentage: 93% silver powder, 1.5% polymer resin, 1% diluent, 1.3% curing agent, 0.2% thixotropic agent, 0% catalyst and 3% organic solvent.
[0126] The silver powder is composed of flake powder with D50 of 3.0 μm and tap density of 4.5 g / mL, spherical powder with D50 of 0.6 μm and tap density of 4.8 g / mL, and spherical powder with D50 of 2 μm and tap density of 6 g / mL, which accounts for 5% of the slurry.
[0127] The polymer resin is the main resin: 0.5% of phenoxy resin PKHH and 0.7% of bisphenol A epoxy resin JER827, and the auxiliary resin is none.
[0128] Diluent: 1% resorcinol diglycidyl ether.
[0129] Curing agent: comprising isocyanate curing agent and auxiliary curing agent, specifically 1.3% G282 isocyanate curing agent, auxiliary curing agent: none.
[0130] Thixotropic agent: 0.2% polyamide wax.
[0131] Catalyst: None.
[0132] Organic solvent: 3% diethylene glycol butyl ether acetate.
[0133] A method for preparing solar silver paste comprises the following steps:
[0134] (1) 3% of diethylene glycol butyl ether acetate organic solvent is mixed in a reaction kettle, 1.5% of a polymer resin is gradually added, the mixture is heated to 85° C., stirred at a speed of 260 r / min until the resin is completely dissolved, allowed to stand, cooled to room temperature, and filtered through a 300-400 mesh cloth to obtain a resin solution;
[0135] (2) taking the prepared resin solution, gradually adding 0.2% polyamide wax thixotropic agent, 1% resorcinol diglycidyl ether, and 1.3% G282 isocyanate curing agent, centrifugally dispersing at 800 rpm for 2 minutes, and fully mixing to obtain an organic carrier;
[0136] (3) Take the prepared organic carrier, add 10% D50 0.6 μm spherical powder and stir, then put it into a centrifugal disperser and centrifuge and stir at speeds of 800 rpm, 1000 rpm and 1200 rpm for 1 min respectively.
[0137] (4) Slowly add the remaining silver powder and stir it manually. After all the silver powder is evenly mixed, put it into the centrifugal disperser and centrifuge it at 800 rpm, 1000 rpm, 1200 rpm, and 1600 rpm for 1 min respectively. After centrifugation, use a three-roller mill to shear and disperse the slurry until the slurry fineness reaches less than 2 μm, and then stop the three rollers.
[0138] (5) Use a 500-mesh sieve to filter out impurities and uneven large particles in the slurry to obtain a finished silver paste.
[0139] Comparative Example 3
[0140] A solar silver paste comprises the following components by mass percentage: 93% silver powder, 1.5% polymer resin, 1% diluent, 1.3% curing agent, 0.2% thixotropic agent, 0% catalyst and 3% organic solvent.
[0141] The silver powder is composed of 5% flaky powder with a D50 of 3.0 μm and a tap density of 4.5 g / mL, 10% spherical powder with a D50 of 0.6 μm and a tap density of 4.8 g / mL, 55% spherical powder with a D50 of 2 μm and a tap density of 6 g / mL, and 23% spherical powder with a D50 of 1 μm and a tap density of 5.8 g / mL.
[0142] The polymer resin is the main resin: 0.5% of phenoxy resin PKHH and 0.7% of bisphenol A epoxy resin jER827, and the auxiliary resin is none.
[0143] Diluent: 1% resorcinol diglycidyl ether.
[0144] Curing agent: comprising isocyanate curing agent and auxiliary curing agent, specifically 1.3% G282 isocyanate curing agent, auxiliary curing agent: none.
[0145] Thixotropic agent: 0.2% polyamide wax.
[0146] Catalyst: None.
[0147] Organic solvent: 3% diethylene glycol butyl ether acetate.
[0148] A method for preparing solar silver paste comprises the following steps:
[0149] (1) 3% of diethylene glycol butyl ether acetate organic solvent is mixed in a reaction kettle, 1.5% of a polymer resin is gradually added, the mixture is heated to 85° C., stirred at a speed of 260 r / min until the resin is completely dissolved, allowed to stand, cooled to room temperature, and filtered through a 300-400 mesh cloth to obtain a resin solution;
[0150] (2) taking the prepared resin solution, gradually adding 0.2% polyamide wax thixotropic agent, 1% resorcinol diglycidyl ether, and 1.3% G282 isocyanate curing agent, centrifugally dispersing at 800 rpm for 2 minutes, and fully mixing to obtain an organic carrier;
[0151] (3) Take the prepared organic carrier, add 10% D50 0.6 μm spherical powder and stir, then put it into a centrifugal disperser and centrifuge and stir at speeds of 800 rpm, 1200 rpm and 1600 rpm for 2 minutes respectively.
[0152] (4) Slowly add the remaining silver powder and stir it manually. After all the silver powder is evenly mixed, put it into the centrifugal disperser and centrifuge it at 800 rpm, 1000 rpm, 1200 rpm, and 1600 rpm for 1 min respectively. After centrifugation, use a three-roller mill to shear and disperse the slurry until the slurry fineness reaches less than 2 μm, and then stop the three rollers.
[0153] (5) Use a 500-mesh sieve to filter out impurities and uneven large particles in the slurry to obtain a finished silver paste.
[0154] Comparative Example 4
[0155] A solar silver paste comprises the following components by mass percentage: 93% silver powder, 1.5% polymer resin, 1% epoxy diluent, 1.3% curing agent, 0.2% thixotropic agent, 0% catalyst and 3% organic solvent.
[0156] The silver powder is composed of 5% flaky powder with a D50 of 3.0 μm and a tap density of 4.5 g / mL, 10% spherical powder with a D50 of 0.6 μm and a tap density of 5.3 g / mL, 55% spherical powder with a D50 of 2 μm and a tap density of 6 g / mL, and 23% spherical powder with a D50 of 1 μm and a tap density of 5.8 g / mL.
[0157] The polymer resin is the main resin: 0.5% of phenoxy resin PKHH and 0.7% of bisphenol A epoxy resin jER827, and the auxiliary resin is 0.3% of 2000ML.
[0158] Epoxy diluent: 1% resorcinol diglycidyl ether.
[0159] Curing agent: comprising isocyanate curing agent and auxiliary curing agent, specifically 1.1% G282 isocyanate curing agent, auxiliary curing agent: none.
[0160] Thixotropic agent: 0.2% polyamide wax.
[0161] Catalyst: None.
[0162] Organic solvent: 3% diethylene glycol butyl ether acetate.
[0163] A method for preparing solar silver paste comprises the following steps:
[0164] (1) 3% of diethylene glycol butyl ether acetate organic solvent is mixed in a reaction kettle, 2.3% of a polymer resin is gradually added, the mixture is heated to 70-95° C., stirred at a speed of 260 r / min until the resin is completely dissolved, allowed to stand, cooled to room temperature, and filtered through a 300-400 mesh cloth to obtain a resin solution;
[0165] (2) taking the prepared resin solution, gradually adding 0.2% polyamide wax thixotropic agent, 1% resorcinol diglycidyl ether, and 1.1% G282 isocyanate curing agent, centrifugally dispersing at 800 rpm for 2 minutes, and fully mixing to obtain an organic carrier;
[0166] (3) Take the prepared organic carrier, add 10% D50 0.6 μm spherical powder and stir, then put it into a centrifugal disperser and centrifuge and stir at speeds of 800 rpm, 1000 rpm and 1200 rpm for 1 min respectively.
[0167] (4) Slowly add the remaining silver powder and stir it manually. After all the silver powder is evenly mixed, put it into the centrifugal disperser and centrifuge it at 800 rpm, 1000 rpm, 1200 rpm, and 1600 rpm for 1 min respectively. After centrifugation, use a three-roller mill to shear and disperse the slurry until the slurry fineness reaches less than 2 μm, and then stop the three rollers.
[0168] (5) Use a 500-mesh sieve to filter out impurities and uneven large particles in the slurry to obtain a finished silver paste.
[0169] Comparative Example 5
[0170] A solar silver paste comprises the following components by mass percentage: 93% silver powder, 1.5% polymer resin, 1% epoxy diluent, 1.3% curing agent, 0.2% thixotropic agent, 0% catalyst and 3% organic solvent.
[0171] The silver powder is composed of 5% of the slurry, with a D50 of 3.0 μm and a tap density of 4.5 g / mL of flake powder; 10% of the slurry, with a D50 of 0.6 μm and a tap density of 4.8 g / mL of spherical powder; 55% of the slurry, with a D50 of 2 μm and a tap density of 6 g / mL of spherical powder; and 23% of the slurry, with a D50 of 1 μm and a tap density of 5.8 g / mL of spherical powder.
[0172] The polymer resin is the main resin: 0.5% phenoxy resin PKHH and 0.7% bisphenol A epoxy resin JER827, and the auxiliary resin is 0.3% 2000ML.
[0173] Epoxy diluent: 1% resorcinol diglycidyl ether.
[0174] Curing agent: comprising isocyanate curing agent and auxiliary curing agent, specifically 1.1% G282 isocyanate curing agent, auxiliary curing agent: 0.2% benzimidazole.
[0175] Thixotropic agent: 0.2% polyamide wax.
[0176] Catalyst: None.
[0177] Organic solvent: 3% diethylene glycol butyl ether acetate.
[0178] A method for preparing solar silver paste comprises the following steps:
[0179] (1) 3% of diethylene glycol butyl ether acetate organic solvent is mixed in a reaction kettle, 1.5% of a polymer resin is gradually added, the mixture is heated to 85° C., stirred at a speed of 260 r / min until the resin is completely dissolved, allowed to stand, cooled to room temperature, and filtered through a 300-400 mesh cloth to obtain a resin solution;
[0180] (2) taking the prepared resin solution, gradually adding 0.2% polyamide wax thixotropic agent, 1% resorcinol diglycidyl ether, 1.1% G282 isocyanate curing agent and 0.2% benzimidazole auxiliary curing agent, centrifugally dispersing at 800 rpm for 2 minutes, and fully mixing to obtain an organic carrier;
[0181] (3) Take the prepared organic carrier, add 10% D50 0.6 μm spherical powder and stir, then put it into a centrifugal disperser and centrifuge and stir at speeds of 800 rpm, 1000 rpm and 1200 rpm for 1 min respectively.
[0182] (4) Slowly add the remaining silver powder and stir it manually. After all the silver powder is evenly mixed, put it into the centrifugal disperser and centrifuge it at 800 rpm, 1000 rpm, 1200 rpm, and 1600 rpm for 1 min respectively. After centrifugation, use a three-roller mill to shear and disperse the slurry until the slurry fineness reaches less than 2 μm, and then stop the three rollers.
[0183] (5) Use a 500-mesh sieve to filter out impurities and uneven large particles in the slurry to obtain a finished silver paste.
[0184] Test example:
[0185] The silver pastes prepared in Examples 1 to 5 and Comparative Examples 1 to 5 were prepared into patterns and cured in an oven at 200°C for 30 minutes. The resistance after curing was measured, and the resistivity was calculated using the resistivity formula. The overlap resistance was calculated using the intercept method, and the viscosity was tested using a plate viscometer. The viscosity ratio corresponding to the intercept rate of 4.62 rpm and 46.6 rpm was recorded as the thixotropic index. The measurement results are shown in Table 1.
[0186] Table 1
[0187]
[0188] As shown in Table 1 above, in Comparative Example 3, compared with Comparative Examples 1-2, the silver powder particle size distribution and silver powder combination are improved, and the resistivity and overlap resistance of the slurry are significantly reduced. This may be because these particle size powders enter and fill the gaps between the original silver powders, improve the effective contact points of the silver powders, and improve the resistivity, while also improving the overlap resistance. In Comparative Example 4, compared with Comparative Example 3, the viscosity of the substrate decreases, the thixotropic index increases, and the resistivity and overlap resistance decrease. It may be that the addition of small molecular polyester improves the viscosity of the slurry, and it has a small amount of hydroxyl groups, which increases the hydrogen bonds of the resin of the slurry and forms a gel-like state. This state is conducive to increasing its thixotropy. This type of resin itself has flexibility and multi-functionality, which improves the rigidity of the original epoxy system of the slurry, thereby promoting its resistivity to decrease, increasing adhesion, and improving overlap impedance. The viscosity of Comparative Example 5 is not significantly different from that of Comparative Example 4. The resistivity and overlapping impedance of Comparative Example 5 are reduced. This may be because the use of imidazole curing agent forms a dual curing effect, improves the curing speed and degree of the slurry, reduces resistance, increases adhesion, and thus improves the overlapping effect.
[0189] Compared with comparative example 5, the resistivity and lap impedance of Example 1 are slightly reduced. The catalyst may increase the dual curing effect and promote the reduction of resistivity and lap resistance, but the impact on the overall performance is not as strong as the latter. Compared with comparative example 5, Example 1 improves the thixotropic index and reduces the viscosity while reducing the resistivity and lap resistance. Compared with the raw materials of Example 1, Example 2 replaces the multi-powder combination scheme with a single silver powder with a wide distribution, but the mechanism of introducing powders of different particle sizes to improve its particle size distribution is consistent with that of Implementation 1, which improves the effective spatial stacking of silver powder. Its resistivity and lap impedance are also smaller than those of Comparative Examples 1 to 5, indicating that a single silver powder with a wide distribution can also have a good spatial stacking effect. However, the lap impedance is larger than that of Implementation 1, which may be related to the small number of small particle size powders. Compared with Example 1, Example 3 changes the resin and its ratio, and finds that its resistivity and lap impedance can also be smaller than those of Comparative Examples 1 to 5, indicating that the resin combination is conducive to improving the conductive properties of the slurry. Compared with Example 1, the viscosity and resistivity of Example 4 and Example 5 are both reduced. Example 4 increases the content of diluent to reduce viscosity, but excessive diluent may cause insufficient curing, resulting in a decrease in resistivity. Example 5 increases the proportion of resin, which reduces the viscosity of the entire slurry. However, the reduction in silver content still brings about the problem of poor resistivity. Therefore, the proportion of flake powder is increased in this example, and the resistivity of the slurry is improved by increasing the content of flake powder.
[0190] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A low resistivity, low temperature solar silver paste, It is characterized in that The raw materials of the silver paste include the following components by mass percentage: 87-93% silver powder, 2-5% resin, 1-2% diluent, 0.5-2% curing agent, 0.01-1% thixotropic agent, 0.01-1% catalyst, and 2-5% organic solvent; The silver powder is composed of flaky powder and spherical powder; the mass ratio of the flaky powder to the spherical powder is 0.01-0.3:1; the spherical powder is one or both of spherical powder and spherical-like powder; The spherical powder is spherical powder I or spherical powder II; the spherical powder I, in terms of weight percentage, includes spherical powders of the following particle sizes: 5-15% D50 is 0.05-0.8 μm, and the tap density is 3-5 g / mL; 65-80% D50 is 2-4 μm, and the tap density is 5-8 g / mL; 14-30% D50 is 1-1.8 μm, and the tap density is 4-6 g / mL; the particle size distribution of the spherical powder II satisfies: D50 is 0.8-1.5 μm, D10 is 0.05-0.5 μm, and D100 is 2-5 μm; The resin is composed of a main resin and an auxiliary resin; the main resin is two or more of bisphenol A epoxy resin, phenoxy resin, bisphenol F epoxy resin, aliphatic epoxy resin, silicone modified epoxy, polyether modified epoxy resin, and epoxidized rubber; the auxiliary resin is at least one of polyether polyol, acrylate polyol, polyester polyol, polyurethane resin, polyester resin, and acrylic resin; the mass ratio of the main resin to the auxiliary resin is 1 to 10:1; The curing agent consists of a main curing agent and an auxiliary curing agent; the main curing agent is a blocked isocyanate curing agent with a deblocking temperature of 80 to 150° C.; the auxiliary curing agent is one or more of an imidazole curing agent, an acid anhydride curing agent, and a dicyandiamide curing agent; the mass ratio of the main curing agent to the auxiliary curing agent is 1.5 to 5:
1.
2. The low resistivity, low temperature solar silver paste according to claim 1, It is characterized in that The D50 of the flaky powder is 2 to 8 μm, and the tap density is 4 to 6 g / mL.
3. The low resistivity, low temperature solar silver paste according to claim 1, It is characterized in that The diluent is epoxy glycidyl ether, and the diluent is one or more of ethylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, 1,4-butanediol diglycidyl ether, glycerol triglycidyl ether, pentaerythritol glycidyl ether, resorcinol diglycidyl ether, trimethylolpropane triglycidyl ether, hexahydrobisphenol A diglycidyl ether, terephthalic acid diglycidyl ether, and sorbitol glycidyl ether.
4. The low resistivity low temperature solar silver paste according to claim 1, It is characterized in that The thixotropic agent is one or more of fumed silica, organic bentonite, modified hydrogenated castor oil and polyamide wax.
5. The low resistivity low temperature solar silver paste according to claim 1, It is characterized in that The catalyst is one or more of CXC1612, CXC1614, XC9206, XC258, CXC1756, XC2007, Vicbase TC3630, VicbaseTC3633, and ICAM-8409; the organic solvent is one or more of propylene carbonate, ethylene glycol ethyl ether acetate, ethylene glycol butyl ether acetate, diethylene glycol butyl ether acetate, dimethyl adipate, diethyl adipate, propylene glycol methyl ether acetate, and terpineol.
6. A method for preparing the low resistivity, low temperature solar silver paste according to any one of claims 1 to 5, It is characterized in that The preparation method comprises the following steps, by mass percentage: (1) adding 2-5% of an organic solvent into a reaction kettle and mixing, then adding 2-5% of a resin, heating and stirring, cooling to room temperature, and filtering to obtain a resin solution; (2) adding 0.01-1% of a catalyst, 0.01-1% of a thixotropic agent, 0.5-2% of a curing agent, and 1-2% of a diluent to the resin solution prepared in step (1), and centrifugally dispersing the mixture to obtain an organic carrier; (3) adding 87-93% of silver powder to the organic carrier prepared in step (2), centrifugally dispersing, shearing and dispersing by a three-roll mill until the slurry fineness is less than 5 μm, filtering, and obtaining a low-resistivity, low-temperature solar silver paste; In step (1), the heating temperature is 70-95° C.; the stirring speed is 200-300 r / min, and the time is 1-2 h; In step (2), the centrifugal dispersion speed is 800-850 rpm and the time is 2-4 min; In step (3), the specific process of the centrifugal dispersion is: dispersing at 800 rpm, 1000 rpm, 1200 rpm, and 1600 rpm, respectively, for 1 to 3 minutes.