An additive method for realizing ultra-wide and ultra-thin welds using a laser and arc composite heat source ribbon wire
By combining laser and arc composite heat source with cuboid ribbon wire, the problems of molding accuracy, residual stress and welding efficiency in existing additive manufacturing technologies are solved, and the ultra-wide and ultra-thin effect of the weld bead and the performance of the weld bead are achieved. promote.
Patent Information
- Application Number
- CN202211297794.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-22
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2042-10-22
AI Technical Summary
The existing additive manufacturing technology has shortcomings in the molding accuracy, residual stress and molten pool controllability of metal components, and the problems of welding efficiency and arc stability are relatively prominent.
Use laser and arc composite heat source to combine with cuboid ribbon wire material, and preheat and guide the welding wire to melt through high-frequency pulse laser energy, adjust the relative positions of the arc welding gun and laser exit head, and set the coordinated working mode of arc current pulse and laser pulse , forming a wider and thinner weld bead.
The ultra-wide and ultra-thin effect of the weld bead is achieved, the residual height of the weld bead is reduced, the heterogeneous nucleation rate at the tail of the molten pool is improved, uniform nucleation and grain refinement are promoted, the bead performance is better, and the arc heat source is Improved stability and manufacturing efficiency.
Smart Images

Figure CN115519252B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of three-dimensional forming and manufacturing, and in particular relates to an additive method for realizing ultra-wide and ultra-thin welds using a laser and arc composite heat source ribbon wire. Background Art
[0002] Additive manufacturing technology is based on computer-aided design, material processing and forming. It uses modern technologies such as the Internet of Things (IoT), artificial intelligence (AI), cyber-physical systems (CPS), big data analysis (BDA), cloud computing, digital twins (DT), and 5G to select spare metal materials or non-metallic materials and stack them layer by layer to produce advanced manufacturing technology with excellent structural performance. Since its development in 1972, this technology has been developing and becoming more and more mature. It has not only made achievements in large-scale fields such as aviation and navigation, but also has broad application prospects in many fields such as micro-structure manufacturing and biomedical engineering. The technical basis of additive manufacturing of metal products is melting and welding. From the current development status, there are two major breakthroughs in additive manufacturing at home and abroad: one is the development from the early laser rapid prototyping of non-metallic materials such as photosensitive resins to the forming and manufacturing of metal structural parts; the other is the deep integration of the flexibility and welding forming technology of high-energy beam heat sources such as lasers, electron beams, and arcs with computer-aided design / manufacturing information technology, realizing customized moldless manufacturing of metal structures and forming a new direction for industrial development.
[0003] The advantages of additive manufacturing are short manufacturing cycle, suitability for the personalized needs of single pieces, manufacturing of large thin-walled parts, manufacturing of difficult-to-process and easy-to-hot-form parts such as titanium alloys, and manufacturing of parts with complex structures. In the fields of aerospace, mechanical manufacturing, etc., in the product development stage, computer peripheral development and innovative education, it has broad development space. At present, additive manufacturing technology is a supplement to traditional mass manufacturing technology, and it faces many new challenges and new problems compared to traditional manufacturing technology. The additive manufacturing of metal components is applied to product research and development, and there are still problems such as high cost of use, low manufacturing efficiency, and unsatisfactory manufacturing accuracy. Its process and equipment research and development are also insufficient, and it has not yet entered large-scale industrial application.
[0004] Arc additive manufacturing technology has the advantages of low cost, high efficiency, multiple controllable parameters, good mechanical properties, and good applicability of metal materials, but there are also some problems that need to be solved: there is a certain gap between the forming accuracy and the net forming parts, the residual stress is large, and the controllability of the molten pool is not good. In traditional welding technology, gas metal arc welding has the advantages of large welding current and high welding efficiency, but the arc is unstable, and the molten pool is easy to overflow and collapse during the forming process; non-metal arc arc welding is stable, but the welding current is small and the welding efficiency is low.
[0005] The arc has the advantages of high thermal efficiency and high droplet deposition rate when used in additive manufacturing, but the arc has high heat input, which can easily cause coarse grain structure inside the metal structure. The open gas-shielded arc action environment is also prone to form porosity defects during the forming process. Summary of the invention
[0006] The purpose of the present invention is to provide an additive method for realizing ultra-wide and ultra-thin welds by using a laser and arc composite heat source strip wire. The use of a rectangular strip wire instead of a cylindrical wire can better spread the molten droplet, which can widen the weld width and reduce the weld excess height. The heat dissipation effect is also better, which can increase the heterogeneous nucleation rate at the tail of the molten pool, promote uniform nucleation, and significantly refine the grain growth during the solidification process of the molten pool, so that the performance of the weld is better.
[0007] The present invention provides a method for adding ultra-wide and ultra-thin welds using a laser and arc composite heat source ribbon wire, which uses an arc heat source to provide the main energy required for melting metal wires, forming molten droplets and forming metal material structures, and uses high-frequency pulse laser energy to preheat and guide the welding wire to melt. The rectangular ribbon wire can make the molten pool wider, and the weld bead also wider. It includes the following steps:
[0008] Step 1: Adjust the relative position of the arc welding gun and the laser output head, set the coordinated working mode of the arc current pulse and the laser pulse, and attach a laser heat source above the ribbon wire so that the laser beam irradiates the ribbon wire. The arc welding gun is located above and behind the ribbon wire, and the emitted oscillating arc beam swings along the path of the laser beam to melt the wire and form a molten pool.
[0009] Step 2: Debug the current and voltage of the equipment, and select parameters such as arc power, gas type and gas flow, wire feeding method and wire feeding speed, and welding speed.
[0010] Step 3, select titanium alloy as the substrate, and use a grinder to grind the area on the substrate surface where additives are needed for a period of time to remove some stains and oxide layers on the surface; then preheat the substrate so that the overall temperature of the substrate reaches a predetermined temperature evenly. Preheating the substrate can remove hydrogen, eliminate residual stress, and reduce severe airflow convection due to excessive temperature difference during additives.
[0011] Step 4, start the additive manufacturing program, the laser works, emits a laser beam with specific parameters, and at the same time, the arc is struck to start the arc and the metal wire is fed to form a molten pool of a certain width; the width of the arc molten pool is 4mm≤B1 / 2≤5mm, and the width of the molten pool is 7mm≤B2 / 2≤9mm.
[0012] Step 5: Allow the plasma arc to continue to advance along a predetermined route until a complete weld is formed.
[0013] Step 6, repeat the operation of step 5 until the entire component is formed.
[0014] Step 7, heat treating the component after material addition in an argon protective atmosphere to obtain a component with better performance;
[0015] Furthermore, in step 1, the relative positions of the arc welding gun and the laser output head are adjusted so that the arc output direction is distributed along the plumb line, the wire and the arc output direction form an angle of 60°, the laser output direction and the arc output direction form an angle of 0 to 30°, and with the forward direction of the workbench as a reference, the laser output point is in front and the arc heat source point is in the back, so that the laser energy acts on the wire to preheat the wire and guide the arc to swing;
[0016] Furthermore, in step 1, the arc spacing, i.e., the distance H between the laser beam and the arc, is adjusted so that the area of the ribbon wire scanned by the laser heat source can be melted by the arc heat source as quickly as possible without the two colliding. The distance between the two is: 6.00mm≤H≤10.00mm.
[0017] Furthermore, in step 1, the action mode of the laser beam is pulse scanning, the pulse laser beam acts on the surface of the ribbon wire to be melted in a Z-shaped trajectory, and the area of the pulse scanning region is ≥ 1 / 2 of the surface area of the ribbon wire, and the pulse scanning frequency is proportional to the movement rate of the arc heat source;
[0018] Furthermore, in step 1, the laser pulse frequency is audible audio frequency 100 Hz to 20 kHz or ultrasonic frequency above 20 kHz, the pulse peak power is not less than 2 kW, and the arc current pulse and the laser pulse are asynchronous pulses.
[0019] Furthermore, in step 2, in order to achieve the additive of strip wires of different lengths, widths and heights, the parameters of the plasma arc include voltage 20V≤U≤40V, where the voltage is the continuously output AC arc voltage; current 60A≤I≤240A, where the current is the continuously output AC arc current; wire feeding speed WFS=2.0m / min, where the wire feeding method is coaxial wire feeding or side-axis wire feeding; welding speed TS=30mm / s; arc power 1200W≤P≤8000W; and arc diameter 6mm≤D≤8mm.
[0020] Furthermore, the preheating treatment of the substrate in step 3 is specifically as follows:
[0021] Before applying the arc, the substrate is preheated to 200-300°C within 20 minutes, and the substrate is kept at this temperature for 5-10 minutes before adding material;
[0022] During the additive process, in order to improve the mechanical properties of the components and reduce the problem of heat accumulation caused by continuous heat input and thus the generation of coarse columnar crystals, a coolant circulation system is added under the substrate to assist in heat dissipation.
[0023] After the addition is completed, the substrate temperature is adjusted to the range of 100-200°C and maintained for 40-50 minutes before stopping to eliminate residual stress and further improve the performance of the obtained component.
[0024] The present invention discloses an additive method for realizing ultra-wide and ultra-thin welds by using a laser and arc composite heat source ribbon wire, using a rectangular ribbon wire to replace a cylindrical wire, and designing a pulsed laser as an auxiliary heat source to preheat and guide the wire, and an arc as a main heat source to work together, thereby obtaining a wider and thinner weld with better performance and better edge quality. The laser plasma generated by the action of the pulsed laser and the material is used to suppress the instability of the pulsed arc, the laser and arc are used to coordinate the pulse to achieve full fusion of the two energy sources, and improve the heat absorption rate of the material to the heat source energy, the heat provided by the pulsed plasma arc is used to achieve the melting of the automatically synchronously fed ribbon wire, and to form a molten droplet, so that it can be deposited and formed, and the designed pulsed plasma arc pulse mode is used to achieve a relatively low average heat input, reduce the internal stress and thermal deformation of the formed component, and play a role in widening the weld. However, in this technology, since the pulse laser is not the main heat source, its frequency needs to be adjusted according to the different sizes of strip welding wire. The power is generally not set too large, and it can only guide the melting of the wire. Moreover, because the wire is a rectangular strip, the formed molten pool may not be so uniform, and it cannot play the role of vibrating the molten pool.
[0025] Compared with the prior art, the present invention has the following significant advantages:
[0026] 1. The present invention uses a plasma arc heat source to provide the main energy required for melting metal wires, forming molten droplets and metal material structure formation. The pulsed laser energy is used to pre-scan the strip wire that is about to be melted, so that the welding wire melts according to the set route and method. The rectangular strip wire replaces the cylindrical wire, and the weld bead is widened, reducing the accumulation of molten droplets and the excess height of the weld bead. At the same time, it can accelerate the escape of gas in the molten pool, reduce macro and micro pores, and slightly improve the structural density.
[0027] 2. The present invention limits the laser beam parameters and combines the coordinated working mode and energy matching method of arc current pulse and laser pulse to ensure that the arc is used as a heat source and the laser beam plays the role of preheating the wire and guiding the arc.
[0028] 3. The present invention uses a rectangular ribbon wire to replace a cylindrical wire, which has a larger cross-sectional area, and the molten droplet is easier to spread, so the spreading area is larger, and the obtained weld area is wider. Similarly, under the condition of a certain volume, the cross-sectional area is larger, the weld excess height is lower, and the forming quality is more exquisite. The metal deposition rate is high, the metal component forming efficiency is high, and the obtained metal has a dense internal structure, uniform and fine grains.
[0029] 4. The arc heat source of the present invention has good stability, can realize low heat input manufacturing, and has low energy consumption and manufacturing cost.
[0030] 5. The present invention can control the heat input by preheating the wire and guiding the arc through the laser heat source, so that the weld plane is more uniform and smooth, the weld shape is more beautiful, and the performance quality is higher. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 Schematic diagram of the structure of the additive method for achieving ultra-wide and ultra-thin welds with ribbon wire using a laser and arc composite heat source.
[0032] Among them: 1 is the power supply; 2 is the substrate; 3 is the arc beam; 4 is the laser beam; 5 is the ribbon wire; 6 is the scanning laser; 7 is the plasma arc additive equipment; 8 is the weld (finished product).
[0033] Figure 2 Schematic diagram of the molten pool morphology and laser path after laser addition of the additional ribbon wire.
[0034] Figure 3 Schematic diagram of the waveform of arc current pulse and laser pulse. The upper part is the laser pulse and the lower part is the arc current pulse. DETAILED DESCRIPTION
[0035] The technical method of the present invention is not limited to the specific implementation modes listed below, but also includes any combination of the specific implementation modes.
[0036] Example 1
[0037] In order to solve the above technical problems, this embodiment provides a method for adding ultra-wide and ultra-thin welds using a laser and arc composite heat source ribbon wire, including the following steps:
[0038] Step 1: Adjust the relative positions of the arc welding gun and the laser output head so that the arc output direction is distributed along the plumb line, the wire and the arc output direction form an angle of 60°, the laser output direction and the arc output direction form an angle of 5°, and with the forward direction of the workbench as a reference, the laser output point is in the front, and the arc heat source point is in the back, so that the laser energy acts on the wire, the arc welding gun is located at the upper back of the strip wire, and the coordinated working mode of the arc current pulse and the laser pulse is set, and the emitted oscillating arc beam swings along the path of the laser beam to melt the wire and form a molten pool.
[0039] Adjust the arc spacing, i.e. the distance H between the laser beam and the arc, so that the area of the ribbon wire scanned by the laser heat source can be melted by the arc heat source as quickly as possible without the two colliding. The distance between the two: H = 10.00 mm.
[0040] The action mode of the laser beam is pulse scanning. The pulse laser beam acts on the surface of the ribbon wire to be melted in a Z-shaped trajectory, and the pulse scanning area is ≥ 1 / 2 of the surface area of the ribbon wire. The pulse scanning frequency is proportional to the movement rate of the arc heat source.
[0041] The second step is to adjust the current and voltage of the equipment, and select the parameters such as arc power, gas type and gas flow, wire feeding speed and welding speed. The parameters of the plasma arc include voltage U = 25V, which is the continuously output AC arc voltage; current I = 150A, which is the continuously output AC arc current; select a rectangular ribbon wire with a width of 8mm and a height of 0.8mm; wire feeding speed WFS = 2.0m / min, and the wire feeding method is coaxial wire feeding or side-axis wire feeding; welding speed TS = 30mm / s; arc power P = 3750W; arc diameter D = 8mm.
[0042] The third step is to use titanium alloy as the substrate and use a grinder to grind the area on the substrate surface where additives are needed for 3 minutes to remove some stains and oxide layers on the surface; before applying the arc, preheat the substrate to 280°C within 20 minutes and keep it warm for 6 minutes before additives are added; during the additive process, in order to improve the mechanical properties of the component and reduce the problem of heat accumulation caused by continuous heat input and the formation of coarse columnar crystals, a coolant circulation system is added under the substrate to assist in heat dissipation; after the additive process is completed, the substrate temperature is adjusted to within 180°C and maintained for 40 minutes before stopping.
[0043] The fourth step is to start the additive manufacturing program, the laser works, emits a laser beam with specific parameters, and at the same time, the arc is struck to start the arc and the metal wire is fed, and the collaborative working mode of the arc current pulse and the laser pulse is set: when the arc current is in non-pulse mode, the laser pulse energy and the arc energy are arbitrarily matched; when the arc current is in pulse mode, the energy matching of the laser pulse and the arc current pulse includes: when the arc current pulse and the laser pulse are synchronous pulses, within an energy matching cycle, the pulse energy matching is peak-to-peak matching; when the arc current pulse and the laser pulse are asynchronous pulses, the laser pulse frequency is at least twice the arc current pulse frequency, within an energy matching cycle, at least one pulse energy matching is peak-to-peak matching, and the remaining pulse energy matching is peak-to-base value matching to form a molten pool of a certain width; the width of the arc molten pool is B1=10mm, and the width of the molten pool after laser recombination is B2=18mm.
[0044] The fifth step is to allow the plasma arc to continue to advance along a predetermined route until a complete weld is formed.
[0045] Step 6: Repeat the operation in step 5 until the entire component is formed.
[0046] The seventh step is to heat treat the component after material addition in an argon protective atmosphere to obtain a component with better performance;
[0047] The component prepared in this embodiment was taken out, and after cleaning the surface, mechanical property tests were performed, including tensile test and hardness test. The tensile strength and elongation after fracture of the additive component are shown in Table 1 below.
[0048] Example 2
[0049] In order to solve the above technical problems, this embodiment provides a method for adding ultra-wide and ultra-thin welds using a laser and arc composite heat source ribbon wire, including the following steps:
[0050] Step 1: Adjust the relative positions of the arc welding gun and the laser output head so that the arc output direction is distributed along the plumb line, the wire and the arc output direction form an angle of 60°, the laser output direction and the arc output direction form an angle of 15°, and with the forward direction of the workbench as a reference, the laser output point is in the front, and the arc heat source point is in the back, so that the laser energy acts on the wire, the arc welding gun is located at the upper rear of the strip wire, and the coordinated working mode of the arc current pulse and the laser pulse is set, and the emitted oscillating arc beam swings along the path of the laser beam to melt the wire and form a molten pool.
[0051] Adjust the arc spacing, i.e. the distance H between the laser beam and the arc, so that the area of the ribbon wire scanned by the laser heat source can be melted by the arc heat source as quickly as possible without the two colliding. The distance between the two: H = 9.00 mm.
[0052] The action mode of the laser beam is pulse scanning. The pulse laser beam acts on the surface of the ribbon wire to be melted in a Z-shaped trajectory, and the pulse scanning area is ≥ 1 / 2 of the surface area of the ribbon wire. The pulse scanning frequency is proportional to the movement rate of the arc heat source.
[0053] The second step is to adjust the current and voltage of the equipment, and select the parameters such as arc power, gas type and gas flow, wire feeding speed and welding speed. The parameters of the plasma arc include voltage U = 24V, which is the continuously output AC arc voltage; current I = 120A, which is the continuously output AC arc current; select a rectangular ribbon wire with a width of 6mm and a height of 0.6mm; wire feeding speed WFS = 2.0m / min, and the wire feeding method is coaxial wire feeding or side-axis wire feeding; welding speed TS = 30mm / s; arc power P = 2880W; arc diameter D = 7mm.
[0054] The third step is to use titanium alloy as the substrate and use a grinder to grind the area on the substrate surface where additives are needed for 3 minutes to remove some stains and oxide layers on the surface; before applying the arc, preheat the substrate to 250°C within 20 minutes and keep it warm for 8 minutes before additives are added; during the additive process, in order to improve the mechanical properties of the component and reduce the problem of heat accumulation caused by continuous heat input and the formation of coarse columnar crystals, a coolant circulation system is added under the substrate to assist in heat dissipation; after the additive process is completed, the substrate temperature is adjusted to within 160°C and maintained for 40 minutes before stopping.
[0055] The fourth step is to start the additive manufacturing process, the laser works, emits a laser beam with specific parameters, and simultaneously ignites the arc to start the arc, starts the wire feeding, and sets the coordinated working mode of the arc current pulse and the laser pulse, which is consistent with Case 1. The width of the arc molten pool is B1 = 9 mm, and the width of the molten pool after laser compounding is B2 = 17 mm.
[0056] The fifth step is to allow the plasma arc to continue to advance along a predetermined route until a complete weld is formed.
[0057] Step 6: Repeat the operation in step 5 until the entire component is formed.
[0058] The seventh step is to heat treat the component after material addition in an argon protective atmosphere to obtain a component with better performance;
[0059] The component prepared in this embodiment was taken out, and after cleaning the surface, mechanical property tests were performed, including tensile test and hardness test. The tensile strength and elongation after fracture of the additive component are shown in Table 1 below.
[0060] Example 3
[0061] In order to solve the above technical problems, this embodiment provides a method for adding ultra-wide and ultra-thin welds using a laser and arc composite heat source ribbon wire, including the following steps:
[0062] Step 1: Adjust the relative positions of the arc welding gun and the laser output head so that the arc output direction is distributed along the plumb line, the wire and the arc output direction form an angle of 60°, the laser output direction and the arc output direction form an angle of 25°, and with the forward direction of the workbench as a reference, the laser output point is in the front, and the arc heat source point is in the back, so that the laser energy acts on the wire, the arc welding gun is located at the upper rear of the strip wire, and the coordinated working mode of the arc current pulse and the laser pulse is set, and the emitted oscillating arc beam swings along the path of the laser beam to melt the wire and form a molten pool.
[0063] Adjust the arc spacing, i.e. the distance H between the laser beam and the arc, so that the area of the ribbon wire scanned by the laser heat source can be melted by the arc heat source as quickly as possible without the two colliding. The distance between the two: H = 8.00 mm.
[0064] The action mode of the laser beam is pulse scanning. The pulse laser beam acts on the surface of the ribbon wire to be melted in a Z-shaped trajectory, and the pulse scanning area is ≥ 1 / 2 of the surface area of the ribbon wire. The pulse scanning frequency is proportional to the movement rate of the arc heat source.
[0065] The second step is to adjust the current and voltage of the equipment, and select the parameters such as arc power, gas type and gas flow, wire feeding speed and welding speed. The parameters of the plasma arc include voltage U = 20V, which is the continuously output AC arc voltage; current I = 70A, which is the continuously output AC arc current; select a rectangular ribbon wire with a width of 5mm and a height of 0.5mm; wire feeding speed WFS = 2.0m / min, and the wire feeding method is coaxial wire feeding or side-axis wire feeding; welding speed TS = 30mm / s; arc power P = 1400W; arc diameter D = 6mm.
[0066] In the third step, titanium alloy is selected as the substrate, and the area on the surface of the substrate that needs to be added is polished for 3 minutes with a grinder to remove some stains and oxide layers on the surface; before applying the arc, the substrate is preheated to 230°C within 16 minutes, and the addition is performed after keeping the temperature for 10 minutes; during the addition process, in order to improve the mechanical properties of the component and reduce the heat accumulation caused by continuous heat input and the problem of coarse columnar crystals, a coolant circulation system is added under the substrate to assist in heat dissipation; after the addition is completed, the substrate temperature is adjusted to within 130°C and maintained for 45 minutes before stopping.
[0067] The fourth step is to start the additive manufacturing process, the laser works, emits a laser beam with specific parameters, and simultaneously ignites the arc to start the arc, starts the wire feeding, and sets the coordinated working mode of the arc current pulse and the laser pulse, which is consistent with Case 1. The width of the arc molten pool is B1 = 9 mm, and the width of the molten pool after laser compounding is B2 = 17 mm.
[0068] The fifth step is to allow the plasma arc to continue to advance along a predetermined route until a complete weld is formed.
[0069] Step 6: Repeat the operation in step 5 until the entire component is formed.
[0070] The seventh step is to heat treat the component after material addition in an argon protective atmosphere to obtain a component with better performance;
[0071] The component prepared in this embodiment was taken out, and after cleaning the surface, mechanical property tests were performed, including tensile test and hardness test. The tensile strength and elongation after fracture of the additive component are shown in Table 1 below.
[0072] Table 1
[0073] Tensile strength / MPa Elongation after break / % Hardness / HV Example 1 1367 15.7 355 Example 2 1293 13.4 356 Example 3 1424 11.8 339
Claims
1. A method for adding material to achieve ultra-wide and ultra-thin welds using a laser and arc composite heat source ribbon wire, characterized in that: The specific steps include: Step 1, adjust the relative positions of the arc welding gun and the laser output head, and set the coordinated working mode of the arc current pulse and the laser pulse, add a laser heat source above the strip wire, so that the laser beam irradiates the strip wire; the arc welding gun is located above and behind the strip wire, and the output oscillating arc beam swings along the path of the laser beam to melt the wire and form a molten pool; Step 2: Debug the current and voltage of the equipment, select the arc power, gas type and gas flow, wire feeding method and wire feeding speed, and welding speed parameters; Step 3: Use titanium alloy as the substrate, and use a grinder to grind the area on the substrate surface where material needs to be added for a period of time to remove some stains and oxide layers on the surface; then preheat the substrate so that the overall temperature of the substrate reaches a predetermined temperature evenly; Step 4, start the additive manufacturing program, the laser works, emits a laser beam with specific parameters, and simultaneously ignites the arc to start the arc and the metal wire starts to feed, forming a molten pool of a certain width; the width of the arc molten pool is 4mm≤B1 / 2≤5mm, and the width of the molten pool is 7mm≤B2 / 2≤9mm; Step 5, let the plasma arc continue to advance along the predetermined route until a complete weld is formed; Step 6, repeat the operation of step 5 until the entire component is formed; Step 7, heat treating the component after material addition in an argon protective atmosphere; In step 1, the relative positions of the arc welding gun, the laser output head and the strip wire are adjusted so that the arc output direction is distributed along the plumb line, the wire and the arc output direction form an angle of 60°, the laser output direction and the arc output direction form an angle of 0-30°, and with the forward direction of the workbench as a reference, the laser output point is in front and the arc heat source point is in the back, so that the laser energy acts on the wire to preheat the wire and guide the arc to swing; In step 1, the action mode of the laser beam is pulse scanning, the pulse laser beam acts on the surface of the ribbon wire to be melted in a Z-shaped trajectory, and the area of the pulse scanning region is ≥ 1 / 2 of the surface area of the ribbon wire, and the pulse scanning frequency is proportional to the movement rate of the arc heat source; In step 3, the specific steps of preheating the substrate are as follows: Before applying the arc, the substrate is preheated to 200-300°C within 20 minutes, and the substrate is kept at this temperature for 5-10 minutes before adding material; During the additive process, in order to improve the mechanical properties of the components and reduce the problem of heat accumulation caused by continuous heat input and thus the generation of coarse columnar crystals, a coolant circulation system is added under the substrate to assist in heat dissipation. After the addition is completed, the substrate temperature is adjusted to the range of 100~200℃ and maintained for 40~50min before stopping to eliminate residual stress and further improve the performance of the obtained component.
2. The method for realizing ultra-wide and ultra-thin welds by using a laser and arc composite heat source ribbon wire according to claim 1, characterized in that: In step 1, adjust the arc spacing, that is, the distance H between the laser beam and the arc, to ensure that the two heat sources will not have a poor laser preheating effect due to the distance being too far, nor will they collide due to the distance being too close; the distance between the two is: 6.00mm≤H≤10.00mm.
3. The method for realizing ultra-wide and ultra-thin welds by using a laser and arc composite heat source ribbon wire according to claim 1, characterized in that: In step 1, the laser pulse frequency is audible sound frequency 100 Hz to 20 kHz or ultrasonic frequency above 20 kHz, the pulse peak power is not less than 2 kW, and the arc current pulse and the laser pulse are asynchronous pulses.
4. The method for realizing ultra-wide and ultra-thin welds by using a laser and arc composite heat source ribbon wire according to claim 1, characterized in that: In step 2, in order to achieve the additive of ribbon wires of different lengths, widths and heights, the parameters of the plasma arc include voltage 20V≤U≤40V, where the voltage is the continuously output AC arc voltage; current 60A≤I≤240A, where the current is the continuously output AC arc current; wire feeding speed WFS=2.0m / min, and the wire feeding method is coaxial wire feeding or side-axis wire feeding; welding speed TS=30mm / s; arc power 1200W≤P≤8000W; and arc diameter 6mm≤D≤8mm.
Citation Information
Patent Citations
Double-laser-beam and electric-arc multi-heat-source composite material adding method
CN111571017A
MIG electric arc double-wire low-heat-input additive manufacturing method for scanning laser-assisted shaping molten pool