A N and Ta ion implanted titanium alloy modified coating and its preparation method and application

By implanting N and Ta ions onto the surface of titanium alloy and combining this with magnetron sputtering of Ta to form the TaN0.1 phase, the problems of poor adhesion and wear of traditional coatings in the bulk environment are solved, and the high wear resistance and stability of multiphase coatings are achieved.

CN115537750BActive Publication Date: 2024-11-08JINAN UNIVERSITY +1
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202211186628.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-27
Publication Date
2024-11-08
Estimated Expiration
2042-09-27

AI Technical Summary

Technical Problem

Traditional titanium alloy surface coatings have poor adhesion in the internal environment, are prone to wear, and single-structure coatings fail during the wear process, thus failing to effectively improve the wear resistance of titanium alloys.

Method used

After N and Ta ion implantation on the surface of titanium alloy, Ta is combined with magnetron sputtering to form TaN0.1 phase, forming a multiphase, multi-layer modified coating, which enhances the bonding ability with the substrate. Furthermore, α-Ta phase is generated by high-temperature magnetron sputtering to improve the hardness and toughness of the coating.

Benefits of technology

It improves the adhesion and wear resistance of the modified titanium alloy coating, enhances the coating's wear resistance, and ensures the stability and protective performance of the coating in the in vivo environment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003866425700000041
    Figure BDA0003866425700000041
Patent Text Reader

Abstract

The present invention belongs to the technical field of biological implant materials, and particularly relates to a titanium alloy modified coating implanted with N and Ta ions, and a preparation method and application thereof. The present invention implants N ions and Ta ions on the surface of a titanium alloy, and then magnetron sputters Ta on the surface of the titanium alloy after the ion implantation, and finally obtains a titanium alloy modified coating. The obtained coating has good mechanical properties and excellent bonding strength with a substrate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of biological implant materials, and particularly relates to a N and Ta ion implanted titanium alloy modified coating and a preparation method and application thereof. Background Art

[0002] At present, preparing friction-reducing and wear-resistant coatings on the surface of titanium alloys is one of the most effective ways to solve the poor wear resistance of titanium alloys. Friction-reducing and wear-resistant coatings generally refer to friction coatings with low friction coefficients and small wear. Enhancing the wear resistance of friction pairs by changing their microstructures or generating metal compounds and ceramics on the surface can reduce or control friction and wear, such as ion implantation, laser cladding, laser shot peening, surface nitriding, micro-arc oxidation, etc. However, traditional single-structure coatings have limitations in the in vivo environment. Therefore, multi-phase, multi-level, and multi-scale hybrid enhanced coatings prepared by different surface composite modification technologies can give full play to the synergy, coupling, and multifunctional response mechanisms between different phases in the coating.

[0003] In ion implantation technology, accelerated ions are guided to the surface of the target material, but the penetration depth of ions implanted into the material surface is generally only 100 to 500 nm. If the coating is too thin, the modified layer will be completely damaged. In addition, during the wear process, the friction pair is in direct contact with the substrate, and the hard particles produced by the worn modified layer will aggravate the wear of the substrate, thereby causing the coating to fail. In addition, the bonding force between the substrate and the coating will also affect the protective performance of the coating. Summary of the invention

[0004] In order to overcome the above-mentioned shortcomings and deficiencies of the prior art, the primary purpose of the present invention is to provide a method for preparing a titanium alloy modified coating by N and Ta ion implantation.

[0005] Another object of the present invention is to provide a titanium alloy modified coating implanted with N and Ta ions obtained by the above method.

[0006] Another object of the present invention is to provide an application of the N and Ta ion implanted titanium alloy modified coating in the preparation of friction reducing and wear resistant materials.

[0007] The purpose of the present invention is achieved through the following solutions:

[0008] A method for preparing a titanium alloy modified coating by implanting N and Ta ions, comprising the following steps:

[0009] N ion implantation and Ta ion implantation are performed on the surface of the titanium alloy, and then Ta is magnetron sputtered on the surface of the titanium alloy after the ion implantation, so as to finally obtain a titanium alloy modified coating.

[0010] The titanium alloy is Ti6Al4V, Ti, Ti-2Al-2.5Zr or Ti-5Al-2.5Sn.

[0011] The titanium alloy surface is degreased before injection.

[0012] The vacuum pressure during the N ion implantation is 2×10 -4 ~5×10 -4 Pa, voltage is 50~80Kv, injection metering is 2×10 17 ~8×10 17 ion / cm 2 Preferably, the vacuum pressure is 5×10 -4 Pa, the voltage is 60Kv, and the injection meter is 5×10 17 ion / cm 2 .

[0013] The vacuum pressure during Ta ion implantation is 2×10 -4 ~5×10 -4 Pa, voltage is 40~70Kv, injection metering is 2×10 17 ~8×10 17 ion / cm 2 Preferably, the vacuum pressure is 5×10 -4 Pa, the voltage is 50Kv, and the injection quantity is 5×10 17 ion / cm 2 .

[0014] The specific operation of magnetron sputtering Ta is to use pure Ta target material and evacuate the vacuum chamber to 5×10 -4 Pa, and heat the chamber temperature to 200-400°C, the power supply power is 1800-2000W, and argon gas is introduced during magnetron sputtering. The magnetron sputtering time is 2-6h.

[0015] A N and Ta ion-implanted titanium alloy modified coating is prepared by the method.

[0016] The invention discloses an application of the titanium alloy modified coating implanted with N and Ta ions in the preparation of friction-reducing and wear-resistant materials.

[0017] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0018] A TaN layer is first formed on the surface of the titanium alloy by ion implantation. Simultaneous implantation of N and Ta can form a TaN0.1 phase, which is beneficial for improving the bonding ability with the substrate.

[0019] Magnetron sputtering is performed on the coating after ion implantation, and the prepared coating contains two phase structures of Ta. Generally, β-Ta will be generated at a low temperature in the early stage of magnetron sputtering, resulting in a hard and brittle coating. The matching degree between the β-Ta lattice constant and the substrate is poor, which can easily lead to weak interface bonding and coating peeling. However, β-Ta is a metastable phase, and the TaN0.1 unstable phase is formed during ion implantation. During the high temperature process of magnetron sputtering, a small amount of N in the ion implanted coating is leaked out. The amount of N leaked out is relatively small, and the magnetron sputtered coating will not be nitrided, but it can ensure that the β-Ta phase is reduced, the generated α-Ta phase is increased, the coating toughness is improved, and the hardness of the Ta coating is improved.

[0020] At the same time, N can increase the sputtering work function of Ta atoms, which further leads to a decrease in the activity of adsorbed Ta atoms moving to the substrate surface, an increase in the nucleation rate, and grain refinement, which further increases the coating strength. DETAILED DESCRIPTION

[0021] The present invention is further described in detail below in conjunction with examples, but the embodiments of the present invention are not limited thereto.

[0022] Unless otherwise specified, the reagents used in the examples can be purchased from the market.

[0023] Example 1

[0024] A method for preparing a wear-resistant coating on a titanium alloy surface by implanting N and Ta ions, comprising the following steps:

[0025] (1) The surface of the Ti6Al4V alloy was ground and polished, then ultrasonically cleaned in ethanol, and dried for later use.

[0026] (2) N ion implantation was performed first, and the vacuum pressure was 4×10 -4 Pa, voltage is 60Kv, and injection dose is 5×10 17 ion / cm 2 Then, Ta element was implanted with ions at a vacuum pressure of 4×10 -4 Pa, the voltage is 50Kv, and the injection dose is 5×10 17 ion / cm 2 When ion implanting Ta, argon (Ar) gas was introduced into the cathode arc source at a flow rate of 6 sccm (standard cubic centimeters per minute).

[0027] (3) Magnetron sputtering Ta

[0028] The specific operation of magnetron sputtering Ta is to use pure Ta target material and evacuate the vacuum chamber to 5×10 -4 Pa, and the chamber temperature was heated to 400°C, the power supply was 2000W, argon gas was introduced during magnetron sputtering, and the magnetron sputtering time was 4h.

[0029] Comparative Example 1

[0030] The difference between this comparative example and Example 1 is that only N ion implantation is performed.

[0031] Comparative Example 2

[0032] The difference between this comparative example and Example 1 is that only N ion implantation and Ta ion implantation are performed.

[0033] Comparative Example 3

[0034] The difference between this comparative example and Example 1 is that only magnetron sputtering of Ta is performed.

[0035] Comparative Example 4

[0036] The difference between this comparative example and Example 1 is that only N ion implantation and magnetron sputtering of Ta are performed.

[0037]

[0038] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A method for preparing a titanium alloy modified coating by implanting N and Ta ions, characterized in that The following steps are involved: N ion implantation and Ta ion implantation are performed on the surface of the titanium alloy, and then Ta is magnetron sputtered on the surface of the titanium alloy after the ion implantation, so as to finally obtain a titanium alloy modified coating; The vacuum pressure during the N ion implantation is 2×10 -4 ~5×10 -4 Pa, voltage is 50~80Kv, injection metering is 2×10 17 ~8×10 17 ion / cm 2 The vacuum pressure during Ta ion implantation is 2×10 -4 ~5×10 -4 Pa, voltage is 40~70Kv, injection metering is 2×10 17 ~8×10 17 ion / cm 2 The specific operation of magnetron sputtering Ta is to use pure Ta target material, evacuate the vacuum chamber to 5×10-4Pa, heat the chamber temperature to 200-400℃, and use a power supply of 1800-2000W. Argon gas is introduced during magnetron sputtering.

2. The preparation method according to claim 1, characterized in that: The vacuum pressure during the N ion implantation is 5×10 -4 Pa, the voltage is 60Kv, and the injection meter is 5×10 17 ion / cm 2 .

3. The preparation method according to claim 1, characterized in that: The vacuum pressure during Ta ion implantation is 5×10 -4 Pa, the voltage is 50Kv, and the injection quantity is 5×10 17 ion / cm 2 .

4. The preparation method according to claim 1, characterized in that: The magnetron sputtering time is 2-6 hours.

5. The preparation method according to claim 1, characterized in that: The titanium alloy is Ti6Al4V, Ti, Ti-2Al-2.5Zr or Ti-5Al-2.5Sn.

6. A titanium alloy modified coating implanted with N and Ta ions, prepared by the method according to any one of claims 1 to 5.

7. Use of the N and Ta ion implanted titanium alloy modified coating according to claim 6 in the preparation of friction reducing and wear resistant materials.

Citation Information

Cited By

  • Wear-resistant hard coating based on TC4 titanium alloy surface ion implantation and ion nitriding as well as preparation method and application of wear-resistant hard coating

    CN121023427A

  • A wear-resistant hard coating based on ion implantation and ion nitriding on a surface of TC4 titanium alloy and a preparation method and application thereof

    CN121023427B