Supported catalyst, preparation method and application thereof, and method for preparing succinic anhydride by hydrogenating maleic anhydride
By using supported catalysts, catalysts containing Ni, Ce and Zr, the problems of low activity and selectivity of existing catalysts are solved, and the preparation of succinic anhydride is achieved at low temperature continuous hydrogenation is achieved, which reduces production costs and energy consumption, and is suitable for large-scale Large-scale industrial production.
Patent Information
- Application Number
- CN202111247219.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-26
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2041-10-26
AI Technical Summary
The existing catalysts have low activity and selectivity in the preparation of succinic anhydride by hydrothermal, high cost, and complex process, so they cannot be used in continuous large-scale industrial production.
Using a supported catalyst, including support and supported active components, containing Ni, Ce and Zr elements, and the support is Al2O3, a catalyst with high catalytic activity and selectivity is prepared by a specific preparation method, which is suitable for low-temperature continuous hydrogenation reaction. .
It improves the activity and selectivity of the catalyst, reduces the reaction temperature and pressure, simplifies the process flow, saves energy consumption, and reduces production costs. It is suitable for large-scale industrial production.
Smart Images

Figure BDA0003321474040000161 
Figure BDA0003321474040000171
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of catalysts, and in particular to a supported catalyst and a preparation method and application thereof, as well as a method for preparing succinic anhydride by hydrogenating maleic anhydride. Background Art
[0002] Succinic anhydride, also known as succinic anhydride, is an important organic synthesis intermediate and fine chemical raw material, which is widely used in food, surfactants, coatings, medicine, agriculture, plastics and other fields. Due to its unique molecular structure, succinic anhydride can undergo hydrolysis, alcoholysis, esterification, halogenation and other reactions. With the development of my country's pesticide, pharmaceutical and petrochemical industries, the demand for succinic anhydride is increasing year by year, especially high-purity succinic anhydride, which has a high degree of external dependence.
[0003] At present, the production methods of succinic anhydride used in industry include: biological fermentation, succinic acid dehydration and maleic anhydride catalytic hydrogenation. Among them, although the biological fermentation method is environmentally friendly, it has high production costs and low product yields, which is difficult to meet the needs of industrial production; the succinic acid dehydration method has a low technical threshold, but the production scale is small and the product quality is low, which is difficult to meet the supply of high-purity succinic anhydride raw material market; the maleic anhydride hydrogenation method has the advantages of simple process flow, convenient operation, high equipment utilization, low operating cost and high product purity, and is currently the most efficient process for producing succinic anhydride.
[0004] Maleic anhydride molecules have one C=C bond and two C=O bonds. Under certain catalytic conditions, selective hydrogenation of the C=C bond can synthesize succinic anhydride; continuing to hydrogenate one of the C=O bonds can synthesize γ-butyrolactone; and then hydrogenating the other C=O bond can synthesize tetrahydrofuran. It can be seen that deep hydrogenation will reduce the selectivity of succinic anhydride. How to control the hydrogenation reaction at the C=C bond hydrogenation stage is the most important problem in the preparation of succinic anhydride by hydrogenation of maleic anhydride. It is necessary to find a suitable catalyst to improve the selectivity of succinic anhydride.
[0005] US5770744 discloses a catalyst for preparing succinic anhydride by catalytic hydrogenation of maleic anhydride and a method for continuously producing succinic anhydride. The process conditions are relatively harsh, the reaction pressure is as high as 38 MPa, and special requirements are placed on the setting and material of the reactor, which limits its large-scale application.
[0006] In the methods disclosed in US1541210 and EP0691335, precious metal Pd is selected as the active component to prepare the catalyst. Although the hydrogenation selectivity is high, the amount of precious metal used accounts for 3.0-10.0% by weight of the total weight of the catalyst, which greatly increases the production cost and is difficult to achieve industrialization.
[0007] CN107597159A discloses a method for preparing a catalyst for preparing succinic anhydride by hydrogenating maleic anhydride with Ni supported on silicon carbide and its application. Although the catalyst has high activity and selectivity, the preparation process is relatively complicated and can only be used for intermittent synthesis reactions, and cannot be applied to continuous large-scale production.
[0008] In summary, the existing catalysts have low activity and succinic anhydride selectivity, high catalyst cost and complex process flow, and cannot be applied to continuous large-scale industrial production. Summary of the invention
[0009] The purpose of the present invention is to overcome the problems in the prior art that the catalyst has low activity and succinic anhydride selectivity, high catalyst cost, complicated process flow and cannot be applied to continuous large-scale production, and to provide a supported catalyst and a preparation method and application thereof, as well as a method for preparing succinic anhydride by hydrogenating maleic anhydride. The supported catalyst has high catalytic activity, a simple preparation method, low cost and can be applied to continuous large-scale industrial production.
[0010] In order to achieve the above object, the first aspect of the present invention provides a supported catalyst, characterized in that the supported catalyst comprises a carrier and an active component supported on the carrier, the active component contains Ni element, Ce element and Zr element, and the carrier contains Al2O3;
[0011] In the supported catalyst, based on the total weight of the supported catalyst, the content of the Ni element is 8-40% by weight, the content of the Ce element is 1-8% by weight, the content of the Zr element is 1-5% by weight, and the content of the carrier is 60-90% by weight, calculated as oxide.
[0012] A second aspect of the present invention provides a method for preparing a supported catalyst, characterized in that the method comprises the following steps:
[0013] (1) performing a first mixing of a Ni-containing precursor compound and a carrier precursor compound to obtain a first mixed solution; the carrier precursor compound contains Al2O3;
[0014] (2) subjecting the first mixed solution to aging and first drying in sequence to obtain a supported catalyst precursor;
[0015] (3) subjecting the supported catalyst precursor to a first contact reaction with a Ce-containing precursor compound and a Zr-containing precursor compound to obtain a base catalyst;
[0016] (4) subjecting the substrate catalyst to a second drying, followed by calcination and shaping to obtain a supported catalyst;
[0017] The amounts of the Ni-containing precursor compound, the Ce-containing precursor compound, the Zr-containing compound and the carrier are such that the prepared catalyst, based on the total weight of the supported catalyst and calculated as oxide, has a Ni content of 8-40% by weight, a Ce content of 1-8% by weight, a Zr content of 1-5% by weight and a carrier content of 60-90% by weight.
[0018] The third aspect of the present invention provides a supported catalyst prepared by the above method.
[0019] A fourth aspect of the present invention provides an application of the above-mentioned supported catalyst and / or the method for preparing the supported catalyst in hydrogenating maleic anhydride to produce succinic anhydride.
[0020] A fifth aspect of the present invention provides a method for preparing succinic anhydride by hydrogenating maleic anhydride, characterized in that the method comprises: in the presence of an activated catalyst, hydrogen and maleic anhydride undergo a second contact reaction to obtain the succinic anhydride;
[0021] Wherein, the activated catalyst is obtained by reducing and activating the above-mentioned supported catalyst with a gas containing hydrogen;
[0022] The reduction activation conditions include: temperature of 350-450° C. and time of 1-8 h.
[0023] Through the above technical scheme, the supported catalyst provided by the present invention, its preparation method and application, and the method for preparing succinic anhydride by hydrogenating maleic anhydride obtain the following beneficial effects:
[0024] The supported catalyst provided by the invention has high activity and selectivity.
[0025] Furthermore, the catalyst prepared by the method provided by the present invention can be used in the continuous hydrogenation of maleic anhydride to produce succinic anhydride at a relatively low reaction temperature (not higher than 140° C.), and has relatively high catalytic activity and selectivity.
[0026] Furthermore, the present invention provides a method for preparing succinic anhydride by hydrogenating maleic anhydride, which has a low catalytic reaction temperature and a relatively low reaction pressure of less than 3 MPa, and can continuously hydrogenate to prepare succinic anhydride, thereby saving energy consumption, simplifying the production operation process, and reducing the production operation cost. DETAILED DESCRIPTION
[0027] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0028] The first aspect of the present invention provides a supported catalyst, characterized in that the supported catalyst comprises a carrier and an active component supported on the carrier, the active component contains Ni element, Ce element and Zr element, and the carrier contains Al2O3;
[0029] In the supported catalyst, based on the total weight of the supported catalyst, the content of the Ni element is 8-40% by weight, the content of the Ce element is 1-8% by weight, the content of the Zr element is 1-5% by weight, and the content of the carrier is 60-90% by weight, calculated as oxide.
[0030] In the present invention, when the supported catalyst meets the above range, it has higher catalytic activity and selectivity.
[0031] According to the present invention, based on the total weight of the supported catalyst, calculated as oxide, the content of the Ni element is 11-25% by weight, the content of the Ce element is 3-6% by weight, the content of the Zr element is 1-3% by weight, and the content of the carrier is 70-85% by weight.
[0032] A second aspect of the present invention provides a method for preparing a supported catalyst, characterized in that the method comprises the following steps:
[0033] (1) performing a first mixing of a Ni-containing precursor compound and a carrier precursor compound to obtain a first mixed solution; the carrier precursor compound contains Al2O3;
[0034] (2) subjecting the first mixed solution to aging and first drying in sequence to obtain a supported catalyst precursor;
[0035] (3) subjecting the supported catalyst precursor to a first contact reaction with a Ce-containing precursor compound and a Zr-containing precursor compound to obtain a base catalyst;
[0036] (4) subjecting the substrate catalyst to a second drying, followed by calcination and shaping to obtain a supported catalyst;
[0037] The amounts of the Ni-containing precursor compound, the Ce-containing precursor compound, the Zr-containing compound and the carrier are such that the prepared catalyst, based on the total weight of the supported catalyst and calculated as oxide, has a Ni content of 8-40% by weight, a Ce content of 1-8% by weight, a Zr content of 1-5% by weight and a carrier content of 60-90% by weight.
[0038] In the present invention, the supported catalyst prepared by the above method can make the catalytic activity and the selectivity of succinic anhydride higher, and the preparation process is simple.
[0039] In the present invention, in step (1), there is no particular limitation on the specific conditions of the first mixing, as long as the Ni-containing precursor compound and the precursor compound of the carrier can be fully and uniformly mixed.
[0040] According to the present invention, the amounts of the Ni-containing precursor compound, the Ce-containing precursor compound, the Zr-containing compound and the carrier are such that the prepared catalyst, based on the total weight of the supported catalyst and calculated as oxide, has a Ni content of 11-25% by weight, a Ce content of 3-6% by weight, a Zr content of 1-3% by weight, and a carrier content of 70-85% by weight.
[0041] In the present invention, the amounts of the Ni-containing precursor compound, the Ce-containing precursor compound, the Zr-containing precursor compound and the carrier are such that the prepared catalyst has higher catalytic activity and selectivity.
[0042] According to the present invention, the Ni-containing precursor compound is a nickel-ammine complex solution.
[0043] Furthermore, the Ce-containing precursor compound is selected from at least one of cerium nitrate, cerium sulfate, cerium chloride and cerium acetate.
[0044] Furthermore, the Zr-containing zirconium precursor compound is selected from at least one of zirconium nitrate, zirconium sulfate, zirconium chloride and zirconium acetate.
[0045] Furthermore, the precursor compound of the carrier is selected from aluminum sol.
[0046] Furthermore, the Ce-containing precursor compound and the Zr-containing precursor compound exist in the form of solutions respectively.
[0047] Furthermore, the Ni-containing precursor compound, the carrier precursor compound, the Ce-containing precursor compound and the Zr-containing precursor compound are preferably nickel-ammine complex solution, aluminum sol, cerium nitrate and zirconium nitrate, respectively, and the prepared catalyst has more excellent catalytic activity and selectivity.
[0048] In the present invention, the content of Al2O3 in the aluminum sol is 10-40% by weight.
[0049] In the present invention, the Ce-containing precursor compound content in the Ce-containing precursor compound solution is 1-10% by weight.
[0050] In the present invention, the content of Zr precursor compound in the Zr precursor compound solution is 1-10% by weight.
[0051] According to the present invention, the method further comprises synthesizing the nickel-ammine complex solution by the following steps: in the presence of a first solvent and aqueous ammonia, a nickel salt and a complexing agent are subjected to a second mixing to obtain a nickel-ammine complex solution.
[0052] Furthermore, the molar ratio of the nickel salt to the complexing agent is 1:0.5-2.
[0053] In the present invention, the first solvent is selected from water, preferably deionized water and / or distilled water, and the amount of the first solvent used is such that the concentration of the prepared nickel ammine complex solution is 0.5-2 mol / L.
[0054] According to the present invention, the nickel salt is selected from at least one of nickel nitrate, nickel sulfate, nickel chloride, basic nickel carbonate and nickel acetate.
[0055] Furthermore, the complexing agent is selected from at least one of monoethanolamine, diethanolamine, triethanolamine and ethylenediaminetetraacetic acid.
[0056] According to the present invention, the second mixing conditions include: temperature of 40-90° C., and stirring time of 1-10 h.
[0057] Furthermore, the second mixing condition also includes adjusting the pH value of the nickel-ammine complex to 9-12.
[0058] In the present invention, the nickel ammine complex solution is synthesized by a one-step method:
[0059] In the presence of a first solvent and aqueous ammonia, the nickel salt and the complexing agent are mixed, the pH value of the solution is adjusted to 9-12, and the solution is stirred at 40-90° C. until all solids are dissolved, thereby obtaining the nickel-ammine complex solution in a one-step method, wherein the molar ratio of the nickel nitrate to the complexing agent is 1:0.5-2.
[0060] In the present invention, the optional range of the nickel salt and the complexing agent is the same as that of the aforementioned nickel salt and the complexing agent, which will not be described in detail here.
[0061] According to the present invention, in step (2), the aging conditions include: temperature of 40-90° C. and time of 12-36 h.
[0062] According to the present invention, in step (3), the conditions of the first contact reaction include: saturation impregnation and / or spraying of the Ce-containing precursor compound and the Zr-containing precursor compound with the supported catalyst precursor.
[0063] In the present invention, the optional range and concentration of the Ce-containing precursor compound and the Zr-containing precursor compound are the same as those of the aforementioned Ce-containing precursor compound and the Zr-containing precursor compound, which will not be described in detail herein.
[0064] In the present invention, the first contact reaction utilizes saturated impregnation and / or spraying to make the preparation process of the supported catalyst simpler.
[0065] According to the present invention, in step (4), the calcination conditions include: temperature of 350-500° C. and time of 2-6 hours.
[0066] According to the present invention, in step (4), there is no particular limitation on the method and shape of molding the supported catalyst. The supported catalyst can be molded by any conventional molding method in the art, such as pressure tableting or extrusion into strips.
[0067] According to the present invention, the conditions for the first drying and the second drying independently include: a temperature of 100-120° C. and a time of 10-20 h.
[0068] In the present invention, the precursor compound aluminum sol containing the carrier is mixed with the nickel ammine complex solution, and after aging and drying, a catalyst precursor with high dispersion activity can be obtained. The supported catalyst prepared from the catalyst precursor has higher catalytic activity and succinic anhydride selectivity.
[0069] According to a preferred embodiment of the present invention:
[0070] (1) in the presence of a first solvent, deionized water and ammonia water, basic nickel carbonate and ethylenediaminetetraacetic acid are mixed for a second time, ammonia gas is introduced during the preparation process, the pH value of the solution is adjusted to 9-11, and the solution is stirred at 40-90° C. until all solids are dissolved to obtain a nickel ammonia complex solution;
[0071] (2) performing a first mixing of the nickel-ammine complex solution and the aluminum sol to obtain a first mixed solution;
[0072] (3) aging the first mixed solution at 40-90° C. for 12-36 hours, and then performing a first drying at 100-120° C. for 10-20 hours to obtain a supported catalyst precursor;
[0073] (4) saturating and / or spraying the supported catalyst precursor with a cerium nitrate solution and a zirconium nitrate solution to obtain a matrix catalyst;
[0074] (5) The base catalyst is calcined at 350-500° C. for 2-6 hours and then molded to obtain a supported catalyst.
[0075] The third aspect of the present invention provides a supported catalyst prepared by the above method.
[0076] In the present invention, the supported catalyst obtained by the above preparation method has higher catalytic activity and selectivity, and is more conducive to application in large-scale industrial production.
[0077] A fourth aspect of the present invention provides an application of the above-mentioned supported catalyst and / or the method for preparing the supported catalyst in hydrogenating maleic anhydride to produce succinic anhydride.
[0078] In the present invention, when the supported catalyst prepared by the method is used in hydrogenating maleic anhydride to produce succinic anhydride, the catalytic reaction temperature and reaction pressure are relatively low, thereby further saving energy consumption.
[0079] A fifth aspect of the present invention provides a method for preparing succinic anhydride by hydrogenating maleic anhydride, characterized in that the method comprises: in the presence of an activated catalyst, hydrogen and maleic anhydride undergo a second contact reaction to obtain the succinic anhydride;
[0080] Wherein, the activated catalyst is obtained by reducing and activating the above-mentioned supported catalyst using a gas containing hydrogen;
[0081] The reduction activation conditions include: temperature of 350-450° C. and time of 1-8 h.
[0082] Furthermore, the hydrogen content in the hydrogen-containing gas is 5-100% by volume.
[0083] In the present invention, the gas containing hydrogen is hydrogen or a mixture of hydrogen and nitrogen.
[0084] In the present invention, there is no limitation on the environment for reduction activation of the supported catalyst, as long as it can be activated. For example, reduction activation can be performed in a fixed bed reactor with a gas space velocity of 10-40 h -1 .
[0085] According to the present invention, the conditions of the second contact reaction include: temperature of 60-150° C. and pressure of 1-3 MPa.
[0086] Furthermore, the molar ratio of the hydrogen to the maleic anhydride is 10-30:1.
[0087] According to the present invention, the maleic anhydride exists in the form of maleic anhydride solution, and the concentration of the maleic anhydride solution is 10-30% by weight.
[0088] According to the present invention, the maleic anhydride solution contains a second solvent, and the second solvent is at least one of tetrahydrofuran, γ-butyrolactone, cyclohexane and 1,4-dioxane.
[0089] Furthermore, the liquid hourly space velocity of maleic anhydride is 0.1-0.5h -1 .
[0090] In the present invention, there is no limitation on the equipment used in the method of preparing succinic anhydride by hydrogenating maleic anhydride, as long as the reaction can be achieved, for example, it can be carried out in a fixed bed reactor.
[0091] According to a preferred embodiment of the present invention:
[0092] (a) In a stainless steel fixed bed reactor, the supported catalyst is heated at 350-450° C. using a mixture of nitrogen and hydrogen (the hydrogen content in the mixture is 5-100% by volume and the hydrogen space velocity is 10-40 h / s). -1 ) reducing for 1-8h to activate and obtain an activated catalyst;
[0093] (b) in the presence of the activated catalyst, hydrogen and maleic anhydride solution (the solvent is selected from at least one of tetrahydrofuran, γ-butyrolactone, cyclohexane and 1,4-dioxane, and the maleic anhydride solution concentration is 10-30 wt%), at 60-150° C., 1-3 MPa, and a liquid hourly space velocity of maleic anhydride of 0.1-0.5 h -1 The second contact reaction is carried out under the condition that the molar ratio of hydrogen to maleic anhydride is 10-30:1;
[0094] (c) condensing the product after the reaction in step (b) to obtain a liquid product, and analyzing the content of each component in the liquid product by gas chromatography. Wherein, the maleic anhydride conversion rate and the selectivity of succinic anhydride are calculated by the following formula:
[0095] Maleic anhydride conversion rate = (Mo-Ma) / Mo×100%
[0096] Selectivity of succinic anhydride = Mi / (Mo-Ma)×100%
[0097] Wherein, Mo is the amount of maleic anhydride, mol;
[0098] Ma—the amount of maleic anhydride remaining after the reaction, mol;
[0099] Mi—the amount of succinic anhydride produced after the reaction, mol.
[0100] The present invention will be described in detail below by way of examples.
[0101] The pressures used in the present invention are all absolute pressures.
[0102] The Al2O3 content in the aluminum sol used below is 20% by weight.
[0103] Unless otherwise specified, the raw materials used in the following examples and comparative examples are all commercially available products.
[0104] In the following preparation examples and comparative preparation examples, the composition and content of the supported catalyst were obtained by XRF testing.
[0105] The following preparation examples are used to illustrate the supported catalyst and the preparation method thereof of the present invention.
[0106] Preparation Example 1
[0107] (1) 125.69 g of basic nickel carbonate (wherein the nickel content in terms of element is 45 wt %), 97.65 g of ethylenediaminetetraacetic acid, 1250 g of deionized water, and 115 g of 25 wt % ammonia water were weighed and mixed, and ammonia gas was introduced to adjust the pH value of the solution to 10.5, and the mixture was stirred at 45° C. until all solids were dissolved to obtain a nickel ammonia complex solution (wherein the nickel ammonia complex concentration was 0.7 mol / L);
[0108] (2) weighing 1520 g of aluminum sol and mixing it with the nickel ammine complex solution obtained in step (1) to obtain a mixed solution;
[0109] (3) Under stirring, aging the mixed solution at 60° C. for 14 h, and then drying at 120° C. for 12 h to obtain a supported catalyst precursor;
[0110] (4) saturating the supported catalyst precursor with a cerium nitrate-zirconium nitrate mixed solution containing 40.36 g Ce(NO3)3·6H2O and 18.97 g Zr(NO3)4·5H2O to obtain a matrix catalyst;
[0111] (5) The base catalyst was dried at 115° C. for 12 h, and then calcined at 400° C. for 4 h to obtain a supported catalyst S1.
[0112] Based on the total weight of the supported catalyst S1, the supported catalyst S1 contains: 18 wt% NiO, 76 wt% Al2O3, 4 wt% CeO2 and 2 wt% ZrO2.
[0113] Preparation Example 2
[0114] (1) 76.81 g of basic nickel carbonate (wherein the nickel content in terms of element is 45 wt %), 59.67 g of ethylenediaminetetraacetic acid, 760 g of deionized water, and 70 g of 25 wt % ammonia water were weighed and mixed, and ammonia gas was introduced to adjust the pH value of the solution to 10.5, and the mixture was stirred at 45° C. until all solids were dissolved to obtain a nickel ammonia complex solution (wherein the nickel ammonia complex concentration was 0.7 mol / L);
[0115] (2) weighing 1700 g of aluminum sol and mixing it with the nickel ammine complex solution obtained in step (1) to obtain a mixed solution;
[0116] (3) Under stirring, aging the mixed solution at 60° C. for 14 h, and then drying at 120° C. for 12 h to obtain a supported catalyst precursor;
[0117] (4) saturating the supported catalyst precursor with a cerium nitrate-zirconium nitrate mixed solution containing 30.27 g Ce(NO3)3·6H2O and 9.49 g Zr(NO3)4·5H2O to obtain a matrix catalyst;
[0118] (5) The base catalyst was dried at 115° C. for 12 h, and then calcined at 400° C. for 4 h to obtain a supported catalyst S2.
[0119] Based on the total weight of the supported catalyst S2, the supported catalyst S2 contains: 11 wt% NiO, 85 wt% Al2O3, 3 wt% CeO2 and 1 wt% ZrO2.
[0120] Preparation Example 3
[0121] (1) 153.62 g of basic nickel carbonate (wherein the nickel content in terms of element is 45 wt %), 119.34 g of ethylenediaminetetraacetic acid, 1550 g of deionized water, and 140 g of 25 wt % ammonia water were weighed and mixed, and ammonia gas was introduced to adjust the pH value of the solution to 10.5, and the mixture was stirred at 45° C. until all solids were dissolved to obtain a nickel ammonia complex solution (wherein the nickel ammonia complex concentration was 0.7 mol / L);
[0122] (2) weighing 1400 g of aluminum sol and mixing it with the nickel ammine complex solution obtained in step (1) to obtain a mixed solution;
[0123] (3) Under stirring, aging the mixed solution at 60° C. for 14 h, and then drying at 120° C. for 12 h to obtain a supported catalyst precursor;
[0124] (4) saturating the supported catalyst precursor with a cerium nitrate-zirconium nitrate mixed solution containing 50.46 g Ce(NO3)3·6H2O and 28.46 g Zr(NO3)4·5H2O to obtain a matrix catalyst;
[0125] (5) The base catalyst was dried at 115° C. for 12 h, and then calcined at 400° C. for 4 h to obtain a supported catalyst S3.
[0126] Based on the total weight of the supported catalyst S3, the supported catalyst S3 contains: 22 wt% NiO, 70 wt% Al2O3, 5 wt% CeO2 and 3 wt% ZrO2.
[0127] Preparation Example 4
[0128] (1) Weigh 264.67 g of Ni(NO3)3·6H2O and mix it with 800 g of deionized water to obtain a nickel nitrate solution;
[0129] (2) weighing 1560 g of aluminum sol and mixing it evenly with the nickel nitrate solution obtained in step (1) to obtain a mixed solution;
[0130] (3) Under stirring, aging the mixed solution at 60° C. for 14 h, and then drying at 120° C. for 12 h to obtain a supported catalyst precursor;
[0131] (4) saturating the supported catalyst precursor with a cerium nitrate-zirconium nitrate mixed solution containing 30.27 g of Ce(NO3)3·6H2O and 18.97 g of Zr(NO3)4·5H2O to obtain a matrix catalyst;
[0132] (5) The base catalyst was dried at 115° C. for 12 h, and then calcined at 400° C. for 4 h to obtain a supported catalyst CS4.
[0133] Based on the total weight of the supported catalyst S4, the supported catalyst S4 contains: 17 wt% NiO, 78 wt% Al2O3, 3 wt% CeO2 and 2 wt% ZrO2.
[0134] Preparation Example 5
[0135] (1) 75.73 g of nickel acetate (wherein the nickel content in terms of element is 45 wt %), 125.17 g of ethylenediaminetetraacetic acid, 1000 g of deionized water, and 115 g of 25 wt % ammonia water were weighed and mixed, and ammonia gas was introduced to adjust the pH value of the solution to 10.5. The solution was stirred at 60° C. until all solids were dissolved to obtain a nickel ammonia complex solution (wherein the nickel ammonia complex concentration was the same as that in Preparation Example 1);
[0136] (2) weighing 1780 g of aluminum sol and mixing it with the nickel ammine complex solution obtained in step (1) to obtain a mixed solution;
[0137] (3) Under stirring, aging the mixed solution at 80° C. for 12 h, and then drying at 110° C. for 18 h to obtain a supported catalyst precursor;
[0138] (4) saturating the supported catalyst precursor with a cerium nitrate-zirconium nitrate mixed solution containing 20.18 g Ce(NO3)3·6H2O and 9.49 g Zr(NO3)4·5H2O to obtain a matrix catalyst;
[0139] (5) The base catalyst was dried at 110° C. for 8 h, and then calcined at 450° C. for 3 h to obtain a supported catalyst S5.
[0140] Based on the total weight of the supported catalyst S5, the supported catalyst S5 contains: 8 wt% NiO, 89 wt% Al2O3, 2 wt% CeO2 and 1 wt% ZrO2.
[0141] Comparative Preparation Example 1
[0142] The catalyst was prepared by the method of Example 1, except that the cerium nitrate and zirconium nitrate impregnation step (4) was not performed in this comparative example. Instead, the catalyst precursor obtained in step (3) was directly subjected to step (5) to prepare catalyst S4.
[0143] Based on the total weight of the catalyst CS1, the catalyst CS1 contains: 18 wt% NiO and 82 wt% Al2O3.
[0144] Comparative Preparation Example 2
[0145] (1) 55.86 g of basic nickel carbonate (wherein the nickel content in terms of element is 45 wt %), 32.54 g of ethylenediaminetetraacetic acid, 550 g of deionized water and 50 g of 25 wt % ammonia water were weighed and mixed, and ammonia gas was introduced to adjust the pH value of the solution to 10.5, and the mixture was stirred at 45° C. until all solids were dissolved to obtain a nickel ammonia complex solution (wherein the nickel ammonia complex concentration was 0.7 mol / L);
[0146] (2) weighing 1860 g of aluminum sol and mixing it with the nickel ammine complex solution obtained in step (1) to obtain a mixed solution;
[0147] (3) Under stirring, aging the mixed solution at 60° C. for 14 h, and then drying at 120° C. for 12 h to obtain a supported catalyst precursor;
[0148] (4) saturating the supported catalyst precursor with a cerium nitrate-zirconium nitrate mixed solution containing 5.05 g Ce(NO3)3·6H2O and 4.74 g Zr(NO3)4·5H2O to obtain a matrix catalyst;
[0149] (5) The base catalyst was dried at 115° C. for 12 h, and then calcined at 400° C. for 4 h to obtain a supported catalyst CS2.
[0150] Based on the total weight of the supported catalyst CS2, the supported catalyst CS2 contains: 6 wt% NiO, 93 wt% Al2O3, 0.5 wt% CeO2 and 0.5 wt% ZrO2.
[0151] Comparative Preparation Example 3
[0152] The catalyst was prepared by the method of Example 1, except that in step (4) of this comparative example, only cerium nitrate solution (with the same concentration as in Preparation Example 1) was used for saturated impregnation to prepare supported catalyst CS3.
[0153] Based on the total weight of the supported catalyst CS3, the supported catalyst CS3 contains: 18 wt% NiO, 78 wt% Al2O3, and 4 wt% CeO2.
[0154] Comparative Preparation Example 4
[0155] The catalyst was prepared by the method of Example 5, except that the aging and first drying step in step (2) and the impregnation step in step (3) were not performed in this comparative example. Instead, the catalyst precursor obtained in step (1) was directly subjected to a first contact reaction with a Ce-containing precursor compound and a Zr-containing precursor compound to obtain a base catalyst, which was then dried and calcined to form a catalyst CS4.
[0156] Based on the total weight of the catalyst CS4, the catalyst CS4 contains: 7 wt% NiO, 89 wt% Al2O3, 3 wt% CeO2 and 1 wt% ZrO2.
[0157] Comparative Preparation Example 5
[0158] (1) 75.73 g of nickel acetate (wherein the nickel content in terms of element is 45 wt %), 125.17 g of ethylenediaminetetraacetic acid, 1000 g of deionized water, and 115 g of 25 wt % ammonia water were weighed and mixed, and ammonia gas was introduced to adjust the pH value of the solution to 10.5, and the mixture was stirred at 45° C. until all solids were dissolved to obtain a nickel ammonia complex solution (wherein the nickel ammonia complex concentration was 0.7 mol / L);
[0159] (2) weighing 1780 g of aluminum sol and mixing it with the nickel ammine complex solution obtained in step (1) to obtain a mixed solution;
[0160] (3) Under stirring, aging the mixed solution at 60° C. for 14 h, drying at 120° C. for 12 h, and then calcining at 400° C. for 4 h to obtain a supported catalyst precursor;
[0161] (4) saturating the supported catalyst precursor with a cerium nitrate-zirconium nitrate mixed solution containing 20.18 g Ce(NO3)3·6H2O and 9.49 g Zr(NO3)4·5H2O (wherein the concentrations of Ce(NO3)3·6H2O and Zr(NO3)4·5H2O are the same as those in Preparation Example 1) to obtain a matrix catalyst;
[0162] (5) The base catalyst was dried at 115° C. for 12 h and molded to obtain a supported catalyst CS5.
[0163] Based on the total weight of the catalyst CS5, the catalyst CS5 contains: 7 wt% NiO, 90 wt% Al2O3, 2 wt% CeO2 and 1 wt% ZrO2.
[0164] The following examples are used to illustrate the application of the supported catalyst of the present invention and the method for preparing succinic anhydride by hydrogenating maleic anhydride.
[0165] Example 1
[0166] The activity of the catalyst obtained in Preparation Example 1 was evaluated by the following method:
[0167] (a) In a stainless steel fixed bed reactor, the supported catalyst prepared in Preparation Example 1 above was heated at 400° C. with a mixture of nitrogen and hydrogen (the hydrogen content in the mixture was 100% by volume and the hydrogen space velocity was 0.3 h / min). -1 ) was reduced for 6 h to activate and obtain an activated catalyst;
[0168] (b) In the presence of the activated catalyst, hydrogen and maleic anhydride solution (the solvent is γ-butyrolactone, the maleic anhydride solution concentration is 20 wt%) are reacted at 90° C., pressure 2.5 MPa, and the liquid hourly space velocity of maleic anhydride is 0.2 h -1 The contact reaction was carried out under the conditions of hydrogen gas and maleic anhydride in a molar ratio of 15:1;
[0169] (c) The product after the reaction in step (b) was condensed to obtain a liquid product, and the content of each component in the liquid product was analyzed by gas chromatography. The conversion rate of maleic anhydride and the selectivity of succinic anhydride were calculated by the following formula. The specific results are shown in Table 1.
[0170] Wherein, the maleic anhydride conversion rate and the succinic anhydride selectivity are calculated by the following formula:
[0171] Maleic anhydride conversion rate = (Mo-Ma) / Mo×100%
[0172] Selectivity of succinic anhydride = Mi / (Mo-Ma)×100%
[0173] Wherein, Mo is the amount of maleic anhydride, mol;
[0174] Ma—the amount of maleic anhydride remaining after the reaction, mol;
[0175] Mi—the amount of succinic anhydride produced after the reaction, mol.
[0176] Embodiment 2-5
[0177] The method of Example 1 was followed, except that the supported catalysts prepared in Preparation Examples 2-5 were used instead of the supported catalyst prepared in Preparation Example 1, and the rest was the same as Example 1. The conversion rate of maleic anhydride and the selectivity of succinic anhydride are shown in Table 1.
[0178] Example 6
[0179] The method of Example 1 was followed, except that in step (b), the solvent was 1,4-dioxane, the concentration of maleic anhydride solution was 15 wt %), the temperature was 70° C., the pressure was 1.5 MPa, and the liquid hourly space velocity of maleic anhydride was 0.4 h -1 The contact reaction was carried out under the following conditions, the molar ratio of hydrogen to maleic anhydride was 20:1, and the rest was the same as in Example 1. The conversion rate of maleic anhydride and the selectivity of succinic anhydride are shown in Table 1.
[0180] Comparative Examples 1-5
[0181] The method of Example 1 was followed, except that the catalysts prepared in Comparative Preparation Examples 1-5 or supported catalysts were used instead of the supported catalyst prepared in Preparation Example 1, and the rest was the same as Example 1. The conversion rate of maleic anhydride and the selectivity of succinic anhydride are shown in Table 1.
[0182] Table 1
[0183]
[0184]
[0185] It can be seen from the results in Table 1 that the supported catalyst provided by the present invention has high catalytic activity and selectivity.
[0186] The method provided by the invention uses nickel ammine complex and aluminum sol as precursor compounds of nickel oxide, aluminum oxide, cerium oxide and zirconium oxide respectively, so that the prepared supported catalyst has better catalytic activity and succinic anhydride selectivity.
[0187] The supported catalyst prepared by the method provided by the present invention can be used for continuous hydrogenation of maleic anhydride to produce succinic anhydride, and the catalytic reaction temperature is relatively low, thereby further saving energy consumption.
[0188] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A method for preparing a supported catalyst, characterized in that: The method comprises the following steps: (1) a Ni-containing precursor compound and a carrier precursor compound are first mixed to obtain a first mixed solution; the carrier precursor compound contains Al2O3; (2) subjecting the first mixed solution to aging and first drying in sequence to obtain a supported catalyst precursor; (3) subjecting the supported catalyst precursor to a first contact reaction with a Ce-containing precursor compound and a Zr-containing precursor compound to obtain a base catalyst; (4) subjecting the substrate catalyst to a second drying, followed by calcination and molding to obtain a supported catalyst; Among them, the amounts of the Ni-containing precursor compound, the Ce-containing precursor compound, the Zr-containing compound and the carrier are such that the prepared catalyst, based on the total weight of the supported catalyst, has a Ni content of 8-40% by weight, a Ce content of 1-8% by weight, a Zr content of 1-5% by weight, and a carrier content of 60-90% by weight.
2. The method according to claim 1, wherein: The amounts of the Ni-containing precursor compound, the Ce-containing precursor compound, the Zr-containing compound and the carrier are such that the prepared catalyst, calculated as oxide, based on the total weight of the supported catalyst, has a Ni content of 11-25% by weight, a Ce content of 3-6% by weight, a Zr content of 1-3% by weight, and a carrier content of 70-85% by weight.
3. The method according to claim 1 or 2, wherein: The Ni-containing precursor compound is a nickel-ammine complex solution; and / or, the Ce-containing precursor compound is selected from at least one of cerium nitrate, cerium sulfate, cerium chloride and cerium acetate; and / or, the Zr-containing zirconium precursor compound is selected from at least one of zirconium nitrate, zirconium sulfate, zirconium chloride and zirconium acetate; And / or, the precursor compound of the support is selected from aluminum sol.
4. The method according to any one of claims 3, wherein: The method further comprises synthesizing the nickel-ammine complex solution by the following steps: in the presence of a first solvent and aqueous ammonia, a nickel salt and a complexing agent are mixed for a second time to obtain a nickel-ammine complex solution; And / or, the molar ratio of the nickel salt to the complexing agent is 1:0.5-2.
5. The method according to claim 4, wherein: The nickel salt is selected from at least one of nickel nitrate, nickel sulfate, nickel chloride, basic nickel carbonate and nickel acetate; And / or, the complexing agent is selected from at least one of monoethanolamine, diethanolamine, triethanolamine and ethylenediaminetetraacetic acid.
6. The method according to claim 4 or 5, wherein: The second mixing conditions include: temperature of 40-90°C and stirring time of 1-10h; And / or, the second mixing condition also includes adjusting the pH value of the nickel ammine complex solution to 9-12.
7. The method according to claim 4 or 5, wherein: In step (2), the aging conditions include: temperature of 40-90°C and time of 12-36h.
8. The method according to claim 4 or 5, wherein: In step (3), the conditions of the first contact reaction include: saturation impregnation and / or spraying of the Ce-containing precursor compound and the Zr-containing precursor compound with the supported catalyst precursor; And / or, in step (4), the calcination conditions include: temperature of 350-500°C and time of 2-6h; And / or, the conditions of the first drying and the second drying each independently include: a temperature of 100-120° C. and a time of 10-20 h.
9. A supported catalyst prepared by the method described in any one of claims 1 to 8.
10. Use of the supported catalyst according to claim 9 or the method for preparing the supported catalyst according to any one of claims 1 to 8 in hydrogenating maleic anhydride to produce succinic anhydride.
11. A method for preparing succinic anhydride by hydrogenating maleic anhydride, characterized in that: The method comprises: in the presence of an activated catalyst, hydrogen and maleic anhydride undergo a second contact reaction to obtain the succinic anhydride; Wherein, the activated catalyst is obtained by reducing and activating the supported catalyst according to claim 9 through a gas containing hydrogen; The reduction activation conditions include: temperature of 350-450° C. and time of 1-8 h.
12. The method according to claim 11, wherein: The conditions of the second contact reaction include: temperature of 60-150° C. and pressure of 1-3 MPa.
13. The method according to claim 11, wherein: The molar ratio of the hydrogen to the maleic anhydride is 10-30:
1.
14. The method according to claim 11 or 12, wherein: The maleic anhydride exists in the form of maleic anhydride solution, and the concentration of the maleic anhydride solution is 10-30% by weight.
15. The method according to claim 11 or 12, wherein: The liquid hourly space velocity of maleic anhydride is 0.1-0.5h -1 .