A method for preparing high-purity, high-density, fine-grained, low-oxygen tungsten target

Through the process of low-temperature vacuum hot pressing and multi-pass small deformation hot rolling combined with hot isostatic pressing, the problem of taking into account the density and grain size of tungsten targets is solved, the oxygen content is reduced, and high-purity, high-density, fine crystals, and low oxygen are achieved. The preparation of tungsten targets improves the quality and performance of the coating.

CN115740452BActive Publication Date: 2024-11-22GRIKIN ADVANCED MATERIALS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211399556.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-09
Publication Date
2024-11-22
Estimated Expiration
2042-11-09

AI Technical Summary

Technical Problem

The existing tungsten target preparation process is difficult to achieve high density and fine grains at the same time, and the high oxygen content affects the performance of the film, resulting in arc discharge and particle phenomena, affecting the yield and thickness uniformity of the coating.

Method used

Low-temperature vacuum hot press sintering to obtain a preformed tungsten target blank with a relative density of 80%-90%. Through multiple passes of small deformation hot rolling, a densified package is formed on the surface layer, and then thermal isostatic sintering is performed to remove the surface layer rolling. The structure is obtained to obtain high-purity, high-density fine crystal low-oxygen tungsten target.

Benefits of technology

The high density and fine grains are achieved, the oxygen content is reduced, and the coarse grain and expensive packaging materials caused by high temperature sintering are avoided, which simplifies the process and reduces costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115740452B_ABST
    Figure CN115740452B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of magnetron sputtering target manufacturing, and discloses a method for preparing a high-purity, high-density, fine-grained, low-oxygen tungsten target. Using W powder with a purity greater than 5N as a raw material, a preformed tungsten target blank with a relative density of 80% to 90% is first obtained by vacuum hot pressing and sintering. Then, a densified surface layer with a relative density of 95% to 99% is formed on the surface of the preformed tungsten target blank within a thickness range of 0.5 to 2 mm by means of multiple passes of small deformation hot rolling, and the density and organizational state of the core remain unchanged. Finally, the tungsten target blank after multiple passes of small deformation rolling is subjected to a densification treatment by hot isostatic pressing sintering without a jacket, and after the treatment, the rolled state organization with a thickness of 0.5 to 2 mm on the surface is removed to obtain a high-purity W target blank with a density of ≥99.5%, an average grain size of ≤10 μm, and an oxygen content of ≤10 ppm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of magnetron sputtering target material manufacturing, and in particular to a method for preparing a high-purity, high-density, fine-grained, low-oxygen tungsten target material. Background Art

[0002] Tungsten target has high melting point (3410℃), high density (19.3g / cm 3 ), high thermal conductivity (165W / (m·K)), high strength, low expansion coefficient (4.6×10 -6 mm -1 ) and high corrosion resistance, and is widely used in the manufacturing process of advanced storage devices. Tungsten targets deposit W / WN films in the gate metal stacking layer, maintain a low gate stack resistivity, and prevent the reaction between W and polysilicon. Therefore, high-purity tungsten targets are key materials for the manufacture of storage devices, and the preparation of high-density, fine-grained, low-oxygen high-purity W targets has become a key technology for achieving excellent coatings. Due to the characteristics of tungsten such as high hardness and large elastic modulus, it is difficult for plastic deformation to achieve densification during its processing, resulting in low density and coarse grains. Low density will produce arcing and particles in the subsequent magnetron sputtering coating process, affecting the yield of the film. Coarse grains affect the uniformity of the coating thickness and the deposition rate. In addition, the oxygen content of high-purity tungsten powder is generally 300-500ppm, which is easy to cause the high oxygen content of the W target blank after sintering. The high oxygen content affects the resistivity of the film and thus the performance of the device.

[0003] W targets are mainly sintered by powder metallurgy process, and the process mainly includes: (1) hot pressing (HP) of tungsten powder followed by hot isostatic pressing (HIP) without a jacket, such as patents US6582535B1, TW201837217A, CN105102670B, CN103567443B; (2) preforming of tungsten powder (which can be performed by hot pressing, cold isostatic pressing (CIP), hot isostatic pressing) to reach a density of 70% to 90%, followed by hot isostatic pressing and sintering with a jacket, the jacket being niobium or tantalum, such as patents US6582535B1, TW201837217A, CN105102670B, CN103567443B; (3) preforming of tungsten powder (which can be performed by hot pressing, cold isostatic pressing (CIP), hot isostatic pressing) to reach a density of 70% to 90%, followed by hot isostatic pressing and sintering with a jacket, the jacket being niobium or tantalum, such as patents US6582535B1, TW201837217A, CN105102670B, CN103567443B; CN103124804B; (3) After cold isostatic pressing of tungsten powder, pressureless sintering in hydrogen atmosphere is performed, and finally hot isostatic pressing without a jacket is performed, such as patents US20070172378A1 and CN103567444B; (4) After cold isostatic pressing of tungsten powder, pressureless sintering in hydrogen atmosphere is performed, and finally hot rolling is performed to improve density, such as patents TW201730360A and CN103805952B; (5) Tungsten powder is subjected to spark plasma sintering (SPS), such as patent CN102046822B.

[0004] The above five forming processes each have their own advantages and disadvantages: (1) Process route 1 adopts the method of hot isostatic pressing without a jacket to prepare high-purity W target material. The preformed W target blank after hot pressing and sintering cannot have through holes, that is, the relative density of the preformed W target blank is required to be >95%. In order to increase the density of the preformed W target blank, high temperature is required to make up for the shortcoming of low hot pressing pressure. High temperature will promote the growth of grains in the tungsten target, which is not conducive to the acquisition of fine-grained tungsten target materials. The grain size of the final W target material is 20-70μm; (2) Process route 2 uses niobium and tantalum materials for sheathing, which is expensive and difficult to process and seal. The process is difficult to implement and the yield is low; (3) Process route 3 uses hydrogen atmosphere pressureless sintering, which requires a high temperature (>1900℃), which is also easy to cause coarse grains inside the W target; (4) Process route 4 finally uses a large deformation hot rolling process, which is easy to produce banded structure and preferential orientation, and the structure is coarse; (5) Process route 5 uses spark plasma sintering process, which is currently only available in laboratory sample preparation and cannot prepare large-sized tungsten target blanks. Summary of the invention

[0005] In view of the deficiencies of the above-mentioned prior art, the present invention provides a method for preparing a high-purity, high-density, fine-grained, low-oxygen tungsten target.

[0006] The present invention is achieved through the following technical solutions.

[0007] A method for preparing a high-purity, high-density, fine-grained, low-oxygen tungsten target material, comprising:

[0008] (1) Using high-purity W powder as raw material;

[0009] (2) sintering high-purity W powder by vacuum hot pressing to obtain a preformed tungsten target blank with a relative density of 80% to 90%;

[0010] (3) subjecting the preformed tungsten target blank to multiple passes of small deformation hot rolling to form a densified surface sheath with a relative density of 95% to 99% within a range of 0.5 to 2 mm thickness on the surface of the preformed tungsten target blank;

[0011] (4) After hot isostatic pressing and sintering the tungsten target blank obtained in step (3), the surface rolled structure is removed to obtain a high-purity, high-density, fine-grained, low-oxygen tungsten target material.

[0012] Furthermore, the purity of the high-purity W powder in step (1) is >5N, and the oxygen content is <500ppm.

[0013] Furthermore, in step (2), the vacuum hot pressing sintering temperature is 1000-1450° C., the sintering pressure is 20-30 MPa, and the sintering time is 1-2 h.

[0014] Furthermore, in step (3), multiple passes of small deformation hot rolling: the deformation of a single pass of hot rolling is ≤3%, and the total deformation is 10% to 15%. If the total deformation in this step is >15%, a rolled strip structure will be generated inside the target material, resulting in a rolled orientation, coarse grains and large internal stress; if the total deformation in this step is <10%, a densified surface layer with a relative density of more than 95% cannot be obtained, and through holes still exist on the surface of the target material, and the subsequent densification treatment cannot be performed by the uncapped HIP method.

[0015] Furthermore, step (4) hot isostatic pressing sintering treatment: the tungsten target blank obtained in step (3) is placed in a hot isostatic pressing furnace for pressing and sintering, the pressing pressure used in the hot isostatic pressing is 120-150 MPa, the sintering temperature is 1600°C-1800°C, and the heat and pressure are maintained for 3-4 hours.

[0016] Furthermore, step (4) removes the surface rolled structure with a thickness of 0.5 to 2 mm.

[0017] Furthermore, a high-purity, high-density, fine-grained, low-oxygen tungsten target is obtained: purity>5N, density≥99.5%, average grain size≤10μm, oxygen content≤10ppm.

[0018] Beneficial technical effects of the present invention:

[0019] (1) Taking into account the requirements of high density and fine grains at the same time: The present invention first adopts low-temperature hot pressing and sintering to obtain a preformed W target blank with low density and fine grains, and then adopts a multi-pass small deformation hot rolling method to form a densification jacket on the surface of the preformed W target blank, and finally obtains a high-purity W target material with high density and fine grains by hot isostatic pressing densification. This avoids the process route 1 and process route 3 in which the density is increased by high-temperature sintering to obtain a preformed W target blank without through holes, and the tungsten target material with fine grains cannot be obtained.

[0020] (2) Simple process and low cost: This technical solution forms a densified sheath on the surface of the preformed W target blank by small deformation hot rolling, avoiding the expensive niobium and tantalum material sheath used in process route 2. The process is simple and the cost is low.

[0021] (3) Low oxygen content: The oxygen content of tungsten powder can be effectively removed by vacuum hot pressing and sintering, reducing it to below 10ppm. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 It is a schematic diagram of the preparation method of the present invention. DETAILED DESCRIPTION

[0023] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0024] The invention mechanism of the present invention is as follows: firstly, a preformed W target blank with fine equiaxed crystals and low oxygen is obtained by low-temperature vacuum hot pressing and sintering; then, the surface layer of the preformed W target blank is densified by multiple small deformation hot rolling processes to eliminate through holes in the surface layer, while the low-density, fine equiaxed crystal structure of the internal preformed W target blank is not destroyed; finally, the W target blank after the small deformation hot rolling process is placed in a hot isostatic pressing furnace for densification treatment, because the through holes on the surface layer of the W target blank after the hot rolling process have been eliminated, the pressure can be transferred to the inside for densification treatment during hot isostatic pressing, and finally a high-density W target blank is obtained; and the internal structure of the W target blank after rolling still maintains a fine equiaxed crystal state, and a fine equiaxed crystal structure can still be obtained after hot isostatic pressing densification, thereby avoiding the problems of banded coarse structure and preferential orientation generated by a large deformation hot rolling process.

[0025] A method for preparing a high-purity, high-density, fine-grained, low-oxygen tungsten target material, comprising:

[0026] (1) Weighing: Weigh the required high-purity W powder as raw material, with a purity of >5N and an oxygen content of <500ppm.

[0027] (2) Vacuum hot pressing sintering: high-purity W powder is preformed by vacuum hot pressing sintering to obtain a preformed tungsten target blank with a relative density of 80% to 90%; wherein the sintering temperature is 1000 to 1450°C, the sintering pressure is 20 to 30 MPa, and the sintering time is 1 to 2 hours.

[0028] (3) Hot rolling: The obtained preformed tungsten target blank is subjected to multiple passes of small deformation hot rolling to form a densified surface sheath with a relative density of 95% to 99% within a range of 0.5 to 2 mm thickness on the surface of the preformed tungsten target blank, while the density and organizational state of the remaining parts remain unchanged; in the multiple passes of small deformation hot rolling, the deformation amount of a single pass of hot rolling is ≤3%, and the total deformation amount is 10% to 15%.

[0029] (4) Hot isostatic pressing sintering: the surface densified tungsten target blank obtained in step (3) is placed in a hot isostatic pressing furnace for pressing and sintering, the pressing pressure used is 120-150 MPa, the sintering temperature is 1600° C.-1800° C., and the temperature and pressure are maintained for 3-4 hours;

[0030] (5) Machining: The densified tungsten target blank obtained in step (4) is machined to remove the surface rolled structure with a thickness of 0.5 to 2 mm, thereby obtaining a high-purity, high-density, fine-grained, low-oxygen tungsten target material with a purity of >5N, a density of ≥99.5%, an average grain size of ≤10 μm, and an oxygen content of ≤10 ppm.

[0031] Example 1

[0032] A method for preparing a high-purity, high-density, fine-grained, low-oxygen tungsten target material, comprising:

[0033] (1) Weighing: Weigh the required high-purity W powder as raw material, with a purity of 5N5 and an oxygen content of 450ppm.

[0034] (2) Vacuum hot pressing sintering: high-purity W powder is preformed by vacuum hot pressing sintering to obtain a preformed tungsten target blank with a relative density of 80.1%; wherein the sintering temperature is 1000°C, the sintering pressure is 20 MPa, and the sintering time is 2 h.

[0035] (3) Hot rolling: The obtained preformed tungsten target blank is subjected to multiple passes of small deformation hot rolling to form a densified surface sheath with a relative density of 95% within a thickness of 0.5 mm on the surface of the preformed tungsten target blank, while the density and organizational state of the remaining parts remain unchanged; the single pass hot rolling deformation amount in the step is 1%, and the total deformation amount is 10%.

[0036] (4) Hot isostatic pressing: the surface densified tungsten target blank obtained in step (3) is placed in a hot isostatic pressing furnace for pressing and sintering. The pressing pressure is 120 MPa, the sintering temperature is 1600° C., and the temperature and pressure are maintained for 4 hours.

[0037] (5) Machining: The densified tungsten target blank obtained in step (4) is machined to remove the surface rolled structure with a thickness of 0.5 mm, thereby obtaining a high-purity, high-density, fine-grained, low-oxygen tungsten target material with a density of 99.5%, an average grain size of 5.0 μm, an oxygen content of 9.3 ppm, and a purity of 5N5.

[0038] Example 2

[0039] A method for preparing a high-purity, high-density, fine-grained, low-oxygen tungsten target material, comprising:

[0040] (1) Weighing: Weigh the required high-purity W powder as raw material, with a purity of 5N5 and an oxygen content of 450ppm.

[0041] (2) Vacuum hot pressing sintering: high-purity W powder is preformed by vacuum hot pressing sintering to obtain a preformed tungsten target blank with a relative density of 84%; wherein the sintering temperature is 1225°C, the sintering pressure is 20 MPa, and the sintering time is 2 h.

[0042] (3) Hot rolling: The obtained preformed tungsten target blank is subjected to multiple passes of small deformation hot rolling to form a densified surface sheath with a relative density of 97% within a thickness of 0.5 mm on the surface of the preformed tungsten target blank, while the density and organizational state of the remaining parts remain unchanged; the deformation amount of a single hot rolling pass in the step is 2%, and the total deformation amount is 13%.

[0043] (4) Hot isostatic pressing: the surface densified tungsten target blank obtained in step (3) is placed in a hot isostatic pressing furnace for pressing and sintering. The pressing pressure is 120 MPa, the sintering temperature is 1600° C., and the temperature and pressure are maintained for 4 hours.

[0044] (5) Machining: The densified tungsten target blank obtained in step (4) is machined to remove the surface rolled structure with a thickness of 0.5 mm, thereby obtaining a high-purity, high-density, fine-grained, low-oxygen tungsten target with a density of 99.5%, an average grain size of 6.1 μm, an oxygen content of 9.0 ppm, and a purity of 5N5.

[0045] Example 3

[0046] A method for preparing a high-purity, high-density, fine-grained, low-oxygen tungsten target material, comprising:

[0047] (1) Weighing: Weigh the required high-purity W powder as raw material, with a purity of 5N5 and an oxygen content of 450ppm.

[0048] (2) Vacuum hot pressing sintering: High-purity W powder is preformed by vacuum hot pressing sintering to obtain a preformed tungsten target blank with a relative density of 87.7%; wherein the sintering temperature is 1450°C, the sintering pressure is 20 MPa, and the sintering time is 2 h.

[0049] (3) Hot rolling: The obtained preformed tungsten target blank is subjected to multiple passes of small deformation hot rolling to form a densified surface sheath with a relative density of 99% within a range of 0.5 mm thickness on the surface of the preformed tungsten target blank, while the density and organizational state of the remaining parts remain unchanged; the deformation amount of a single hot rolling pass in the step is 3%, and the total deformation amount is 15%.

[0050] (4) Hot isostatic pressing: the surface densified tungsten target blank obtained in step (3) is placed in a hot isostatic pressing furnace for pressing and sintering. The pressing pressure is 120 MPa, the sintering temperature is 1600° C., and the temperature and pressure are maintained for 4 hours.

[0051] (5) Machining: The densified tungsten target blank obtained in step (4) is machined to remove the surface rolled structure with a thickness of 0.5 mm, thereby obtaining a high-purity, high-density, fine-grained, low-oxygen tungsten target with a density of 99.6%, an average grain size of 6.7 μm, an oxygen content of 8.8 ppm, and a purity of 5N5.

[0052] Example 4

[0053] A method for preparing a high-purity, high-density, fine-grained, low-oxygen tungsten target material, comprising:

[0054] (1) Weighing: Weigh the required high-purity W powder as raw material, with a purity of 5N5 and an oxygen content of 450ppm.

[0055] (2) Vacuum hot pressing sintering: High-purity W powder is preformed by vacuum hot pressing sintering to obtain a preformed tungsten target blank with a relative density of 82.3%; wherein the sintering temperature is 1000° C., the sintering pressure is 30 MPa, and the sintering time is 2 h.

[0056] (3) Hot rolling: The obtained preformed tungsten target blank is subjected to multiple passes of small deformation hot rolling to form a densified surface layer with a relative density of 95% within a thickness of 1.5 mm on the surface of the preformed tungsten target blank, while the density and organizational state of the remaining parts remain unchanged; the single pass hot rolling deformation amount in the step is 1%, and the total deformation amount is 10%.

[0057] (4) Hot isostatic pressing: the surface densified tungsten target blank obtained in step (3) is placed in a hot isostatic pressing furnace for pressing and sintering. The pressing pressure is 120 MPa, the sintering temperature is 1600° C., and the temperature and pressure are maintained for 4 hours.

[0058] (5) Machining: The densified tungsten target blank obtained in step (4) is machined to remove the surface rolled structure with a thickness of 1.5 mm, thereby obtaining a high-purity, high-density, fine-grained, low-oxygen tungsten target material with a density of 99.6%, an average grain size of 5.3 μm, an oxygen content of 8.9 ppm, and a purity of 5N5.

[0059] Example 5

[0060] A method for preparing a high-purity, high-density, fine-grained, low-oxygen tungsten target material, comprising:

[0061] (1) Weighing: Weigh the required high-purity W powder as raw material, with a purity of 5N5 and an oxygen content of 450ppm.

[0062] (2) Vacuum hot pressing sintering: High-purity W powder is preformed by vacuum hot pressing sintering to obtain a preformed tungsten target blank with a relative density of 86.4%; wherein the sintering temperature is 1225°C, the sintering pressure is 30 MPa, and the sintering time is 2 h.

[0063] (3) Hot rolling: The obtained preformed tungsten target blank is subjected to multiple passes of small deformation hot rolling to form a densified surface sheath with a relative density of 97% within a thickness of 1.5 mm on the surface of the preformed tungsten target blank, while the density and organizational state of the remaining parts remain unchanged; the deformation amount of a single hot rolling pass in the step is 2%, and the total deformation amount is 13%.

[0064] (4) Hot isostatic pressing: the surface densified tungsten target blank obtained in step (3) is placed in a hot isostatic pressing furnace for pressing and sintering. The pressing pressure is 120 MPa, the sintering temperature is 1600° C., and the temperature and pressure are maintained for 4 hours.

[0065] (5) Machining: The densified tungsten target blank obtained in step (4) is machined to remove the surface rolled structure with a thickness of 1.5 mm, thereby obtaining a high-purity, high-density, fine-grained, low-oxygen tungsten target with a density of 99.6%, an average grain size of 6.5 μm, an oxygen content of 8.2 ppm, and a purity of 5N5.

[0066] Example 6

[0067] A method for preparing a high-purity, high-density, fine-grained, low-oxygen tungsten target material, comprising:

[0068] (1) Weighing: Weigh the required high-purity W powder as raw material, with a purity of 5N5 and an oxygen content of 450ppm.

[0069] (2) Vacuum hot pressing sintering: high-purity W powder is preformed by vacuum hot pressing sintering to obtain a preformed tungsten target blank with a relative density of 89.5%; wherein the sintering temperature is 1450°C, the sintering pressure is 30 MPa, and the sintering time is 2 h.

[0070] (3) Hot rolling: The obtained preformed tungsten target blank is subjected to multiple passes of small deformation hot rolling to form a densified surface sheath with a relative density of 99% within a thickness of 1.5 mm on the surface of the preformed tungsten target blank, while the density and organizational state of the remaining parts remain unchanged; the deformation amount of a single hot rolling pass in the step is 3%, and the total deformation amount is 15%.

[0071] (4) Hot isostatic pressing: the surface densified tungsten target blank obtained in step (3) is placed in a hot isostatic pressing furnace for pressing and sintering. The pressing pressure is 120 MPa, the sintering temperature is 1600° C., and the temperature and pressure are maintained for 4 hours.

[0072] (5) Machining: The densified tungsten target blank obtained in step (4) is machined to remove the surface rolled structure with a thickness of 1.5 mm, thereby obtaining a high-purity, high-density, fine-grained, low-oxygen tungsten target with a density of 99.7%, an average grain size of 7.2 μm, an oxygen content of 7.9 ppm, and a purity of 5N5.

[0073] Example 7

[0074] A method for preparing a high-purity, high-density, fine-grained, low-oxygen tungsten target material, comprising:

[0075] (1) Weighing: Weigh the required high-purity W powder as raw material, with a purity of 5N5 and an oxygen content of 450ppm.

[0076] (2) Vacuum hot pressing sintering: high-purity W powder is preformed by vacuum hot pressing sintering to obtain a preformed tungsten target blank with a relative density of 89.5%; wherein the sintering temperature is 1450°C, the sintering pressure is 30 MPa, and the sintering time is 2 h.

[0077] (3) Hot rolling: The obtained preformed tungsten target blank is subjected to multiple passes of small deformation hot rolling to form a densified surface sheath with a relative density of 95% within a 2 mm thickness range on the surface of the preformed tungsten target blank, while the density and organizational state of the remaining parts remain unchanged; the single pass hot rolling deformation amount in the step is 1%, and the total deformation amount is 10%.

[0078] (4) Hot isostatic pressing: the surface densified tungsten target blank obtained in step (3) is placed in a hot isostatic pressing furnace for pressing and sintering. The pressing pressure is 120 MPa, the sintering temperature is 1700° C., and the temperature and pressure are maintained for 4 hours.

[0079] (5) Machining: The densified tungsten target blank obtained in step (4) is machined to remove the surface rolled structure with a thickness of 2 mm, thereby obtaining a high-purity, high-density, fine-grained, low-oxygen tungsten target with a density of 99.8%, an average grain size of 8.4 μm, an oxygen content of 7.3 ppm, and a purity of 5N5.

[0080] Example 8

[0081] A method for preparing a high-purity, high-density, fine-grained, low-oxygen tungsten target material, comprising:

[0082] (1) Weighing: Weigh the required high-purity W powder as raw material, with a purity of 5N5 and an oxygen content of 450ppm.

[0083] (2) Vacuum hot pressing sintering: high-purity W powder is preformed by vacuum hot pressing sintering to obtain a preformed tungsten target blank with a relative density of 89.5%; wherein the sintering temperature is 1450°C, the sintering pressure is 30 MPa, and the sintering time is 2 h.

[0084] (3) Hot rolling: The obtained preformed tungsten target blank is subjected to multiple passes of small deformation hot rolling to form a densified surface layer with a relative density of 97% within a 2 mm thickness range on the surface of the preformed tungsten target blank, while the density and organizational state of the remaining parts remain unchanged; the deformation amount of a single hot rolling pass in the step is 2%, and the total deformation amount is 13%.

[0085] (4) Hot isostatic pressing: the surface densified tungsten target blank obtained in step (3) is placed in a hot isostatic pressing furnace for pressing and sintering. The pressing pressure is 120 MPa, the sintering temperature is 1800° C., and the temperature and pressure are maintained for 4 hours.

[0086] (5) Machining: The densified tungsten target blank obtained in step (4) is machined to remove the surface rolled structure with a thickness of 2 mm, thereby obtaining a high-purity, high-density, fine-grained, low-oxygen tungsten target with a density of 99.8%, an average grain size of 8.8 μm, an oxygen content of 6.9 ppm, and a purity of 5N5.

[0087] Example 9

[0088] A method for preparing a high-purity, high-density, fine-grained, low-oxygen tungsten target material, comprising:

[0089] (1) Weighing: Weigh the required high-purity W powder as raw material, with a purity of 5N5 and an oxygen content of 450ppm.

[0090] (2) Vacuum hot pressing sintering: high-purity W powder is preformed by vacuum hot pressing sintering to obtain a preformed tungsten target blank with a relative density of 89.5%; wherein the sintering temperature is 1450°C, the sintering pressure is 30 MPa, and the sintering time is 2 h.

[0091] (3) Hot rolling: The obtained preformed tungsten target blank is subjected to multiple passes of small deformation hot rolling to form a densified surface sheath with a relative density of 99% within a 2 mm thickness range on the surface of the preformed tungsten target blank, while the density and organizational state of the remaining parts remain unchanged; the single pass hot rolling deformation amount in the step is 3%, and the total deformation amount is 15%.

[0092] (4) Hot isostatic pressing: the surface densified tungsten target blank obtained in step (3) is placed in a hot isostatic pressing furnace for pressing and sintering. The pressing pressure is 150 MPa, the sintering temperature is 1600° C., and the temperature and pressure are maintained for 4 hours.

[0093] (5) Machining: The densified tungsten target blank obtained in step (4) is machined to remove the surface rolled structure with a thickness of 2 mm, thereby obtaining a high-purity, high-density, fine-grained, low-oxygen tungsten target with a density of 99.8%, an average grain size of 9.2 μm, an oxygen content of 6.5 ppm, and a purity of 5N5.

[0094] Example 10

[0095] A method for preparing a high-purity, high-density, fine-grained, low-oxygen tungsten target material, comprising:

[0096] (1) Weighing: Weigh the required high-purity W powder as raw material, with a purity of 5N5 and an oxygen content of 450ppm.

[0097] (2) Vacuum hot pressing sintering: high-purity W powder is preformed by vacuum hot pressing sintering to obtain a preformed tungsten target blank with a relative density of 89.5%; wherein the sintering temperature is 1450°C, the sintering pressure is 30 MPa, and the sintering time is 2 h.

[0098] (3) Hot rolling: The obtained preformed tungsten target blank is subjected to multiple passes of small deformation hot rolling to form a densified surface sheath with a relative density of 97% within a 2 mm thickness range on the surface of the preformed tungsten target blank, while the density and organizational state of the remaining parts remain unchanged; the deformation amount of a single hot rolling pass in the step is 2%, and the total deformation amount is 12%.

[0099] (4) Hot isostatic pressing: the surface densified tungsten target blank obtained in step (3) is placed in a hot isostatic pressing furnace for pressing and sintering. The pressing pressure is 150 MPa, the sintering temperature is 1700° C., and the temperature and pressure are maintained for 4 hours.

[0100] (5) Machining: The densified tungsten target blank obtained in step (4) is machined to remove the surface rolled structure with a thickness of 2 mm, thereby obtaining a high-purity, high-density, fine-grained, low-oxygen tungsten target material with a density of 99.9%, an average grain size of 9.5 μm, an oxygen content of 6.1 ppm, and a purity of 5N5.

[0101] Embodiment 11

[0102] A method for preparing a high-purity, high-density, fine-grained, low-oxygen tungsten target material, comprising:

[0103] (1) Weighing: Weigh the required high-purity W powder as raw material, with a purity of 5N5 and an oxygen content of 450ppm.

[0104] (2) Vacuum hot pressing sintering: high-purity W powder is preformed by vacuum hot pressing sintering to obtain a preformed tungsten target blank with a relative density of 89.5%; wherein the sintering temperature is 1450°C, the sintering pressure is 30 MPa, and the sintering time is 2 h.

[0105] (3) Hot rolling: The obtained preformed tungsten target blank is subjected to multiple passes of small deformation hot rolling to form a densified surface sheath with a relative density of 97% within a 2 mm thickness range on the surface of the preformed tungsten target blank, while the density and organizational state of the remaining parts remain unchanged; the deformation amount of a single hot rolling pass in the step is 2%, and the total deformation amount is 12%.

[0106] (4) Hot isostatic pressing: the surface densified tungsten target blank obtained in step (3) is placed in a hot isostatic pressing furnace for pressing and sintering. The pressing pressure is 150 MPa, the sintering temperature is 1800° C., and the temperature and pressure are maintained for 4 hours.

[0107] (5) Machining: The densified tungsten target blank obtained in step (4) is machined to remove the surface rolled structure with a thickness of 2 mm, thereby obtaining a high-purity, high-density, fine-grained, low-oxygen tungsten target material with a density of 99.9%, an average grain size of 9.8 μm, an oxygen content of 5.8 ppm, and a purity of 5N5.

[0108] Comparative Example 1

[0109] 1. Weighing: Weigh the corresponding weight of W powder, purity 5N5, oxygen content 400ppm.

[0110] 2. Vacuum hot pressing sintering: The W powder is preformed by vacuum hot pressing sintering to obtain a preformed tungsten target blank with a relative density of 95.6%. In this step, the sintering temperature is 1800° C., the sintering pressure is 30 MPa, and the sintering time is 2 hours.

[0111] 3. Hot isostatic pressing: The obtained preformed W target blank is placed in a hot isostatic pressing furnace for pressing and sintering. The pressing pressure used for hot isostatic pressing is 150MPa, the sintering temperature is 1800℃, and the temperature and pressure are kept for 4 hours. A high-purity W target with a density of 99.2%, an average grain size of 23μm, an oxygen content of 5.7ppm, and a purity of 5N5 is obtained.

[0112] Comparative Example 2

[0113] 1. Weighing: Weigh the corresponding weight of W powder, purity 5N5, oxygen content 320ppm.

[0114] 2. Vacuum hot pressing sintering: The W powder is preformed by vacuum hot pressing sintering to obtain a preformed tungsten target blank with a relative density of 96.2%. In this step, the sintering temperature is 2000° C., the sintering pressure is 30 MPa, and the sintering time is 2 hours.

[0115] 3. Hot isostatic pressing: The obtained preformed W target blank is placed in a hot isostatic pressing furnace for pressing and sintering. The pressing pressure used for hot isostatic pressing is 150MPa, the sintering temperature is 1800℃, and the temperature and pressure are kept for 4 hours. A high-purity W target with a density of 99.5%, an average grain size of 65μm, an oxygen content of 5.3ppm, and a purity of 5N5 is obtained.

[0116] Comparative Example 3

[0117] 1. Weighing: Weigh the corresponding weight of W powder, purity 5N5, oxygen content 320ppm.

[0118] 2. Vacuum hot pressing sintering: The W powder is preformed by vacuum hot pressing sintering to obtain a preformed tungsten target blank with a relative density of 82.3%. In this step, the sintering temperature is 1000° C., the sintering pressure is 30 MPa, and the sintering time is 2 hours.

[0119] 3. Degassing and sealing: Place the preformed W target blank into the Nb sleeve for degassing and sealing.

[0120] 4. Hot isostatic pressing: Place the package after degassing and sealing into a hot isostatic pressing furnace for pressing and sintering. The pressing pressure used for hot isostatic pressing is 120MPa, the sintering temperature is 1600℃, and the heat and pressure are maintained for 4h.

[0121] 5. Machining: After machining to remove the Nb sheath, a high-purity W target with a density of 99.6%, an average grain size of 6.5 μm, an oxygen content of 17.8 ppm, and a purity of 5N is obtained.

[0122] Comparative Example 4

[0123] 1. Weighing: Weigh the corresponding weight of W powder, purity 5N5, oxygen content 320ppm.

[0124] 2. Vacuum hot pressing sintering: The W powder is preformed by vacuum hot pressing sintering to obtain a preformed tungsten target blank with a relative density of 89.5%. In this step, the sintering temperature is 1450° C., the sintering pressure is 30 MPa, and the sintering time is 2 hours.

[0125] 3. Degassing and sealing: Place the preformed W target blank into the Nb sleeve for degassing and sealing.

[0126] 4. Hot isostatic pressing: Place the package after degassing and sealing into a hot isostatic pressing furnace for pressing and sintering. The pressing pressure used for hot isostatic pressing is 150MPa, the sintering temperature is 1800℃, and the heat and pressure are maintained for 4h.

[0127] 5. Machining: After machining to remove the Nb sheath, a high-purity W target with a density of 99.9%, an average grain size of 9.8 μm, an oxygen content of 16.6 ppm, and a purity of 5N is obtained.

[0128] Comparative Example 5

[0129] 1. Weighing: Weigh the corresponding weight of W powder, purity 5N, oxygen content 320ppm.

[0130] 2. Cold isostatic pressing: The weighed W powder is placed in a rubber package as a raw material and pressed by cold isostatic pressing at a pressure of 300 MPa for 15 minutes to obtain a W target blank with a relative density of 76.1%.

[0131] 3. Pressureless sintering in hydrogen atmosphere: The W target blank after cold isostatic pressing is placed in a sintering furnace for sintering. Hydrogen is introduced for protection during the sintering process. The sintering temperature is 2300°C and the temperature is kept for 10 hours. A W target blank with a relative density of 92.3% is obtained.

[0132] 4. Hot rolling: The W target blank pressurelessly sintered in hydrogen atmosphere is heated and then rolled to obtain a high-purity W target with a relative density of 99.9%, an average grain size of 105 μm, an oxygen content of 14.2 ppm, and a purity of 5N.

[0133] The main manufacturing processes and performance results of the W targets in Examples 1 to 11 and Comparative Examples 1 to 5 are shown in Table 1.

[0134] Table 1 Main manufacturing process and performance of W target material in implementation case

[0135]

[0136] It can be seen from the above table that compared with comparative examples 1 and 2, the density of the high-purity W target material finally obtained in the embodiment is greater than or equal to that of comparative examples 1 and 2, and the average grain size of the embodiment is significantly smaller than that of comparative examples 1 and 2, indicating that the present patent can avoid high-temperature hot pressing and sintering by means of multiple passes of small deformation hot rolling, thereby obtaining a high-density, fine-grained high-purity W target material; compared with comparative example 3 and comparative example 11, it can be seen that the relative density and average grain size of the target material obtained by the embodiment and the comparative example using the same hot pressing process and hot isostatic pressing process are consistent, but the oxygen content of the embodiment is significantly lower than that of the comparative example, indicating that the embodiment can obtain a target material with a lower oxygen content by using multiple passes of small deformation hot rolling to densify the target surface instead of the comparative example sheathing, and avoid the use of expensive Nb sheathing, which is more economical; the relative density of the high-purity W target material obtained; compared with comparative example 5, it can be seen that the high-purity W target material obtained by the patent of the present invention has a smaller average grain size and a lower oxygen content. Therefore, this patent can obtain high-purity W target materials with high density, fine grains and low oxygen content.

[0137] The above is only a preferred embodiment of the present invention and does not limit the invention. It should be pointed out that for ordinary technicians in this field, under the technical enlightenment provided by the present invention, other equivalent improvements can be made, all of which can achieve the purpose of the present invention and should be regarded as the protection scope of the present invention.

Claims

1. A method for preparing a high-purity, high-density, fine-grained, low-oxygen tungsten target. It is characterized in that The method comprises: (1) Using high-purity W powder as raw material, the purity of the high-purity W powder is >5N, and the oxygen content is <500ppm; (2) sintering high-purity W powder by vacuum hot pressing to obtain a preformed tungsten target blank with a relative density of 80% to 90%; (3) subjecting the preformed tungsten target blank to multiple passes of small deformation hot rolling, controlling the deformation of a single pass of hot rolling to ≤3%, and the total deformation to 10% to 15%, and forming a densified surface sheath with a relative density of 95% to 99% within a range of 0.5 to 2 mm thickness on the surface of the preformed tungsten target blank; (4) After hot isostatic pressing and sintering the tungsten target blank obtained in step (3), the surface rolled structure is removed to obtain a high-purity, high-density, fine-grained, low-oxygen tungsten target material, wherein the purity of the high-purity, high-density, fine-grained, low-oxygen tungsten target material is greater than 5N, the density is greater than 99.5%, the average grain size is less than 10 μm, and the oxygen content is less than 10 ppm.

2. A method for preparing a high-purity, high-density, fine-grained, low-oxygen tungsten target according to claim 1, It is characterized in that In step (2), the vacuum hot pressing sintering temperature is 1000-1450° C., the sintering pressure is 20-30 MPa, and the sintering time is 1-2 h.

3. A method for preparing a high-purity, high-density, fine-grained, low-oxygen tungsten target according to claim 1, It is characterized in that Step (4) hot isostatic pressing sintering treatment: the tungsten target blank obtained in step (3) is placed in a hot isostatic pressing furnace for pressing and sintering. The pressing pressure used in the hot isostatic pressing is 120-150 MPa, the sintering temperature is 1600° C.-1800° C., and the heat and pressure are maintained for 3-4 hours.