Perovskite nanoparticles and preparation methods and applications thereof

The preparation of perovskite nanoparticles through self-propagation reaction method and quenching method solves the problems of long reaction periods and difficult preparation of complex component compounds in the prior art, and achieves the rapid preparation and high catalytic activity of perovskite nanoparticles. Suitable for carbon monoxide oxidation catalysis.

CN116081695BActive Publication Date: 2024-11-22TSINGHUA UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310187676.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-24
Publication Date
2024-11-22
Estimated Expiration
2043-02-24

AI Technical Summary

Technical Problem

The existing perovskite nanoparticle preparation methods have long reaction cycles, and there are limitations in preparing complex component compounds, which are difficult to meet the needs of industrial production.

Method used

Perovskite nanoparticles were prepared by self-propagation reaction method and quenching method. By heating the solution in the self-propagation reactor, it turned into a viscous liquid, and then triggered a redox reaction. Small particle size and porous were prepared by quenching liquid nitrogen. Structured perovskite nanoparticles shorten the reaction cycle and improve the uniformity and controllability of the preparation.

Benefits of technology

The rapid preparation of perovskite nanoparticles is achieved, and the product has a high specific surface area and good catalytic activity. It is suitable for catalyzing carbon monoxide oxidation reaction, significantly increasing the oxidation rate of carbon monoxide.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116081695B_ABST
    Figure CN116081695B_ABST
Patent Text Reader

Abstract

The invention discloses perovskite nanoparticles and a preparation method and application thereof. The method for preparing perovskite nanoparticles comprises: providing a first solution; providing a second solution; mixing the first solution with the second solution, adding glycine to the mixed solution to obtain a third solution; placing the third solution in a self-propagating reactor, heating the third solution at a first temperature to evaporate the solvent; the third solution is converted into a viscous liquid, the temperature in the self-propagating reactor is increased to a second temperature, and a self-propagating reaction is initiated; calcining the reaction product obtained by the self-propagating reaction; quenching the calcined product to obtain perovskite nanoparticles, the chemical formula of the perovskite nanoparticles is (BiFeO3) (1‑x) ‑(SrTiO3) x , 0≤x≤1. Multiple raw materials can be completely mixed in the liquid phase, so that the prepared product has better uniformity; self-propagating combined with rapid cooling can obtain small-sized and loose and porous perovskite nanoparticles; the reaction cycle is short and the controllability is strong; the product has a certain catalytic CO oxidation activity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of material preparation, and in particular to perovskite nanoparticles and a preparation method and application thereof. Background Art

[0002] The controllable and large-scale synthesis of perovskite nanoparticles is a research topic of great significance. On the one hand, nanoparticles have rich physical and chemical properties due to their high specific surface area and size effect, and have been widely used in a variety of structural and functional materials. On the other hand, the unique crystal structure of the perovskite system and the d-electron effect of the transition metal elements make it an important research system in the fields of optoelectronics, ferroelectrics, ferromagnetism and pyroelectrics. However, many current methods for preparing perovskite nanoparticles based on hydrothermal, sol-gel and traditional solid-phase methods require long-term mixing or sintering, which may also have certain limitations in the preparation of compounds with complex components and actual industrial production.

[0003] Therefore, the current methods for preparing perovskite nanoparticles still need to be improved. Summary of the invention

[0004] In order to at least alleviate or solve at least one of the above-mentioned problems to a certain extent, one object of the present invention is to propose a method for preparing perovskite nanoparticles with a short reaction cycle and strong controllability. Another object of the present invention is to propose the use of perovskite nanoparticles prepared by this method in catalyzing the oxidation of carbon monoxide.

[0005] In one aspect of the present invention, the present invention provides a method for preparing perovskite nanoparticles. According to an embodiment of the present invention, the method for preparing perovskite nanoparticles includes: providing a first solution, wherein the first solution contains Bi 3+ and Fe 3 + and NO3 - ; Providing a second solution, the second solution containing Ti 4+ and Sr 2+ and NO3 - ; mixing the first solution with the second solution, adding glycine to the mixed solution to obtain a third solution; placing the third solution in a self-propagating reactor, heating the third solution at a first temperature to evaporate the solvent; converting the third solution into a viscous liquid, raising the temperature in the self-propagating reactor to a second temperature to initiate a self-propagating reaction; calcining the reaction product obtained by the self-propagating reaction; quenching the calcined product to obtain perovskite nanoparticles, the chemical formula of the perovskite nanoparticles being (BiFeO3) (1-x) -(SrTiO3) x, 0≤x≤1. Thus, a variety of raw materials can be completely mixed in the liquid phase, so that the final product has better uniformity; the liquid phase quickly transforms into the solid phase during the self-propagating process, and further combined with rapid cooling, small-sized and loose and porous perovskite nanoparticles can be obtained; the method is used to prepare perovskite nanoparticles, with a short reaction cycle and strong controllability. By adjusting the ratio of raw materials in the solution, the atomic ratio of each element in the product can be well controlled; the perovskite nanoparticles prepared by this method can be used to catalyze carbon monoxide oxidation reactions and have good catalytic effects.

[0006] According to an embodiment of the present invention, the first solution is obtained by fully dissolving Bi(NO3)3·5H2O and Fe(NO3)3·9H2O in deionized water, and the total concentration of metal ions in the first solution is 0.1M-0.5M. Thus, nitrate containing crystal water can be fully dissolved in deionized water, and the metal ions in the first solution have a suitable concentration.

[0007] According to an embodiment of the present invention, the second solution is obtained by the following steps: mixing Ti[O(C4H9)]4 with deionized water to hydrolyze Ti[O(C4H9)]4 to generate TiO(OH)2; adding nitric acid solution to generate TiO(OH)2 from TiO(NO3)2; adding SrCO3 at a molar ratio of 1:1 between titanium and strontium, and obtaining the second solution after the gas is completely released, wherein the total concentration of metal ions in the second solution is 0.1M-0.5M. Thus, both titanium and strontium can be dissolved in deionized water in the form of ions, and the metal ions in the second solution have a suitable concentration.

[0008] According to an embodiment of the present invention, in the third solution, the ratio of the total molar number of metal ions to the molar number of glycine is 1: 2 to 2: 1. Thus, each substance in the reaction raw material has a suitable molar ratio, which is conducive to full utilization of the raw materials, thereby facilitating improvement of the yield of the product.

[0009] According to an embodiment of the present invention, the first temperature is 80° C.-200° C., and / or the second temperature is 300° C.-500° C. Thus, most of the solvent in the third solution is evaporated at the first temperature, and after the third solution is converted into a viscous liquid, a rapid redox reaction is initiated at the second temperature to obtain solid phase particles.

[0010] According to an embodiment of the present invention, the calcination temperature is 600° C.-1100° C. Thus, the reaction product in the self-propagating reactor can be further decomposed by calcination to obtain perovskite phase product particles.

[0011] According to an embodiment of the present invention, the rapid cooling is achieved by using liquid nitrogen, so that the calcined product can be rapidly cooled by liquid nitrogen to obtain a nano-sized perovskite phase product.

[0012] In another aspect of the present invention, the present invention provides a perovskite nanoparticle. According to an embodiment of the present invention, the perovskite nanoparticle is prepared by the method described above, and the chemical formula of the perovskite nanoparticle is (BiFeO3) (1-x) -(SrTiO3) x , 0≤x≤1. Therefore, the perovskite nanoparticles have high activity and specific surface area and can be used as a catalyst.

[0013] According to an embodiment of the present invention, the particle size of the perovskite nanoparticles is 50 nm-100 nm. Therefore, the perovskite nanoparticles have a smaller particle size, which is beneficial to further improve their specific surface area and catalytic activity.

[0014] In another aspect of the present invention, the present invention proposes that the aforementioned perovskite nanoparticles are used to catalyze the carbon monoxide oxidation reaction. The aforementioned perovskite nanoparticles are used as catalysts to catalyze the carbon monoxide oxidation reaction, which can significantly increase the oxidation rate of carbon monoxide and rapidly convert carbon monoxide into carbon dioxide. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0016] Figure 1 A flow chart of a method for preparing perovskite nanoparticles according to one embodiment of the present invention is shown;

[0017] Figure 2 The X-ray diffraction patterns of the perovskite nanoparticles of Examples 1 to 4 of the present invention are shown;

[0018] Figure 3 The catalytic activity test results of the perovskite nanoparticles of Examples 1 to 4 of the present invention for catalyzing CO oxidation are shown. DETAILED DESCRIPTION

[0019] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and cannot be understood as limiting the present invention.

[0020] In one aspect of the present invention, the present invention provides a method for preparing perovskite nanoparticles. According to an embodiment of the present invention, reference is made to Figure 1 , the method for preparing perovskite nanoparticles may include the following steps:

[0021] S100: providing a first solution.

[0022] In this step, a first solution is provided, wherein the first solution contains Bi 3+ and Fe 3+ and NO3 - , NO3 - It acts as an oxidant in the subsequent self-propagating reaction and calcination process.

[0023] According to some embodiments of the present invention, the first solution is obtained by fully dissolving Bi(NO3)3·5H2O and Fe(NO3)3·9H2O in deionized water. Specifically, Bi(NO3)3·5H2O and Fe(NO3)3·9H2O can be added to deionized water in a certain proportion, and stirred to fully dissolve the solid matter. According to some specific embodiments of the present invention, in the first solution, Bi 3+ The molar concentration and Fe 3+ The molar concentrations are the same, so that the atomic ratio of bismuth element to iron element in the final product is 1:1.

[0024] According to some embodiments of the present invention, the total concentration of metal ions in the first solution may be 0.1M-0.5M. For example, the total concentration of metal ions in the first solution may be 0.1M, 0.2M, 0.3M, 0.4M, 0.5M, etc. Thus, the metal ions in the first solution have a suitable concentration, which facilitates the subsequent removal of the solvent by evaporation.

[0025] S200: providing a second solution.

[0026] In this step, a second solution is provided, wherein the second solution contains Ti 4+ and Sr 2+ and NO3 - , NO3 - It acts as an oxidant in the subsequent self-propagating reaction and calcination process.

[0027] According to some embodiments of the present invention, the second solution can be obtained by the following steps: mixing Ti[O(C4H9)]4 with deionized water to hydrolyze Ti[O(C4H9)]4 to generate TiO(OH)2; adding nitric acid solution to generate TiO(OH)2 from TiO(NO3)2; adding SrCO3 in a molar ratio of titanium to strontium of 1:1, and obtaining the second solution after the gas is completely released.

[0028] According to some specific embodiments of the present invention, tetrabutyl titanate Ti[O(C4H9)]4 can be mixed with deionized water in a mass ratio of 1:5, and Ti[O(C4H9)]4 can be fully hydrolyzed to generate TiO(OH)2 through ultrasound and / or stirring. Subsequently, a nitric acid solution is added, and the concentration of the nitric acid solution can be 5M. The mixture is fully reacted to obtain a clear solution, and TiO(OH)2 generates TiO(NO3)2. SrCO3 is added in a molar ratio of titanium to strontium of 1:1, and SrCO3 is slowly added while stirring to obtain a second solution after the gas is completely released.

[0029] According to some embodiments of the present invention, the total concentration of metal ions in the second solution is 0.1M-0.5M. For example, the total concentration of metal ions in the second solution may be 0.1M, 0.2M, 0.3M, 0.4M, 0.5M, etc. Thus, the metal ions in the second solution have a suitable concentration, which facilitates the subsequent removal of the solvent by evaporation.

[0030] It should be noted that there is no particular order in which the first solution and the second solution are prepared. The first solution can be prepared first and then the second solution; the second solution can be prepared first and then the first solution; the first solution and the second solution can also be prepared at the same time, that is, the preparation time of the first solution and the second solution can partially overlap.

[0031] S300: mixing the first solution and the second solution, and adding glycine to the mixed solution to obtain a third solution.

[0032] According to an embodiment of the present invention, according to the chemical formula of the perovskite nanoparticles (BiFeO3) (1-x) -(SrTiO3) x , 0≤x≤1, the first solution is mixed with the second solution, glycine is added to the mixed solution, and after sufficient stirring, a uniform third solution is obtained.

[0033] It should be noted that when x=0, the second solution does not need to be prepared, and glycine can be directly added to the first solution to obtain the third solution, and the chemical formula of the final product is BiFeO3; when x=1, the first solution does not need to be prepared, and glycine can be directly added to the second solution to obtain the third solution, and the chemical formula of the final product is SrTiO3.

[0034] According to some embodiments of the present invention, in the third solution, the ratio of the total molar number of metal ions to the molar number of glycine can be 1: 2 to 2: 1. For example, in the third solution, the ratio of the total molar number of metal ions to the molar number of glycine can be 1: 2, 3: 4, 1: 1, 3: 2, 2: 1. Thus, the total molar number of metal ions and the molar number of glycine are within a suitable range, and the subsequent glycine is used as a fuel in the self-propagating reactor to better maintain the self-propagating reaction.

[0035] S400: placing the third solution in a self-propagating reactor, and heating the third solution at a first temperature to evaporate the solvent.

[0036] According to an embodiment of the present invention, after obtaining the third solution, the third solution is placed in a self-propagating reactor, and the third solution is heated at a first temperature to evaporate the solvent. During the heating process, a large number of bubbles are generated in the third solution, causing the solvent to evaporate, thereby removing most of the solvent in the third solution.

[0037] According to some embodiments of the present invention, the first temperature may be 80°C-200°C. For example, the first temperature may be 80°C, 100°C, 120°C, 150°C, 170°C, 200°C, etc. At the above temperatures, the solvent in the third solution may be evaporated and removed in a relatively short time, and no self-propagating reaction may be triggered.

[0038] S500: The third solution is transformed into a viscous liquid, and the temperature in the self-propagating reactor is increased to a second temperature to initiate a self-propagating reaction.

[0039] According to an embodiment of the present invention, after the third solution is converted into a viscous liquid, the temperature in the self-propagating reactor is raised to a second temperature, which may be 300°C-500°C, for example, the second temperature may be 300°C, 350°C, 400°C, 450°C, 500°C, etc., thereby inducing a self-propagating reaction (oxidation-reduction reaction) to generate a solid phase product. It should be noted that most of the solvent in the third solution is evaporated and removed, and a small amount of solvent still exists in the viscous liquid. Further removal of the solvent in the subsequent self-propagating reaction process can obtain a reaction product with a pore structure.

[0040] S600: calcining the reaction product obtained by the self-propagating reaction.

[0041] According to an embodiment of the present invention, after the self-propagating reaction is completed, the reaction product in the self-propagating reactor is taken out and calcined, so that the reaction product obtained in the self-propagating reactor is further decomposed to obtain perovskite phase product particles. Gas is also generated during the calcination process, so that the calcined product has a richer pore structure, thereby increasing the specific surface area of ​​the product.

[0042] According to some embodiments of the present invention, the calcination temperature may be 600°C-1100°C, for example, the calcination temperature may be 600°C, 700°C, 800°C, 900°C, 1100°C, 1100°C, etc. Thus, by calcining the self-propagating reaction product at the above temperature, the reaction product can be fully decomposed to obtain a perovskite phase product.

[0043] According to some embodiments of the present invention, the calcination temperature may be 600° C. and the calcination time may be 1 hour. Thus, calcination for 1 hour can fully decompose the self-propagating reaction product, and the reaction time is short, which is beneficial to shortening the preparation cycle of perovskite nanoparticles.

[0044] According to some other embodiments of the present invention, during the calcination process, the temperature may be kept at 600° C. for 1 hour, and then the temperature may be increased to 1100° C. and kept at this temperature for another hour.

[0045] S700: Rapidly cooling the calcined product to obtain perovskite nanoparticles.

[0046] According to an embodiment of the present invention, after calcination, the calcined product can be rapidly cooled to obtain perovskite nanoparticles. The chemical formula of the perovskite nanoparticles is (BiFeO3) (1-x) -(SrTiO3) x , 0≤x≤1, where x can be 0, 0.25, 0.5, 0.75, 1, etc. Rapid cooling of the calcined product can effectively prevent further growth of the grains during the furnace cooling process, which is beneficial to reducing the particle size of the perovskite phase product and increasing the specific surface area of ​​the perovskite particles, thereby improving the catalytic activity of the product.

[0047] According to some embodiments of the present invention, rapid cooling is achieved by using liquid nitrogen. For example, the calcined product can be placed in liquid nitrogen to rapidly cool the calcined product. Rapid cooling of the calcined product by using liquid nitrogen can stabilize the high-temperature phase and is conducive to the formation of a single phase. Compared with furnace cooling, rapid cooling by using liquid nitrogen significantly shortens the annealing time and can effectively prevent the grains from continuing to grow. Different from the internal stress state at the grain boundary, under liquid nitrogen conditions, large particles tend to break from the grain boundary to obtain nanoparticles with smaller particle size, and the specific surface area will increase. After the liquid nitrogen evaporates, well-dispersed perovskite nanoparticles can be obtained.

[0048] The overall reaction equation (unbalanced) is as follows:

[0049] (1-x)Bi 3+ +(1-x)Fe 3+ +xSr 2+ +xTi 4+ +H3O + +C2H5NO2→(BiFeO3) (1-x) -(SrTiO3) x +CO2+N2+O2+H2O.

[0050] The method proposed by the present invention is used to prepare perovskite nanoparticles. The reaction raw materials are mixed in the liquid phase, and the mixing is more uniform, which is conducive to improving the uniformity of the product; soluble salts are used as raw materials, and the soluble salts are fully mixed in the liquid phase as precursors. Compared with mixed solid-phase raw material powders, it has the advantages of uniformity and shortened cycle. The method can obtain different products (including oxides with complex components) by adjusting the proportion of raw materials in the solution, and has strong controllability and easy operation; using a liquid-based self-propagating reaction combined with a quenching method, shortening the annealing time can inhibit the growth of grains, and a rich pore structure can be obtained by the rapid evaporation of the solution, with rapid reaction, short cycle, and small product particle size, large specific surface area, and rich active sites on the surface, and high catalytic activity. This method has the prospect of realizing large-scale production of perovskite nanoparticles, and the product can be used to remove the reaction system of carbon monoxide gas produced by incomplete combustion of fossil fuels.

[0051] In another aspect of the present invention, the present invention provides a perovskite nanoparticle. According to an embodiment of the present invention, the perovskite nanoparticle is prepared by the method described above, and the chemical formula of the perovskite nanoparticle is (BiFeO3) (1-x) -(SrTiO3) x , 0≤x≤1, where x can be 0, 0.25, 0.5, 0.75, 1, etc. The perovskite nanoparticles have uniform composition, high activity and high specific surface area, and can be used as a catalyst. Taking x as 0.5 as an example, (BiFeO3) 0.5 -(SrTiO3) 0.5 That is Bi 0.5 Sr 0.5 Fe 0.5 Ti 0.5 O3 is a uniform hexagonal perovskite phase compound.

[0052] According to an embodiment of the present invention, the particle size of the perovskite nanoparticles may be 50 nm-100 nm. Thus, the perovskite nanoparticles have a smaller particle size, which is beneficial to further increase their specific surface area and activity, thereby improving the catalytic performance of the perovskite nanoparticles.

[0053] In another aspect of the present invention, the present invention proposes that the aforementioned perovskite nanoparticles are used to catalyze the carbon monoxide oxidation reaction. The aforementioned perovskite nanoparticles are used to catalyze the carbon monoxide oxidation reaction, which can significantly increase the reaction rate of the carbon monoxide oxidation reaction and quickly convert carbon monoxide into carbon dioxide. The perovskite nanoparticles can be used in a reaction system for removing carbon monoxide gas generated by incomplete combustion of fossil fuels.

[0054] The present invention will be described below by specific examples, and it will be appreciated by those skilled in the art that the following specific examples are only for illustrative purposes, and do not limit the scope of the present invention in any way. In addition, in the following examples, unless otherwise specified, the materials and equipment used are all commercially available. If in the following examples, specific processing conditions and processing methods are not clearly described, then conditions and methods known in the art can be used to process.

[0055] Example 1: Synthesis and catalytic performance of BiFeO3 nanoparticles

[0056] (1) Bi(NO3)3·5H2O and Fe(NO3)3·9H2O are fully dissolved in deionized water at a molar ratio of 1:1 to obtain a first solution, wherein the total concentration of metal ions in the first solution is 0.2 M.

[0057] (2) Glycine is added to the first solution, with the total molar number of metal ions and the molar number of glycine being 2:1, and the mixture is stirred thoroughly to obtain a third solution.

[0058] (3) The third solution is placed in a self-propagating reactor, and the third solution is heated at 200° C. to evaporate the solvent.

[0059] (4) After the third solution is transformed into a viscous liquid, the temperature in the self-propagating reactor is increased to 400° C. to initiate a self-propagating reaction.

[0060] (5) After the self-propagating reaction is completed and completely cooled, the reaction product in the self-propagating reactor is taken out, placed in an alumina porcelain boat, and calcined in a tube furnace under air atmosphere at a heating rate of 10 °C min -1 Raise the temperature to calcination temperature 600℃ and keep it for 1h.

[0061] (6) After the heat preservation is completed, the calcined product is immediately taken out and placed in liquid nitrogen for rapid cooling to obtain perovskite nanoparticles BiFeO3.

[0062] The prepared BiFeO3 nanoparticles were used for carbon monoxide oxidation. 100 mg of BiFeO3 sample was mixed with 300 mg of quartz sand in an atmosphere of CO:O2:Ar=0.8:20:79.2 (molar ratio) at a space velocity of 60000 ml g -1 h -1 , testing its catalytic carbon monoxide oxidation performance.

[0063] Example 2: (BiFeO3) 0.75 -(SrTiO3) 0.25 Nanoparticle synthesis and catalytic performance

[0064] (1) Bi(NO3)3·5H2O and Fe(NO3)3·9H2O are fully dissolved in deionized water at a molar ratio of 1:1 to obtain a first solution, wherein the total concentration of metal ions in the first solution is 0.2 M.

[0065] (2) Tetrabutyl titanate Ti[O(C4H9)]4 is mixed with deionized water in a mass ratio of 1:5, and Ti[O(C4H9)]4 is fully hydrolyzed to generate TiO(OH)2 by ultrasonication and stirring. Subsequently, a 5M nitric acid solution is added to react until a clear solution is obtained, and TiO(OH)2 generates TiO(NO3)2; SrCO3 is added in a molar ratio of titanium to strontium of 1:1, and a second solution is obtained after the gas is completely released. The total concentration of metal ions in the second solution is 0.2M.

[0066] (3) The first solution and the second solution are mixed at a volume ratio of 3:1, and glycine is added to the mixed solution so that the ratio of the total molar number of metal ions to the molar number of glycine is 2:1. The mixture is stirred thoroughly to obtain a third solution.

[0067] (4) placing the third solution in a self-propagating reactor, and heating the third solution at 200° C. to evaporate the solvent.

[0068] (5) After the third solution is transformed into a viscous liquid, the temperature in the self-propagating reactor is increased to 400° C. to initiate a self-propagating reaction.

[0069] (6) After the self-propagating reaction is completed and completely cooled, the reaction product in the self-propagating reactor is taken out, placed in an alumina porcelain boat, and calcined in a tube furnace under air atmosphere at a heating rate of 10 °C min -1 Raise the temperature to 600°C and keep it for 1 hour. Continue to raise the temperature to 1100°C and keep it for 1 hour.

[0070] (7) After the 1100°C heat preservation is completed, the calcined product is immediately taken out and placed in liquid nitrogen for rapid cooling to obtain perovskite nanoparticles (BiFeO3) 0.75 -(SrTiO3) 0.25 .

[0071] The prepared (BiFeO3) 0.75 -(SrTiO3) 0.25 Nanoparticles were used for carbon monoxide oxidation. 100 mg of sample was mixed with 300 mg of quartz sand in an atmosphere of CO:O2:Ar=0.8:20:79.2 at a space velocity of 60000 ml g -1 h -1 , testing its catalytic carbon monoxide oxidation performance.

[0072] Example 3: (BiFeO3)0.5 -(SrTiO3) 0.5 Nanoparticle synthesis and catalytic performance

[0073] (1) Bi(NO3)3·5H2O and Fe(NO3)3·9H2O are fully dissolved in deionized water at a molar ratio of 1:1 to obtain a first solution, wherein the total concentration of metal ions in the first solution is 0.2 M.

[0074] (2) Tetrabutyl titanate Ti[O(C4H9)]4 is mixed with deionized water in a mass ratio of 1:5, and Ti[O(C4H9)]4 is fully hydrolyzed to generate TiO(OH)2 by ultrasonication and stirring. Subsequently, a 5M nitric acid solution is added to react until a clear solution is obtained, and TiO(OH)2 generates TiO(NO3)2; SrCO3 is added in a molar ratio of titanium to strontium of 1:1, and a second solution is obtained after the gas is completely released. The total concentration of metal ions in the second solution is 0.2M.

[0075] (3) The first solution and the second solution are mixed in a volume ratio of 1:1, and glycine is added to the mixed solution so that the ratio of the total molar number of metal ions to the molar number of glycine is 1:1. The mixture is stirred thoroughly to obtain a third solution.

[0076] (4) placing the third solution in a self-propagating reactor, and heating the third solution at 200° C. to evaporate the solvent.

[0077] (5) After the third solution is transformed into a viscous liquid, the temperature in the self-propagating reactor is increased to 400° C. to initiate a self-propagating reaction.

[0078] (6) After the self-propagating reaction is completed and completely cooled, the reaction product in the self-propagating reactor is taken out, placed in an alumina porcelain boat, and calcined in a tube furnace under air atmosphere at a heating rate of 10 °C min -1 Raise the temperature to 600°C and keep it for 1 hour. Continue to raise the temperature to 1100°C and keep it for 1 hour.

[0079] (7) After the 1100°C heat preservation is completed, the calcined product is immediately taken out and placed in liquid nitrogen for rapid cooling to obtain perovskite nanoparticles (BiFeO3) 0.5 -(SrTiO3) 0.5 .

[0080] The prepared (BiFeO3) 0.5 -(SrTiO3) 0.5 Nanoparticles were used for carbon monoxide oxidation. 100 mg of sample was mixed with 300 mg of quartz sand in an atmosphere of CO:O2:Ar=0.8:20:79.2 at a space velocity of 60000 ml g -1h -1 , testing its catalytic carbon monoxide oxidation performance.

[0081] Example 4: Synthesis and catalytic performance of SrTiO3 nanoparticles

[0082] (1) Tetrabutyl titanate Ti[O(C4H9)]4 and deionized water are mixed in a mass ratio of 1:5, and Ti[O(C4H9)]4 is fully hydrolyzed to generate TiO(OH)2 by ultrasonication and stirring. Subsequently, a 5M nitric acid solution is added to react until a clear solution is obtained, and TiO(OH)2 generates TiO(NO3)2; SrCO3 is added in a molar ratio of titanium to strontium of 1:1, and a second solution is obtained after the gas is completely released. The total concentration of metal ions in the second solution is 0.2M.

[0083] (2) Glycine is added to the second solution, with the ratio of the total molar number of metal ions to the molar number of glycine being 2:1, and the mixture is stirred thoroughly to obtain a third solution.

[0084] (3) The third solution is placed in a self-propagating reactor, and the third solution is heated at 200° C. to evaporate the solvent.

[0085] (4) After the third solution is transformed into a viscous liquid, the temperature in the self-propagating reactor is increased to 400° C. to initiate a self-propagating reaction.

[0086] (5) After the self-propagating reaction is completed and completely cooled, the reaction product in the self-propagating reactor is taken out, placed in an alumina porcelain boat, and calcined in a tube furnace under air atmosphere at a heating rate of 10 °C min -1 Raise the temperature to calcination temperature 1100°C and keep warm for 1 hour.

[0087] (6) After the 1100°C heat preservation is completed, the calcined product is immediately taken out and placed in liquid nitrogen for rapid cooling to obtain perovskite nanoparticles SrTiO3.

[0088] The prepared SrTiO3 nanoparticles were used for carbon monoxide oxidation. 100 mg of SrTiO3 sample was mixed with 300 mg of quartz sand in an atmosphere of CO:O2:Ar=0.8:20:79.2 (molar ratio) at a space velocity of 60000 ml g -1 h -1 , testing its catalytic carbon monoxide oxidation performance.

[0089] X-ray diffraction experiments were performed on the perovskite nanoparticles prepared in Examples 1 to 4. Figure 2The X-ray diffraction patterns of the perovskite nanoparticles of Examples 1 to 4 are shown in FIG. The sample of Example 1 is BiFeO3; compared with the sample of Example 1, the main body of the sample of Example 2 is transferred to the SrTiO3 phase, and there is a part of the Bi2O3 impurity phase at about 27.8°, which can be eliminated by adjusting the raw material ratio; the sample of Example 3 is a perovskite phase, and no obvious impurity phase is generated; the main body of the sample of Example 4 is a SrTiO3 phase, and no obvious impurity phase is generated.

[0090] Figure 3 The test results of the perovskite nanoparticles of Examples 1 to 4 for carbon monoxide oxidation are shown. As shown in Figure 3, BiFeO3 nanoparticles catalyze carbon monoxide oxidation, and the temperature at which carbon monoxide is completely converted is about 205°C; (BiFeO3) 0.75 -(SrTiO3) 0.25 Nanoparticles catalyze carbon monoxide oxidation, and the temperature for complete conversion of carbon monoxide is about 238°C; (BiFeO3) 0.5 -(SrTiO3) 0.5 The nanoparticles catalyze the oxidation of carbon monoxide, and the temperature at which carbon monoxide is completely converted is about 228°C; the SrTiO3 nanoparticles catalyze the oxidation of carbon monoxide, and the temperature at which carbon monoxide is completely converted is about 240°C. It can be seen that the samples prepared in each embodiment can be used to catalyze the oxidation of carbon monoxide. As a catalyst, the perovskite nanoparticles prepared by the method proposed in the present invention have good catalytic carbon monoxide oxidation performance and high catalytic activity.

[0091] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "some specific embodiments", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment are included in at least one embodiment of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in a suitable manner in any one or more embodiments or examples. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of different embodiments or examples, unless they are contradictory. In addition, it should be noted that in this specification, the terms "first", "second" and "third" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated.

[0092] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A use of perovskite nanoparticles in catalyzing carbon monoxide oxidation reaction, characterized in that: The preparation steps of the perovskite nanoparticles include: Provide a first solution, wherein the first solution contains Bi 3+ and Fe 3+ and NO 3- ; Provide a second solution, wherein the second solution contains Ti 4+ and Sr 2+ and NO 3- ; mixing the first solution and the second solution, and adding glycine to the mixed solution to obtain a third solution; placing the third solution in a self-propagating reactor, and heating the third solution at a first temperature to evaporate the solvent; The third solution is transformed into a viscous liquid, and the temperature in the self-propagating reactor is increased to a second temperature to initiate a self-propagating reaction; calcining the reaction product obtained by the self-propagating reaction; The calcined product is rapidly cooled to obtain perovskite nanoparticles, wherein the chemical formula of the perovskite nanoparticles is (BiFeO3) (1-x) -(SrTiO3) x , 0≤x≤0.5; The quenching is achieved by using liquid nitrogen; The particle size of the perovskite nanoparticles is 50nm-100nm.

2. The use according to claim 1, characterized in that The first solution is obtained by fully dissolving Bi(NO3)3·5H2O and Fe(NO3)3·9H2O in deionized water, and the total concentration of metal ions in the first solution is 0.1M-0.5M.

3. The use according to claim 1, characterized in that The second solution is obtained by the following steps: Mix Ti[O(C4H9)]4 with deionized water to hydrolyze Ti[O(C4H9)]4 to generate TiO(OH)2; Add nitric acid solution to convert TiO(OH)2 into TiO(NO3)2; SrCO3 is added in a molar ratio of titanium to strontium of 1:1, and the second solution is obtained after the gas is completely released. The total concentration of metal ions in the second solution is 0.1M-0.5M.

4. The use according to any one of claims 1 to 3, characterized in that In the third solution, the ratio of the total molar number of metal ions to the molar number of glycine is 1:2 to 2:

1.

5. The use according to any one of claims 1 to 3, characterized in that The first temperature is 80°C-200°C, and / or the second temperature is 300°C-500°C.

6. The use according to any one of claims 1 to 3, characterized in that The calcination temperature is 600°C-1100°C.