A composite film and device for oil-water separation with wide applicability and preparation method

By performing hot pressing and femtosecond laser treatment on titanium foil and polytetrafluoroethylene powder, an oil-water separation membrane with a wide range of adaptability was prepared, which solved the problem of the existing technology being difficult to simultaneously process light oil and water and heavy oil and water mixtures. , achieving efficient and long-life oil-water separation effect.

CN114986951BActive Publication Date: 2024-10-29YICHUN PINGSHUN ENVIRONMENTAL PROTECTION TECHNOLOGY CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202210519085.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-12
Publication Date
2024-10-29
Estimated Expiration
2042-05-12

AI Technical Summary

Technical Problem

Existing oil-water separation technology is difficult to simultaneously separate mixtures of light oil and water and heavy oil and water, and traditional methods have problems such as low efficiency, narrow application range, and secondary pollution.

Method used

Titanium foil and polytetrafluoroethylene (PTFE) powder are used to prepare composite films through a hot pressing process, and femtosecond laser is used for surface roughening and drilling to form superhydrophobic/superoleophilic and superhydrophilic/underwater superphobic The surface properties of oil are used to construct an oil-water separation membrane with a wide range of adaptability.

Benefits of technology

It achieves efficient separation of different types of oil-water mixtures, improves the separation rate and service life, and ensures the applicability and industrial application value of the device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114986951B_ABST
    Figure CN114986951B_ABST
Patent Text Reader

Abstract

The present invention is a composite film and device for oil-water separation with wide applicable performance and a preparation method, and relates to a method for preparing an oil-water separation film on a composite functional material using laser, the method uses titanium foil and polytetrafluoroethylene powder as raw materials, and adopts a hot pressing process to prepare a composite film in which the upper and lower layers are polytetrafluoroethylene and titanium foil respectively; using a femtosecond laser, the upper and lower surfaces of the composite film are respectively subjected to laser roughening treatment at a relatively low energy density, so that the surface of one side of polytetrafluoroethylene presents super-hydrophobic / super-oleophilic wetting characteristics, and the surface of one side of the titanium foil presents super-hydrophilic / underwater super-oleophobic wetting characteristics; the composite film after roughening is punched, and the two composite films prepared are respectively installed at the two ends of a "T-type" oil-water separation device, ensuring that the different sides of the film face the oil-water mixture, and obtaining an oil-water separation device with wide applicable performance. The present invention has the advantages of simple method, high efficiency, and low cost, and the prepared oil-water separation device has a wide range of applications, and can efficiently and massively process oil-water mixtures.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of functional materials and laser micro-processing, and more specifically, relates to a method for preparing an oil-water separation film on a composite functional material by using laser. Background Art

[0002] As the source of human life, water pollution has always attracted widespread attention. At present, many industries and fields, such as the petroleum industry, catering industry, metallurgy industry, mining industry, textile and leather industry, and national defense industry, produce a large amount of oily wastewater every year. If it is directly discharged, it will cause serious pollution to the water body; at the same time, frequent crude oil spills will cause a large number of animals and plants in the ocean and rivers to die, causing serious damage to their ecological balance. Therefore, how to deal with oily wastewater will become a global problem and challenge in solving environmental pollution problems.

[0003] In order to separate oily wastewater, distillation, gravity, centrifugation, flotation, adsorption, coagulation, salting out and biological methods can be used according to the different physical, chemical and biological characteristics of water and oil phases. However, these methods still have the disadvantages of high energy consumption, low efficiency, narrow scope of application and possible secondary pollution, which greatly limits their scope of application. Therefore, it is particularly urgent to develop a low-cost, high-efficiency and widely applicable oil-water separation technology.

[0004] Due to the inconsistency of the surface tension of the oil phase and the water phase, the wetting properties on the surface of some functional materials are inconsistent. By utilizing this difference in wettability, under the action of the liquid's own gravity or external pressure, one component can be selectively allowed to penetrate through the film micropores, while the other component cannot penetrate through the film micropores, thereby achieving the separation of the oil-water mixture. Compared with traditional separation technology, membrane separation technology has the advantages of low operating cost, high separation efficiency, no secondary pollution and a wide range of applications.

[0005] As a typical hydrophobic polymer material (intrinsic water contact angle is about 114°), polytetrafluoroethylene (PTFE) has become an ideal material for preparing oil-water separation membranes because of its good resistance to high and low temperatures, chemical corrosion resistance, aging resistance, and good electrical insulation.

[0006] Titanium is a rare metal with good high and low temperature resistance, excellent ductility and plasticity. At the same time, its hardness is comparable to that of steel, but its mass is only half of that of steel of the same volume. At room temperature, titanium metal does not react with most strong acids, strong bases, or even aqua regia, and has good corrosion resistance, making it another ideal material for preparing oil-water separation membranes.

[0007] Compared with other construction methods, laser processing technology has the advantages of a wide range of processable materials, good regional selective processing, low pollution, and non-contact. In particular, it can perform precision processing with the help of computer software control, which makes it show great advantages in the preparation of oil-water separation membranes.

[0008] At present, there are many methods for constructing oil-water separation films on different functional materials using different methods. Jun Liu et al. reported in the journal (Surface & Coatings Technology, 2016, 307: 171-176) that a superhydrophilic and underwater superoleophobic film was obtained by spraying chitosan-silicon nanoparticles on a stainless steel mesh. Although the preparation method is simple and efficient, the long-term applicability of the oil-water separation film is poor due to the low adhesion between the coating and the stainless steel substrate material. At the same time, its inherent superhydrophilic / superoleophobic wetting properties make it mainly suitable for separating mixtures formed by light oil and water, while the mixture formed by heavy oil and water, due to the high density of heavy oil, is in the lower layer of the solution. During the separation process, the heavy oil will form a barrier layer, making the separation of such oil-water mixtures difficult to achieve, and its application is subject to certain limitations. Zhongli Qin et al. proposed in the journal (Material & Design, 2019, 184: 108200-108208) that a film that can be used for oil-water separation can be prepared by using picosecond infrared laser to roughen the surface of polytetrafluoroethylene film first and then laser etch and drill holes. Although this preparation method can obtain films with different separation properties, due to its unique super-hydrophobic / super-oleophilic properties, it is mainly suitable for separating mixtures formed by heavy oil and water. For mixtures formed by light oil and water, the light oil has a low density, and the denser water layer below will form a barrier layer, making the separation of such oil-water mixtures more difficult to achieve. Chunai Dai et al. published a paper in the journal (Soft Matter, 2014, 10 (40): 8116-8122) on the preparation of super-hydrophobic / super-oleophilic oil-water separation membranes using copper mesh as the substrate by combining chemical oxidation and impregnation. In order to overcome the difficulty in separating the mixture of light oil and water (the water phase is located at the bottom of the oil-water mixture due to its high density, thus forming a barrier layer), the separation device is tilted at a certain angle to allow the light oil to penetrate and flow out of the separation device smoothly. However, the device is only suitable for the separation of oil-water mixtures with a small volume, and is difficult to adapt to the separation of large quantities of oil-water mixtures. In summary, although oil-water separation membranes with different properties can be successfully constructed by different methods, they all face the difficulty of being suitable for separating mixtures formed by light oil and water and mixtures formed by heavy oil and water at the same time, which limits their application range to a certain extent. Therefore, it is particularly necessary to find a membrane or device with a wide range of applications, which can be applied to the separation of large quantities of oil-water mixtures, and can be simply and efficiently implemented in industrial production. Summary of the invention

[0009] In view of the above defects or improvement needs of the prior art, the present invention provides a method for preparing an oil-water separation device with a wide range of applicable performance, which uses titanium foil and poly-PTFE powder as raw materials, and prepares a composite film material with upper and lower layers of titanium foil and PTFE respectively through a hot pressing process, and then uses a femtosecond laser to roughen the upper and lower surfaces of the composite material, and then uses a femtosecond laser to punch holes on the surface of the composite film material after double-sided roughening, thereby obtaining a film material with adjustable oil-water separation rate (flow rate), high separation efficiency, and suitable for separating different types of oil-water mixtures. This solves the technical problem that the existing oil-water separation film cannot be used for large-scale separation of mixtures formed by light oil and water and mixtures formed by heavy oil and water at the same time.

[0010] In order to achieve the above object, according to one aspect of the present invention, a method for preparing a composite film for oil-water separation with wide applicable performance is provided, comprising the following steps:

[0011] (S1) Preparation of composite film: Titanium foil and PTFE powder are used as raw materials, and a composite film material with a PTFE layer and a titanium foil layer as the upper and lower layers is prepared by hot pressing process; before the hot pressing process is implemented, the roughened titanium foil is ultrasonically cleaned in acetone, ethanol and distilled water for 10 min, and after drying, a layer of silane coupling agent is coated on its surface; and a layer of PTFE powder is covered on its surface;

[0012] (S2) Laser roughening the surface of the composite material: using a femtosecond laser to perform laser scanning on the upper and lower surfaces of the composite material in step (S1), respectively, so that the surface of the PTFE side of the composite material exhibits super hydrophobic / super oleophilic wetting properties, and the surface of the titanium foil side exhibits super hydrophilic / underwater super oleophobic wetting properties;

[0013] (S3) laser drilling: setting an appropriate laser drilling spacing and drilling diameter, and using a femtosecond laser to perform laser drilling on the surface of the composite film material in step (2), thereby obtaining an oil-water separation film with excellent adaptability;

[0014] (S4) Preparation of oil-water separation device: Take two oil-water separation composite films prepared in step (3), one of which has its PTFE side facing the inside of the device, and the other has its titanium foil side facing inward, and fix them respectively on both sides of a "T-shaped" oil-water separation device, thereby obtaining a device that can separate different types of oil-water mixtures in large quantities.

[0015] Preferably, in the above step (S1), the thickness of the titanium foil is 0.05-1.00 mm;

[0016] Preferably, the total thickness of the composite film material prepared in the above step (S1) wherein the upper and lower layers are respectively a polytetrafluoroethylene layer and a titanium foil layer is 0.10-2.00 mm.

[0017] Preferably, in the composite film material preparation process in the above step (S1), the hot pressing temperature is 330-450°C, the hot pressing pressure is 2-6Mpa, and the hot pressing time is preferably 0.5-1.5h.

[0018] Preferably, the laser scanning method in the above step (S2) is grid scanning, and the laser scanning etching will construct a rough surface composed of micrometer size and nanometer size on the upper surface and lower surface of the composite film material respectively;

[0019] The wavelength of the femtosecond laser in step (S2) is in the infrared, visible or ultraviolet band, the laser power is preferably 0.5-10W, the laser pulse frequency is preferably 200KHz-1MHz, the laser scanning line spacing is preferably 6-50μm, and the laser scanning speed is preferably 100-1500mm / s.

[0020] Preferably, in the above step (S2), after the composite film is roughened by laser, the water static contact angle of the PTFE side surface is greater than 150°, and the oil static contact angle is less than 10°. After the composite film is roughened by laser, the oil static contact angle of the titanium foil side surface under water is greater than 150°, and the water static contact angle is less than 10°.

[0021] Preferably, the step (S3) above adopts femtosecond laser drilling, and the hole punched is preferably a tapered through hole. The through hole is preferably laser-drilled from one side of the roughened titanium foil, and the radius of the tapered through hole is 0.5 μm-200 μm.

[0022] A composite film for oil-water separation with wide applicable performance, the composite film is divided into an upper layer and a lower layer, the upper layer and the lower layer are a PTFE layer and a titanium foil layer respectively; wherein the surface of one side of the PTFE exhibits super-hydrophobic / super-oleophilic wetting properties; the surface of one side of the titanium foil exhibits super-hydrophilic / underwater super-oleophobic wetting properties; the total thickness of the composite film material of the PTFE layer and the titanium foil layer is 0.10-2.00 mm; the surface of the composite film material is laser-punched, and the distance between the holes is 250 μm.

[0023] Preferably, the diameter of the pores is 20 to 160 μm.

[0024] Preferably, the composite film is made of titanium foil and PTFE powder as raw materials, and a hot pressing process is adopted to prepare a composite film material in which the upper and lower layers are PTFE layer and titanium foil layer respectively.

[0025] An oil-water separation device, wherein the two composite films are respectively installed positively and negatively at the two ends of the oil-water separation device.

[0026] In general, the above technical solutions conceived by the present invention can achieve the following beneficial effects compared with the prior art:

[0027] (1) The present invention specifically selects titanium foil as the raw material for preparing the composite film. First, after laser processing, the surface of the titanium foil exhibits superhydrophilicity and underwater superoleophobicity, making it an ideal film material for preparing oil-water mixture separation. Secondly, the titanium foil has good resistance to high and low temperatures and acid and alkali corrosion, so that the separation film prepared from the titanium foil can be used in any harsh environment, effectively improving the applicability of the prepared composite film in separating oil-water mixtures. Finally, as a metal material, titanium foil has excellent mechanical strength. Using it as a raw material to prepare oil-water separation film materials can effectively improve the performance of the composite film material in supporting the gravity destruction of the oil-water mixture and extend the actual application life of the composite film.

[0028] (2) In the present invention, PTFE powder is specially selected as the raw material for preparing the composite film. First, PTFE is a typical hydrophobic material. After laser processing, the surface of PTFE exhibits super-hydrophobic and super-oleophilic properties, which is another ideal material for preparing the separation of oil-water mixture. Secondly, PTFE has good resistance to high and low temperatures, chemical corrosion, and aging, so that the separation film prepared by PTFE can be used in any harsh environment, effectively improving the applicability of the prepared composite film material.

[0029] (3) In the present invention, the surface of one side of the titanium foil of the composite film material exhibits superhydrophilicity and underwater superoleophobicity, while the surface of the polytetrafluoroethylene side exhibits superhydrophobicity and superoleophilicity, and the wetting properties of the two surfaces are exactly opposite. Utilizing the opposite wetting properties, in the design of an actual oil-water separation device, when one side of the titanium foil of the composite film material faces the oil-water mixture, the water phase in the mixture can selectively permeate and pass through the composite film material, while the oil phase cannot; and when the PTFE side of the composite film material faces the oil-water mixture, the oil phase in the mixture can selectively permeate and pass through the composite film material, while the water phase cannot. Therefore, in the design of the oil-water separation device, two processed composite film materials are set, and the different sides of the two film materials are facing the oil-water mixture, which can ensure that the oil phase and the water phase can simultaneously permeate and pass through the two films, thereby ensuring that the device can be used to separate various types of oil-water mixtures.

[0030] (4) By utilizing the characteristics of laser processing, such as high precision, good controllability and high efficiency, and the characteristics that the process parameters and processing graphics of the processing process can be quickly changed and designed directly by the computer, it is possible to achieve high-efficiency preparation of oil-water separation membranes with different separation rates (flow rates) and sizes, making it have strong engineering application value. (5) Under the same experimental conditions, the present invention can increase the oil-water separation rate by about 50% and increase the service life to 2.9 times the original service life. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 Composite film preparation process flow chart;

[0032] The process is as follows: titanium foil surface sandblasting roughening treatment → cleaning → surface modification → powder coating → hot pressing → composite film;

[0033] Figure 2 The process flow chart of preparing the composite film with oil-water separation function is as follows: laser roughening the surface of one side of the titanium foil → laser roughening the surface of one side of the polytetrafluoroethylene → laser drilling;

[0034] Figure 3 Scanning electron microscope image of the surface morphology of the oil-water composite film obtained after laser roughening and drilling (observed from the polytetrafluoroethylene side);

[0035] Figure 4 (a) and (b) are schematic diagrams of the static contact angles of water and oil (1,2-dichloroethane) on one side of the tetrafluoroethylene composite film prepared in step (2);

[0036] Figure 5 (a) and (b) are schematic diagrams of the static contact angles of water and oil (1,2-dichloroethane) on one side of the composite thin film titanium foil prepared in step (2);

[0037] Figure 6 Schematic diagram of the design of the prepared membrane for oil-water mixture separation device. DETAILED DESCRIPTION

[0038] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In addition, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0039] The present invention provides a method for preparing an oil-water separation device with wide applicable performance, characterized in that it comprises the following steps:

[0040] (1) Preparation of composite film: Titanium foil and PTFE powder are used as raw materials, and a hot pressing process is adopted to prepare a composite film material with a polytetrafluoroethylene layer and a titanium foil layer as the upper and lower layers. In step (1), since polytetrafluoroethylene and titanium foil are heterogeneous materials, the bonding strength between them is not high. In order to improve the bonding strength between the two materials in the prepared composite film, before the hot pressing process is implemented, the pressing surface of the titanium foil is first treated by sandblasting, which can effectively improve the roughness of the titanium foil surface, thereby increasing the mechanical interlocking force between the two materials and increasing the bonding strength; at the same time, the silane coupling agent is applied to the roughened titanium foil surface, which can effectively improve the interface performance between the titanium foil and the PTFE material and increase the bonding strength.

[0041] (2) Laser roughening of the composite surface: The upper and lower surfaces of the composite material obtained in step (1) are laser roughened using a femtosecond laser. By changing the laser processing parameters, the surface of the composite material PTFE side shows superhydrophobic / superoleophilic wetting properties, while the surface of the titanium foil side shows superhydrophilic / underwater superoleophobic wetting properties. In step (2), the purpose of laser processing the upper and lower surfaces of the composite material is to increase the roughness of the upper and lower surfaces, so that the PTFE surface exhibits superhydrophobic / superoleophilic wetting properties, while the titanium foil surface exhibits superhydrophilic and underwater superoleophobic wetting properties. In the process of roughening the upper and lower surfaces of the composite film material, due to the different etching thresholds of the PTFE and titanium foil materials, the selected laser processing parameters are inconsistent. However, due to the limitation of the thin thickness of the prepared composite film, the laser processing parameters used for surface roughening are usually carried out at a lower laser power and a faster scanning rate. If the laser processing power is too high, the material on the upper or lower surface of the composite film will be completely etched away.

[0042] (3) Laser drilling: Set appropriate laser drilling spacing and aperture, and use femtosecond laser to perform laser drilling on the surface of the composite film material obtained in step (2), so as to obtain an oil-water separation film with a wide range of adaptability. In step (3), the purpose of the laser processing method is to construct through holes of different apertures in the composite film obtained in (2) according to the requirements of the engineering design. Since the composite film material needs to be punched through, the required laser power is relatively large and the scanning speed is relatively low during the processing. However, in order to prevent the existence of thermal effects during the processing from causing the constructed through holes to deform, thereby affecting the oil-water separation performance of the film, it is usually required that the laser scanning speed used in the drilling process should not be too low. The hole shape is preferably a conical through hole with a small bottom and a large top, that is, a large hole close to the laser gun.

[0043] (4) Preparation of oil-water separation device: Take two composite films prepared in (3), fix them on both sides of the "T-shaped" oil-water separation device, and place different sides of the two film materials facing the oil-water mixture. The simultaneous use of two composite film materials in step (4) is to ensure that when the prepared oil-water separation device separates any type of oil-water mixture, the presence of a certain liquid phase in the oil-water mixture will not become a barrier layer for another liquid phase in the separation process, thereby ensuring that the oil-water separation device has a wide range of applicability. In step (4), the orientations of the two oil-water separation films must be kept inconsistent, that is, the titanium foil surface of one of the films faces the oil-water mixture to be separated. Since the surface exhibits superhydrophilic and underwater superoleophobic wetting properties, the water phase in the mixture will penetrate and pass through the film, while the oil phase will be blocked and cannot pass through; at the same time, the PTFE surface of the other film faces the oil-water mixture to be separated. Since the surface exhibits superhydrophobic / superoleophilic wetting properties, the oil phase in the mixture will penetrate and pass through the film, while the water phase will be blocked and cannot pass through. Therefore, by simply utilizing the different orientations of the two oil-water separation composite films, the oil phase and water phase in different types of oil-water mixtures can be separated from the two films respectively, effectively improving its scope of application.

[0044] In a preferred embodiment, the purpose of roughening the titanium foil surface by sandblasting in step (1) of the present invention is to improve the bonding strength between the titanium foil and PTFE in the prepared composite film, and to prevent peeling due to poor bonding between the material layers during subsequent use. Since the surface of the titanium foil raw material used in the present invention is relatively smooth, if PTFE powder is directly applied to its surface and subjected to a hot pressing process, the bonding strength between the two material layers is usually not high. Therefore, the roughness of the titanium foil surface can be increased by sandblasting, which is conducive to the formation of a mechanical locking structure that is mutually hooked and interlocked between the titanium foil layer and the PTFE layer at the interface, thereby enhancing the bonding strength between the two material layers.

[0045] The present invention selects sandblasting to roughen the surface of the titanium foil because sandblasting has high efficiency, low cost, simple and convenient operation.

[0046] In a preferred embodiment, the purpose of treating the titanium foil surface with a silane coupling agent in step (1) of the present invention is also to improve the bonding strength between the titanium foil layer and the PTFE material in the composite film. Titanium foil and PTFE are two heterogeneous materials, metal and organic, respectively, and their interface properties are poor. As a classic interface modifier, the use of silane coupling agent can effectively improve the bonding strength between the two materials.

[0047] In the preparation of the composite film of the present invention, the hot pressing process is preferably 330-450° C., the hot pressing pressure is preferably 2-6 MPa, and the hot pressing time is preferably 0.5-1.5 h.

[0048] In some embodiments, the total thickness of the prepared composite film material is 0.10-2.00 mm, wherein the thickness of the titanium foil material is 0.05-1.00 mm.

[0049] In some embodiments, the laser scanning method used in step (2) to roughen the surfaces on both sides of the composite film is preferably grid scanning. The laser etching roughening can construct a conical micron-sized protrusion structure on the film surface. At the same time, the surface of the micron protrusion structure is also covered with a large number of nano protrusions and hole structures. The rough structure makes the wettability of the constructed surface is isotropic.

[0050] According to the Wenzel model in wetting theory, it can be seen that the presence of rough structures will amplify the wettability of the solid surface. Therefore, laser roughening treatment will make the surface of one side of the composite film PTFE more hydrophobic and oleophilic, making it a super-hydrophobic / super-oleophilic surface. At the same time, the hydrophilicity and oleophobicity of the titanium foil surface after roughening treatment are stronger, making it a super-hydrophilic / underwater super-oleophobic surface. Therefore, laser roughening will amplify the wettability of the surfaces on both sides of the composite material at the same time, and the wettability on both sides is completely opposite.

[0051] The present invention utilizes the difference in wetting properties on both sides of the composite film, and it can be applied to separate different types of oil-water mixtures. Wherein, after coarsening, one side of the composite film PTFE presents super-hydrophobic / super-oleophilic wetting properties. If the surface is directed toward the oil-water mixture, only the oil phase therein can be passed, and the water phase cannot pass, and it is suitable for separating the mixture formed by heavy oil and water. And after coarsening, one side of the composite film titanium foil presents super-hydrophilic / underwater super-oleophobicity. If the surface is directed toward the oil-water mixture, only the water phase therein can be passed, and the oil phase cannot pass, and it is suitable for separating the mixture formed by light oil and water. Therefore, by utilizing the difference in the composite film direction after coarsening, different types of oil-water mixtures can be separated.

[0052] The present invention uses a high-power, low-scanning-speed laser to drill holes in a composite film, with the aim of constructing a large number of through holes in the composite film, so that under the action of the liquid's own gravity or external force, liquid close to the membrane material can penetrate and pass through, while liquid incompatible with the membrane material cannot spread on its surface and appears in a droplet shape. When the droplet radius is larger than the diameter of the through hole, even under the action of the liquid's own gravity or external force, it cannot penetrate and pass through the through hole, thereby achieving separation of the oil-water mixture.

[0053] The present invention utilizes computer software to accurately design the aperture of the processed through hole and the number of through holes per unit area. Combined with the characteristics of laser precision processing, oil-water separation films with different flow rates can be constructed according to the needs of engineering design, thereby meeting different engineering needs for oil-water separation.

[0054] In the present invention, the bond energy of the CF bond in the PTFE material is relatively large, and titanium foil belongs to a metal material. The laser etching thresholds of these two materials are relatively high. In order to obtain a better roughened surface and punched hole shape, a femtosecond laser is specially selected to roughen and punch the composite film, rather than a nanosecond laser and a picosecond laser. The main reason is that the pulse width of the femtosecond laser is in the femtosecond order, and the peak energy of the laser is high. In the process of processing the composite film, it is mainly "cold" etching, and there is less thermal effect during the etching process, making it easier to build a richer micro-nano structure on the surface of the composite film. However, nanosecond lasers and picosecond lasers have larger pulse widths, lower peak energy, and larger thermal effects during the processing process, resulting in fewer nanostructures when the surface is roughened, and the roughening effect is not ideal. At the same time, when using nanosecond lasers and picosecond lasers for punching, the larger thermal effect will also cause deformation problems in the punched through holes.

[0055] In a preferred embodiment, a "T-shaped" oil-water separation device is used in step (4) of the present invention. By utilizing the different orientations of the two oil-water separation composite membranes, the oil phase and the water phase in different types of oil-water mixtures can be separated from the two sides of the "T-shaped" oil-water separation device, thereby effectively improving its applicability.

[0056] The following are examples:

[0057] Example 1

[0058] (1) Preparation of composite film material: The process flow for preparing the composite film material of the present invention is shown in Figure 1 As shown, the sequence is: sandblasting roughening treatment of titanium foil surface → cleaning → surface treatment → powder spreading → hot pressing molding → composite film. The specific steps are: lay a titanium foil with a thickness of 0.1 mm flat and fix it on a horizontal platform, then perform sandblasting roughening treatment on its surface. The sandblasting uses refined quartz sand with a particle size of about 0.2 mm. Then, the roughened titanium foil is ultrasonically cleaned in acetone, ethanol and distilled water for 10 min respectively. After drying, a layer of silane coupling agent is coated on its surface, and it is placed in a hot pressing molding machine, and a layer of PTFE powder is covered on its surface for hot pressing molding. The hot pressing temperature is 350°C, the pressure is 3 Mpa, and the hot pressing is 0.5 h.

[0059] Figure 2 The process flow chart for preparing a composite film with oil-water separation function is as follows: laser roughening the surface of one side of the titanium foil → laser roughening the surface of one side of the polytetrafluoroethylene → laser drilling.

[0060] (2) Laser roughening: The composite film prepared in step (1) is placed and fixed on a laser processing platform, and a femtosecond laser with a wavelength of 800 nm and a focused spot diameter of 20 μm is used. The grid scanning method is used to first perform laser roughening on the surface of the titanium foil side of the composite film. The laser processing parameters are: laser power of 3 W, pulse frequency of 200 KHz, scanning speed of 1500 mm / s, and scanning spacing of 25 μm. Then, the surface of the PTFE side of the composite film is laser roughened. The laser processing parameters are: laser power of 3 W, pulse frequency of 400 KHz, scanning speed of 1000 mm / s, and scanning spacing of 30 μm.

[0061] (3) Laser drilling: According to the design requirements of the oil-water separation project, the designed hole diameter is 80 μm and the hole spacing is 250 μm. Then, a femtosecond laser with a wavelength of 800 nm and a focused spot diameter of 20 μm is used to drill holes in the composite film roughened in step (2) at a relatively high laser power. When drilling, ensure that the titanium foil surface of the composite film faces upward. The laser parameters for drilling are: laser power of 10 W, pulse frequency of 200 KHz, and scanning speed of 200 mm / s.

[0062] Figure 3 This is a scanning electron microscope image of the surface morphology of the composite film after laser roughening and drilling (observed from the polytetrafluoroethylene side). It can be seen that the surface of the composite film PTFE side is covered with a large number of micron-sized cone protrusions. This rough structure can effectively improve its wetting performance. At the same time, the film surface is also covered with neatly arranged through-hole array structures, with a distance of 250μm between holes, which is achieved with the help of laser drilling. Figure 4 (a) and (b) are the static contact angles of water and oil (1,2-dichloroethane) on one side of the composite film PTFE surface prepared in step (2). It can be seen that the laser roughening and drilling treatment makes the surface of one side of the composite film PTFE show super hydrophobic / super oleophilic wetting properties; Figure 5 (a) and (b) are schematic diagrams of the static contact angles of water and oil (1,2-dichloroethane) on one side of the surface of the composite thin film titanium foil prepared in step (2). It can be seen that the laser roughening and drilling treatment makes the surface of one side of the composite thin film titanium foil show superhydrophilic / underwater superoleophobic wetting properties, which is also extremely beneficial to improving the efficiency of oil-water separation.

[0063] (4) Preparation of oil-water separation device: Figure 6 Schematic diagram of the design of the prepared film for oil-water mixture separation device. The specific steps are: install the two composite films prepared in (3) at the two ends of the "T-shaped" oil-water separation device respectively, and during installation, ensure that the different sides of the two composite film materials face the oil-water mixture.

[0064] The oil-water separation performance of the prepared oil-water separation device was measured. A mixture of petroleum ether and water (volume ratio 1:1) was used as the measuring medium. After 5 parallel experiments, the results showed that it took 52.4 seconds for 1000 ml of oil-water mixture to pass through the oil-water separation device with a membrane area of ​​30 mm × 30 mm, and its total flow rate was 21.2 L / (m 2 ·s), and at the same time, after measurement, the corresponding oil-water separation efficiency reached 98.55%.

[0065] Example 2

[0066] (1) Preparation of composite film materials: A titanium foil with a thickness of 0.08 mm was placed flat and fixed on a horizontal surface, and then subjected to surface roughening treatment by sandblasting. The sandblasting material used was refined quartz sand with a particle size of about 0.1 mm. After cleaning and drying, a layer of silane coupling agent was coated on its surface, and it was placed in a hot pressing machine. Then, an appropriate amount of PTFE powder was covered on its surface and hot pressed. The hot pressing temperature was 330 °C, the pressure was 2.5 MPa, and the hot pressing was performed for 1 h.

[0067] (2) Laser roughening: The composite film prepared in step (1) is placed and fixed on a laser processing platform, and a femtosecond laser with a wavelength of 1030 nm and a focused spot diameter of 20 μm is used. The grid scanning method is used to roughen the surface of the titanium foil side of the composite film. The roughening treatment parameters are: laser power of 3.5 W, pulse frequency of 100 KHz, scanning speed of 1300 mm / s, and scanning spacing of 25 μm. Then, the surface of the PTFE side of the composite film is roughened. The laser processing parameters are: laser power of 4 W, pulse frequency of 200 KHz, scanning speed of 900 mm / s, and scanning spacing of 30 μm.

[0068] (3) The drilling diameters were designed to be 20 μm, 40 μm, 60 μm, 80 μm, 100 μm, 120 μm, 140 μm, and 160 μm, respectively. The distance between through holes was 300 μm. A femtosecond laser with a wavelength of 1030 nm and a focused spot diameter of 20 μm was used for drilling. The drilling parameters were: laser power of 12 W, pulse frequency of 400 kHz, and scanning speed of 150 mm / s.

[0069] The radius of the tapered through hole is 0.5 μm-200 μm.

[0070] (4) Preparation of oil-water separation device: The two oil-water separation composite films prepared in (3) are installed at the two ends of the "T-shaped" oil-water separation device. During installation, ensure that different sides of the two film materials face the oil-water mixture.

[0071] Using a mixture of 1,2-dichloroethane and water as the medium, the oil-water separation efficiency and flow rate were tested. The results are shown in Table 1.

[0072] Table 1 Separation efficiency and flow rate of oil-water separation devices with different through-hole diameters

[0073] .

[0074] It can be seen from Table 1 that as the through-hole diameter continues to increase, the flow rate of oil and water separated by the oil-water separation device continues to increase, while the corresponding oil-water separation efficiency continues to decrease.

[0075] (5) Comparative test of separation rate (flow rate) and service life

[0076] A single-layer titanium foil and a single-layer polytetrafluoroethylene film, both of which were 0.20 mm thick, were selected and processed under the same process conditions as those for preparing the composite film. Then, the two films were installed in a "T-type" oil-water separation device. The separation rate and service life of the oil-water mixture were tested and compared with the composite film of the present invention. The results are shown in Table 2.

[0077] Table 2 Comparison of separation rate and service life between single-layer film and composite film

[0078] .

[0079] It can be seen from Table 2 that, under the condition of keeping the membrane separation efficiency almost the same, the oil-water separation rate of the composite membrane can be increased by about 50%, and the service life can be increased to 2.9 times the original service life.

Claims

1. A method for preparing a composite film for oil-water separation with wide applicability, characterized in that: The steps include: (S1) Preparation of composite film: Titanium foil and PTFE powder are used as raw materials, and a composite film material with a PTFE layer and a titanium foil layer as the upper and lower layers is prepared by hot pressing process; before the hot pressing process is implemented, the titanium foil that has been roughened by sandblasting is ultrasonically cleaned in acetone, ethanol and distilled water for 10 min, and after drying, a layer of silane coupling agent is coated on its surface; and a layer of PTFE powder is covered on its surface; (S2) Laser roughening the surface of the composite material: using a femtosecond laser to perform laser scanning on the upper and lower surfaces of the composite material in step (S1), respectively, so that the surface of the PTFE side of the composite material exhibits super hydrophobic / super oleophilic wetting properties, and the surface of the titanium foil side exhibits super hydrophilic / underwater super oleophobic wetting properties; (S3) laser drilling: setting an appropriate laser drilling spacing and drilling diameter, and using a femtosecond laser to perform laser drilling on the surface of the composite film material in step (2), thereby obtaining an oil-water separation film with excellent adaptability; (S4) Preparation of oil-water separation device: Take two oil-water separation composite films prepared in step (3), one of which has its PTFE side facing the inside of the device, and the other has its titanium foil side facing the inside, and fix them on both sides of a "T-shaped" oil-water separation device, respectively, to obtain a device that can separate different types of oil-water mixtures in large quantities.

2. The preparation method according to claim 1, characterized in that In the step (S1), the thickness of the titanium foil is 0.05-1.00 mm; The total thickness of the composite film material prepared in the step (S1) is 0.10-2.00 mm, with the upper and lower layers being respectively a polytetrafluoroethylene layer and a titanium foil layer.

3. The preparation method according to claim 1, characterized in that: In the step (S1) of preparing the composite film material, the hot pressing temperature is 330-450°C, the hot pressing pressure is 2-6Mpa, and the hot pressing time is 0.5-1.5h.

4. The preparation method according to claim 1, characterized in that: In the step (S2), the laser scanning method is grid scanning, and the laser scanning etching will construct a rough surface composed of micrometer size and nanometer size on the upper surface and the lower surface of the composite film material respectively; The femtosecond laser wavelength in the step (S2) is in the infrared, visible or ultraviolet band, the laser power is 0.5-10W, the laser pulse frequency is 200KHz-1MHz, the laser scanning line spacing is 6-50μm, and the laser scanning speed is 100-1500mm / s.

5. The preparation method according to claim 1, characterized in that: In the step (S2), after the composite film is roughened by laser, the water static contact angle of the PTFE side surface is greater than 150°, and the oil static contact angle is less than 10°; after the composite film is roughened by laser, the oil static contact angle of the titanium foil side surface under water is greater than 150°, and the water static contact angle is less than 10°.

6. The preparation method according to claim 1, characterized in that: The step (S3) uses femtosecond laser drilling, and the hole punched is a tapered through hole; the through hole is laser-drilled from one side of the roughened titanium foil, and the radius of the tapered through hole is 0.5 μm-200 μm.

Citation Information

Patent Citations

  • Method for preparing oil and water separation film by utilizing picosecond laser equipment

    CN109396665A

  • Stress-induced surface wettability continuous transformation Janus composite film, and preparation method and application thereof

    CN113384919A

  • Membrane separation oil-water separation device

    CN215387711U