A kind of efficient degumming method of industrial hemp fiber

By using the catalyst MnFe2O4 auxiliary Fenton system in the industrial hemp fiber degumming process, combining alkaline pretreatment and deep degumming of oxygen bleach liquid, the problems of low efficiency and environmental pollution in traditional processes are solved, and low cost and high efficiency are achieved , good environmentally friendly degumming effect.

CN116397336BActive Publication Date: 2024-11-12QIQIHAR UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310444545.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-24
Publication Date
2024-11-12
Estimated Expiration
2043-04-24

AI Technical Summary

Technical Problem

The traditional industrial hemp degumming process has problems such as long cycle, low efficiency, serious environmental pollution, high cost and fiber damage, especially the chemical degumming method causes serious damage to the environment and hemp fibers.

Method used

The catalyst MnFe2O4 assisted Fenton system is used to deguard under weak acid conditions, combined with alkaline pretreatment and oxygen bleach liquid in-depth deguarding, reducing the amount of chemical reagents and reaction time, improving the deguarding efficiency, and reducing costs through catalyst recovery.

Benefits of technology

The degumming process of industrial hemp fiber with low cost, high efficiency and environmental protection has been achieved, which reduces the residual glue rate, increases the breaking strength and whiteness of the fiber, reduces environmental pollution, and can reuse the catalyst, reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116397336B_ABST
    Figure CN116397336B_ABST
Patent Text Reader

Abstract

The invention discloses an efficient degumming method for industrial hemp fiber, which comprises the following steps: 1) preparing a catalyst MnFe2O4; 2) pre-treating industrial hemp under alkaline conditions, and then washing with water; 3) further degumming the industrial hemp fiber under weak acid conditions under the action of Fenton reagent H2O2, FeSO4·7H2O and catalyst MnFe2O4, and then washing with water; 4) recovering the catalyst; 5) performing deep degumming and bleaching treatment on the industrial hemp fiber with oxygen bleaching liquid, washing with water, and drying. Compared with other chemical degumming methods, the method of the invention uses less chemical reagents, has a shorter reaction time, has less environmental pollution, and has lower cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of degumming process methods, in particular to a high-efficiency degumming method for industrial hemp fibers. Background Art

[0002] Industrial hemp contains approximately 70% cellulose and 30% non-cellulose components. These non-cellulose components, also defined as pectin, play a dual role in the hemp phloem as both nutrition and bonding. The pectin content is tightly connected to the cellulose fibers and embedded in them, making it impossible for the individual fibers to separate freely from each other. Therefore, the removal of these pectin components from the raw hemp is the focus of industrial hemp fiber processing before the spinning process or large-scale industrial use.

[0003] Traditional industrial hemp degumming processes include natural water microbial degumming, mechanical degumming, chemical degumming and bio-enzyme degumming. Natural water microbial degumming uses microorganisms in water for degumming. Its disadvantages are long cycle, low efficiency, high labor intensity, large amount of water required, and serious environmental pollution; mechanical degumming method degumming is not thorough, fiber breakage leads to poor separation and short fiber length, which makes fiber spinning difficult; bio-enzyme degumming can reduce degumming costs, reduce environmental pollution and increase the production rate of refined hemp, and after enzyme degumming, the fiber is fluffy and soft, the average length increases, and the short fiber rate is low, but the current activity of bio-enzymes is not high enough, the degumming rate is low, and it takes a long time and the lignin removal is not obvious. Traditional chemical degumming uses chemical reagents for degumming. A large amount of chemicals and water are required in the degumming process, which not only consumes a lot of energy but also seriously pollutes the environment. At the same time, due to the use of a large amount of strong acid and alkali under high temperature conditions, the damage to hemp fibers is great. Summary of the invention

[0004] The present invention aims to solve one of the technical problems in the related art to at least a certain extent. To this end, the present invention provides a degumming method for industrial hemp fiber with less chemical reagent usage, shorter reaction time, less environmental pollution and lower cost.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] The embodiment of the present invention provides a method for degumming industrial hemp fiber, comprising the following steps:

[0007] 1) preparing catalyst MnFe2O4;

[0008] 2) Pre-treating industrial hemp under alkaline conditions and then washing with water;

[0009] 3) Under weak acid conditions, the industrial hemp fiber is further degummed under the action of Fenton reagent H2O2, FeSO4·7H2O and catalyst MnFe2O4, and then washed;

[0010] 4) recovering the catalyst;

[0011] 5) The industrial hemp fiber is subjected to in-depth degumming and bleaching treatment with oxygen bleaching liquid, followed by washing and drying.

[0012] The hemp fiber degumming process of the present invention has the characteristics of low cost, high benefit, high environmental protection, etc. The refined hemp obtained by the present invention has low residual glue rate, good breaking strength, good fiber softness and whiteness, soft fiber performance, and ideal hand feel and gloss. In addition, the catalyst MnFe2O4 in the present invention greatly promotes the degumming effect of Fenton on industrial hemp, so that the degumming time is short, the amount of alkali used is small, the alkali concentration in the wastewater is low, and environmental pollution is reduced. The catalyst MnFe2O4 can be reused after preparation, which reduces the cost and has good application prospects.

[0013] In some embodiments, step 1) is: using FeCl3 and MnCl2 with a molar ratio of 2:1 as raw materials, ethylene glycol as solvent, adjusting the pH to 7-8 with sodium acetate, reacting at 180°C for 8-12 hours, cooling, separating the precipitate with a magnet, washing alternately with deionized water and anhydrous ethanol for 3 times, and drying to constant weight to obtain the product.

[0014] In some embodiments, in step 2), industrial hemp is added to water at a bath ratio of 1:10-30, the NaOH concentration is 1-2 g / L, treated at 50-60° C. for 50-60 minutes, and washed with water until the pH value of the washing solution is neutral.

[0015] Preferably, in step 2), industrial hemp is added to water at a bath ratio of 1:20, the NaOH concentration is 2 g / L, treated at 60° C. for 60 minutes, and washed with water until the pH value of the washing solution is neutral.

[0016] In some embodiments, in step 3), industrial hemp is added with Fenton reagent and catalyst MnFe2O4 according to a bath ratio of 1:10-30, the concentrations of Fenton reagent are 3.5-7wt% H2O2, 0.25-0.5wt% FeSO4·7H2O, and the concentration of MnFe2O4 is 0.01-0.03wt%, respectively. The pH is adjusted to pH=5 with citric acid and sodium bicarbonate, treated at 50-60°C for 50-60min, and washed with water until the pH value of the washing solution is neutral.

[0017] In the embodiment of the present invention, the concentration of FeSO4·7H2O in the Fenton reagent is 0.25-0.5wt%. If the amount of FeSO4·7H2O added is too much, iron mud and fiber coloring will occur. If the amount of FeSO4·7H2O added is too little, the degumming effect is poor. Therefore, the concentration of FeSO4·7H2O is controlled to be 0.25-0.5wt% in the present application, and 3.5-7wt% H2O2 is matched according to the concentration range of FeSO4·7H2O, and the two react completely. In addition, the embodiment of the present invention enhances the activity of H2O2 in the Fenton system by adding the catalyst MnFe2O4. The inventors found that the addition of too much MnFe2O4 will damage the fiber, and the addition of too little MnFe2O4 has a weak activation effect in the Fenton system. Therefore, the addition of MnFe2O4 is controlled to be 0.01-0.03wt% in the present application.

[0018] Preferably, in step 3), industrial hemp is added with Fenton reagent and catalyst MnFe2O4 according to a bath ratio of 1:30, the concentrations of Fenton reagent are 6wt% H2O2, 0.4wt% FeSO4·7H2O, and the concentration of MnFe2O4 is 0.017wt%, and the pH is adjusted to pH=5 with citric acid and sodium bicarbonate, treated at 60°C for 60min, and washed with water until the pH value of the washing solution is neutral.

[0019] In some embodiments, in step 4), the catalyst is separated by a magnet, the water is drained, and the catalyst is collected again and placed in a 50° C. oven to dry to constant weight for next use.

[0020] In some embodiments, in step 5), industrial hemp is added to a bleaching solution at a bath ratio of 1:10 to 30, wherein the concentration of hydrogen peroxide is 10 to 14 g / L, the concentration of Na2CO3 is 1 to 2 g / L, the concentration of sodium silicate is 2 to 4 g / L, and the concentration of sodium sulfite is 0.5 to 1 g / L. The bleaching solution is treated at 80 to 100° C. for 80 to 100 minutes, washed with water until the pH value is neutral, and dried to a fiber dry state.

[0021] Preferably, in step 5), industrial hemp is added to a bleaching solution at a bath ratio of 1:30, wherein the concentration of hydrogen peroxide is 14 g / L, the concentration of Na2CO3 is 2 g / L, the concentration of sodium silicate is 2 g / L, and the concentration of sodium sulfite is 1 g / L. The bleaching solution is treated at 90° C. for 100 minutes, washed with water until the pH value is neutral, and dried to a fiber dry state.

[0022] The beneficial effects of the present invention are:

[0023] (1) The process flow of hemp fiber degumming of the present invention is as follows: MnFe2O4 preparation - pretreatment - MnFe2O4 assisted Fenton system oxidation degumming treatment - catalyst recovery - oxygen bleaching - water washing - drying. It has the characteristics of low cost, high efficiency and high environmental protection. The refined hemp obtained by the present invention has low residual glue rate, good breaking strength, good fiber softness and whiteness, soft fiber performance, and ideal hand feel and gloss.

[0024] (2) The catalyst MnFe2O4 greatly promoted the Fenton degumming of industrial hemp. Under low pH conditions, the Fe in FeSO4·7H2O reacted with H2O2 to form a 2+ The oxidation system formed produces hydroxyl radicals (·OH) with strong oxidation activity, which then react with organic compounds to effectively decompose high-molecular organic matter that is difficult to degrade into small molecular particles, and completely decompose into CO2 and H2O2. This shortens the degumming time, reduces the amount of alkali used, reduces the concentration of alkali in the wastewater, reduces environmental pollution, and the catalyst MnFe2O4 can be reused after preparation, which reduces costs and has good application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is the SEM image of the catalyst prepared in Example 1.

[0026] Figure 2 This is a SEM image of hemp fiber after treatment according to the method of Example 1. DETAILED DESCRIPTION

[0027] The embodiments of the present invention are described in detail below. The embodiments described below are exemplary and are only used to explain the present invention, and should not be understood as limiting the present invention.

[0028] Unless defined otherwise herein, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application belongs.

[0029] Where values ​​are described herein as a range, it should be understood that such disclosure includes disclosure of all possible sub-ranges within that range, as well as specific values ​​falling within that range, regardless of whether a specific value or a specific sub-range is explicitly stated.

[0030] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.

[0031] The physical properties of the hemp fiber prepared by the degumming method of the present invention were tested, and the following test data were obtained: the breaking strength was tested by an LLY-06E electronic single fiber strength tester, the stretching distance was 20 mm / min, the stretching number was 20 times, and the average value was taken.

[0032] The reference standard for testing the residual glue rate is GB / T18147.2-2008.

[0033] The reference standard for whiteness testing is GB / T17644-2008.

[0034] The COD value in degumming wastewater is in accordance with the standard GB11914-1989.

[0035] Example 1

[0036] A degumming method for industrial hemp fiber comprises the following steps:

[0037] 1) Preparation of catalyst MnFe2O4

[0038] Use 30 ml of ethylene glycol as solvent, adjust the acidity to 7-8 with 2.7 g of sodium acetate, add 0.002 mol of MnCl2·4H2O and 0.004 mol of FeCl3·6H2O, react in a reactor at 180°C for 10 hours after fully dissolving, suck out with a magnet after cooling, wash alternately with deionized water and anhydrous ethanol for 3 times, and dry to constant weight to obtain the product.

[0039] 2) Pre-treat industrial hemp under alkaline conditions and then wash with water;

[0040] The conditions are: industrial hemp is added to water at a bath ratio of 1:20, the NaOH concentration is 2g / L, treated at 60°C for 60 minutes, and washed with water until the pH value of the washing solution is neutral.

[0041] 3) Chemical degumming

[0042] Add Fenton reagent and catalyst MnFe2O4 to industrial hemp at a bath ratio of 1:30. The concentrations of Fenton reagent are 6wt% H2O2, 0.4wt% FeSO4·7H2O, and 0.017wt% MnFe2O4. Adjust the pH to pH=5 with citric acid and sodium bicarbonate, treat at 60℃ for 60min, and wash with water until the pH of the washing solution is neutral.

[0043] 4) Catalyst recovery:

[0044] Use a magnet to suck the catalyst to the bottom and drain the water; collect the catalyst again and dry it in a 50℃ oven to constant weight for next use;

[0045] 5) Oxygen bleaching, then water washing and drying.

[0046] The conditions are: industrial hemp is added to the bleaching solution at a bath ratio of 1:30. In the bleaching solution, the concentration of hydrogen peroxide is 14g / L, the concentration of Na2CO3 is 2g / L, the concentration of sodium silicate is 2g / L, and the concentration of sodium sulfite is 1g / L. It is treated at 90℃ for 100 minutes, washed with water until the pH value is neutral, and dried to a fiber dry state.

[0047] Figure 1 The SEM image of the catalyst prepared in step 1) is shown. Figure 1 It can be seen that MnFe2O4 presents uniform nanocrystals and has a good intermediate structure, which is conducive to the reaction.

[0048] Figure 2 The SEM image of the hemp fiber after the method of Example 1 is shown. Figure 2 It can be seen that the hydrogen bonds between the cellulose fibers in the figure are opened, resulting in an increase in the contacting non-crystalline areas. Between these areas of the fiber, macromolecular components such as colloid and lignin are removed, the fiber surface is smooth, and the fibers are well separated.

[0049] Example 2

[0050] A degumming method for industrial hemp fiber comprises the following steps:

[0051] 1) Preparation of catalyst MnFe2O4

[0052] Use 30 ml of ethylene glycol as solvent, adjust the acidity to 7-8 with 2.7 g of sodium acetate, add 0.002 mol of MnCl2·4H2O and 0.004 mol of FeCl3·6H2O, react in a reactor at 180°C for 10 hours after fully dissolving, suck out with a magnet after cooling, wash alternately with deionized water and anhydrous ethanol for 3 times, and dry to constant weight to obtain the product.

[0053] 2) Pre-treat industrial hemp under alkaline conditions and then wash with water;

[0054] The conditions are: industrial hemp is added to water at a bath ratio of 1:30, the NaOH concentration is 1g / L, treated at 60°C for 60 minutes, and washed with water until the pH value of the washing solution is neutral.

[0055] 3) Chemical degumming

[0056] Add Fenton reagent and catalyst MnFe2O4 to industrial hemp at a bath ratio of 1:30. The concentrations of Fenton reagent are 3.5wt% H2O2, 0.25wt% FeSO4·7H2O, and 0.017wt% MnFe2O4. Adjust the pH to pH=5 with citric acid and sodium bicarbonate, treat at 50℃ for 50min, and wash with water until the pH of the washing solution is neutral.

[0057] 4) Catalyst recovery:

[0058] Use a magnet to suck the catalyst to the bottom and drain the water; collect the catalyst again and dry it in a 50℃ oven to constant weight for next use;

[0059] 5) Oxygen bleaching, then water washing and drying.

[0060] The conditions are: industrial hemp is added to the bleaching solution at a bath ratio of 1:20. In the bleaching solution, the concentration of hydrogen peroxide is 10g / L, the concentration of Na2CO3 is 1g / L, the concentration of sodium silicate is 2g / L, and the concentration of sodium sulfite is 0.5g / L. It is treated at 90℃ for 90 minutes, washed with water until the pH value is neutral, and dried to a fiber dry state.

[0061] Example 3

[0062] A degumming method for industrial hemp fiber comprises the following steps:

[0063] 1) Preparation of catalyst MnFe2O4

[0064] Use 30 ml of ethylene glycol as solvent, adjust the acidity to 7-8 with 2.7 g of sodium acetate, add 0.002 mol of MnCl2·4H2O and 0.004 mol of FeCl3·6H2O, react in a reactor at 180°C for 10 hours after fully dissolving, suck out with a magnet after cooling, wash alternately with deionized water and anhydrous ethanol for 3 times, and dry to constant weight to obtain the product.

[0065] 2) Pre-treat industrial hemp under alkaline conditions and then wash with water;

[0066] The conditions are: industrial hemp is added to water at a bath ratio of 1:30, the NaOH concentration is 1.5g / L, treated at 55°C for 55 minutes, and washed with water until the pH value of the washing solution is neutral.

[0067] 3) Chemical degumming

[0068] Add Fenton reagent and catalyst MnFe2O4 to industrial hemp at a bath ratio of 1:30. The concentrations of Fenton reagent are 5wt% H2O2, 0.35wt% FeSO4·7H2O, and 0.025wt% MnFe2O4. Adjust the pH to pH=5 with citric acid and sodium bicarbonate, treat at 55℃ for 55min, and wash with water until the pH of the washing solution is neutral.

[0069] 4) Catalyst recovery:

[0070] Use a magnet to suck the catalyst to the bottom and drain the water; collect the catalyst again and dry it in a 50℃ oven to constant weight for next use;

[0071] 5) Oxygen bleaching, then water washing and drying.

[0072] The conditions are: industrial hemp is added to the bleaching solution at a bath ratio of 1:30. In the bleaching solution, the concentration of hydrogen peroxide is 12g / L, the concentration of Na2CO3 is 1.5g / L, the concentration of sodium silicate is 3g / L, and the concentration of sodium sulfite is 0.7g / L. It is treated at 90℃ for 90 minutes, washed with water until the pH value is neutral, and dried to a fiber dry state.

[0073] Example 4

[0074] A degumming method for industrial hemp fiber comprises the following steps:

[0075] 1) Preparation of catalyst MnFe2O4

[0076] Use 30 ml of ethylene glycol as solvent, adjust the acidity to 7-8 with 2.7 g of sodium acetate, add 0.002 mol of MnCl2·4H2O and 0.004 mol of FeCl3·6H2O, react in a reactor at 180°C for 10 hours after fully dissolving, suck out with a magnet after cooling, wash alternately with deionized water and anhydrous ethanol for 3 times, and dry to constant weight to obtain the product.

[0077] 2) Pre-treat industrial hemp under alkaline conditions and then wash with water;

[0078] The conditions are: industrial hemp is added to water at a bath ratio of 1:30, the NaOH concentration is 2g / L, treated at 60°C for 60 minutes, and washed with water until the pH value of the washing solution is neutral.

[0079] 3) Chemical degumming

[0080] Add Fenton reagent and catalyst MnFe2O4 to industrial hemp at a bath ratio of 1:30. The concentrations of Fenton reagent are 7wt% H2O2, 0.5wt% FeSO4·7H2O, and 0.03wt% MnFe2O4. Adjust the pH to pH=5 with citric acid and sodium bicarbonate, treat at 60℃ for 60min, and wash with water until the pH of the washing solution is neutral.

[0081] 4) Catalyst recovery:

[0082] Use a magnet to suck the catalyst to the bottom and drain the water; collect the catalyst again and dry it in a 50℃ oven to constant weight for next use;

[0083] 5) Oxygen bleaching, then water washing and drying.

[0084] The conditions are: industrial hemp is added to the bleaching solution at a bath ratio of 1:10. In the bleaching solution, the concentration of hydrogen peroxide is 14g / L, the concentration of Na2CO3 is 2g / L, the concentration of sodium silicate is 4g / L, and the concentration of sodium sulfite is 1g / L. It is treated at 100℃ for 100 minutes, washed with water until the pH value is neutral, and dried to a fiber dry state.

[0085] Comparative Example 1

[0086] Different from Example 2, no catalyst MnFe2O4 is used in Comparative Example 1.

[0087] Comparative Example 2

[0088] In Comparative Example 2, step 3) is:

[0089] Add H2O2 and catalyst MnFe2O4 to industrial hemp at a bath ratio of 1:30, with H2O2 concentration of 3.5wt% and MnFe2O4 concentration of 0.017wt%. Adjust the pH to pH=5 with citric acid and sodium bicarbonate, treat at 60℃ for 60min, and wash with water until the pH of the washing solution is neutral.

[0090] The other steps are the same as in Example 2.

[0091] Comparative Example 3

[0092] In Comparative Example 3, the catalyst used is porous g-C3N4 instead of the catalyst MnFe2O4 in Example 2.

[0093] The preparation method of porous g-C3N4 is as follows: first grind 2.5g of melamine for 5 minutes, then mix 2.5g of cyanuric acid and grind for 10 minutes; then place it in 100m of ethanol solution, stir for 2h, and ultrasonicate for 1h. Then evaporate the ethanol solution in a 90℃ water bath to obtain a supramolecular precursor. Then, heat the obtained supramolecular precursor from room temperature to 550℃ at a heating rate of 1.5℃ / min, and then calcine at a constant temperature for 6h to obtain it.

[0094] The chemical degumming conditions of step 3) are as follows: add Fenton reagent and catalyst porous g-C3N4 to industrial hemp at a bath ratio of 1:30, the concentrations of Fenton reagent are 5% H2O2, 0.35% FeSO4·7H2O, and the concentration of g-C3N4 is 0.025%, adjust the pH to pH=5 with citric acid and sodium bicarbonate, treat at 55°C for 55 minutes, wash with water until the pH value of the washing solution is neutral, and treat at 60°C for 60 minutes under xenon lamp irradiation.

[0095] The other steps are the same as in Example 2.

[0096] Comparative Example 4

[0097] In Comparative Example 4, the catalyst used is g-C3N4 / TiO2 instead of the catalyst MnFe2O4 in Example 2.

[0098] Preparation of g-C3N4 / TiO2: Mix g-C3N4 (the preparation method of which is shown in Comparative Example 3) and TiO2 in a mass ratio of 1:1, place in a muffle furnace, calcine at a temperature of 550°C, and calcine for 2 hours to obtain the product.

[0099] The chemical degumming conditions of step 3) are as follows: add Fenton reagent and catalyst g-C3N4 / TiO2 to industrial hemp at a bath ratio of 1:30, the concentrations of Fenton reagent are 5% H2O2, 0.35% FeSO4·7H2O, and the concentration of g-C3N4 / TiO2 is 0.025%, adjust the pH to pH=5 with citric acid and sodium bicarbonate, treat at 55°C for 55 minutes, wash with water until the pH value of the washing solution is neutral, and treat at 60°C for 60 minutes under xenon lamp irradiation.

[0100] The other steps are the same as in Example 2.

[0101] Comparative Example 5

[0102] In comparative example 5, step 1) is:

[0103] Use 30 ml of ethylene glycol as solvent, adjust the acidity to 7-8 with 2.7 g of sodium acetate, add 0.006 mol of MnCl2·4H2O and 0.012 mol of FeCl3·6H2O, react in a reactor at 180°C for 10 hours after fully dissolving, suck out with a magnet after cooling, wash alternately with deionized water and anhydrous ethanol for 3 times, and dry to constant weight to obtain the product.

[0104] The other steps are the same as in Example 2.

[0105] Comparative Example 6

[0106] The degumming method of industrial hemp fiber in Comparative Example 6 comprises the following steps:

[0107] 1) Preparation of catalyst MnFe2O4

[0108] Use 30ml ethylene glycol as solvent, adjust the acidity to 7-8 with 2.7g sodium acetate, add 0.002mol MnCl2.4H2O and 0.004mol FeCl3.6H2O, react in a reactor at 180℃ for 10h after fully dissolving, suck out with a magnet after cooling, wash 3 times with deionized water and anhydrous ethanol alternately, and dry to constant weight to obtain the product.

[0109] 2) Pre-treat industrial hemp under alkaline conditions and then wash with water;

[0110] The conditions are: industrial hemp is added to water at a bath ratio of 1:40, the NaOH concentration is 3g / L, treated at 70°C for 70 minutes, and washed with water until the pH value of the washing solution is neutral.

[0111] 3) Chemical degumming

[0112] Add Fenton reagent and catalyst MnFe2O4 to industrial hemp at a bath ratio of 1:40. The concentrations of Fenton reagent are 8% H2O2, 0.6% FeSO4·7H2O, and 0.035% MnFe2O4. Adjust the pH to pH=5 with citric acid and sodium bicarbonate, treat at 70℃ for 70min, and wash with water until the pH of the washing solution is neutral.

[0113] 4) Catalyst recovery:

[0114] Use a magnet to suck the catalyst to the bottom and drain the water; collect the catalyst again and dry it in a 50℃ oven to constant weight for next use;

[0115] 5) Oxygen bleaching, then water washing and drying.

[0116] The conditions are: industrial hemp is added to the bleaching solution at a bath ratio of 1:40. In the bleaching solution, the concentration of hydrogen peroxide is 15g / L, the concentration of Na2CO3 is 3g / L, the concentration of sodium silicate is 5g / L, and the concentration of sodium sulfite is 1.5g / L. It is treated at 110℃ for 110 minutes, washed with water until the pH value is neutral, and dried to a fiber dry state.

[0117] The residual rubber rate, breaking strength, whiteness and COD value in the degumming wastewater of Examples 1-4 and Comparative Examples 1-6 are shown in Table 1.

[0118] Table 1 Test data of Examples 1-4 and Comparative Examples 1-6

[0119]

[0120]

[0121] In summary, the industrial hemp fiber degumming process of the present invention has a residual gum rate of 5.86-6.81% after degumming, a breaking strength of 30.12-32.65CN, a whiteness of 26.78-28.92, a good degumming effect, a COD value of 15000-16000mg / L, and is beneficial to environmental protection. Among them, the effect of embodiment 1 is better.

[0122] It can be seen from Example 2 and Comparative Example 1 that when MnFe2O4 is not added and other conditions remain unchanged, the residual glue rate of Comparative Example 1 is 12.87%, the breaking strength is 48.51cN, the whiteness is 25.01%, and the COD value is 16375mg / L. By comparison, it can be seen that the fiber residual glue rate of Comparative Example 1 is relatively high after degumming, indicating that its degumming effect is slightly poor; the whiteness is low, indicating that the bleaching effect is not good. The reason why the degumming and bleaching effect of Example 2 is better than that of Comparative Example 1 is that the addition of MnFe2O4 increases the activity of H2O2 in the Fenton system and enhances the oxidation effect of H2O2, which can not only destroy a large number of double bond structures, but also destroy the chromophores of the pigment and the chromophores in the lignin, producing a bleaching effect.

[0123] It can be seen from Example 2 and Comparative Example 2 that when FeSO4·7H2O is not added and other conditions remain unchanged, the residual glue rate of Comparative Example 2 is 15.32%, the breaking strength is 49.52cN, the whiteness is 29.43%, and the COD value is 22409mg / L. By comparison, it can be seen that the effect of degumming treatment in Comparative Example 2 is not as good as that in Example 2. The reason for this is that FeSO4·7H2O plays a great role in the Fenton system. Fe in FeSO4·7H2O 2+ The oxidation system formed by H2O2 produces hydroxyl free radicals (·OH) with strong oxidative activity, which decomposes hemp, Fe 2+ After oxidation, it becomes Fe 3+ , H2O2 can convert Fe 3+ Reduction to Fe 2+ At the same time, hydroxyl radicals (·OH) are produced, and this cycle continuously stimulates the production of hydroxyl radicals (·OH) to fully decompose the hemp.

[0124] It can be seen from the data of residual glue rate and fiber breaking strength of Example 2, Comparative Example 3 and Comparative Example 4 that g-C3N4 and g-C3N4 / TiO2 do not play a significant role in Fenton system degumming. This may be due to the uneven irradiation of the xenon lamp during the degumming reaction due to the opacity of the hemp fiber, which increases the difficulty of actual production. Although the COD value is lower than other chemical degumming processes, these two catalysts are not easy to recover compared with MnFe2O4, and increase the production cost.

[0125] It can be seen from Example 2 and Comparative Example 5 that the amount of FeCl3.6H2O and MnCl2.4H2O is changed in the preparation of MnFe2O4 in Comparative Example 5, and the residual glue rate of Comparative Example 1 is 6.71%, the breaking strength is 25.12cN, the whiteness is 23.69%, and the COD value is 16213mg / L. By comparison, it can be seen that the residual glue rate of the fiber after degumming in Comparative Example 5 is slightly lower, but its strength is greatly reduced and the whiteness is also poor. The reason for the analysis is that the color of the MnFe2O4 catalyst prepared according to this amount is darker, which will cause fiber coloring, enhance the catalytic effect, but cause greater damage to the fiber.

[0126] It can be seen from Example 2 and Comparative Example 6 that the catalyst MnFe2O4 remains unchanged, and in other steps, the amount of chemical reagents increases, the temperature increases, and the time increases. The residual glue rate of Comparative Example 6 is 5.79%, the breaking strength is 24.85cN, the whiteness is 28.95%, and the COD value is 15946mg / L. By comparison, it can be seen that although the residual glue rate of the fiber after degumming in Comparative Example 6 is low, the strength is greatly reduced. The reason for this is that the amount of chemicals used in the degumming process increases, the time is prolonged, and the temperature increases, which greatly damages the hemp fiber.

[0127] In the present invention, the terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" etc. mean that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the described specific features, structures, materials or characteristics may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0128] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A method for degumming industrial hemp fiber, characterized in that: The steps include: 1) 0.002 mol MnCl2∙4H2O and 0.004 mol FeCl3∙6H2O were used as raw materials, ethylene glycol was used as solvent, and the pH was adjusted to 7-8 with sodium acetate. The reaction was carried out at 180°C for 8-12 hours. After cooling, the precipitate was separated by a magnet, washed alternately with deionized water and anhydrous ethanol for 3 times, and dried to constant weight to obtain the catalyst MnFe2O4. 2) Add industrial hemp to water at a bath ratio of 1:10-30, with a NaOH concentration of 1-2 g / L, and treat at 50-60°C for 50-60 minutes, then wash with water until the pH value of the washing solution is neutral; 3) Add Fenton reagent and catalyst MnFe2O4 to industrial hemp at a bath ratio of 1:10-30. The concentrations of Fenton reagent are 3.5-7wt% H2O2, 0.25-0.5wt% FeSO4∙7H2O, and 0.01-0.03wt% MnFe2O4. Adjust the pH to 5 with citric acid and sodium bicarbonate, treat at 50-60℃ for 50-60min, and wash with water until the pH value of the washing solution is neutral. 4) Recover the catalyst; 5) Industrial hemp is added to bleaching solution at a bath ratio of 1:10~30, wherein the concentration of hydrogen peroxide is 10~14 g / L, the concentration of Na2CO3 is 1~2 g / L, the concentration of sodium silicate is 2~4 g / L, and the concentration of sodium sulfite is 0.5~1 g / L. The bleaching solution is treated at 80~100℃ for 80~100 minutes, washed with water until the pH value is neutral, and dried to a fiber dry state.

2. A method for degumming industrial hemp fiber according to claim 1, characterized in that: In step 2), industrial hemp is added with water at a bath ratio of 1:20, the NaOH concentration is 2 g / L, treated at 60°C for 60 minutes, and washed with water until the pH value of the washing solution is neutral.

3. The method for degumming industrial hemp fiber according to claim 1, characterized in that: In step 3), industrial hemp was added with Fenton reagent and catalyst MnFe2O4 according to a bath ratio of 1:

30. The concentrations of Fenton reagent were 6wt% H2O2, 0.4 wt% FeSO4∙7H2O, and 0.017 wt% MnFe2O4. The pH was adjusted to pH=5 with citric acid and sodium bicarbonate, treated at 60℃ for 60min, and washed with water until the pH value of the washing solution was neutral.

4. The method for degumming industrial hemp fiber according to claim 1, characterized in that: In step 4), the catalyst is separated by a magnet, the water is drained, the catalyst is collected again, and placed in a 50°C oven to dry to constant weight for next use.

5. The method for degumming industrial hemp fiber according to claim 1, characterized in that: In step 5), industrial hemp is added with bleaching solution at a bath ratio of 1:30, wherein the concentration of hydrogen peroxide is 14 g / L, the concentration of Na2CO3 is 2 g / L, the concentration of sodium silicate is 2 g / L, and the concentration of sodium sulfite is 1 g / L. The bleaching solution is treated at 90°C for 100 minutes, washed with water until the pH value is neutral, and dried to a fiber dry state.