A kind of enteromorpha fiber pulp board manufacturing process

Through multi-step process, the problem of single processing method and poor refinement of the existing Ultimate fiber pulp board is solved, and the processing precision and water absorption effect are improved, and the use of Ultimate fiber is fully utilized. The value of fiber.

CN116103959BActive Publication Date: 2024-11-29SHENZHEN XINHONGJIA TECH CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202310010764.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-05
Publication Date
2024-11-29
Estimated Expiration
2043-01-05

AI Technical Summary

Technical Problem

The existing Ultimate fiber pulp board production process is relatively single, resulting in poor processing refinement, less water absorption effect, and the inability to fully utilize the value of Ultimate fiber.

Method used

Multi-step processes are adopted, including salvage, drying, decomposition, cutting, steaming, grinding and making mesh. Through these steps, Ultimate fibers are finely processed to improve their processing precision.

Benefits of technology

The processing precision of Ultimate fiber pulp board is improved, making it more suitable for non-woven fabrics, diapers, sanitary napkins and adult incontinence pads, enhancing its water absorption effect and making full use of Ultimate fiber value.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a process for making a pulp board of enteromorpha fiber, comprising the steps of a) salvaging; b) drying; c) removing impurities; d) cutting; e) boiling; f) grinding; g) making a net, wherein the step a) salvaging is to salvage the enteromorpha grown out of the water surface in the selected pond area by a salvage ship at 5 a.m. every day. The invention salvages, dries and removes impurities of the enteromorpha, and then improves the processed enteromorpha by boiling and grinding, thereby improving the refinement of the production steps of the enteromorpha fiber pulp board production process, making the internal structure of the enteromorpha fiber pulp board more delicate, and making it more suitable for application in non-woven fabrics, diapers, sanitary napkins and adult incontinence pads, thereby improving the processing refinement, and solving the problem that the processing method of the existing enteromorpha fiber pulp board production process is relatively single, and is generally manufactured directly by drying and grinding, and the processing refinement degree is poor, resulting in its water absorption effect is not obvious, and the value of the enteromorpha fiber cannot be fully utilized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of enteromorpha fiber products, in particular to a process for producing an enteromorpha fiber pulp board. Background Art

[0002] Enteromorpha is an algae plant of the Ulvaceae family and the Enteromorpha genus. The algae is bright green and composed of a single layer of cells, which are arranged into tubes or adhered into ribbons. The cell arrangement depends on the species. It is mononuclear and has lamellar chloroplasts. The plant height can reach 1 meter, and the base has a disc-shaped holdfast composed of rhizoid filaments.

[0003] Enteromorpha fiber can be formed into pulp board after processing, which can be used in non-woven fabrics, diapers, sanitary napkins and adult incontinence pads. However, the existing Enteromorpha fiber pulp board production process is relatively simple, and is generally manufactured directly by drying and grinding. The degree of processing refinement is poor, resulting in its water absorption effect is not obvious, and the value of Enteromorpha fiber cannot be fully utilized.

[0004] Therefore, it is necessary to design and transform the processing method of the Enteromorpha fiber pulp board production process to effectively improve the processing fineness of the Enteromorpha fiber. Summary of the invention

[0005] In order to solve the problems raised in the above-mentioned background technology, the purpose of the present invention is to provide a process for producing a pulp board of Enteromorpha fiber, which has the advantage of improving the processing fineness, and solves the problem that the existing process for producing Enteromorpha fiber pulp board is relatively single in processing method, and is generally manufactured directly by drying and grinding, and the processing fineness is poor, resulting in its water absorption effect is not obvious, and the value of Enteromorpha fiber cannot be fully utilized.

[0006] To achieve the above object, the present invention provides the following technical solution: a process for making a pulp board of enteromorpha fiber, comprising the steps of a) salvaging; b) drying; c) removing impurities; d) cutting; e) steaming; f) grinding; and g) making a net:

[0007] Step a) Salvage: At 5 a.m. every day, the Enteromorpha growing out of the water in the selected pond area is salvaged by a salvage boat and sent to the processing area before 7 a.m.;

[0008] Step b) drying: continuously drying the enteromorpha by a drum dryer;

[0009] Step c) impurity removal: placing the dried Enteromorpha into a vibrating screening machine for screening, so that the impurities inside the Enteromorpha are separated from the Enteromorpha;

[0010] Step d) cutting: feeding the Enteromorpha into a G500 cutting machine for cutting, and forming Enteromorpha fiber strips with a width of 4 to 7 mm after cutting;

[0011] Step e) steaming: placing the cut Enteromorpha fiber strips into a steaming pot and steaming them at a temperature of 140 to 150° C. for 30 to 35 minutes;

[0012] Step f) grinding: grinding the cooked Enteromorpha fibers using a Raymond mill to separate and refine the Enteromorpha fibers;

[0013] Step g) web making: the ground Enteromorpha fibers are wet-webbed and dried to obtain Enteromorpha pulp board.

[0014] As a preferred embodiment of the present invention, in the step a) salvage, a cross bar is installed in front of the hull, and a scoop net is installed on the wings of the fishing boat, and a crane is provided. The scoop net consists of a steel frame mesh and a 10m long net sleeve. When the fishing boat is sailing, the enteromorpha automatically falls into the net bag from the steel frame mesh, and then is uniformly packed by the transport ship with a crane and transported back to the fishing port for unloading.

[0015] As a preferred embodiment of the present invention, in the step b) of drying, the enteromorpha is dried in a drum dryer at a temperature of 200-250° C. for 10-15 minutes.

[0016] As a preferred embodiment of the present invention, in step c) of removing impurities, a vibrating screening machine is used to vibrate and strike the Enteromorpha so that impurities adsorbed on the surface of the Enteromorpha fall directly to the outside of the Enteromorpha.

[0017] As a preferred embodiment of the present invention, in the step d) of cutting, the Enteromorpha fiber needs to be rolled up by a winder before cutting to form a cylindrical state, and then cut from its end face by a cutter.

[0018] As a preferred embodiment of the present invention, in step e) steam cooking, a sodium hypochlorite solution is added during the steam cooking process for bleaching, and 20 liters of sodium hypochlorite solution is added for every 180 liters of aqueous solution.

[0019] As a preferred embodiment of the present invention, in step f) grinding, the Enteromorpha fibers ground by the Raymond mill flow into the interior of the coarse pulp pool, and then the Enteromorpha fiber slurry is beaten by a pulping machine and further refined after being processed by a fine pulping machine.

[0020] As a preferred embodiment of the present invention, the step g) of making a net comprises filtering the Enteromorpha fiber slurry using a rotary wing screen, then feeding the filtered Enteromorpha fiber slurry into a long-web multi-cylinder paper machine using a headbox for wet web forming, then drying it in a steam dryer at a temperature of 200°C, and then winding the dried Enteromorpha fiberboard using a winder.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] 1. The present invention salvages, dries and removes impurities from the enteromorpha, and then improves the processed enteromorpha by steaming and grinding, thereby improving the refinement of the production steps of the enteromorpha fiber pulp board production process, making its internal structure more delicate and more suitable for application in non-woven fabrics, diapers, sanitary napkins and adult incontinence pads, thereby improving the advantage of processing refinement, and solving the problem that the existing enteromorpha fiber pulp board production process has a relatively single processing method, which is generally manufactured directly by drying and grinding, and the degree of processing refinement is poor, resulting in its water absorption effect is not obvious, and the value of the enteromorpha fiber cannot be fully utilized. DETAILED DESCRIPTION

[0023] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] The present invention provides a process for making a pulp board of enteromorpha fiber, comprising the steps of a) salvaging; b) drying; c) removing impurities; d) cutting; e) steaming; f) grinding; and g) making a net.

[0025] Step a) Salvage: At 5 a.m. every day, the Enteromorpha growing out of the water in the selected pond area is salvaged by a salvage boat and sent to the processing area before 7 a.m.;

[0026] Step b) drying: continuously drying the enteromorpha by a drum dryer;

[0027] Step c) impurity removal: placing the dried Enteromorpha into a vibrating screening machine for screening, so that the impurities inside the Enteromorpha are separated from the Enteromorpha;

[0028] Step d) cutting: feeding the Enteromorpha into a G500 cutting machine for cutting, and forming Enteromorpha fiber strips with a width of 4 to 7 mm after cutting;

[0029] Step e) steaming: placing the cut Enteromorpha fiber strips into a steaming pot and steaming them at a temperature of 140 to 150° C. for 30 to 35 minutes;

[0030] Step f) grinding: grinding the cooked Enteromorpha fibers using a Raymond mill to separate and refine the Enteromorpha fibers;

[0031] Step g) web making: the ground Enteromorpha fibers are wet-webbed and dried to obtain Enteromorpha pulp board.

[0032] The present invention is further configured as follows: step a) salvage, a cross bar is installed in front of the hull, a scoop net is installed on the wings of the fishing boat, and a lifting rod is provided, the scoop net is composed of a steel frame net mouth and a 10-m-long net sleeve, when the fishing boat is sailing, the enteromorpha automatically falls into the net bag from the steel frame net mouth, and then is uniformly packed by the transport ship with a lifting rod and transported back to the fishing port for unloading.

[0033] The present invention is further configured as follows: step b) drying, the enteromorpha is dried in a drum drying machine at a temperature of 200 to 250° C. for 10 to 15 minutes.

[0034] The present invention is further configured as follows: Step c) impurity removal, using a vibration screening machine to vibrate and beat the Enteromorpha, so that the impurities adsorbed on the surface of the Enteromorpha directly fall to the outside of the Enteromorpha.

[0035] The present invention is further configured as follows: in step d) cutting, the enteromorpha fiber needs to be rolled up by a winder before cutting to form a cylindrical state, and then cut from its end face by a cutter.

[0036] The present invention is further configured as follows: step e) cooking, during which sodium hypochlorite solution is added for bleaching, and 20 liters of sodium hypochlorite solution is added for every 180 liters of aqueous solution.

[0037] The present invention is further configured as follows: step f) grinding, the Enteromorpha fiber ground by the Raymond mill flows into the interior of the coarse pulp pool, and then the Enteromorpha fiber slurry is beaten by a pulping machine and further refined after being processed by a fine pulping machine.

[0038] The present invention is further configured as follows: step g) web making, using a rotary wing screen to filter the Enteromorpha fiber slurry, and then using a headbox to feed the filtered Enteromorpha fiber slurry into the interior of a long-web multi-cylinder paper machine for wet web forming, and then drying it in a steam dryer at a temperature of 200°C, and then using a winder to wind up the dried Enteromorpha fiberboard.

[0039] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0040] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A process for producing enteromorpha fiber pulp board, characterized in that: The method comprises the steps of a) fishing; b) drying; c) removing impurities; d) cutting; e) boiling; f) grinding; and g) making a net. Step a) Salvage: At 5 a.m. every day, the Enteromorpha growing out of the water in the selected pond area is salvaged by a salvage ship, and is uniformly sent to the processing area before 7 a.m., a cross bar is installed in front of the hull, and a sling net is installed on the wings of the fishing boat, and a sling net is equipped. The sling net consists of a steel frame net mouth and a 10-meter-long net sleeve. When the fishing boat is sailing, the Enteromorpha automatically falls into the net bag from the steel frame net mouth, and then is uniformly packed by the transport ship with a sling and transported back to the fishing port for unloading; Step b) drying: continuously drying the enteromorpha in a drum dryer, wherein the enteromorpha is dried in the drum dryer at a temperature of 200 to 250° C. for 10 to 15 minutes; Step c) impurity removal: placing the dried Enteromorpha into a vibrating screening machine for screening to separate the impurities inside the Enteromorpha from the Enteromorpha, and using the vibrating screening machine to vibrate and beat the Enteromorpha so that the impurities adsorbed on the surface of the Enteromorpha directly fall to the outside of the Enteromorpha; Step d) cutting: feeding the Enteromorpha into a G500 cutting machine for cutting, and forming Enteromorpha fiber strips with a width of 4 to 7 mm after cutting. In the step d) cutting, the Enteromorpha fiber needs to be rolled up by a winding machine before cutting to form a cylindrical state, and then cut from its end face by the cutting machine; Step e) cooking: putting the cut Enteromorpha fiber strips into a cooking pot and cooking them at a temperature of 140 to 150° C. for 30 to 35 minutes, adding a sodium hypochlorite solution for bleaching during the cooking process, and adding 20 liters of sodium hypochlorite solution for every 180 liters of aqueous solution; Step f) grinding: grinding the Enteromorpha fibers after cooking by using a Raymond mill to separate and refine the Enteromorpha fibers, the Enteromorpha fibers ground by the Raymond mill flow into a rough pulp tank, and then the Enteromorpha fiber slurry is beaten by a pulping machine and further refined by a fine pulping machine; Step g) web making: the ground Enteromorpha fibers are wet-webbed and dried to obtain Enteromorpha pulp board, the Enteromorpha fiber slurry is filtered using a rotary wing screen, and then the filtered Enteromorpha fiber slurry is fed into a long-web multi-cylinder paper machine using a headbox for wet web forming, and then dried in a steam dryer at a temperature of 200°C, and then the dried Enteromorpha fiber board is rolled up using a winder.

Citation Information

Patent Citations

  • Method for preparing freshness-retaining bag containing enteromorpha fiber

    CN103061209A