A non-film-forming and highly anti-adhesive styrene acrylic core-shell emulsion and preparation method thereof

Through technical means such as designing core-shell structures and using chain transfer agents, the problem of acrylate copolymer emulsions returning to sticking at high temperatures is solved, and low-cost and efficient anti-adhesion and boiling resistance are achieved, which is suitable for pressure-sensitive adhesives and Wood paint and other scenes.

CN117362530BActive Publication Date: 2024-11-26QINGYUAN HUMAN NEW MATERIAL TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311201973.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-18
Publication Date
2024-11-26
Estimated Expiration
2043-09-18

AI Technical Summary

Technical Problem

The problem of re-adhesion of acrylate copolymer emulsions at high temperatures limits its application scenarios with high anti-adhesion requirements, such as the use of pressure-sensitive adhesives and wood coatings, and the existing solutions are costly.

Method used

The preparation method of non-film-forming high-resistance styrene core-shell emulsion is adopted. By designing the core-shell structure, the interpenetrating network structure and internal and external cross-linking are formed, and the branching degree is reduced, and the boiling resistance and anti-stickness properties are improved. The dense spatial network structure is further crosslinked by self-crosslinking monomers and silicon modified monomers.

Benefits of technology

It has achieved the improvement of the anti-viscosity and boiling resistance of the paint film at low cost, reduced the migration of ethanol, and the formulation process is simple, the emulsion is stable, and it has wide application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117362530B_ABST
    Figure CN117362530B_ABST
Patent Text Reader

Abstract

The invention discloses a non-film-forming high anti-adhesive styrene acrylic core-shell emulsion and a preparation method thereof. The non-film-forming emulsion prepared by the method has excellent water boiling resistance, good compatibility, high anti-adhesiveness and ethanol migration resistance, meets the good compatibility of paper / pulp coating paint systems, provides excellent anti-adhesive performance, and has outstanding water boiling resistance and ethanol migration resistance; meets food grade requirements, can reduce the amount of coating additives used, greatly reduces costs, is environmentally friendly, has a simple production process, and has good market prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of organic coatings, and in particular relates to a method for preparing a non-film-forming and highly anti-adhesive styrene acrylic core-shell emulsion. Background Art

[0002] Acrylic copolymer emulsion has excellent weather resistance, acid and alkali resistance, scrub resistance, and high adhesion, and is widely used in many fields such as textiles, paper products, pressure-sensitive adhesives, coatings, and leather processing; with the upgrade of the plastic ban, many paper-over-plastic composite products, plastic synthetic paper, and coated paper have gradually become the objects of elimination by the packaging and printing industry because they cannot meet the environmental protection requirements of recyclability, repulpability, and biodegradability. Therefore, products with functional coatings on paper have become products that are urgently needed in the market. However, acrylates have the common problem of being hot and viscous and cold and brittle. For application scenarios with high anti-adhesion requirements, it is difficult to overcome the problem of high-temperature re-adhesion. This defect limits its application, especially in pressure-sensitive adhesives and wood coatings. At present, the two main ways to solve this problem at home and abroad are to add wax emulsions or nano-silicon and increase its intramolecular / intermolecular crosslinking; but the cost is necessarily expensive. Therefore, the market urgently needs a low-priced, excellent anti-adhesion, and well-compatible resin to solve this problem. Summary of the invention

[0003] In view of the problems existing in the prior art, the present invention provides a method for preparing a non-film-forming and highly anti-adhesive styrene acrylic core-shell emulsion.

[0004] In order to solve the above technical problems, the present invention adopts the following technical solution: a non-film-forming and highly anti-adhesive styrene acrylic core-shell emulsion, comprising the following material compositions in parts by weight:

[0005] Hard monomer 60-85 parts

[0006] Soft monomer 10-20 parts

[0007] Functional monomer 2-5 copies

[0008] Cross-linking monomer 3-7 parts

[0009] Silane coupling agent 0.5-1.2 parts

[0010] 1.5-2.2 parts of polymerizable emulsifier

[0011] Initiator 0.25-1 part

[0012] Oxidant 0.2-0.6 parts

[0013] Reducing agent 0.1-0.3 parts

[0014] 2-4 parts ammonia water

[0015] Antibacterial agent 0.005-3 parts

[0016] 60-100 parts of deionized water

[0017] The hard monomer is one or more of styrene, α-methylstyrene, methyl methacrylate, tert-butyl methacrylate, and isobornyl methacrylate;

[0018] The soft monomer is one or more of n-butyl acrylate, isooctyl acrylate, 2-ethylhexyl acrylate, and lauryl acrylate;

[0019] The cross-linking monomer is one or more of ethylene glycol dimethacrylate, diethylene glycol dimethacrylate, γ-aminopropyl triethoxysilane, hydroxyethyl acrylamide, hydroxymethyl acrylamide, and polyethylene glycol (400) dimethacrylate;

[0020] The polymerizable emulsifier is ammonium allyl fatty alcohol sulfate and / or sodium allyl fatty alcohol sulfate.

[0021] Preferably, 0.4 to 1 part of a chain transfer agent is further included, wherein the chain transfer agent is one or more of n-dodecyl mercaptan, isododecyl mercaptan, and dimethyl styrene diode.

[0022] Preferably, the functional monomer is one or more of acrylic acid, methacrylic acid, itaconic acid, hydroxyethyl methacrylate, and hydroxypropyl methacrylate.

[0023] Preferably, the oxidant is tert-butyl hydroperoxide; the reducing agent is one or more of ascorbic acid, isoascorbic acid, bleaching agent, sodium sulfite, Brüggemann FF6M; the initiator is one or more of potassium persulfate and ammonium persulfate; the bactericide is one or more of methylisothiazolinone and 1,2-benzisothiazolin-3-one.

[0024] Preferably, the silane coupling agent is one or more of γ-aminopropyltriethoxysilane, γ-glycidyloxypropyltrimethoxysilane and γ(methacryloyloxy)propyltrimethoxysilane.

[0025] As a preference, the mass parts of each substance composition are as follows:

[0026] 4-8 parts of n-butyl acrylate, 6-9 parts of 2-ethylhexyl acrylate, 20-28 parts of styrene, 30-45 parts of methyl methacrylate, 8-12 parts of alpha-methyl styrene, 2-5 parts of acrylic acid, 1.5-2.2 parts of polymerizable emulsifier, 0.5-1.2 parts of silane coupling agent, 3-7 parts of cross-linking monomer, 0.4-1 parts of chain transfer agent, 0.25-1 parts of initiator, 0.2-0.6 parts of oxidant, 0.1-0.3 parts of reducing agent, 0.005-0.3 parts of antibacterial agent, 2-4 parts of ammonia water and 60-100 parts of deionized water.

[0027] The present invention also provides a method for preparing the non-film-forming and highly anti-adhesive styrene acrylic core-shell emulsion, comprising the following steps:

[0028] Step S1, preparation of pre-emulsion:

[0029] 20-50 parts of hard monomer, 2-10 parts of soft monomer, 0.5-2 parts of crosslinking monomer, 2-5 parts of functional monomer and 0.6-1.5 parts of polymerizable emulsifier are added to deionized water, and emulsified in a high-speed homogenizing emulsifier to obtain a core layer pre-emulsion;

[0030] 25-40 parts of hard monomer, 5-10 parts of soft monomer, 2-5 parts of crosslinking monomer, 0.2-0.8 parts of chain transfer agent, 0.5-1.2 parts of silane coupling agent and 0.1-0.5 parts of polymerizable emulsifier are added into deionized water, and emulsified in a high-speed homogenizing emulsifier to obtain a shell pre-emulsion;

[0031] Step S2, preparation of kettle bottom liquid: add an appropriate amount of polymerizable emulsifier to deionized water, stir and dissolve to obtain kettle bottom liquid, which is set aside; in addition, add 0.2-0.6 parts of initiator to deionized water, stir and dissolve to prepare an initiator solution, which is set aside;

[0032] Step S3, core emulsion polymerization: the bottom liquid of the kettle is heated to 80±3°C under stirring, and then part of the initiator solution is added thereto, and the temperature is kept for at least 15 minutes; then, the core layer pre-emulsion liquid obtained in step S2 is added dropwise to the reactor at a stirring speed of 150-200 rpm, and the dropping time is controlled to be 1.5-2.5 hours. After the dropping is completed, an appropriate amount of ammonia water is added to neutralize and stir evenly;

[0033] Step S4, shell emulsion polymerization: continue to add the shell pre-emulsion obtained in step S1 and the remaining initiator solution to the reaction system in a dropwise manner, and control the dropwise addition to be completed within 1.5-2.5 hours; after the dropwise addition is completed, keep the reaction at 75-80°C for 1-2 hours, and then cool to 70±3°C;

[0034] Step S5, then, simultaneously adding the oxidant and the reductant to the reaction system dropwise within 40±10 minutes, keeping the temperature for 30-50 minutes, raising the temperature to 85±3°C and keeping the temperature for at least 1 hour; finally, cooling the temperature to below 40°C, adding the bactericide, and stirring evenly to obtain a non-film-forming and highly anti-adhesive styrene acrylic core-shell emulsion;

[0035] Preferably, the components of the core layer pre-emulsion in step S1 are as follows: 25 parts of methyl methacrylate, 10 parts of styrene, 5 parts of n-butyl acrylate, 1 part of ethylene glycol dimethacrylate or dimethacrylate, and 3 parts of acrylic acid;

[0036] The components of the shell pre-emulsion are as follows: 15 parts of styrene, 10 parts of α-methylstyrene, 8-18 parts of methyl methacrylate, 7 parts of isooctyl acrylate, 3 parts of diethylene glycol dimethacrylate, 1 part of hydroxyethyl acrylamide, 1 part of γ-aminopropyl triethoxysilane, and 0.5 parts of dimethylstyrene diode.

[0037] Beneficial effects. Compared with the prior art, the present invention has the following advantages: 1. By designing the core-shell structure, the transition layer between the core and the shell forms an inter-transfer network structure, and intermolecular and intramolecular crosslinking is formed inside and outside the core and the shell, thereby improving the resistance to boiling, adhesion and ethanol migration. Self-crosslinking monomers and silicon-modified self-crosslinking monomers are used in the shell layer, so that the paint film can be further crosslinked after film formation to form a denser spatial network structure, thereby having better anti-adhesion performance. 2. Chain transfer agents are used to reduce the degree of branching, so that the ends of the molecular chains have a certain degree of crosslinking while having a lower degree of branching, so that the molecular chains have better regularity, thereby having better resistance to boiling and lower ethanol migration. 3. The formulation process is simple, the cost is low, the emulsion has high stability, can be produced and scaled up repeatedly, and has good compatibility and universality, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] In order to more clearly illustrate the technical solution of the embodiment of the present invention, the following is a brief introduction to the drawings required for describing the embodiment. Among them:

[0039] Figure 1 This is the infrared spectrum of the non-film-forming and highly anti-adhesive styrene acrylic core-shell emulsion;

[0040] Figure 2 It is a differential scanning calorimetry curve of non-film-forming and highly anti-adhesive styrene acrylic core-shell emulsion;

[0041] Figure 3 This is the particle size and distribution diagram of the non-film-forming and highly anti-adhesive styrene acrylic core-shell emulsion. DETAILED DESCRIPTION

[0042] The present invention is further illustrated below in conjunction with the accompanying drawings and specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. After reading the present invention, modifications to various equivalent forms of the present invention by those skilled in the art all fall within the scope defined by the appended claims of the present application.

[0043] Description of the relationship between the Chinese names and English abbreviations of the substances involved in the present invention:

[0044]

[0045] 1. Preparation of non-film-forming and highly anti-adhesive styrene acrylic core-shell emulsion

[0046] Example 1

[0047] Step S1, preparation of pre-emulsion: adding 25 parts of methyl methacrylate, 5 parts of n-butyl acrylate, 3 parts of acrylic acid and 10 parts of styrene monomer and 0.3 parts of polymerizable emulsifier into 30 parts of deionized water, and emulsifying them in a high-speed homogenizing emulsifier at a speed of 1500 r / min to form a core layer pre-emulsion A; similarly, adding 15 parts of styrene, 18 parts of methyl methacrylate, 7 parts of n-butyl acrylate, 0.3 parts of polymerizable emulsifier and 30 parts of deionized water; emulsifying them in a high-speed homogenizing emulsifier at a speed of 1500 r / min to form a shell layer pre-emulsion B;

[0048] Step S2, preparation of polymerization reaction stock solution: 1.2 parts of polymerizable emulsifier are taken into a reaction kettle, 80 parts of deionized water are added, and the mixture is stirred and dissolved at 40±3° C.; the mixture is prepared into a kettle bottom solution C for standby use; 0.3 parts of potassium persulfate are weighed and dissolved in 20 parts of deionized water to prepare an initiator solution D for standby use;

[0049] Step S3, core emulsion polymerization: the bottom liquid C of the reactor is heated to 80±3°C at a speed of 250rpm / min, and then 1 / 2 of the initiator solution D is added to the bottom liquid C of the reactor, and the temperature is kept for 15min; then the core layer pre-emulsified liquid obtained in step S1 is added dropwise to the bottom liquid of the reactor, and the addition is completed over 2h. After the addition is completed, 2 parts of ammonia water are added to neutralize and stirred for 10min;

[0050] Step S4, shell emulsion polymerization: continue to drip the shell pre-emulsion obtained in step S1 and the remaining 1 / 2 of the initiator solution D into the reaction system at the same time, and drip it for 2 hours; after the dripping is completed, keep the reaction at 80°C for 1.5 hours, and then cool it to 70±3°C;

[0051] Step S5, then, 0.4 parts of oxidant TBHP and 0.2 parts of reducing agent FF6M are respectively diluted with 4 parts of deionized water, and then simultaneously added dropwise to the reaction system within 40±10 minutes, and after keeping warm for 40 minutes, the temperature is raised to 85±3° C. and kept warm for 1 hour; finally, the temperature is lowered to below 40° C., 0.01 parts of antibacterial agent MIT is added, and the mixture is stirred evenly to obtain a non-film-forming and highly anti-adhesive styrene acrylic core-shell emulsion, which has a slightly white and bluish appearance;

[0052] Embodiment 2-8

[0053] Compared with Example 1, the difference of this example is that the types and addition amounts of the reaction materials are different, as shown in Tables 1 and 2 for details.

[0054] Example 9

[0055] Compared with Example 1, the difference of this example is that, in addition to the different types and addition amounts of the reaction materials, there are also the following differences in the preparation process: the core layer and shell layer monomers are pre-emulsified and added dropwise, the core layer is added dropwise first, and then the shell layer is added dropwise. In this process, when the shell layer monomer is added dropwise by 70%, 3 parts of diethylene glycol dimethacrylate, 1 part of γ-aminopropyl triethoxysilane, 1 part of hydroxyethyl acrylamide, and dimethyl styrene diode are pre-emulsified together and then continued to be added dropwise, and the initiator is added dropwise simultaneously.

[0056] Table 1 shows the addition amount of each component of the core layer pre-emulsion in each embodiment.

[0057]

[0058] Table 2 shows the addition amount of each component of the shell pre-emulsion in each embodiment.

[0059]

[0060] The non-film-forming high anti-adhesive styrene acrylic core-shell emulsion obtained in each example was prepared into a cured film according to the following method to test various properties:

[0061] First, the substrate selection: special test paper (Golden Sun 210g / m2 uncoated food base paper) (Note: the test paper sample size is 10cm*5cm), special test glass plate (75*25*1mm slide).

[0062] Emulsion preparation: Use low Tg film-forming resin (optionally homemade) to assist film formation, and match it with non-film-forming, highly anti-adhesive styrene acrylic core-shell emulsion to prepare a mixed emulsion for polar application performance testing, with a mass ratio of (6.5:3.5).

[0063] Finally, use OSP-15# wire rod to coat the test paper with a dry coating weight of about 5-7g / ㎡, number the test paper samples according to the serial number, and then put the test paper samples into an oven set at 120℃, and place each numbered paper sample for 50 seconds to solidify into a film.

[0064] 2. Performance Test

[0065] The cured film prepared by the above method was tested for hot water resistance, oil resistance and anti-rebound performance. The test methods for each performance are as follows:

[0066] Water resistance test: According to the provisions of GB / T1733-1993 "Determination of water resistance of paint film", the test can meet the requirements of water boiling resistance in normal use scenarios. In addition, the present invention also uses the following more intuitive method for detection: Take a glass slide sample coated with barrier resin prepared according to the above method. Put it in a hot water thermostat box with a temperature of (70±5)℃, and the liquid surface completely immerses the glass substrate. Take it out after 2 hours, dry it with filter paper, and record whether the paint film has loss of gloss, discoloration, blistering, wrinkling, shedding, rusting and other phenomena and the recovery time. 3 samples are measured for each sample. The test results show that it does not turn white after 2 hours of water boiling, the surface does not lose gloss, fall off, wrinkle or bubble, and the water boiling resistance is excellent.

[0067] The 95% ethanol migration test refers to the test specified in GB31604.8-2016 and can meet the migration requirements for food contact materials.

[0068] Heat-resistance test: Take a paper sample coated with barrier resin prepared according to the above method, cut it into square pieces of 5 cm in length and width, and stack them together with the coating surface facing the coating surface (face to face) and the back of the paper facing the coating surface (back to back), press it with a 5KG weight, put it in a 60℃ oven for 6 hours, take it out and cool it down, and both the face to face and the back to back can fall off naturally, which can meet the high heat-resistance requirements of the barrier coating. The test results of the properties of the cured films obtained in each embodiment are shown in Table 3.

[0069] Table 3 is the test results of the cured film properties obtained in each embodiment

[0070]

[0071] From the test results of each embodiment, it can be seen that:

[0072] Example 1: When no cross-linking agent and a monomer with greater steric hindrance are used, the anti-adhesion and water boiling resistance are poor, and the migration amount of 95% ethanol is large.

[0073] Examples 2 and 3: By comparing Examples 2 and 3, it can be found that the use of a soft monomer with large steric hindrance - isooctyl acrylate and a rigid monomer with large steric hindrance - α-methylstyrene in the shell layer can reduce the degree of freedom by restricting the internal rotation of the single bond, thereby reducing the flexibility of the chain segment to improve its anti-adhesion performance.

[0074] Embodiment 4, 5 and 6: By comparing embodiment 4 / 5 and 6, it can be found that by using diethylene glycol dimethacrylate, an internal cross-linking monomer with a certain hydrophilicity, in the core layer, the shell layer and the core-shell layer, a spatial network three-dimensional structure can be formed inside the molecular chain segment to form a certain degree of chemical cross-linking. The cross-linking monomer can bridge the molecular chain segments and form a staggered grid structure between the molecular chains through the cross-linking points. At the same time, the ethoxy group of the internal cross-linking monomer has a certain hydrophilicity and can form hydrogen bonds between molecules to form physical cross-linking. In addition, the internal cross-linking monomer of the core-shell layer will form an interpenetrating network structure in the core-shell layer for transition, so that the transition layer between the core and shell also has strength and density, thereby having better anti-sticking performance, water boiling resistance and lower ethanol migration.

[0075] Example 7: It can be found from Example 7 that further use of a self-crosslinking external crosslinking monomer hydroxyethyl acrylamide and a certain amount of external crosslinking silicon-modified silane coupling agent in the shell layer can further crosslink and cure after the emulsion is constructed and film-formed, so that the paint film has lower segment flexibility and chain rotation freedom, thereby making the paint film surface have better anti-stick properties.

[0076] Example 8: It can be found from Example 8 that using a certain amount of chain transfer agent in the shell layer will reduce the degree of branching while giving the polymer chain segments a certain degree of crosslinking, so that the chain segments have a certain regularity and repeatability, and the paint film can have better water boiling resistance and anti-stick properties.

[0077] Example 9: It can be found from Example 9 that by using a new dropping process, pre-emulsifying and dropping the internal and external crosslinking agents and chain transfer agents in the later stage of dropping, the crosslinking can be distributed as evenly as possible on the outer surface of the core-shell structure shell, and the outer surface has a lower degree of branching, thereby having better anti-sticking properties, water boiling resistance and lower ethanol migration.

[0078] The main innovations of the present invention are:

[0079] 1. By designing the core-shell structure, the transition layer between the core and shell forms an interpenetrating network structure, and intermolecular and intramolecular crosslinking is formed inside and outside the core and shell, thereby improving the resistance to boiling, adhesion and ethanol migration. Self-crosslinking monomers and silicon-modified self-crosslinking monomers are used in the shell layer, so that the paint film can be further cross-linked after film formation to form a denser spatial network structure, thereby having better anti-adhesion properties.

[0080] 2. Use chain transfer agents to reduce the degree of branching, so that the molecular chain ends have a certain degree of crosslinking while having a lower degree of branching, so that the molecular chain has better regularity, thus having better water boiling resistance and lower ethanol migration.

[0081] 3. The formulation process is simple, the cost is low, the emulsion has high stability, can be produced and scaled up repeatedly, and has good compatibility and universality, and has broad application prospects.

Claims

1. A method for preparing a non-film-forming, highly anti-adhesive styrene acrylic core-shell emulsion, characterized in that The following steps are involved: Step S1, preparation of pre-emulsion: 25 parts of methyl methacrylate, 10 parts of styrene, 5 parts of n-butyl acrylate, 1 part of ethylene glycol dimethacrylate, 3 parts of acrylic acid and 0.6-1.5 parts of a polymerizable emulsifier are added to deionized water, and emulsified in a high-speed homogenizing emulsifier to obtain a core layer pre-emulsion; 15 parts of styrene, 10 parts of α-methylstyrene, 8-18 parts of methyl methacrylate, 7 parts of isooctyl acrylate, 3 parts of diethylene glycol dimethacrylate, 1 part of hydroxyethyl acrylamide, 1 part of γ-aminopropyl triethoxysilane, 0.5 parts of α-methylstyrene dimer and 0.1-0.5 parts of a polymerizable emulsifier are added to deionized water, and emulsified in a high-speed homogenizing emulsifier to obtain a shell pre-emulsion; Step S2, preparation of kettle bottom liquid: add an appropriate amount of polymerizable emulsifier to deionized water, stir and dissolve to obtain kettle bottom liquid, which is set aside; in addition, add 0.2-0.6 parts of initiator to deionized water, stir and dissolve to prepare an initiator solution, which is set aside; Step S3, core emulsion polymerization: the bottom liquid of the kettle is heated to 80±3°C under stirring, and then part of the initiator solution is added thereto, and the temperature is kept for at least 15 minutes; then, the core layer pre-emulsion liquid obtained in step S1 is added to the reactor in a dropwise manner at a stirring speed of 150-200 rpm, and the dropping time is controlled to be 1.5-2.5 hours. After the dropping is completed, an appropriate amount of ammonia water is added to neutralize and stir evenly; Step S4, shell emulsion polymerization: continue to add the shell pre-emulsion obtained in step S1 and the remaining initiator solution to the reaction system in a dropwise manner, and control the dropwise addition to be completed within 1.5-2.5 hours; after the dropwise addition is completed, keep the reaction at 75-80°C for 1-2 hours, and then cool to 70±3°C; Step S5, then, simultaneously adding the oxidant and the reductant to the reaction system dropwise within 40±10 min, keeping the temperature for 30-50 min, raising the temperature to 85±3° C. and keeping the temperature for at least 1 h; finally, cooling the temperature to below 40° C., adding the antibacterial agent, and stirring evenly to obtain a non-film-forming and highly anti-adhesive styrene acrylic core-shell emulsion; The polymerizable emulsifier is ammonium allyl fatty alcohol sulfate and / or sodium allyl fatty alcohol sulfate.

2. The method for preparing the non-film-forming high anti-adhesive styrene acrylic core-shell emulsion according to claim 1, characterized in that: The oxidant is tert-butyl hydroperoxide; the reducing agent is one or more of ascorbic acid, isoascorbic acid, bleaching agent, sodium sulfite, and Brüggemann FF6M; the initiator is one or more of potassium persulfate and ammonium persulfate; and the antibacterial agent is one or more of methylisothiazolinone and 1,2-benzisothiazolin-3-one.