A silicon-germanium-antimony-tellurium doped target material and preparation method thereof
By mixing silicon powder and GexSbyTez powder and then performing wet ball milling and vacuum hot pressing, a silicon-doped germanium antimony tellurium target material is prepared, which solves the problem of the complicated preparation process of silicon-doped germanium antimony tellurium film in the existing technology and realizes silicon The uniform distribution of doping amount and efficient doping simplify the process flow.
Patent Information
- Application Number
- CN202310661181.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-06
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-06-06
AI Technical Summary
The process of preparing silicon-doped germanium antimony tellurium thin films in the existing technology is complex and difficult to control, especially in the dual-target sputtering method, which requires precise control of sputtering conditions to ensure the consistency and performance of the film composition.
By mixing silicon powder and GexSbyTez powder and then performing wet ball milling and vacuum hot pressing, a silicon-doped germanium antimony tellurium target is prepared, which simplifies the sputtering process. The silicon-doped germanium antimony tellurium target is directly used for coating, which reduces the difficulty of preparation. .
It achieves uniform distribution and efficient doping of silicon doping amount, meets the basic requirements for silicon doping amount of germanium antimony tellurium thin films, simplifies the process flow and reduces the difficulty of preparation.
Smart Images

Figure BDA0004269072980000081
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of target material production, and in particular to a silicon-germanium-antimony-tellurium doped target material and a preparation method thereof. Background Art
[0002] Currently, the most studied chalcogenide phase change material in PCRAM applications is GeTe-Sb 2 Te 3 Pseudo-binary alloys, such as Ge 1 Sb 2 Te 4 ,Ge 2 Sb 2 Te 5 and Ge 1 Sb 4 Te 7 Etc. This series of materials has an extremely fast crystallization speed and there is a significant electrical difference between the amorphous and crystalline states of the material, which can meet the requirements of PCRAM devices for phase change storage medium layers. However, the need for a high thermal threshold during the phase change process has become an obstacle to the storage of pure germanium antimony telluride thin films. Studies have shown that silicon doping helps the amorphous stability of germanium antimony telluride thin films, reduces the RESET voltage of the material, and reduces device power consumption. To achieve the above effects, the existing solution is to prepare the film by sputtering coating (PVD); the raw material for sputtering can be Ge x Sb y Te z The target material is matched with the pure Si target material to achieve the purpose of doping Si into the GeSbTe film. x Sb y Te z The sputtering conditions for both Si target material and pure Si target material are extremely demanding, and the sputtering process is difficult to control, which will result in low product yield.
[0003] Jiang Yifan of Nanjing University mentioned the following on page 3 in his paper "Study on the Effect of Silicon Doping on the Properties of Chalcogenide Phase Change Material Germanium Antimony Telluride Thin Films": "In this chapter, GST and Si-GST films were prepared by electron beam evaporation, and the thermally induced phase change kinetics of the films were studied by in-situ resistance testing and the results of different films were compared. The in-situ variable temperature resistance test method showed that compared with pure GST films, Si-GST films have higher crystallization temperature and crystalline resistivity, and these physical quantities will further increase with the increase of Si doping concentration, which indicates that Si-GST films have better non-quality thermal stability and can effectively reduce the power consumption of PCRAM devices;
[0004] Then, the crystallization activation energy and amorphous conductivity activation energy of GST and S-GST films were calculated using the experimental data of temperature-variable resistors, and it was found that the values of both activation energies would increase with the increase of Si doping concentration. The value of crystallization activation energy increased from 2.99 eV before Si doping to 4.09 eV after Si doping, indicating that more energy is required for the crystallization of Si-GST film, thereby improving the amorphous thermal stability of the film: and the value of amorphous conductivity activation energy increased from 0.404 eV before Si doping to 0.31 eV after Si doping, indicating that Si doping changed the energy band structure of the crystalline GST film;
[0005] In the in-situ constant temperature resistance test experiment, the experimental data showed that the incubation time required for the crystallization of Si-GST film was longer than that of GST film at the same annealing temperature, thus confirming that Si-GST has better amorphous thermal stability;
[0006] And through the analysis of the film crystallization model, it was found that after Si doping, the Avrami coefficient of the film decreased significantly from about 2.70 to about 1.30, while the crystallization activation energy increased from 3.11eV to 4.17eV. "
[0007] It is not difficult to see that the addition of silicon into the germanium antimony telluride film can increase the crystallization temperature and crystalline resistance of the germanium antimony telluride film. At the same time, within a certain range, the crystallization activation energy of the film will increase with the increase of silicon doping concentration, which means that the silicon-doped germanium antimony telluride film requires more energy for crystallization, thereby improving the amorphous thermal stability of the film; and the amorphous conductivity activation energy of the film also increases with the increase of silicon doping concentration, indicating that silicon doping changes the energy band structure of the amorphous germanium antimony telluride film.
[0008] Combining the above literature, it is not difficult to find that silicon doping has multi-faceted and multi-dimensional beneficial effects on improving the performance of germanium antimony telluride thin films; and in the prior art, there are also many precedents for preparing silicon-doped germanium antimony telluride thin films;
[0009] Chinese patent application 201610742155.1 discloses a method for preparing doped Ge with a fixed atomic ratio based on an analytical method. 2 Sb 2 Te 5 The method of phase change film is to calculate the deposition thickness ratio of the two targets according to the doping atomic ratio, and then determine the sputtering power of the two targets to prepare A x (Ge 2 Sb 2 Te 5 ) 100-xA film, where A is the doping element, x is the percentage of doping atoms in the doped film to be prepared, and the sputtering power of the two targets is adjusted after the test to obtain a film with the required doping atomic ratio; the specific preparation steps are: calculating the thickness ratio of the deposited films of the two targets, the deposition rate of the corresponding films of the two targets, selecting the substrate and pretreatment, determining the sputtering power of the two targets, sputtering coating, detecting the chemical composition of the film and comparing it with the target film, and fine-tuning the sputtering power to prepare GGe that meets the doping atomic ratio 2 Sb 2 Te 5 film;
[0010] It can be seen that the above scheme provides a method for preparing germanium antimony telluride thin films doped with other elements. However, by observing paragraphs 7-21 of the scheme, it is not difficult to see that this scheme obtains germanium antimony telluride thin films containing doped elements by a dual-target sputtering method, and before sputtering, it is necessary to calculate the deposition film thickness ratio of the two targets and the film deposition rate of the two targets during co-sputtering, and select the substrate and pre-treat and adjust the sputtering power of the two targets; on the one hand, the scheme can purposefully and clearly set the sputtering process parameters through the above treatment, which is fast and efficient; and by accurately controlling the sputtering power of the two targets, it is possible to accurately control the film composition;
[0011] But at the same time, the preparation process of germanium antimony telluride target containing doped elements has high technical content, is slightly complicated to implement, and requires very precise control. If the silicon element can be directly doped into the target material, the silicon-doped germanium antimony telluride target material can be directly used for coating, thereby reducing the calculation of the thin film deposition rate and the control of the sputtering speed during dual-target sputtering.
[0012] Chinese patent application 201910905550.0 discloses a method for preparing a carbon-doped germanium antimony tellurium phase change target, which comprises the following steps: using elemental germanium, elemental antimony and elemental tellurium as raw materials, performing vacuum induction melting, ball milling and screening to obtain germanium antimony tellurium powder; dispersing the germanium antimony tellurium powder and carbon black in a reaction system containing acrylamide, and obtaining polyacrylamide colloid in which germanium antimony tellurium powder and carbon black are evenly distributed through polymerization reaction; calcining the polyacrylamide colloid in which germanium antimony tellurium powder and carbon black are distributed in an oxygen-free environment to obtain carbon-doped germanium antimony tellurium powder; vacuum hot pressing sintering the carbon-doped germanium antimony tellurium powder to obtain a carbon-doped germanium antimony tellurium phase change target;
[0013] This scheme uses polyacrylamide and carbon black as carbon sources. In the process of forming polyacrylamide colloid, the germanium antimony telluride powder and carbon black powder are suspended in the solution by stirring, so as to achieve the purpose of fully mixing the carbon black powder and the germanium antimony telluride powder. This solves the problem that when high-energy ball milling or other mechanical mixing is used in the prior art, the carbon powder agglomerates due to its softness, which makes it difficult to mix the carbon powder and the germanium antimony telluride powder evenly. In addition, when the polyacrylamide colloid is thermally decomposed, the carbon-carbon double bonds produced have greater activity and are easy to produce physical and chemical reactions with the germanium antimony telluride particles to achieve uniform mixing of the powders, effectively solving the problem of uneven doping caused by agglomeration of carbon particles in the existing carbon-doped germanium antimony telluride target; but although carbon and silicon belong to the same main group of elements, whether the preparation method of carbon-doped germanium antimony telluride phase change target can be easily applied to silicon-doped germanium antimony telluride phase change target remains to be discussed.
[0014] The problem that this solution needs to solve is: how to develop a germanium antimony telluride target material doped with silicon to reduce the difficulty of preparing silicon-doped germanium antimony telluride thin films. Summary of the invention
[0015] The purpose of the present application is to develop a germanium antimony telluride target material, and the germanium antimony telluride target material is doped with silicon element to reduce the difficulty of preparing silicon-doped germanium antimony telluride thin films.
[0016] Unless otherwise specified in this application: nM represents nanomole / liter, μM represents micromole / liter, mM represents millimole / liter, and M represents mole / liter;
[0017] A method for preparing a silicon-germanium-antimony-tellurium doped target comprises the following steps:
[0018] Step 1: Mix silicon powder, Ge x Sb y Te z The powders are mixed and the mass of silicon powder accounts for 2-10% of the total mass of the powders, and then wet ball milling and drying are performed to obtain silicon-germanium-antimony-tellurium doped powders;
[0019] Step 2: vacuum hot pressing the silicon-germanium-antimony-telluride powder obtained in step 1 to obtain a silicon-germanium-antimony-telluride blank;
[0020] Step 3: Mechanically process the silicon-germanium-antimony-telluride blank obtained in step 2 to obtain a silicon-germanium-antimony-telluride target.
[0021] Preferably, the Ge in step 1 x Sb y Te z The purity of the powder is not less than 5N, and Ge x Sb y Te z In powder, 1≤x≤2, 2≤y≤4, 4≤z≤7, Ge x Sby Te z The particle size of the powder is less than 10 microns.
[0022] Preferably, the silicon powder in step 1 is silicon powder with a particle size less than 10 microns obtained by crushing polycrystalline silicon with a purity of 4 to 7N.
[0023] Preferably, step 1 is specifically: silicon powder, Ge x Sb y Te z The powder mixture is then placed in a vacuum ball mill, and grinding balls are added, with the mass ratio of grinding balls to materials being 2 to 4:1. Then an organic solvent is added and the mixture is vacuumed to 10 -2 Pa, followed by wet ball milling at a speed of 60-100 r / min for 2-4 h;
[0024] The organic solvent is selected from at least one of anhydrous ethanol and isopropanol;
[0025] The grinding balls are zirconium balls or stainless steel balls.
[0026] Preferably, step 2 is specifically as follows: firstly, the silicon-germanium-antimony-tellurium powder doped with silicon-germanium-antimony-tellurium obtained in step 1 is placed in a graphite mold for compaction, and then the graphite mold is placed in a vacuum hot pressing furnace for pre-pressing, the pre-pressing pressure is 2-5 MPa, and the time is 3-5 min;
[0027] Then the furnace door is closed, the furnace is evacuated to 5-10Pa, and the temperature is raised to 500-600°C at a rate of 5-10°C / min for insulation for 90-130min. During the insulation process, when the insulation time reaches 30-50min, the pressure is increased to 30-35MPa and maintained for 60-80min. After the insulation and pressure maintenance, the pressure is slowly reduced to 10MPa, cooled with the furnace, the furnace door is opened, and the doped germanium antimony tellurium blank is obtained after demolding.
[0028] Preferably, step 3 specifically comprises: grinding and machining the germanium antimony telluride blank obtained in step 2 to obtain a silicon-doped germanium antimony telluride target.
[0029] In addition, a silicon-germanium-antimony-telluride target is disclosed, which is prepared by the above-mentioned silicon-germanium-antimony-telluride target preparation method. The germanium-antimony-telluride target is doped with silicon element, and the doping amount of silicon element is 2-10% by mass percentage.
[0030] Preferably, the grain size of the Germanium Antimony Telluride target is less than 6 μm.
[0031] Preferably, the oxygen content in the germanium antimony telluride target is less than 800 ppm.
[0032] The beneficial effect of the present application is that the silicon doping amount in the silicon-germanium-antimony-telluride target material obtained by the method for preparing the silicon-germanium-antimony-telluride target material disclosed in the present application reaches 2 to 10 wt %, which can meet the basic requirements for the silicon doping amount in the silicon-germanium-antimony-telluride film, and at the same time can solve the problem of complex process when preparing thin films using traditional double-target sputtering, thereby reducing the difficulty of preparing silicon-germanium-antimony-telluride thin films. DETAILED DESCRIPTION
[0033] In the description of the present invention, it should be noted that, if the specific conditions are not specified in the examples, the experiments were carried out according to conventional conditions or the conditions recommended by the manufacturer. The reagents or instruments used, if the manufacturer is not specified, are all conventional products that can be purchased commercially.
[0034] The present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0035] Example 1
[0036] Select polysilicon raw materials, first grind the raw materials and clean the outer surface, then crush them into particles with a particle size ranging from 50 to 100 meshes, then wet grind, vacuum dry and sieve to obtain finished raw materials A with a particle size less than 10 microns;
[0037] Then select Ge with a particle size less than 10 microns 2 Sb 2 Te 5 Powder raw material B.
[0038] Step 1: Mix raw materials A and B according to Si:Ge 2 Sb 2 Te 5 =2:98 mass ratio, put it into the vacuum ball mill, put a certain mass of zirconium balls, where the mass ratio of material to zirconium balls is 2:1, add isopropanol at the same time, and evacuate to 10 - 2 After Pa, wet grinding and mixing were carried out; the ball mill speed was 100r / min, the wet grinding time was 2h, and the wet grinding was allowed to stand for 1.5h after completion;
[0039] The material after ball milling and standing was taken out and placed in a vacuum drying oven for drying at a temperature of 100° C. for 1 h to obtain silicon-germanium-antimony-tellurium powder.
[0040] Step 2: Place the silicon-germanium-antimony-tellurium powder in step 1 into a mold with graphite paper on all sides, flatten it with a spoon, and then compact the powder with a tamping hammer. Then, place graphite paper, graphite gasket and graphite indenter on top of the powder in sequence, and then place it in a vacuum hot pressing furnace so that the pressure column and the center of the mold are aligned;
[0041] First, pre-press at 2T / min, the pre-press pressure is 3MPa, maintain for 3min and then release the pressure;
[0042] Then the furnace door was closed, and the vacuum was evacuated until the vacuum degree in the furnace reached 8Pa. Then heating was started, and the temperature was raised to 500°C at a rate of 5°C / min. The temperature was kept warm for 130 minutes. During the heat preservation process, the pressure was increased to 35MPa when the heat preservation time reached 50 minutes, and then the temperature was kept warm and pressure maintained for 80 minutes. After the heat preservation and pressure maintenance was completed, the pressure was slowly reduced to 10MPa, and the furnace was cooled. The furnace door was opened, and the doped germanium antimony tellurium blank was obtained after demolding.
[0043] Step 3: The rough target material is ground and tested for density, composition and purity to obtain a silicon-doped germanium antimony tellurium target material with a relative density of 99.2%, uniform composition and a purity of 5N.
[0044] Example 2
[0045] Step 1: Mix raw materials A and B according to Si:Ge 2 Sb 2 Te 5 =4:96 mass ratio, put it into the vacuum ball mill, put a certain mass of stainless steel balls, and the mass ratio of material to stainless steel balls is 3:1, and put anhydrous ethanol at the same time, and evacuate to 10 -2 After Pa, wet grinding and mixing were carried out. The ball mill speed was 80r / min, the wet grinding time was 3h, and the wet grinding was left to stand for 2h;
[0046] The material after the ball mill was left to stand was taken out and placed in a vacuum drying oven for drying at a temperature of 90° C. for 1.5 h to obtain silicon-germanium-antimony-tellurium powder.
[0047] Step 2: Place the silicon-germanium-antimony-tellurium powder in step 1 into a mold with graphite paper on all sides, flatten it with a spoon, and then compact the powder with a tamping hammer. Then, place graphite paper, graphite gasket and graphite indenter on top of the powder in sequence, and then place it in a vacuum hot pressing furnace so that the pressure column and the center of the mold are aligned;
[0048] First, pre-press at 2T / min, the pre-press pressure is 5MPa, maintain for 5min and then release the pressure;
[0049] Then the furnace door was closed, and the vacuum was evacuated until the vacuum degree in the furnace reached 5Pa. Then heating was started, and the temperature was increased to 600°C at a rate of 10°C / min. The temperature was kept warm for 100 minutes. During the heat preservation process, when the heat preservation time reached 30 minutes, the pressure was increased to 32MPa, and then the temperature was kept warm and pressure maintained for 70 minutes. After the heat preservation and pressure maintenance was completed, the pressure was slowly reduced to 10MPa, and the furnace was cooled. The furnace door was opened, and the doped germanium antimony tellurium blank was obtained after demolding.
[0050] Step 3: Grind the rough target material, and perform density, component, and purity tests to obtain a silicon-doped germanium antimony tellurium target material with a relative density of 99.3%, uniform component, and a purity of 5N.
[0051] Example 3
[0052] Step 1: Mix raw materials A and B according to Si:Ge 2 Sb 2 Te 5 =10:90 mass ratio, put it into the vacuum ball mill, put a certain mass of zirconium balls, where the mass ratio of material to zirconium balls is 2:1, add anhydrous ethanol at the same time, and evacuate to 10 -2 After Pa, wet grinding and mixing were carried out; the ball mill speed was 60r / min, the wet grinding time was 4h, and the wet grinding was completed and left to stand for 1h;
[0053] The material after ball milling and standing was taken out and placed in a vacuum drying oven for drying at a temperature of 80° C. for 2 h to obtain a uniformly mixed silicon-germanium-antimony-tellurium doped powder.
[0054] Step 2: Place the silicon-germanium-antimony-tellurium powder in step 1 into a mold with graphite paper on all sides, flatten it with a spoon, and then compact the powder with a tamping hammer. Then, place graphite paper, graphite gasket and graphite indenter on top of the powder in sequence, and then place it in a vacuum hot pressing furnace so that the pressure column and the center of the mold are aligned;
[0055] First, pre-press at 3T / min, with a pre-pressing pressure of 5MPa, and release the pressure after maintaining for 4min;
[0056] Then the furnace door was closed, and the vacuum was evacuated until the vacuum degree in the furnace reached 10Pa. Then heating was started, and the temperature was raised to 550°C at a rate of 8°C / min. The temperature was kept warm for 90 minutes. During the heat preservation process, the pressure was increased to 33MPa when the heat preservation time reached 40 minutes, and then the temperature was kept warm and pressure maintained for 60 minutes. After the heat preservation and pressure maintenance was completed, the pressure was slowly reduced to 10MPa, and the furnace was cooled. The furnace door was opened, and the doped germanium antimony tellurium blank was obtained after demolding.
[0057] Step 3: Grind the rough target material, and perform density, component, and purity tests to obtain a silicon-doped germanium antimony tellurium target material with a relative density of 99.1%, uniform component, and a purity of 5N.
[0058] Comparative Example 1
[0059] The method is basically the same as Example 1, except that in step 1, after wet grinding, the material is directly taken out and placed in a vacuum drying box for drying.
[0060] Comparative Example 2
[0061] The method is basically the same as Example 1, except that a carbon raw material is used instead of a silicon raw material.
[0062] Performance Test:
[0063] Density test: Archimedes drainage method is used to test the density of the target material.
[0064] Silicon content and oxygen content test: XRD is used to detect the silicon content at three different locations of a single sample, and the oxygen content is also detected at the same time.
[0065] Grain size: SEM
[0066] The test results are shown in Table 1:
[0067] Table 1
[0068]
[0069] Result analysis:
[0070] 1. It can be seen from Examples 1-3 and Comparative Example 1 that when the standing step is omitted after the wet ball milling in step 1, the difference in silicon content at each position increases significantly. This also proves that in the preparation process of silicon-germanium-antimony-tellurium target, standing after wet milling is an indispensable step. We speculate that the reason for this phenomenon may be that during the wet milling process, the particles are subjected to strong impact and wear, resulting in differences in particle size, shape and distribution. In addition, the medium added during the wet ball milling process sometimes has uneven horizontal distribution; standing can cause tiny displacements and particle arrangement in the powder through forces such as gravity and surface tension, thereby affecting the distribution of the particles, causing the particles to change from densely packed to more evenly distributed.
[0071] 2. It can be seen from Examples 1-3 and Comparative Example 2 that when carbon is used instead of silicon, the uniformity and density of the prepared target material are significantly reduced. It is not difficult to see that the above preparation method is not suitable for preparing carbon-doped germanium antimony telluride targets; and the polyacrylamine used in the preparation method of carbon-doped germanium antimony telluride targets is not only used as a raw material for preparing colloids, but also provides 20% of carbon elements. Therefore, this method cannot be directly used to prepare silicon-doped germanium antimony telluride targets, and the silicon-doped germanium antimony telluride targets in this application have been proved by experiments to have poor uniformity of the carbon-doped germanium antimony telluride targets.
[0072] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A method for preparing a silicon-germanium-antimony-tellurium doped target material. It is characterized in that The following steps are involved: Step 1: Mix silicon powder, Ge x Sb y Te z The powders are mixed and the mass of silicon powder accounts for 2-10% of the total mass of the powders, and then wet ball milling, standing and drying are performed to obtain silicon-germanium-antimony-tellurium doped powders; Step 2: vacuum hot pressing the silicon-germanium-antimony-telluride powder obtained in step 1 to obtain a silicon-germanium-antimony-telluride blank; Step 3: machining the silicon-germanium-antimony-telluride blank obtained in step 2 to obtain a silicon-germanium-antimony-telluride target; The standing time is 1 to 2 hours.
2. The method for preparing the silicon-germanium-antimony-telluride target according to claim 1, It is characterized in that Step 1Ge x Sb y Te z The purity of the powder is not less than 5N, and Ge x Sb y Te z In the powder, 1≤x≤2, 2≤y≤4, 4≤z≤7, the Ge x Sb y Te z The particle size of the powder is less than 10 microns.
3. The method for preparing the silicon-germanium-antimony-telluride target according to claim 1, It is characterized in that The silicon powder in step 1 is silicon powder with a particle size of less than 10 microns obtained by crushing polycrystalline silicon with a purity of 4 to 7N.
4. The method for preparing the silicon-germanium-antimony-telluride target according to claim 1, It is characterized in that The step 1 is specifically as follows: silicon powder, Ge x Sb y Te z The powder mixture is then placed in a vacuum ball mill, and grinding balls are added, with the mass ratio of grinding balls to materials being 2 to 4:
1. Then an organic solvent is added and the mixture is vacuumed to 10 -2 Pa, followed by wet ball milling at a speed of 60-100 r / min for 2-4 h; The organic solvent is selected from at least one of anhydrous ethanol and isopropanol; The grinding balls are zirconium balls or stainless steel balls.
5. The method for preparing the silicon-germanium-antimony-telluride target according to claim 1, It is characterized in that The step 2 is specifically as follows: firstly, the silicon-germanium-antimony-tellurium powder obtained in step 1 is placed in a graphite mold for compaction, and then the graphite mold is placed in a vacuum hot pressing furnace for pre-pressing, the pre-pressing pressure is 2-5 MPa, and the time is 3-5 minutes; Then the furnace door is closed, the furnace is evacuated to 5-10Pa, and the temperature is raised to 500-600°C at a rate of 5-10°C / min for insulation for 90-130min. During the insulation process, when the insulation time reaches 30-50min, the pressure is increased to 30-35MPa and maintained for 60-80min. After the insulation and pressure maintenance, the pressure is slowly reduced to 10MPa, cooled with the furnace, the furnace door is opened, and the doped germanium antimony tellurium blank is obtained after demolding.
6. The method for preparing the silicon-germanium-antimony-telluride target according to claim 1, It is characterized in that The step 3 specifically comprises: grinding and machining the germanium antimony telluride blank obtained in step 2 to obtain a silicon-doped germanium antimony telluride target.
7. A silicon-germanium-antimony-tellurium doped target, It is characterized in that The method for preparing a silicon-doped germanium-antimony-telluride target material according to any one of claims 1 to 6, wherein the germanium-antimony-telluride target material is doped with silicon element, and the doping amount of the silicon element is 2 to 10% by mass.
8. The silicon-germanium-antimony-telluride doped target according to claim 7, It is characterized in that The grain size of the germanium antimony tellurium target material is less than 6 μm.
9. The silicon-germanium-antimony-telluride target according to claim 7, It is characterized in that The oxygen content in the germanium antimony tellurium target is less than 800 ppm.
Citation Information
Patent Citations
Method for preparing phase-change film with fixed atomic ratio and doped with Ge2Sb2Te5 on basis of analytical method
CN106191773A
Preparation method of carbon-doped germanium-antimony-tellurium phase change target material
CN110527960A
Preparation methods for germanium-antimony-tellurium powder and target material
CN110342473A
Method for fabricating ceramic materials
US4800051A