A method for preparing high-strength and high-toughness degradable melt-blown nonwoven material

Through premix and melt blending, high-strength and high-strength polylactic acid melt-blown nonwoven materials are prepared, which solves the problems of complex processes, high cost and insufficient degradability, and achieves fully degradable, high-strength and high-strength and high-strength and toughness Material preparation.

CN116219636BActive Publication Date: 2024-11-29DONGHUA UNIV

Patent Information

Application Number
CN202310099130.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-09
Publication Date
2024-11-29
Estimated Expiration
2043-02-09

AI Technical Summary

Technical Problem

The existing modified polylactic acid meltblown nonwoven fabrics have complex processes, long time, high cost, and often neglect the degradability of added materials, resulting in solvent volatility problems, making it difficult to achieve fully degradable, high strength and high toughness material preparation.

Method used

Polylactic acid slices and polybutylene succinate slices are used as raw materials to prepare high-strength and high-strength polylactic acid meltblown nonwoven materials through premix, melt blending, hot melt forming and other steps, and control the dispersed phase morphology structure to achieve Improved strength of the material.

Benefits of technology

It realizes a meltblown nonwoven polylactic acid with a simple preparation process, solvent-free volatile, fully degradable, high-strength and high-toughness polylactic acid meltblown nonwoven materials, reducing production costs and meeting the requirements of sustainable development.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004085903960000011
    Figure HDA0004085903960000011
  • Figure HDA0004085903960000012
    Figure HDA0004085903960000012
  • Figure HDA0004085903960000021
    Figure HDA0004085903960000021
Patent Text Reader

Abstract

The invention discloses a method for preparing a high-strength and high-toughness degradable melt-blown nonwoven material, comprising the following steps: S1, premixing: using polylactic acid slices and polybutylene succinate slices as raw materials, premixing under certain conditions to obtain polylactic acid / polybutylene succinate premixed slices; S2, melt blending: injecting the obtained polylactic acid / polybutylene succinate premixed slices into a twin-screw extruder for melting, and extruding into a thin stream of melt through a metering pump and a hanger-type die head; S3, hot melt molding: stretching and shearing the melt through a high-temperature and high-speed airflow to obtain fibers, and then collecting them through a receiving device through self-bonding into a web to obtain polylactic acid melt-blown nonwoven materials with different morphological structures. The preparation method of the invention only requires one blending, and no additional device is required to achieve the improvement of the strength and toughness of the polylactic acid melt-blown nonwoven material. In addition, the invention uses polylactic acid and polybutylene succinate as raw materials, which can achieve full degradability and meet the requirements of sustainable development.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of nonwoven fabrics, and particularly relates to a method for preparing a high-strength and high-toughness degradable melt-blown nonwoven material. Background Art

[0002] The meltblown nonwoven process uses high-speed hot air to stretch the polymer melt stream extruded from the die spinneret, thereby forming ultrafine fibers and condensing them on a condensing screen or roller, and relying on self-bonding to become a nonwoven fabric. The meltblown nonwoven material prepared by this process has the characteristics of large specific surface area, high porosity, and fluffy structure. It is widely used in filtration, warmth preservation, medical and health fields. However, most of the meltblown nonwoven materials are currently based on polypropylene raw materials, which are non-renewable resources and waste is not easy to degrade, which brings a burden to resources and the environment. With the continuous enhancement of people's ecological awareness and environmental awareness, degradable meltblown nonwoven materials have become a research hotspot.

[0003] Polylactic acid is a thermoplastic aliphatic polyester, which is recognized as the most promising biodegradable material to replace polypropylene. However, due to the high glass transition temperature and slow crystallization rate of polylactic acid, polylactic acid melt-blown nonwoven materials have the disadvantages of large brittleness and poor mechanical properties, making it difficult to mass-produce and apply. Therefore, researchers have made various modifications to polylactic acid materials, and the following related reports have been made in order to obtain polylactic acid melt-blown nonwoven fabrics with excellent performance.

[0004] A Chinese patent (publication number CN105088542B) discloses a high elongation modified polylactic acid SMS composite nonwoven material and a preparation method, and specifically discloses the following technical scheme: 5 to 30 parts of polyamide elastomer and 70 to 95 parts of polylactic acid by mass are used as raw materials, and a polylactic acid blended melt-blown nonwoven material is obtained by melt-blowing. The longitudinal strength of the obtained melt-blown nonwoven material is 40-150N / 5cm, and the longitudinal elongation at break is 60-130%. The material manufactured by this method has excellent toughness, but ignores the non-degradable characteristics of polyamide.

[0005] A Chinese patent (publication number CN113293517B) discloses a polylactic acid elastic ultrafine fiber nonwoven material and its preparation method and application, and specifically discloses the following technical scheme: 10 to 20 parts of polyethylene glycol, 10 to 20 parts of nanocellulose, 20 to 40 parts of bio-based elastomer and 60 to 70 parts of polylactic acid by mass are used as raw materials, and a polylactic acid blended melt-blown nonwoven material is obtained by melt-blowing. The longitudinal strength of the obtained melt-blown nonwoven material is 50-80N / 5cm, and the longitudinal elongation at break is 56-75%. The material manufactured by this method has high toughness, but the method is complex, time-consuming, and costly, and requires three blendings and an additional multi-stage hot stretching device.

[0006] The above-mentioned existing modified polylactic acid melt-blown nonwoven fabrics mainly focus on adding reinforcing and toughening materials at the same time, and improving the phase interface. Although the effects of reinforcing and toughening can be achieved, the process is complicated, time-consuming, and costly, and the degradability of the added materials is often ignored, resulting in solvent volatilization problems. Therefore, how to produce a fully degradable, high-strength and high-toughness polylactic acid melt-blown nonwoven material through a simple process has become an urgent problem to be solved in the industry.

[0007] The morphology of the dispersed phase in the blend has a great influence on the mechanical properties. The dispersed phase morphology of binary blends is mainly divided into single-phase continuous structure, two-phase staggered structure and two-phase continuous structure. Among them, the in-situ microfibril structure and the two-phase continuous structure in the single-phase continuous structure have become hot areas of polymer blending research. The in-situ microfibril structure refers to the structure in which the dispersed phase exists in the matrix in the form of microfibrils. The higher orientation of the microfibrils is conducive to the increase of mechanical strength; the two-phase continuous structure refers to the network structure in which the polymer system penetrates each other, which is conducive to the conduction of stress. However, there is no relevant research report on the strengthening and toughening modification of polylactic acid melt-blown nonwoven materials by controlling the morphological structure of the dispersed phase.

[0008] Polybutylene succinate (PBS) is a fully biodegradable polymer material with good biocompatibility and toughness. Summary of the invention

[0009] In view of the problems existing in the above-mentioned prior art, the present invention provides a method for preparing a polylactic acid melt-blown nonwoven material with simple preparation process, non-toxicity, harmlessness, full degradability, high strength and high toughness.

[0010] In order to achieve the above purpose, the present invention adopts the following technical solutions

[0011] A method for preparing a high-strength and high-toughness polylactic acid melt-blown nonwoven material comprises the following steps:

[0012] S1. Premixing: Using polylactic acid chips and polybutylene succinate chips as raw materials, premixing under certain conditions to prepare polylactic acid / polybutylene succinate premixed chips;

[0013] S2, melt blending: inject the prepared polylactic acid / polybutylene succinate premixed slices into a twin-screw extruder for melting, and extrude into a thin stream of melt through a metering pump and a hanger-type die head;

[0014] S3. Hot melt forming: The obtained thin stream melt is stretched and sheared by high-temperature and high-speed airflow to obtain fibers, which are then self-bonded into a web and collected by a receiving device to obtain a polylactic acid melt-blown nonwoven material.

[0015] Preferably, in step S1, the polylactic acid chips and polybutylene succinate chips need to be dried before premixing.

[0016] Preferably, the drying treatment condition is vacuum drying, the vacuum drying temperature is 40-100° C., and the vacuum drying time is 12-72 h.

[0017] Preferably, in step S1, the premixing temperature is room temperature, and the premixing time is 10-40 minutes.

[0018] Preferably, in step S2, the screw extruder is divided into four temperature zones, and the temperatures of the four temperature zones are: 170-200°C, 180-210°C, 190-230°C, and 220-250°C, respectively.

[0019] Preferably, in step S2, the temperature of the hanger-shaped die head is 230-260°C.

[0020] Preferably, in step S2, the melt extrusion rate of the combination of the twin-screw extruder and the hanger-type die head is 20-90 g / min;

[0021] Preferably, in step S3, the temperature of the high-temperature, high-speed airflow is 240-290° C.; the speed of the high-temperature, high-speed airflow is 100-300 m / s; and the receiving distance of the receiving device is 5-40 cm.

[0022] Preferably, in terms of mass fractions, the mass ratio of the polylactic acid slices to the polybutylene succinate slices is 20-95:5-80.

[0023] The second object of the present invention is to provide a high-strength and high-toughness polylactic acid melt-blown nonwoven material obtained by the above-mentioned preparation method, wherein the high-strength and high-toughness polylactic acid melt-blown nonwoven material is any one of an in-situ microfiber structure, a two-phase continuous structure or an island structure.

[0024] Preferably, the high-strength and high-toughness polylactic acid melt-blown nonwoven material has an average diameter of 3-15 μm.

[0025] The third object of the present invention is to provide the application of the high-strength and high-toughness polylactic acid melt-blown nonwoven material in the field of protection.

[0026] The present invention has the following beneficial effects:

[0027] (1) The present invention aims to utilize the stress characteristics of different stages of the melt-blowing process and the high cooling rate of the melt-blowing process to construct different dispersed phase morphological structures to strengthen and toughen polylactic acid melt-blown nonwoven materials. By using polylactic acid chips and polybutylene succinate chips as raw materials, and sequentially undergoing premixing, melt extrusion, high-temperature and high-speed airflow stretching and shearing, and self-bonding web-forming processes, while controlling the ratio of the matrix material and the reinforcing material and the temperature and rate of the high-temperature and high-speed airflow, a high-strength and high-toughness polylactic acid melt-blown nonwoven material is obtained. Specifically, the shear force inside the screw is first utilized to disperse PBS in the form of spherical droplets in PLA, and then, through die extrusion and hot air flow under specific conditions, the PBS spherical droplets are evolved into specific structures of different forms (such as in-situ microfiber structure, two-phase continuous structure, and island structure) in the PLA matrix. The preparation method of the present invention only requires one blending, and no additional device is required to achieve the improvement of the strength and toughness of the polylactic acid melt-blown nonwoven material.

[0028] (2) The preparation method of the present invention does not have the problem of solvent volatilization, that is, there is no pollution problem in the preparation process; in addition, the present invention uses polylactic acid and polybutylene succinate as raw materials, which can be fully degradable, and the final products are carbon dioxide and water, which meets the requirements of sustainable development. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0030] Figure 1 Schematic diagram of the structure of the meltblown nonwoven device used in Example 1 of the present invention;

[0031] Figure 2 Schematic diagram of the formation of different structures of polylactic acid blended melt-blown fibers;

[0032] Figure 3 This is a SEM image of the cross-sectional morphology of the polylactic acid blended melt-blown fiber prepared in Example 1-3; wherein, Figure 3 a is a SEM image of the melt-blown fiber prepared in Example 1 parallel to the fiber direction;

[0033] Figure 3 b is a SEM image of the melt-blown fiber prepared in Example 2 parallel to the fiber direction; Figure 3 c is a SEM image of the melt-blown fiber prepared in Example 3 parallel to the fiber direction; Figure 3 d is a SEM image perpendicular to the fiber direction of the melt-blown fiber obtained in Example 1; Figure 3e is a SEM image perpendicular to the fiber direction of the melt-blown fiber obtained in Example 2; Figure 3 f is a SEM image of the meltblown fiber prepared in Example 3, perpendicular to the fiber direction. DETAILED DESCRIPTION

[0034] In the following description, specific details such as specific system structures, technologies, etc. are provided for the purpose of illustration rather than limitation, so as to provide a thorough understanding of the embodiments of the present invention. However, it should be clear to those skilled in the art that the present invention may be implemented in other embodiments without these specific details. In other cases, detailed descriptions of well-known systems, devices, circuits, and methods are omitted to prevent unnecessary details from obstructing the description of the present invention.

[0035] Example 1

[0036] refer to Figure 1 , a method for preparing a high-strength and high-toughness polylactic acid melt-blown nonwoven material comprises the following steps:

[0037] S1. Dry polylactic acid slices with a weight average molecular weight of 70,000 and polybutylene succinate slices with a weight average molecular weight of 65,000 at 50° C. under vacuum conditions for 24 h, then weigh 8 kg of the dried polylactic acid slices and 2 kg of the polybutylene succinate slices and premix them in a high-speed mixer for 20 min;

[0038] S2, inject the premixed slices into a twin-screw extruder for melting, and extrude them into melt streams through a metering pump and a hanger-type die head. The temperatures of the four temperature zones of the twin-screw extruder are 170°C, 190°C, 215°C, and 250°C, respectively, the temperature of the hanger-type die head is 250°C, and the extrusion rate is 40g / min;

[0039] S3. The extruded melt stream is placed under a high-temperature, high-speed airflow at a temperature of 260°C and a speed of 150 m / s to form fibers, and the fibers are self-bonded into a web by the residual heat of the fiber cortex on a receiving device with a receiving distance of 10 cm to obtain a polylactic acid melt-blown nonwoven material.

[0040] See the production process flow chart of high-strength and high-toughness polylactic acid meltblown nonwoven materials Figure 1 , Figure 1 The meanings of the marks are as follows: 1. Feed inlet; 2. Motor; 3. Twin-screw extruder; 4. Filter; 5. Metering pump; 6. Hanger-type die head; 7. Spinneret hole; 8. Gas hole; 9. Receiving device.

[0041] The morphology of the (polylactic acid) meltblown (nonwoven material) fibers obtained in this embodiment parallel to the fiber direction and perpendicular to the fiber direction was observed by SEM. The results are as follows: Figure 3 a and Figure 3 d. Figure 3 a and Figure 3 d The results show that the (polylactic acid) meltblown (nonwoven material) fibers prepared in the embodiment present an in-situ microfiber structure (see Figure 2 ), that is, polybutylene succinate exists in the polylactic acid matrix in the form of microfibers. According to the standard GB / T3923.1-2013, the longitudinal strength of the nonwoven material is 65N / 5cm, and the elongation at break is 24.62%.

[0042] Example 2

[0043] The preparation method of high-strength and high-toughness polylactic acid melt-blown nonwoven material comprises the following steps:

[0044] S1. Dry polylactic acid slices with a weight average molecular weight of 70,000 and polybutylene succinate slices with a weight average molecular weight of 65,000 at 50° C. under vacuum conditions for 24 hours, then weigh 5 kg of the dried polylactic acid slices and 5 kg of the polybutylene succinate slices and place them in a high-speed mixer for premixing for 20 minutes;

[0045] S2, the premixed slices are injected into a twin-screw extruder for melting, and extruded into a melt stream through a metering pump and a hanger-type die head. The temperatures of the four temperature zones of the twin-screw extruder are 170°C, 190°C, 215°C, and 250°C, respectively, the temperature of the hanger-type die head is 260°C, and the extrusion rate is 50g / min;

[0046] S3. The extruded melt stream is placed under an air flow at a temperature of 280° C. and a speed of 220 m / s to form fibers, and the fibers are self-bonded into a web by the residual heat of the fiber cortex on a receiving device with a receiving distance of 10 cm to obtain a polylactic acid melt-blown nonwoven material.

[0047] The morphology of the obtained (polylactic acid) meltblown (nonwoven material) fibers parallel to the fiber direction and perpendicular to the fiber direction was observed by SEM. The results are as follows: Figure 3 b and Figure 3 As shown in e. Figure 3 b and Figure 3 As a result, the (polylactic acid) meltblown (nonwoven material) fibers obtained in this embodiment have a two-phase continuous structure (see Figure 2 ), that is, polybutylene succinate and polylactic acid interpenetrate each other to form a network structure. According to the standard GB / T 3923.1-2013, the longitudinal strength of the nonwoven material is 53N / 5cm, and the elongation at break is 40.54%.

[0048] Example 3

[0049] The preparation method of high-strength and high-toughness polylactic acid melt-blown nonwoven material comprises the following steps:

[0050] S1, taking a polylactic acid slice with a weight average molecular weight of 70,000 and a polybutylene succinate slice with a weight average molecular weight of 65,000 and drying them under vacuum conditions at a drying temperature of 50° C. for 24 hours;

[0051] S2, take 4kg of the dried polylactic acid slices and 6kg of polybutylene succinate slices and premix them in a high-speed mixer for 20min;

[0052] S3, the premixed slices are injected into a twin-screw extruder for melting, and extruded into a melt stream through a metering pump and a hanger-type melt-blown die head. The temperatures of the four temperature zones of the extruder are 170°C, 190°C, 215°C, and 250°C, respectively, the temperature of the hanger-type die head is 250°C, and the extrusion rate is 60g / min;

[0053] S4. The extruded melt stream is placed under an air flow at a temperature of 270°C and a speed of 180 m / s to form fibers, and the fibers are self-bonded into a web by the residual heat of the fiber cortex on a receiving device with a receiving distance of 10 cm to obtain a polylactic acid melt-blown nonwoven material.

[0054] The morphology of the obtained (polylactic acid) meltblown (nonwoven material) fibers parallel to the fiber direction and perpendicular to the fiber direction was observed by SEM. The results are as follows: Figure 3 c and Figure 3 f. Figure 3 c and Figure 3 As can be seen from the results, the (polylactic acid) meltblown (nonwoven material) fibers obtained in this embodiment have an island-in-the-sea structure (see Figure 2 ), that is, polylactic acid exists in the form of spherical droplets in the polybutylene succinate matrix. According to the standard GB / T 3923.1-2013, the longitudinal strength of the nonwoven material is 21N / 5cm, and the elongation at break is 4.49%.

[0055] Comparative Example 1

[0056] The steps are basically the same as those in Example 1, except that the content of polylactic acid chips is 2 kg, and the content of polybutylene succinate chips is 8.5 kg.

[0057] Experimental results: It is difficult to form continuous fibers and spinning is impossible; further increasing the temperature of the die head and the airflow to 265°C and 285°C respectively, the polylactic acid blended melt-blown nonwoven material obtained on the receiving device with a receiving distance of 10 cm has many material points caused by insufficiently drawn fibers.

[0058] According to the standard GB / T 3923.1-2013, the longitudinal strength of the obtained nonwoven material is 5N / 5cm, and the elongation at break is 1.01%. The comparative results show that when the proportion of polybutylene succinate is large, it is difficult to melt extrude in the spinning temperature range of pure polylactic acid melt-blown nonwoven material, and the spinnability is poor.

[0059] Comparative Example 2

[0060] The steps are basically the same as those in Example 2, except that the air flow velocity is 300 m / s.

[0061] Experimental results: Meltblown nonwoven materials have almost no strength.

[0062] The comparative example results show that when the air flow velocity is too high, long fibers cannot be formed and the spinnability is poor.

[0063] Comparative Example 3

[0064] The steps are basically the same as those in Example 3, except that the temperature of the air flow is 235°C.

[0065] Experimental results: The fibers are coarse and the yarns are seriously paralleled, making the meltblown nonwoven material feel harder.

[0066] The comparative example results show that when the air flow temperature is too low, the polymer cannot be sufficiently stretched and the resulting melt-blown nonwoven material has poor skin affinity.

[0067] Comparative Example 4

[0068] S1, drying polylactic acid slices with a weight average molecular weight of 70,000 at 50° C. under vacuum conditions for 24 hours;

[0069] S2, weigh 10 kg of dried polylactic acid slices, inject them into a twin-screw extruder for melting, and extrude them into melt streams through a metering pump and a hanger-type die head. The temperatures of the four temperature zones of the extruder are 170°C, 190°C, 215°C, and 250°C, respectively, the temperature of the hanger-type die head is 250°C, and the extrusion rate is 50g / min;

[0070] S3. The extruded melt stream is formed into fibers under the action of an air flow at a temperature of 270° C. and a speed of 150 m / s, and is self-bonded into a web by the residual heat of the fiber cortex on a receiving device with a receiving distance of 10 cm to obtain a polylactic acid melt-blown nonwoven material.

[0071] According to the standard GB / T 3923.1-2013, the longitudinal strength of the nonwoven material is 14N / 5cm, and the elongation at break is 1.28%. Comparative Example 4 shows that the strength and toughness of pure polylactic acid meltblown nonwoven material are relatively poor.

[0072] The present invention is not limited to the above-mentioned specific implementation modes. Various changes made by ordinary technicians in this field based on the above-mentioned concepts without creative work are all within the protection scope of the present invention.

Claims

1. A method for preparing a high-strength and high-toughness degradable melt-blown nonwoven material, characterized in that: The following steps are involved: S1. Premixing: Using polylactic acid chips and polybutylene succinate chips as raw materials, premixing under certain conditions to prepare polylactic acid / polybutylene succinate premixed chips; S2, melt blending: inject the prepared polylactic acid / polybutylene succinate premixed slices into a twin-screw extruder for melting, and extrude into a thin stream of melt through a metering pump and a hanger-type die head; S3, hot melt forming: the obtained thin stream melt is stretched and sheared by high temperature and high speed airflow to obtain fibers, which are then self-bonded into a web and collected by a receiving device to obtain a polylactic acid melt-blown nonwoven material; In step S2, the screw extruder is divided into four temperature zones, and the temperatures of the four temperature zones are: 170-200°C, 180-210°C, 190-230°C, and 220-250°C; The temperature of the coat-hanger die is 230-260°C; the melt extrusion rate of the combined device of the twin-screw extruder and the coat-hanger die is 20-90g / min; In step S3, the temperature of the high-temperature, high-speed airflow is 240-290° C., the speed of the high-temperature, high-speed airflow is 100-300 m / s, and the receiving distance of the receiving device is 5-40 cm; Calculated by weight, the weight ratio of the polylactic acid slice to the polybutylene succinate slice is 20-95:5-80.

2. The method for preparing a high-strength and high-toughness degradable melt-blown nonwoven material according to claim 1, characterized in that: In step S1, the polylactic acid slices and polybutylene succinate slices need to be dried before premixing.

3. The method for preparing a high-strength and high-toughness degradable melt-blown nonwoven material according to claim 2, characterized in that: The drying treatment condition is vacuum drying, the vacuum drying temperature is 40-100° C., and the vacuum drying time is 12-72 hours.

4. The method for preparing a high-strength and high-toughness degradable melt-blown nonwoven material according to claim 1, characterized in that: In step S1, the premixing temperature is room temperature, and the premixing time is 10-40 minutes.

5. A high-strength and high-toughness polylactic acid melt-blown nonwoven material prepared by the preparation method according to any one of claims 1 to 4, characterized in that: The high-strength and high-toughness polylactic acid melt-blown nonwoven material is any one of an in-situ microfiber structure, a two-phase continuous structure or an island structure, and the average diameter of the high-strength and high-toughness polylactic acid melt-blown nonwoven material is 3-15 μm.

6. Application of the high-strength and high-toughness polylactic acid melt-blown nonwoven material as claimed in claim 5 in the field of protection.

Citation Information

Patent Citations

  • A kind of high elongation modified polylactic acid sms composite nonwoven material and preparation method

    CN105088542B

  • A polylactic acid elastic microfiber nonwoven material, its preparation method and application

    CN113293517B

  • Biodegradable polylactic acids for use in forming fibers

    CN101563391A

  • Fully-degradable polylactic acid fiber melt-blowing nonwoven and preparation method thereof

    CN101824708A

  • Preparation method of high-strength and high-toughness PLA (polylactic acid) and in-situ nanofiber composite

    CN106009559A

Cited By

  • A high-strength, high-toughness, fully biodegradable alloy fiber, its preparation method and application