High-hardness, high-wear-resistance and high-toughness hot work die steel and preparation method thereof
Through the smelting and forging method combining high C, low Si, high Mo composition design and multi-process smelting and forging methods, the problem of insufficient hardness, wear resistance and toughness in high-end industrial applications is solved, and high hardness and wear resistance are achieved and high toughness mold steel preparation to meet modern industrial needs.
Patent Information
- Application Number
- CN202411189373.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-03
AI Technical Summary
Existing mold steels are difficult to meet the needs of high hardness, high wear resistance and high toughness in high industrial applications, and there are problems of inhomogeneity of components and insufficient organizational regulation in smelting and forging processes.
Adopt high C, low Si and high Mo composition design, combined with electric furnace smelting, vacuum refining, continuous casting electrode blank, annealing and forging technology, and ensure uniform distribution of carbides and austenite grains through solid solution + spheroidization treatment technology. Refine and improve the mechanical properties of the material.
It realizes high hardness, wear resistance and toughness of mold steel, significantly improves the purity and tissue uniformity of the material, and meets the requirements of modern industry for high-end molds.
Smart Images

Figure CN119061311A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of die steel preparation, in particular to a hot working die steel with high hardness, high wear resistance and high toughness and a preparation method thereof. Background Art
[0002] With the development of modern industry, molds are used more and more widely. In automobiles, electronics, instruments and meters, home appliances, aerospace, building materials, motors and communication equipment, about 60%-80% of the parts are processed and formed by molds, so it is called the "mother of industry". It is estimated that the ratio of molds to related industries is about 1:100, that is, 100 million yuan of mold development can drive 10 billion yuan of related industries. Summary of the invention
[0004] The purpose of the present invention is to provide a method for preparing a hot working die steel with high hardness, high wear resistance and high toughness. The method is based on the commonly used hot working die steel H13, adopts the composition design concept of high C, low Si and high Mo to design the composition, and adds special smelting, forging and heat treatment processes, so that the prepared product has excellent purity, uniformity of structure and mechanical properties. The mold made of this material can better meet the requirements of modern industrial production for high-end molds.
[0005] In order to achieve the purpose of the above invention, a method for preparing a hot working die steel with high hardness, high wear resistance and high toughness is provided, and the main steps are as follows:
[0006] S1. Electric furnace smelting:
[0007] According to the component content of hot working die steel, blast furnace molten iron (ratio ≥ 60%), shearing charge and bulk surplus steel are prepared, CaO, CaF2, aluminum block and dolomite are added, and the steel is melted and smelted in an electric furnace; after slagging, CaO, cleaning agent and aluminum block are added before tapping, and the tapping temperature is ≥ 1620℃;
[0008] Among them, the component contents of hot working die steel are, by mass percentage, C 0.40%-0.45%, Mn 0.30%-0.50%, Si 0.20%-0.50%, S≤0.001%, P≤0.008%, Cr 4.90%-5.10%, Mo 2.30%-2.60%, V 0.50%-0.70%, and the rest is Fe, and the residual gas content is, H≤1.5ppm, O≤13ppm, N≤90ppm; the residual harmful elements Cu≤0.05%, Ti, Sn, Pb are all ≤0.002%;
[0009] S2, ladle refining furnace refining:
[0010] The ladle refining furnace is heated, and slag CaO, CaF2, and C-Si powder are added to reduce and adjust the slag system;
[0011] S3, vacuum refining furnace refining:
[0012] The integrated RH vacuum tank is equipped with an advanced vacuum pump, and the vacuum degree is ≤15Pa. After degassing, sampling and analysis are performed. After the components are qualified, argon gas is softly blown into the hanging bag.
[0013] S4, continuous casting electrode billet:
[0014] The superheat of the first furnace is 20-35℃, and the continuous casting furnace is 18-30℃; the continuous casting speed is 0.13-0.20m / min, and three-stage electromagnetic stirring is adopted;
[0015] S5. Electrode blank annealing:
[0016] Annealing the electrode blank after continuous casting in step S4;
[0017] S6, electroslag remelting:
[0018] The electrode blank obtained in step S5 is surface-polished and smelted using a binary slag system of calcium fluoride and alumina to obtain an electroslag ingot;
[0019] S7, Forging:
[0020] The electroslag ingot obtained in step S6 is heated to 1260-1300° C., kept warm for 15-30 hours for diffusion homogenization, and then forged into a rectangular flat billet by roughing, drawing and forging. The intermediate billet is then heated to 1280° C. again, kept warm for 15-30 hours for diffusion homogenization, and then subjected to multi-directional upsetting and drawing in the three directions of X, Y and Z to the finished product size;
[0021] S8, heat treatment after forging:
[0022] The forging blank obtained in step S7 is subjected to post-forging extreme cooling control to inhibit the precipitation of grain boundary carbides;
[0023] S9, solution + spheroidizing initial treatment:
[0024] The forging blank after the post-forging heat treatment in step S8 is subjected to a solid solution + spheroidizing initial treatment;
[0025] S10, solution + spheroidizing final treatment;
[0026] The forging blank obtained in step S9 is subjected to a final treatment of solid solution + spheroidization.
[0027] Specifically, in step S1, the proportion of molten iron in the blast furnace is ≥ 60%.
[0028] Specifically, in step S3, under vacuum conditions, the circulation flow rate is ≥100t / min, the processing time is ≥35 minutes, and the residual gas H is ensured to be ≤1.5ppm, N ≤80ppm. After the vacuum degassing is completed, sampling and analysis are performed, and argon gas is blown into the hanging bag after the components are qualified.
[0029] Furthermore, in step S3, the soft blowing time of argon gas is 18 to 39 minutes, and the bag temperature is 1550 to 1568°C.
[0030] Specifically, in step S5, the annealing temperature is 840-860°C, the holding time is 1-1.5 min / mm, and the furnace is cooled to below 350°C before being taken out of the furnace.
[0031] Specifically, in step S6, the starting melting rate value of the steady-state stage of electroslag smelting is 7-10 kg / min, and the end melting rate value is 5.0-8.0 kg / min, and then the furnace is shut down to cool for 80-100 minutes before being sent to the forging process.
[0032] Specifically, in step S8, the specific operation of the extreme cooling control after forging is: water cooling once to the temperature of the large surface of the billet ≤ 250°C; then loading into a heat treatment furnace, heating to 960-990°C, keeping warm for 15-20 hours, furnace cooling to 730-750°C, keeping warm for 25-40 hours for complete annealing + isothermal annealing treatment.
[0033] Specifically, in step S9, the specific operation of the solid solution + spheroidizing initial treatment is: placing the workpiece obtained in step S8 into a heating furnace and heating it to 1030-1070°C with the furnace, keeping it warm, and then cooling it by direct water cooling; after cooling, placing the workpiece into an annealing furnace, heating it to 830-860°C, keeping it warm for 15-30h, furnace cooling it to 730-750°C, keeping it warm for 25-50h for spheroidizing annealing, and then furnace cooling it to below 350°C and air cooling it to room temperature.
[0034] Specifically, in step S10, the specific operation of the solution + spheroidizing final treatment is: placing the workpiece obtained in step S9 into a heating furnace and heating it to 1000-1020°C with the furnace, keeping it warm, and then cooling it by direct water cooling; after cooling, placing the workpiece into an annealing furnace, heating it to 830-860°C, keeping it warm for 15-30h, furnace cooling it to 690-740°C, keeping it warm for 25-50h for spheroidizing annealing, and then furnace cooling it to below 350°C and air cooling it to room temperature.
[0035] As the carbon content increases, the total amount of carbides in the material increases. First, the forged carbides are fully dissolved into the matrix through the first high-temperature solid solution temperature, and then the carbides are treated at a higher spheroidizing temperature so that the carbides can be evenly distributed in the ferrite matrix, preparing for the second solid solution + spheroidizing treatment.
[0036] The second solid solution at a lower temperature is to dissolve the Cr carbides that are easy to coarsen on the basis of the first solid solution, and at the same time, the grain boundaries retain enough V and Mo carbides to pin the austenite grain boundaries and inhibit the coarsening of austenite grains. At the same time, matching the lower secondary spheroidization temperature makes the precipitated carbides finer and more evenly distributed. Small and uniform carbides are easier to fully dissolve into the matrix during the vacuum heat treatment heating process of the mold, and the strengthening and toughening effect is better. At the same time, matching the fine austenite grains, the mold has good toughness. Matching with high carbon, a mold with high hardness, high wear resistance and high toughness is finally obtained.
[0037] Another object of the present invention is to provide a hot working die steel with high hardness, high wear resistance and high toughness, wherein the components are, by mass percentage, C 0.40% to 0.45%, Mn 0.30% to 0.50%, Si 0.20% to 0.50%, S≤0.001%, P≤0.008%, Cr 4.90% to 5.10%, Mo 2.30% to 2.60%, V 0.50% to 0.70%, and the rest is Fe, and the residual gas content is, H≤1.5ppm, O≤13ppm, N≤90ppm; the residual harmful elements Cu≤0.05%, Ti, Sn, and Pb are all ≤0.002%.
[0038] The method for preparing a hot working die steel with high hardness, high wear resistance and high toughness of the present invention has the following advantages compared with the prior art:
[0039] (1) The composition design concept of high C, low Si, and high Mo is used to design the composition, laying the foundation for achieving high hardness, high wear resistance, and high toughness of the mold;
[0040] (2) Blast furnace iron is used in the electric furnace smelting batch, which improves the initial purity of the raw materials;
[0041] (3) The use of integrated vacuum degassing equipment is more effective in degassing and removing inclusions than VD;
[0042] (4) The use of continuous casting billet electrodes has better uniformity of head and tail composition than die-cast electrodes;
[0043] (5) The use of full annealing + isothermal annealing treatment process can eliminate tissue inheritance better than conventional post-forging stress relief annealing;
[0044] (6) The microstructure control and austenite grain refinement effects of the double ultrafine treatment are better than those of the conventional single ultrafine treatment. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 This is a photo of the austenite grain size of the hot working die steel obtained in Example 1;
[0046] Figure 2 This is a crystal phase photo of the hot working die steel obtained in Example 1;
[0047] Figure 3 This is a photo of the austenite grain size of the hot working die steel obtained in Example 2;
[0048] Figure 4 This is a crystal phase photograph of the hot working die steel obtained in Example 2;
[0049] Figure 5 This is a photo of the austenite grain size of the hot working die steel obtained in Example 3;
[0050] Figure 6 This is a crystal phase photograph of the hot working die steel obtained in Example 3;
[0051] Figure 7 This is a photo of the austenite grain size of the hot working die steel obtained in Example 4;
[0052] Figure 8 This is a crystal phase photograph of the hot working die steel obtained in Example 4;
[0053] Fig. 9 This is a photo of the austenite grain size of the hot working die steel obtained in Example 5;
[0054] Fig.10 This is a crystal phase photograph of the hot working die steel obtained in Example 5. DETAILED DESCRIPTION
[0055] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments.
[0056] Example 1
[0057] A hot working die steel, which is basically composed of the elements shown in Table 1 according to mass fraction:
[0058] Table 1
[0059]
[0060]
[0061] The preparation method thereof mainly comprises the following steps:
[0062] S1. Electric furnace smelting:
[0063] According to the component content of hot working die steel, blast furnace molten iron (ratio ≥ 60%), shear charge and bulk surplus steel are prepared, CaO, CaF2, aluminum block and dolomite are added, and the steel is melted and smelted in an electric furnace; the molten steel temperature is 1640°C for oxidation and slagging, and alloy material, lime and fluorite are added after slagging to adjust the chemical composition and dephosphorize. The tapping temperature is 1630°C, and aluminum wire is added during the tapping process. The aluminum wire is added at 1.0 kg / t for deoxidation.
[0064] S2, ladle refining furnace refining:
[0065] After smelting in the electric furnace, the molten steel is transferred into the ladle, hoisted to the refining furnace seat, and slag materials CaO, CaF2, and C-Si powder are added to reduce and make white slag. According to the actual composition, alloy materials are added to complete the composition fine-tuning, desulfurization, and deoxidation operations; after the operation is completed, the white slag is removed, and then reheated and new slag is added for secondary white slag making to further remove inclusions in the steel; in the process of secondary white slag making, aluminum wire and calcium wire are added for composite deoxidation; the amount of aluminum wire and calcium wire is added according to 1.0kg / t.
[0066] S3, RH vacuum refining furnace refining:
[0067] The integrated RH vacuum tank is equipped with an advanced vacuum pump and has a vacuum degree of 12Pa. Under vacuum conditions, the circulation flow rate is 120t / min and the processing time is 37 minutes. After the vacuum degassing is completed, the residual gas H is ≤1.0ppm and N is ≤80ppm. Samples are taken for analysis. After the components are qualified, argon is blown into the hanging bag. The soft blowing time of argon is 25min and the hanging bag temperature is 1560℃.
[0068] S4, continuous casting electrode billet:
[0069] The superheat of the first furnace is 30℃, and that of the continuous casting furnace is 25℃; the continuous casting speed is 0.16m / min, and three-stage electromagnetic stirring is adopted.
[0070] S5. Electrode blank annealing:
[0071] The electrode blank after continuous casting in step S4 is annealed at a temperature of 850°C and a holding time of 1.5 min / mm, and the furnace is cooled to 340°C before being taken out of the furnace;
[0072] S6, electroslag remelting:
[0073] The electrode blank obtained in step S5 is surface polished and smelted using a binary slag system of calcium fluoride and alumina. The starting melting rate value in the steady-state stage of electroslag smelting is 8.5 kg / min and the end melting rate value is 6.0 kg / min. An electroslag ingot is obtained, and then the furnace is shut down for cooling for 90 minutes before being sent to a forging process.
[0074] S7, Forging:
[0075] The electroslag ingot obtained in step S6 is heated to 1280°C and kept at this temperature for 25 hours for diffusion homogenization, and then forged into a rectangular flat billet by roughing and drawing, and then the intermediate billet is heated to 1280°C again and kept at this temperature for 25 hours for diffusion homogenization. Multi-directional upsetting and drawing in the three directions of X, Y and Z are performed to the finished product size;
[0076] S8, post-forging pretreatment
[0077] The forging blank obtained in step S7 is subjected to extreme cooling control after forging to inhibit the precipitation of carbides at the grain boundaries: water-cooling is performed once to a large surface temperature of 240°C; then the blank is loaded into a heat treatment furnace, heated to 980°C, kept warm for 20 hours, furnace-cooled to 740°C, kept warm for 35 hours for complete annealing + isothermal annealing treatment.
[0078] S9, solution + spheroidizing initial treatment:
[0079] The workpiece obtained in step S8 is placed in a heating furnace and heated to 1040°C. After keeping the temperature, the workpiece is cooled by direct water cooling. After cooling, the workpiece is placed in an annealing furnace, heated to 860°C, kept at the temperature for 25 hours, cooled to 740°C in the furnace, kept at the temperature for 40 hours for spheroidizing annealing, and then cooled to 300°C in the furnace and air-cooled to room temperature.
[0080] S10, solution + spheroidizing final treatment:
[0081] The workpiece obtained in step S9 is placed in a heating furnace and heated to 1010°C. After keeping the temperature, it is cooled by direct water cooling. After cooling, the workpiece is placed in an annealing furnace, heated to 850°C, kept at this temperature for 25 hours, furnace cooled to 710°C, kept at this temperature for 40 hours for spheroidizing annealing, and then furnace cooled to 300°C and air cooled to room temperature.
[0082] Example 2
[0083] A hot working die steel, which is basically composed of the elements shown in Table 2 according to mass fraction:
[0084] Table 2
[0085]
[0086] The preparation method thereof mainly comprises the following steps:
[0087] S1. Electric furnace smelting:
[0088] According to the component content of hot working die steel, blast furnace molten iron (ratio ≥ 60%), shear charge and bulk surplus steel are prepared, CaO, CaF2, aluminum block and dolomite are added, and the steel is melted and smelted in an electric furnace; the molten steel temperature is 1640°C for oxidation and slagging, and alloy material, lime and fluorite are added after slagging to adjust the chemical composition and dephosphorize. The tapping temperature is 1630°C, and aluminum wire is added during the tapping process. The aluminum wire is added at 1.0 kg / t for deoxidation.
[0089] S2, ladle refining furnace refining:
[0090] After smelting in the electric furnace, the molten steel is transferred into the ladle, hoisted to the refining furnace seat, and slag materials CaO, CaF2, and C-Si powder are added to reduce and make white slag. According to the actual composition, alloy materials are added to complete the composition fine-tuning, desulfurization, and deoxidation operations; after the operation is completed, the white slag is removed, and then reheated and new slag is added for secondary white slag making to further remove inclusions in the steel; in the process of secondary white slag making, aluminum wire and calcium wire are added for composite deoxidation; the amount of aluminum wire and calcium wire is added according to 1.0kg / t.
[0091] S3, vacuum refining furnace refining:
[0092] The integrated vacuum tank is equipped with an advanced vacuum pump, and the vacuum degree is 12Pa. Under vacuum conditions, the circulation flow is 120t / min, and the processing time is 37 minutes. After the vacuum degassing is completed, the residual gas H is ≤1.0ppm, and N is ≤80ppm. Samples are taken for analysis. After the components are qualified, argon is blown into the hanging bag. The soft blowing time of argon is 25min, and the hanging bag temperature is 1560℃.
[0093] S4, continuous casting electrode billet:
[0094] The superheat of the first furnace is 30℃, and that of the continuous casting furnace is 25℃; the continuous casting speed is 0.16m / min, and three-stage electromagnetic stirring is adopted.
[0095] S5. Electrode blank annealing:
[0096] The electrode blank after continuous casting in step S4 is annealed at a temperature of 850°C and a holding time of 1.5 min / mm, and the furnace is cooled to 340°C before being taken out of the furnace;
[0097] S6, electroslag remelting:
[0098] The electrode blank obtained in step S5 is surface polished and smelted using a binary slag system of calcium fluoride and alumina. The starting melting rate value in the steady-state stage of electroslag smelting is 8.5 kg / min and the end melting rate value is 6.0 kg / min. An electroslag ingot is obtained, and then the furnace is shut down for cooling for 90 minutes before being sent to a forging process.
[0099] S7, Forging:
[0100] The electroslag ingot obtained in step S6 is heated to 1280°C and kept at this temperature for 25 hours for diffusion homogenization, and then forged into a rectangular flat billet by roughing and drawing, and then the intermediate billet is heated to 1280°C again and kept at this temperature for 25 hours for diffusion homogenization. Multi-directional upsetting and drawing in the three directions of X, Y and Z are performed to the finished product size;
[0101] S8, post-forging pretreatment
[0102] The forging blank obtained in step S7 is subjected to extreme cooling control after forging to inhibit the precipitation of carbides at the grain boundaries: water-cooling is performed once to a large surface temperature of 240°C; then the blank is loaded into a heat treatment furnace, heated to 980°C, kept warm for 20 hours, furnace-cooled to 740°C, kept warm for 35 hours for complete annealing + isothermal annealing treatment.
[0103] S9, solution + spheroidizing initial treatment:
[0104] The workpiece obtained in step S8 is placed in a heating furnace and heated to 1040°C. After keeping the temperature, the workpiece is cooled by direct water cooling. After cooling, the workpiece is placed in an annealing furnace, heated to 860°C, kept at the temperature for 25 hours, cooled to 740°C in the furnace, kept at the temperature for 40 hours for spheroidizing annealing, and then cooled to 300°C in the furnace and air-cooled to room temperature.
[0105] S10, solution + spheroidizing final treatment:
[0106] The workpiece obtained in step S9 is placed in a heating furnace and heated to 1010°C. After keeping the temperature, it is cooled by direct water cooling. After cooling, the workpiece is placed in an annealing furnace, heated to 850°C, kept at this temperature for 25 hours, furnace cooled to 710°C, kept at this temperature for 40 hours for spheroidizing annealing, and then furnace cooled to 300°C and air cooled to room temperature.
[0107] Example 3
[0108] A hot working die steel, which is basically composed of the elements shown in Table 3 according to mass fraction:
[0109] Table 3
[0110]
[0111] The preparation method thereof mainly comprises the following steps:
[0112] S1. Electric furnace smelting:
[0113] According to the component content of hot working die steel, blast furnace molten iron (ratio ≥ 60%), shear charge and bulk surplus steel are prepared, CaO, CaF2, aluminum block and dolomite are added, and the steel is melted and smelted in an electric furnace; the molten steel temperature is 1640°C for oxidation and slagging, and alloy material, lime and fluorite are added after slagging to adjust the chemical composition and dephosphorize. The tapping temperature is 1630°C, and aluminum wire is added during the tapping process. The aluminum wire is added at 1.0 kg / t for deoxidation.
[0114] S2, ladle refining furnace refining:
[0115] After smelting in the electric furnace, the molten steel is transferred into the ladle, hoisted to the refining furnace seat, and slag materials CaO, CaF2, and C-Si powder are added to reduce and make white slag. According to the actual composition, alloy materials are added to complete the composition fine-tuning, desulfurization, and deoxidation operations; after the operation is completed, the white slag is removed, and then reheated and new slag is added for secondary white slag making to further remove inclusions in the steel; in the process of secondary white slag making, aluminum wire and calcium wire are added for composite deoxidation; the amount of aluminum wire and calcium wire is added according to 1.0kg / t.
[0116] S3, vacuum refining furnace refining:
[0117] The integrated vacuum tank is equipped with an advanced vacuum pump, and the vacuum degree is 12Pa. Under vacuum conditions, the circulation flow is 120t / min, and the processing time is 37 minutes. After the vacuum degassing is completed, the residual gas H is ≤1.0ppm, and N is ≤80ppm. Samples are taken for analysis. After the components are qualified, argon is blown into the hanging bag. The soft blowing time of argon is 25min, and the hanging bag temperature is 1560℃.
[0118] S4, continuous casting electrode billet:
[0119] The superheat of the first furnace is 30℃, and that of the continuous casting furnace is 25℃; the continuous casting speed is 0.16m / min, and three-stage electromagnetic stirring is adopted.
[0120] S5. Electrode blank annealing:
[0121] The electrode blank after continuous casting in step S4 is annealed at a temperature of 850°C and a holding time of 1.5 min / mm, and the furnace is cooled to 340°C before being taken out of the furnace;
[0122] S6, electroslag remelting:
[0123] The electrode blank obtained in step S5 is surface polished and smelted using a binary slag system of calcium fluoride and alumina. The starting melting rate value in the steady-state stage of electroslag smelting is 8.5 kg / min and the end melting rate value is 6.0 kg / min. An electroslag ingot is obtained, and then the furnace is shut down for cooling for 90 minutes before being sent to a forging process.
[0124] S7, Forging:
[0125] The electroslag ingot obtained in step S6 is heated to 1280°C and kept at this temperature for 25 hours for diffusion homogenization, and then forged into a rectangular flat billet by roughing and drawing, and then the intermediate billet is heated to 1280°C again and kept at this temperature for 25 hours for diffusion homogenization. Multi-directional upsetting and drawing in the three directions of X, Y and Z are performed to the finished product size;
[0126] S8, post-forging pretreatment
[0127] The forging blank obtained in step S7 is subjected to extreme cooling control after forging to inhibit the precipitation of carbides at the grain boundaries: water-cooling is performed once to a large surface temperature of 240°C; then the blank is loaded into a heat treatment furnace, heated to 980°C, kept warm for 20 hours, furnace-cooled to 740°C, kept warm for 35 hours for complete annealing + isothermal annealing treatment.
[0128] S9, solution + spheroidizing initial treatment:
[0129] The workpiece obtained in step S8 is placed in a heating furnace and heated to 1040°C. After keeping the temperature, the workpiece is cooled by direct water cooling. After cooling, the workpiece is placed in an annealing furnace, heated to 860°C, kept at the temperature for 25 hours, cooled to 740°C in the furnace, kept at the temperature for 40 hours for spheroidizing annealing, and then cooled to 300°C in the furnace and air-cooled to room temperature.
[0130] S10, solution + spheroidizing final treatment:
[0131] The workpiece obtained in step S9 is placed in a heating furnace and heated to 1010°C. After keeping the temperature, it is cooled by direct water cooling. After cooling, the workpiece is placed in an annealing furnace, heated to 850°C, kept at this temperature for 25 hours, furnace cooled to 710°C, kept at this temperature for 40 hours for spheroidizing annealing, and then furnace cooled to 300°C and air cooled to room temperature.
[0132] Example 4
[0133] A hot working die steel, which is basically composed of the elements shown in Table 4 according to mass fraction:
[0134] Table 4
[0135]
[0136] The preparation method thereof mainly comprises the following steps:
[0137] S1. Electric furnace smelting:
[0138] According to the component content of hot working die steel, blast furnace molten iron (ratio ≥ 60%), shear charge and bulk surplus steel are prepared, CaO, CaF2, aluminum block and dolomite are added, and the steel is melted and smelted in an electric furnace; the molten steel temperature is 1640°C for oxidation and slagging, and alloy material, lime and fluorite are added after slagging to adjust the chemical composition and dephosphorize. The tapping temperature is 1630°C, and aluminum wire is added during the tapping process. The aluminum wire is added at 1.0 kg / t for deoxidation.
[0139] S2, ladle refining furnace refining:
[0140] After smelting in the electric furnace, the molten steel is transferred into the ladle, hoisted to the refining furnace seat, and slag materials CaO, CaF2, and C-Si powder are added to reduce and make white slag. According to the actual composition, alloy materials are added to complete the composition fine-tuning, desulfurization, and deoxidation operations; after the operation is completed, the white slag is removed, and then reheated and new slag is added for secondary white slag making to further remove inclusions in the steel; in the process of secondary white slag making, aluminum wire and calcium wire are added for composite deoxidation; the amount of aluminum wire and calcium wire is added according to 1.0kg / t.
[0141] S3, vacuum refining furnace refining:
[0142] The integrated vacuum tank is equipped with an advanced vacuum pump, and the vacuum degree is 12Pa. Under vacuum conditions, the circulation flow is 120t / min, and the processing time is 37 minutes. After the vacuum degassing is completed, the residual gas H is ≤1.0ppm, and N is ≤80ppm. Samples are taken for analysis. After the components are qualified, argon is blown into the hanging bag. The soft blowing time of argon is 25min, and the hanging bag temperature is 1560℃.
[0143] S4, continuous casting electrode billet:
[0144] The superheat of the first furnace is 30℃, and that of the continuous casting furnace is 25℃; the continuous casting speed is 0.16m / min, and three-stage electromagnetic stirring is adopted.
[0145] S5. Electrode blank annealing:
[0146] The electrode blank after continuous casting in step S4 is annealed at a temperature of 850°C and a holding time of 1.5 min / mm, and the furnace is cooled to 340°C before being taken out of the furnace;
[0147] S6, electroslag remelting:
[0148] The electrode blank obtained in step S5 is surface polished and smelted using a binary slag system of calcium fluoride and alumina. The starting melting rate value in the steady-state stage of electroslag smelting is 8.5 kg / min and the end melting rate value is 6.0 kg / min. An electroslag ingot is obtained, and then the furnace is shut down for cooling for 90 minutes before being sent to a forging process.
[0149] S7, Forging:
[0150] The electroslag ingot obtained in step S6 is heated to 1280°C and kept at this temperature for 25 hours for diffusion homogenization, and then forged into a rectangular flat billet by roughing and drawing, and then the intermediate billet is heated to 1280°C again and kept at this temperature for 25 hours for diffusion homogenization. Multi-directional upsetting and drawing in the three directions of X, Y and Z are performed to the finished product size;
[0151] S8, post-forging pretreatment
[0152] The forging blank obtained in step S7 is subjected to extreme cooling control after forging to inhibit the precipitation of carbides at the grain boundaries: water-cooling is performed once to a large surface temperature of 240°C; then the blank is loaded into a heat treatment furnace, heated to 980°C, kept warm for 20 hours, furnace-cooled to 740°C, kept warm for 35 hours for complete annealing + isothermal annealing treatment.
[0153] S9, solution + spheroidizing initial treatment:
[0154] The workpiece obtained in step S8 is placed in a heating furnace and heated to 1040°C. After keeping the temperature, the workpiece is cooled by direct water cooling. After cooling, the workpiece is placed in an annealing furnace, heated to 860°C, kept at the temperature for 25 hours, cooled to 740°C in the furnace, kept at the temperature for 40 hours for spheroidizing annealing, and then cooled to 300°C in the furnace and air-cooled to room temperature.
[0155] S10, solution + spheroidizing final treatment:
[0156] The workpiece obtained in step S9 is placed in a heating furnace and heated to 1010°C. After keeping the temperature, it is cooled by direct water cooling. After cooling, the workpiece is placed in an annealing furnace, heated to 850°C, kept at this temperature for 25 hours, furnace cooled to 710°C, kept at this temperature for 40 hours for spheroidizing annealing, and then furnace cooled to 300°C and air cooled to room temperature.
[0157] Example 5
[0158] A hot working die steel, which is basically composed of the elements shown in Table 5 according to mass fraction:
[0159] Table 5
[0160]
[0161] The preparation method thereof mainly comprises the following steps:
[0162] S1. Electric furnace smelting:
[0163] According to the component content of hot working die steel, blast furnace molten iron (ratio ≥ 60%), shear charge and bulk surplus steel are prepared, CaO, CaF2, aluminum block and dolomite are added, and the steel is melted and smelted in an electric furnace; the molten steel temperature is 1640°C for oxidation and slagging, and alloy material, lime and fluorite are added after slagging to adjust the chemical composition and dephosphorize. The tapping temperature is 1630°C, and aluminum wire is added during the tapping process. The aluminum wire is added at 1.0 kg / t for deoxidation.
[0164] S2, ladle refining furnace refining:
[0165] After smelting in the electric furnace, the molten steel is transferred into the ladle, hoisted to the refining furnace seat, and slag materials CaO, CaF2, and C-Si powder are added to reduce and make white slag. According to the actual composition, alloy materials are added to complete the composition fine-tuning, desulfurization, and deoxidation operations; after the operation is completed, the white slag is removed, and then reheated and new slag is added for secondary white slag making to further remove inclusions in the steel; in the process of secondary white slag making, aluminum wire and calcium wire are added for composite deoxidation; the amount of aluminum wire and calcium wire is added according to 1.0kg / t.
[0166] S3, vacuum refining furnace refining:
[0167] The integrated vacuum tank is equipped with an advanced vacuum pump, and the vacuum degree is 12Pa. Under vacuum conditions, the circulation flow is 120t / min, and the processing time is 37 minutes. After the vacuum degassing is completed, the residual gas H is ≤1.0ppm, and N is ≤80ppm. Samples are taken for analysis. After the components are qualified, argon is blown into the hanging bag. The soft blowing time of argon is 25min, and the hanging bag temperature is 1560℃.
[0168] S4, continuous casting electrode billet:
[0169] The superheat of the first furnace is 30℃, and that of the continuous casting furnace is 25℃; the continuous casting speed is 0.16m / min, and three-stage electromagnetic stirring is adopted.
[0170] S5. Electrode blank annealing:
[0171] The electrode blank after continuous casting in step S4 is annealed at a temperature of 850°C and a holding time of 1.5 min / mm, and the furnace is cooled to 340°C before being taken out of the furnace;
[0172] S6, electroslag remelting:
[0173] The electrode blank obtained in step S5 is surface polished and smelted using a binary slag system of calcium fluoride and alumina. The starting melting rate value in the steady-state stage of electroslag smelting is 8.5 kg / min and the end melting rate value is 6.0 kg / min. An electroslag ingot is obtained, and then the furnace is shut down for cooling for 90 minutes before being sent to a forging process.
[0174] S7, Forging:
[0175] The electroslag ingot obtained in step S6 is heated to 1280°C and kept at this temperature for 25 hours for diffusion homogenization, and then forged into a rectangular flat billet by roughing and drawing, and then the intermediate billet is heated to 1280°C again and kept at this temperature for 25 hours for diffusion homogenization. Multi-directional upsetting and drawing in the three directions of X, Y and Z are performed to the finished product size;
[0176] S8, post-forging pretreatment
[0177] The forging blank obtained in step S7 is subjected to extreme cooling control after forging to inhibit the precipitation of carbides at the grain boundaries: water-cooling is performed once to a large surface temperature of 240°C; then the blank is loaded into a heat treatment furnace, heated to 980°C, kept warm for 20 hours, furnace-cooled to 740°C, kept warm for 35 hours for complete annealing + isothermal annealing treatment.
[0178] S9, solution + spheroidizing initial treatment:
[0179] The workpiece obtained in step S8 is placed in a heating furnace and heated to 1040°C. After keeping the temperature, the workpiece is cooled by direct water cooling. After cooling, the workpiece is placed in an annealing furnace, heated to 860°C, kept at the temperature for 25 hours, cooled to 740°C in the furnace, kept at the temperature for 40 hours for spheroidizing annealing, and then cooled to 300°C in the furnace and air-cooled to room temperature.
[0180] S10, solution + spheroidizing final treatment:
[0181] The workpiece obtained in step S9 is placed in a heating furnace and heated to 1010°C. After keeping the temperature, it is cooled by direct water cooling. After cooling, the workpiece is placed in an annealing furnace, heated to 850°C, kept at this temperature for 25 hours, furnace cooled to 710°C, kept at this temperature for 40 hours for spheroidizing annealing, and then furnace cooled to 300°C and air cooled to room temperature.
[0182] In order to verify the comprehensive performance of the hot working die steel provided by the preparation method of the present invention, the inventors took 5 samples of the hot working die steel blanks obtained in Examples 1 to 5 to test the ball destructure, unnotched impact toughness, and austenite grain size. The test data are shown in Table 6:
[0183] Table 6
[0184]
[0185] From Table 6 and Figures 1 to 10 visible:
[0186] 1. As Figures 1 to 10As shown in the figure, the microstructure of the mold material in the spheroidized annealed state is uniform, and the fine spheroidal secondary carbides are evenly distributed on the ferrite matrix. According to the NADCA#207-2011 standard, the grade is ≤AS5; the spheroidized structure is conducive to full dissolution during the austenitization process, reducing the number and size of undissolved carbides; and then dispersed and precipitated during the tempering process to achieve the purpose of improving impact toughness;
[0187] 2. Increasing the carbon content in the mold steel material composition can greatly improve the hardness and wear resistance of the mold material; at the same time, a reasonable preheat treatment process allows the alloy element carbides to be evenly distributed in the ferrite matrix, while obtaining fine austenite grains. In the subsequent mold steel quenching and tempering process, carbides of Mo, Cr, and V are dispersed and precipitated from the matrix. It is these fine precipitated phases that play a role in dispersion strengthening during use, while matching the fine austenite grains to improve the comprehensive performance of the material. The single unnotched lateral impact energy of the core of the mold material is ≥350J, and the average unnotched lateral impact performance is ≥370J;
[0188] 3. It can be concluded from the microstructure photographs taken in Examples 1 to 10 that there is no liquid precipitation carbide.
[0189] It can be seen that the hot working die steel prepared by the preparation method has high hardness, high strength, high wear resistance, high erosion resistance, high toughness and high crack resistance.
Claims
1. A method for preparing a hot working die steel with high hardness, high wear resistance and high toughness, characterized in that: The main steps are as follows: S1. Electric furnace smelting: According to the component content of hot working die steel, blast furnace molten iron, shearing charge and bulk surplus steel are prepared, CaO, CaF2, aluminum block and dolomite are added, and the steel is melted and smelted in an electric furnace; after slagging, CaO, cleaning agent and aluminum block are added before tapping, and the tapping temperature is ≥1620℃; Among them, the component contents of hot working die steel are, by mass percentage, C 0.40%-0.45%, Mn 0.30%-0.50%, Si 0.20%-0.50%, S≤0.001%, P≤0.008%, Cr 4.90%-5.10%, Mo 2.30%-2.60%, V 0.50%-0.70%, and the rest is Fe, and the residual gas content is, H≤1.5ppm, O≤13ppm, N≤90ppm; the residual harmful elements Cu≤0.05%, Ti, Sn, Pb are all ≤0.002%; S2, ladle refining furnace refining: The ladle refining furnace is heated, and slag CaO, CaF2, and C-Si powder are added to reduce and adjust the slag system; S3, vacuum refining furnace refining: The integrated vacuum tank is equipped with an advanced vacuum pump, and the vacuum degree is ≤15Pa. After degassing, sampling and analysis are performed. If the components are qualified, argon gas is softly blown into the hanging bag. S4, continuous casting electrode billet: The superheat of the first furnace is 20-35℃, and the continuous casting furnace is 18-30℃; the continuous casting speed is 0.13-0.20m / min, and three-stage electromagnetic stirring is adopted; S5. Electrode blank annealing: Annealing the electrode blank after continuous casting in step S4; S6, electroslag remelting: The electrode blank obtained in step S5 is surface-polished and smelted using a binary slag system of calcium fluoride and alumina to obtain an electroslag ingot; S7, Forging: The electroslag ingot obtained in step S6 is heated to 1260-1300° C., kept warm for 15-30 hours for diffusion homogenization, and then forged into a rectangular flat billet by roughing, drawing and forging. The intermediate billet is then heated to 1280° C. again, kept warm for 15-30 hours for diffusion homogenization, and then subjected to multi-directional upsetting and drawing in the three directions of X, Y and Z to the finished product size; S8, heat treatment after forging: The forging blank obtained in step S7 is subjected to post-forging extreme cooling control to inhibit the precipitation of grain boundary carbides; S9, solution + spheroidizing initial treatment: The forging blank after the post-forging heat treatment in step S8 is subjected to a solid solution + spheroidizing initial treatment; S10, solution + spheroidizing final treatment; The forging blank obtained in step S9 is subjected to a final treatment of solid solution + spheroidization.
2. The method for preparing a hot working die steel with high hardness, high wear resistance and high toughness according to claim 1, characterized in that: In step S1, the proportion of blast furnace molten iron is ≥ 60%.
3. The method for preparing a hot working die steel with high hardness, high wear resistance and high toughness according to claim 1, characterized in that: In step S3, under vacuum conditions, the circulation flow rate is ≥100t / min, the processing time is ≥35 minutes, and the residual gas H is ensured to be ≤1.5ppm, N ≤80ppm. After the vacuum degassing is completed, sampling and analysis are performed, and argon gas is blown into the hanging bag after the components are qualified.
4. The method for preparing a hot working die steel with high hardness, high wear resistance and high toughness according to claim 3, characterized in that: In step S3, the soft blowing time of argon is 18 to 39 minutes, and the bag temperature is 1550 to 1568°C.
5. The method for preparing a hot working die steel with high hardness, high wear resistance and high toughness according to claim 1, characterized in that: In step S5, the annealing temperature is 840-860°C, the holding time is 1-1.5 min / mm, and the furnace is cooled to below 350°C before being taken out of the furnace.
6. The method for preparing a hot working die steel with high hardness, high wear resistance and high toughness according to claim 1, characterized in that: In step S6, the starting melting rate value of the steady-state stage of electroslag smelting is 7-10 kg / min, and the end melting rate value is 5.0-8.0 kg / min, and then the furnace is shut down and cooled for 80-100 minutes before being sent to the forging process.
7. The method for preparing a hot working die steel with high hardness, high wear resistance and high toughness according to claim 1, characterized in that: In step S8, the specific operation of the extreme cooling control after forging is: water cooling once to the temperature of the large surface of the billet ≤ 250°C; then loading into a heat treatment furnace, heating to 960-990°C, keeping warm for 15-20 hours, furnace cooling to 730-750°C, keeping warm for 25-40 hours for complete annealing + isothermal annealing treatment.
8. The method for preparing a hot working die steel with high hardness, high wear resistance and high toughness according to claim 1, characterized in that: In step S9, the specific operation of the solution + spheroidizing initial treatment is: placing the workpiece obtained in step S8 into a heating furnace and heating it to 1030-1070°C with the furnace, keeping it warm, and then cooling it by direct water cooling; after cooling, placing the workpiece into an annealing furnace, heating it to 830-860°C, keeping it warm for 15-30h, cooling it in the furnace to 730-750°C, keeping it warm for 25-50h for spheroidizing annealing, and then cooling it in the furnace to below 350°C and air cooling it to room temperature.
9. The method for preparing a hot working die steel with high hardness, high wear resistance and high toughness according to claim 8, characterized in that: In step S10, the specific operation of the solution + spheroidizing final treatment is: placing the workpiece obtained in step S9 into a heating furnace and heating it to 1000-1020°C with the furnace, keeping it warm, and then cooling it by direct water cooling; after cooling, placing the workpiece into an annealing furnace, heating it to 830-860°C, keeping it warm for 15-30h, cooling it in the furnace to 690-740°C, keeping it warm for 25-50h for spheroidizing annealing, and then cooling it in the furnace to below 350°C and air cooling it to room temperature.
10. The hot working die steel prepared by the method for preparing hot working die steel with high hardness, high wear resistance and high toughness according to any one of claims 1 to 9, characterized in that: Its component contents are, by mass percentage, C 0.40%-0.45%, Mn 0.30%-0.50%, Si 0.20%-0.50%, S≤0.001%, P≤0.008%, Cr 4.90%-5.10%, Mo2.30%-2.60%, V 0.50%-0.70%, and the rest is Fe. The residual gas content is, H≤1.5ppm, O≤13ppm, N≤90ppm; the residual harmful elements Cu≤0.05%, Ti, Sn, and Pb are all ≤0.002%.
Citation Information
Cited By
Hot and cold working dual-purpose high-toughness die steel and preparation method thereof
CN116377309A