A UV-curable nanoimprint material and manufacturing process

Through the combination of specific components and process steps, ultraviolet curing nanoimprinted materials with high UV curing activity and good interface affinity are formed, solving the problem of insufficient mechanical properties and thermal stability of existing materials and achieving high precision and stable imprinting effect at high temperatures.

CN117806122BActive Publication Date: 2024-11-22GERMANLITHO CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311850788.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-29
Publication Date
2024-11-22
Estimated Expiration
2043-12-29

AI Technical Summary

Technical Problem

The existing ultraviolet cured nanoimprint materials have low mechanical properties and poor thermal stability, making it difficult to meet the imprinting needs in high-precision and high-temperature environments.

Method used

Using 4-methylaminopyridine, sulfonic acid compounds, initiators, thioglycolic acid, silane compounds, triethylamine and aliphatic polyurethane acrylate, the high UV curing activity and good Interface affinity for ultraviolet curing nanoimprinting materials.

Benefits of technology

It improves the mechanical properties and thermal stability of the material, and achieves stable performance maintenance and high-precision imprinting effect in high-temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004640960420000141
    Figure BDA0004640960420000141
Patent Text Reader

Abstract

The invention discloses a material and manufacturing process for ultraviolet light-cured nanoimprinting, which comprises dissolving 4-methylaminopyridine and a sulfonic acid compound in toluene to obtain a powder, preparing a pretreatment initiator and a grafting initiator, and mixing aliphatic polyurethane acrylate, a lipid compound, a pretreatment triethoxysilane and a grafting initiator to form a solution. The material finally obtained can be used for nanoimprinting technology. Compared with the prior art, the process is simple and has good controllability, and also has good thermal stability and tensile strength, and provides an effective method for the preparation of ultraviolet light-cured nanoimprinting materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of ultraviolet light curing materials, and in particular to an ultraviolet light curing nanoimprint material and a manufacturing process. Background Art

[0002] UV curing technology is a fast curing technology commonly used in the fields of coatings, inks, adhesives, etc. It uses ultraviolet light to activate photosensitizers, triggering chemical reactions, so that the coating or adhesive cures into a hard and wear-resistant state in a short time. Compared with traditional thermal curing or chemical curing methods, UV curing has the characteristics of fast curing, solvent-free and environmentally friendly, excellent performance, and fine control. It greatly improves production efficiency, reduces the emission of volatile organic compounds, is more environmentally friendly, has excellent wear resistance, chemical resistance, heat resistance and optical transparency, and achieves precise control of curing speed and performance.

[0003] UV-curable nanoimprint materials are materials designed for nanoimprint technology, combining the characteristics of UV-curing technology and nano-scale materials. It is usually composed of the following components: matrix material, nanoparticles, photosensitizer, and auxiliary additives. The matrix material is the main body of the UV-curable nanoimprint material, which can be a polymer, resin or adhesive. The matrix material is quickly cured under the irradiation of ultraviolet light to form a solid structure. Nanoparticles are tiny particles added to the matrix material with specific shapes, sizes and surface properties. These nanoparticles can be used to achieve nanoscale patterns and structures, providing high-resolution and precise imprinting effects. Photosensitizers are key components in the UV-curing process, which can absorb ultraviolet light and initiate chemical reactions. The selection and concentration of photosensitizers affect the curing speed and performance parameters. Auxiliary additives can be used to adjust the material's viscosity, fluidity, adhesion and wear resistance to meet the requirements of specific applications.

[0004] UV-curable nanoimprint materials can be used in various fields, such as microelectronics manufacturing, optical component preparation, biosensors, etc. They can achieve rapid replication and high-precision processing of fine patterns through nanoimprint technology, providing an effective tool for the preparation of nanoscale devices and structures.

[0005] China's authorized invention patent CN103279011B discloses a mercapto-olefin UV-curable nanoimprint material, which is composed of a low-viscosity, multi-functional liquid prepolymer, a photoinitiator, an auxiliary agent and a diluent. The low-viscosity, multi-functional liquid prepolymer is composed of a (silicon-containing) mercapto monomer and a (silicon-containing) olefin monomer. Both the (silicon-containing) mercapto monomer and the (silicon-containing) olefin monomer contain two or more curable cross-linking functional groups, and the curable cross-linking functional groups are mercapto or carbon-carbon unsaturated double bonds. The liquid prepolymer accounts for 5%-90% of the total mass of the material, the mass of the diluent accounts for 95%-10% of the total mass of the material, the mass of the photoinitiator is 1%-5% of the mass of the liquid prepolymer, and the mass of the auxiliary agent is 0.01%-10% of the mass of the liquid prepolymer. The invention has the characteristics of low viscosity, fast curing, complete curing in air, and low shrinkage. Based on the spin coating process, it can be used as a UV-curable nanoimprint adhesive to achieve large-area UV-curable nanoimprinting and economically and efficiently produce patterns with key dimensions less than 100 nanometers. However, the mechanical properties of the UV-curable nanoimprint material prepared by the invention are low and the thermal stability is poor. Summary of the invention

[0006] In view of the deficiencies in the prior art, the technical problem to be solved by the present invention is to provide a UV-curable nanoimprint material and a manufacturing process having high mechanical properties and thermal stability.

[0007] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solutions:

[0008] A manufacturing process of a UV-curable nanoimprint material is as follows:

[0009] Step 1, dissolving 4-methylaminopyridine and a sulfonic acid compound in hot toluene respectively, then mixing with stirring while keeping warm, cooling to room temperature, and vacuum filtering and drying to obtain a powder;

[0010] Step 2, adding the initiator, thioglycolic acid and the powder prepared in step 1 to toluene, stirring under high temperature reflux overnight under nitrogen atmosphere, and then removing toluene from the reactant by rotary evaporation under reduced pressure to obtain a crude product, diluting it with dichloromethane, and then washing it with a saturated sodium bicarbonate aqueous solution and water respectively, collecting the organic phase and drying it with anhydrous magnesium sulfate overnight to obtain a pretreated initiator;

[0011] Step 3, mixing the silane compound, the pre-treated initiator prepared in step 2, triethylamine and dichloromethane, and stirring under a nitrogen atmosphere to obtain a grafting initiator;

[0012] Step 4, stirring and mixing triethoxysilane, water and anhydrous ethanol, standing the mixture to clarify, adding hydrochloric acid while stirring, and leaving the mixture at room temperature overnight to obtain pretreated triethoxysilane;

[0013] Step 5: Mix and stir the aliphatic polyurethane acrylate, lipid compound, pretreated triethoxysilane and the grafting initiator prepared in step 3 until a uniform solution is formed, and then maintain vacuum to remove bubbles formed during the stirring process to obtain a UV-curable nanoimprint material.

[0014] Preferably, the manufacturing process of the UV-curable nanoimprint material is as follows, in parts by weight:

[0015] Step 1, dissolving 8 to 12 parts of 4-methylaminopyridine and 8 to 12 parts of a sulfonic acid compound in 80 to 120 parts of toluene at 60 to 80° C., then stirring and mixing for 1 to 3 hours, cooling to room temperature, and vacuum filtering and drying to obtain a powder;

[0016] Step 2, adding 20 to 30 parts of initiator, 8 to 13 parts of thioglycolic acid and 0.5 to 0.8 parts of the powder prepared in step 1 to 80 to 120 parts of toluene, refluxing and stirring at 110 to 130° C. under a nitrogen atmosphere overnight, then removing toluene from the reactants by rotary evaporation under reduced pressure, diluting the obtained crude product with 70 to 90 parts of dichloromethane, and then washing with 400 to 600 parts of saturated sodium bicarbonate aqueous solution and 200 to 400 parts of water respectively, collecting the organic phase and drying it with anhydrous magnesium sulfate overnight to obtain a pretreated initiator;

[0017] Step 3, 4 to 6 parts of the silane compound, 5 to 7 parts of the pre-treated initiator prepared in step 2, 0.1 to 0.3 parts of triethylamine and 25 to 35 parts of dichloromethane are mixed, and stirred at 30 to 50° C. for 1 to 3 hours under a nitrogen atmosphere to obtain a grafting initiator;

[0018] Step 4, 18 to 22 parts of triethoxysilane, 4 to 6 parts of water and 8 to 10 parts of anhydrous ethanol are stirred and mixed for 1 to 3 hours, and after the mixture is allowed to stand and clarified, 0.1 to 0.3 parts of 5 to 20 wt % hydrochloric acid are added under stirring, and the mixture is left at room temperature overnight to obtain pretreated triethoxysilane;

[0019] Step 5: Mix and stir 35-45 parts of aliphatic polyurethane acrylate, 8-12 parts of lipid compounds, 0.7-0.9 parts of pretreated triethoxysilane and 0.7-0.9 parts of the grafting initiator prepared in step 3 until a uniform solution is formed, and then maintain vacuum at 40-60° C. for 5-15 minutes to remove bubbles formed during the stirring process to obtain a UV-curable nanoimprint material.

[0020] The initiator is at least one of 2-[4-(2-hydroxy-2-methyl-1-oxypropyl)phenoxy]acetic acid, 2-hydroxy-1-[4-(2-hydroxypropoxy)phenyl]-2-methylpropan-1-one, N-acetylmuramyl-L-alanine-D-isoglutamine-L-lysine, and 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone.

[0021] The sulfonic acid compound is at least one of 5-amino-2-chlorotoluene-5-sulfonic acid and p-toluenesulfonic acid.

[0022] The silane compound is at least one of 3-glycidyloxypropyltriethoxysilane and 3-(2,3-epoxypropyloxy)propyltrimethoxysilane.

[0023] The lipid compound is at least one of 1,6-hexanediol dimethacrylate and octadecyl methacrylate.

[0024] A method for using a UV-curable nanoimprint material is as follows:

[0025] S1, prepare the imprinting mold and substrate;

[0026] S2, coating the ultraviolet light curing nanoimprint material on the surface of the imprinting part of the imprinting mold at an ambient temperature of 18 to 25°C;

[0027] S3, using ultraviolet irradiation to perform primary curing on the surface of the imprinting part of the imprinting mold, with an irradiation dose of 800 to 1200 mJ to fix the imprinting material;

[0028] S4, after heating at 90-110° C., using an imprinting mold to imprint the substrate, and then using ultraviolet rays to expose and cure the substrate, with an irradiation dose of 1000-2000 mJ, to obtain an imprinted product.

[0029] In the manufacturing process of the UV-curable nanoimprint material, the role of each raw material is as follows:

[0030] The role of 4-methylaminopyridine and 5-amino-2-chlorotoluene-5-sulfonic acid in step 1 is to participate in the reaction of the subsequent steps as reactants, possibly provide active groups, promote the reaction, and ultimately form the pretreatment initiator and grafting initiator required for preparing UV-curable nanoimprint materials.

[0031] 2-[4-(2-Hydroxy-2-methyl-1-oxypropyl)phenoxy]acetic acid: as one of the reactants, it participates in the reaction and may be used to form a pretreatment initiator.

[0032] 2-Hydroxy-1-[4-(2-hydroxypropoxy)phenyl]-2-methylpropan-1-one: as one of the reactants, it participates in the reaction and may be used to form a pretreatment initiator.

[0033] Thioglycolic acid: As one of the reactants, it participates in the reaction and may be used to form a pretreatment initiator.

[0034] The powder prepared in step 1: as an additive, it may act as a cross-linking agent in the reaction.

[0035] 3-Glycidyloxypropyltriethoxysilane: As one of the reactants, it participates in the reaction and may be used to form a grafting initiator.

[0036] Triethylamine: As one of the reactants, it may be used to adjust the reaction conditions and promote the reaction.

[0037] Dichloromethane: As a solvent, it is used to provide a reaction medium for the reaction and adjust the concentration of the reaction system.

[0038] Triethoxysilane: As one of the reactants, it participates in the reaction and may be used to form pre-treated triethoxysilane.

[0039] Anhydrous ethanol: may be used to adjust reaction conditions and promote the reaction.

[0040] Hydrochloric acid: used to adjust reaction conditions and promote the reaction.

[0041] Aliphatic polyurethane acrylate: As the main matrix material, it provides the basic properties and characteristics of the material.

[0042] Octadecanyl methacrylate: May participate in the reaction and be used to adjust the performance and characteristics of the material.

[0043] Compared with the prior art, the present invention has the following beneficial effects:

[0044] 1) The UV-curable nanoimprint material prepared by the present invention has good interface affinity and can form good contact with the surface of the nano-mold, which is beneficial to the transfer and replication of the imprint process.

[0045] 2) The UV-curable nanoimprint material prepared by the present invention has high UV-curing activity. Under UV irradiation, the material can be quickly cured and hardened, thereby realizing a fast nanoimprint process.

[0046] 3) The imprinted product obtained by using the UV-curable nanoimprint material prepared by the present invention has good thermal stability and can maintain its performance in a high temperature environment.

[0047] 4) The imprinted product obtained by using the UV-curable nanoimprint material prepared by the present invention increases the cross-linking points of the material, strengthens the network structure of the material, and thus improves its mechanical properties. Therefore, the prepared material may have a higher tensile strength, which helps to cope with stress and deformation during the imprinting process. DETAILED DESCRIPTION

[0048] Main sources of substances:

[0049] Aliphatic polyurethane acrylate: Shanghai Zhenlishi Network Technology Co., Ltd., product number: EBECRYL 1290.

[0050] 2-[4-(2-Hydroxy-2-methyl-1-oxopropyl)phenoxy]acetic acid: English name: 2-[4-(2-Hydroxy-2-methyl-1-oxopropyl)phenoxy]acetic acid, CAS: 119462-61-2.

[0051] N-Acetylmuramyl-L-alanine-D-isoglutaminyl-L-lysine: English name: N-Acetylmuramyl-L-alanyl-D-isoglutaminyl-L-lysin, CAS: 56816-17-2.

[0052] 2-Hydroxy-1-[4-(2-hydroxypropoxy)phenyl]-2-methylpropan-1-one: English name: 2-hydroxy-1-[4-(2-hydroxypropoxy)phenyl]-2-methyl-propan-1-one, CAS: 700368-63-4.

[0053] Example 1

[0054] A manufacturing process of a UV-curable nanoimprint material is as follows:

[0055] Step 1, dissolve 10 g of 4-methylaminopyridine and 10 g of 5-amino-2-chlorotoluene-5-sulfonic acid in 100 g of 70° C. toluene, then stir and mix for 2 h, cool to room temperature, and vacuum filter and dry to obtain a powder;

[0056] Step 2, adding 25g of 2-[4-(2-hydroxy-2-methyl-1-oxypropyl)phenoxy]acetic acid, 11g of mercaptoacetic acid and 0.7g of the powder prepared in step 1 to 100g of toluene, reflux and stir at 125°C under a nitrogen atmosphere overnight, then removing toluene from the reactant by rotary evaporation under reduced pressure to obtain a crude product, diluting it with 80g of dichloromethane, then washing it with 500g of a saturated sodium bicarbonate aqueous solution and 300g of water, respectively, collecting the organic phase and drying it with anhydrous magnesium sulfate overnight to obtain a pretreated initiator;

[0057] Step 3, 5 g of 3-glycidyloxypropyltriethoxysilane, 6 g of the pre-treated initiator prepared in step 2, 0.2 g of triethylamine and 30 g of dichloromethane were mixed, and stirred at 40° C. for 2 h under a nitrogen atmosphere to obtain a grafting initiator;

[0058] Step 4, 20 g of triethoxysilane, 5 g of water and 9 g of anhydrous ethanol were stirred and mixed for 2 h, and after the mixture was allowed to stand to clarify, 0.2 g of 10 wt % hydrochloric acid was added under stirring, and the mixture was left at room temperature overnight to obtain pretreated triethoxysilane;

[0059] Step 5: Mix and stir 40 g of aliphatic polyurethane acrylate, 10 g of octadecyl methacrylate, 0.8 g of pretreated triethoxysilane and 0.8 g of the grafting initiator prepared in step 3 until a uniform solution is formed, and then maintain it in vacuum at 50° C. for 10 min to remove bubbles formed during the stirring process to obtain a UV-curable nanoimprint material.

[0060] A method for using a UV-curable nanoimprint material is as follows:

[0061] S1, prepare the imprinting mold and substrate;

[0062] S2, coating the ultraviolet light curing nanoimprint material on the surface of the imprint part of the imprint mold at an ambient temperature of 20°C;

[0063] S3, using ultraviolet irradiation to perform primary curing on the surface of the imprinting part of the imprinting mold, with an irradiation dose of 1000mJ to fix the imprinting material;

[0064] S4. After heating at 100° C., the substrate is imprinted using an imprinting mold, and then the substrate is exposed and cured using ultraviolet rays with an irradiation dose of 1200 mJ to obtain an imprinted product.

[0065] Example 2

[0066] A manufacturing process of a UV-curable nanoimprint material is as follows:

[0067] Step 1, dissolve 10 g of 4-methylaminopyridine and 10 g of 5-amino-2-chlorotoluene-5-sulfonic acid in 100 g of 70° C. toluene, then stir and mix for 2 h, cool to room temperature, and vacuum filter and dry to obtain a powder;

[0068] Step 2, adding 25g of 2-hydroxy-1-[4-(2-hydroxypropoxy)phenyl]-2-methylpropane-1-one, 11g of mercaptoacetic acid and 0.7g of the powder prepared in step 1 to 100g of toluene, refluxing with stirring at 125°C under a nitrogen atmosphere overnight, then removing toluene from the reactant by rotary evaporation under reduced pressure to obtain a crude product, diluting with 80g of dichloromethane, then washing with 500g of a saturated sodium bicarbonate aqueous solution and 300g of water, respectively, collecting the organic phase and drying it with anhydrous magnesium sulfate overnight to obtain a pretreated initiator;

[0069] Step 3, 5 g of 3-glycidyloxypropyltriethoxysilane, 6 g of the pre-treated initiator prepared in step 2, 0.2 g of triethylamine and 30 g of dichloromethane were mixed, and stirred at 40° C. for 2 h under a nitrogen atmosphere to obtain a grafting initiator;

[0070] Step 4, 20 g of triethoxysilane, 5 g of water and 9 g of anhydrous ethanol were stirred and mixed for 2 h, and after the mixture was allowed to stand to clarify, 0.2 g of 10 wt % hydrochloric acid was added under stirring, and the mixture was left at room temperature overnight to obtain pretreated triethoxysilane;

[0071] Step 5: Mix and stir 40 g of aliphatic polyurethane acrylate, 10 g of octadecyl methacrylate, 0.8 g of pretreated triethoxysilane and 0.8 g of the grafting initiator prepared in step 3 until a uniform solution is formed, and then maintain it in vacuum at 50° C. for 10 min to remove bubbles formed during the stirring process to obtain a UV-curable nanoimprint material.

[0072] The method of using the UV-curable nanoimprint material is the same as that in Example 1.

[0073] Example 3

[0074] A manufacturing process of a UV-curable nanoimprint material is as follows:

[0075] Step 1, dissolve 10 g of 4-methylaminopyridine and 10 g of 5-amino-2-chlorotoluene-5-sulfonic acid in 100 g of 70° C. toluene, then stir and mix for 2 h, cool to room temperature, and vacuum filter and dry to obtain a powder;

[0076] Step 2, adding 25g of N-acetyl wall acyl-L-alanine-D-isoglutamine-L-lysine, 11g of thioglycolic acid and 0.7g of the powder prepared in step 1 to 100g of toluene, stirring at reflux at 125°C overnight under a nitrogen atmosphere, then removing toluene from the reactant by rotary evaporation under reduced pressure to obtain a crude product, diluting it with 80g of dichloromethane, then washing it with 500g of a saturated sodium bicarbonate aqueous solution and 300g of water, respectively, collecting the organic phase and drying it with anhydrous magnesium sulfate overnight to obtain a pre-treated initiator;

[0077] Step 3, 5 g of 3-glycidyloxypropyltriethoxysilane, 6 g of the pre-treated initiator prepared in step 2, 0.2 g of triethylamine and 30 g of dichloromethane were mixed, and stirred at 40° C. for 2 h under a nitrogen atmosphere to obtain a grafting initiator;

[0078] Step 4, 20 g of triethoxysilane, 5 g of water and 9 g of anhydrous ethanol were stirred and mixed for 2 h, and after the mixture was allowed to stand to clarify, 0.2 g of 10 wt % hydrochloric acid was added under stirring, and the mixture was left at room temperature overnight to obtain pretreated triethoxysilane;

[0079] Step 5: Mix and stir 40 g of aliphatic polyurethane acrylate, 10 g of octadecyl methacrylate, 0.8 g of pretreated triethoxysilane and 0.8 g of the grafting initiator prepared in step 3 until a uniform solution is formed, and then maintain it in vacuum at 50° C. for 10 min to remove bubbles formed during the stirring process to obtain a UV-curable nanoimprint material.

[0080] The method of using the UV-curable nanoimprint material is the same as that in Example 1.

[0081] Example 4

[0082] A manufacturing process of a UV-curable nanoimprint material is as follows:

[0083] Step 1, dissolve 10 g of 4-methylaminopyridine and 10 g of 5-amino-2-chlorotoluene-5-sulfonic acid in 100 g of 70° C. toluene, then stir and mix for 2 h, cool to room temperature, and vacuum filter and dry to obtain a powder;

[0084] Step 2, 12.5g of 2-[4-(2-hydroxy-2-methyl-1-oxypropyl)phenoxy]acetic acid, 12.5g of 2-hydroxy-1-[4-(2-hydroxypropoxy)phenyl]-2-methylpropane-1-one, 11g of mercaptoacetic acid and 0.7g of the powder prepared in step 1 are added to 100g of toluene, and refluxed at 125°C under a nitrogen atmosphere with stirring overnight, and then toluene is removed from the reactants by rotary evaporation under reduced pressure to obtain a crude product, which is diluted with 80g of dichloromethane, and then washed with 500g of a saturated sodium bicarbonate aqueous solution and 300g of water, respectively, and the organic phase is collected and dried over anhydrous magnesium sulfate overnight to obtain a pre-treated initiator;

[0085] Step 3, 5 g of 3-glycidyloxypropyltriethoxysilane, 6 g of the pre-treated initiator prepared in step 2, 0.2 g of triethylamine and 30 g of dichloromethane were mixed, and stirred at 40° C. for 2 h under a nitrogen atmosphere to obtain a grafting initiator;

[0086] Step 4, 20 g of triethoxysilane, 5 g of water and 9 g of anhydrous ethanol were stirred and mixed for 2 h, and after the mixture was allowed to stand to clarify, 0.2 g of 10 wt % hydrochloric acid was added under stirring, and the mixture was left at room temperature overnight to obtain pretreated triethoxysilane;

[0087] Step 5: Mix and stir 40 g of aliphatic polyurethane acrylate, 10 g of octadecyl methacrylate, 0.8 g of pretreated triethoxysilane and 0.8 g of the grafting initiator prepared in step 3 until a uniform solution is formed, and then maintain it in vacuum at 50° C. for 10 min to remove bubbles formed during the stirring process to obtain a UV-curable nanoimprint material.

[0088] The method of using the UV-curable nanoimprint material is the same as that in Example 1.

[0089] Comparative Example 1

[0090] A manufacturing process of a UV-curable nanoimprint material is as follows:

[0091] Step 1, dissolving 10 g of 4-methylaminopyridine and 10 g of p-toluenesulfonic acid in 100 g of 70° C. toluene respectively, then stirring and mixing for 2 h, cooling to room temperature, and vacuum filtering and drying to obtain a powder;

[0092] Step 2, adding 25g of 2-[4-(2-hydroxy-2-methyl-1-oxypropyl)phenoxy]acetic acid, 11g of mercaptoacetic acid and 0.7g of the powder prepared in step 1 to 100g of toluene, reflux and stir at 125°C under a nitrogen atmosphere overnight, then removing toluene from the reactant by rotary evaporation under reduced pressure to obtain a crude product, diluting it with 80g of dichloromethane, then washing it with 500g of a saturated sodium bicarbonate aqueous solution and 300g of water, respectively, collecting the organic phase and drying it with anhydrous magnesium sulfate overnight to obtain a pretreated initiator;

[0093] Step 3, 5 g of 3-glycidyloxypropyltriethoxysilane, 6 g of the pre-treated initiator prepared in step 2, 0.2 g of triethylamine and 30 g of dichloromethane were mixed, and stirred at 40° C. for 2 h under a nitrogen atmosphere to obtain a grafting initiator;

[0094] Step 4, 20 g of triethoxysilane, 5 g of water and 9 g of anhydrous ethanol were stirred and mixed for 2 h, and after the mixture was allowed to stand to clarify, 0.2 g of 10 wt % hydrochloric acid was added under stirring, and the mixture was left at room temperature overnight to obtain pretreated triethoxysilane;

[0095] Step 5: Mix and stir 40 g of aliphatic polyurethane acrylate, 10 g of octadecyl methacrylate, 0.8 g of pretreated triethoxysilane and 0.8 g of the grafting initiator prepared in step 3 until a uniform solution is formed, and then maintain it in vacuum at 50° C. for 10 min to remove bubbles formed during the stirring process to obtain a UV-curable nanoimprint material.

[0096] The method of using the UV-curable nanoimprint material is the same as that in Example 1.

[0097] Comparative Example 2

[0098] A manufacturing process of a UV-curable nanoimprint material is as follows:

[0099] Step 1, dissolve 10 g of 4-methylaminopyridine and 10 g of 5-amino-2-chlorotoluene-5-sulfonic acid in 100 g of 70° C. toluene, then stir and mix for 2 h, cool to room temperature, and vacuum filter and dry to obtain a powder;

[0100] Step 2, adding 25g of 2-[4-(2-hydroxy-2-methyl-1-oxypropyl)phenoxy]acetic acid, 11g of mercaptoacetic acid and 0.7g of the powder prepared in step 1 to 100g of toluene, reflux and stir at 125°C under a nitrogen atmosphere overnight, then removing toluene from the reactant by rotary evaporation under reduced pressure to obtain a crude product, diluting it with 80g of dichloromethane, then washing it with 500g of a saturated sodium bicarbonate aqueous solution and 300g of water, respectively, collecting the organic phase and drying it with anhydrous magnesium sulfate overnight to obtain a pretreated initiator;

[0101] Step 3, 5 g of 3-(2,3-epoxypropoxy)propyltrimethoxysilane, 6 g of the pre-treated initiator prepared in step 2, 0.2 g of triethylamine and 30 g of dichloromethane were mixed, and stirred at 40° C. for 2 h under a nitrogen atmosphere to obtain a grafting initiator;

[0102] Step 4, 20 g of triethoxysilane, 5 g of water and 9 g of anhydrous ethanol were stirred and mixed for 2 h, and after the mixture was allowed to stand to clarify, 0.2 g of 10 wt % hydrochloric acid was added under stirring, and the mixture was left at room temperature overnight to obtain pretreated triethoxysilane;

[0103] Step 5: Mix and stir 40 g of aliphatic polyurethane acrylate, 10 g of octadecyl methacrylate, 0.8 g of pretreated triethoxysilane and 0.8 g of the grafting initiator prepared in step 3 until a uniform solution is formed, and then maintain it in vacuum at 50° C. for 10 min to remove bubbles formed during the stirring process to obtain a UV-curable nanoimprint material.

[0104] The method of using the UV-curable nanoimprint material is the same as that in Example 1.

[0105] Comparative Example 3

[0106] A manufacturing process of a UV-curable nanoimprint material is as follows:

[0107] Step 1, dissolve 10 g of 4-methylaminopyridine and 10 g of 5-amino-2-chlorotoluene-5-sulfonic acid in 100 g of 70° C. toluene, then stir and mix for 2 h, cool to room temperature, and vacuum filter and dry to obtain a powder;

[0108] Step 2, adding 25 g of 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone, 11 g of thioglycolic acid and 0.7 g of the powder prepared in step 1 to 100 g of toluene, refluxing with stirring at 125° C. under a nitrogen atmosphere overnight, then removing toluene from the reactant by rotary evaporation under reduced pressure to obtain a crude product, diluting it with 80 g of dichloromethane, and then washing it with 500 g of a saturated sodium bicarbonate aqueous solution and 300 g of water, respectively, collecting the organic phase and drying it with anhydrous magnesium sulfate overnight to obtain a pretreated initiator;

[0109] Step 3, 5 g of 3-glycidyloxypropyltriethoxysilane, 6 g of the pre-treated initiator prepared in step 2, 0.2 g of triethylamine and 30 g of dichloromethane were mixed, and stirred at 40° C. for 2 h under a nitrogen atmosphere to obtain a grafting initiator;

[0110] Step 4, 20 g of triethoxysilane, 5 g of water and 9 g of anhydrous ethanol were stirred and mixed for 2 h, and after the mixture was allowed to stand to clarify, 0.2 g of 10 wt % hydrochloric acid was added under stirring, and the mixture was left at room temperature overnight to obtain pretreated triethoxysilane;

[0111] Step 5: Mix and stir 40 g of aliphatic polyurethane acrylate, 10 g of octadecyl methacrylate, 0.8 g of pretreated triethoxysilane and 0.8 g of the grafting initiator prepared in step 3 until a uniform solution is formed, and then maintain it in vacuum at 50° C. for 10 min to remove bubbles formed during the stirring process to obtain a UV-curable nanoimprint material.

[0112] The method of using the UV-curable nanoimprint material is the same as that in Example 1.

[0113] Comparative Example 4

[0114] A manufacturing process of a UV-curable nanoimprint material is as follows:

[0115] Step 1, dissolve 10 g of 4-methylaminopyridine and 10 g of 5-amino-2-chlorotoluene-5-sulfonic acid in 100 g of 70° C. toluene, then stir and mix for 2 h, cool to room temperature, and vacuum filter and dry to obtain a powder;

[0116] Step 2, adding 25g of 2-[4-(2-hydroxy-2-methyl-1-oxypropyl)phenoxy]acetic acid, 11g of mercaptoacetic acid and 0.7g of the powder prepared in step 1 to 100g of toluene, reflux and stir at 125°C under a nitrogen atmosphere overnight, then removing toluene from the reactant by rotary evaporation under reduced pressure to obtain a crude product, diluting it with 80g of dichloromethane, then washing it with 500g of a saturated sodium bicarbonate aqueous solution and 300g of water, respectively, collecting the organic phase and drying it with anhydrous magnesium sulfate overnight to obtain a pretreated initiator;

[0117] Step 3, 5 g of 3-glycidyloxypropyltriethoxysilane, 6 g of the pre-treated initiator prepared in step 2, 0.2 g of triethylamine and 30 g of dichloromethane were mixed, and stirred at 40° C. for 2 h under a nitrogen atmosphere to obtain a grafting initiator;

[0118] Step 4, 20 g of triethoxysilane, 5 g of water and 9 g of anhydrous ethanol were stirred and mixed for 2 h, and after the mixture was allowed to stand to clarify, 0.2 g of 10 wt % hydrochloric acid was added under stirring, and the mixture was left at room temperature overnight to obtain pretreated triethoxysilane;

[0119] Step 5: 40 g of aliphatic polyurethane acrylate, 10 g of 1,6-hexanediol dimethacrylate, 0.8 g of pretreated triethoxysilane and 0.8 g of the grafting initiator prepared in step 3 are mixed and stirred until a uniform solution is formed, and then maintained in vacuum at 50° C. for 10 min to remove bubbles formed during the stirring process, thereby obtaining a UV-curable nanoimprint material.

[0120] The method of using the UV-curable nanoimprint material is the same as that in Example 1.

[0121] Comparative Example 5

[0122] A manufacturing process of a UV-curable nanoimprint material is as follows:

[0123] Step 1, dissolving 10 g of 4-methylaminopyridine and 10 g of p-toluenesulfonic acid in 100 g of 70° C. toluene respectively, then stirring and mixing for 2 h, cooling to room temperature, and vacuum filtering and drying to obtain a powder;

[0124] Step 2, adding 25 g of 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone, 11 g of thioglycolic acid and 0.7 g of the powder prepared in step 1 to 100 g of toluene, refluxing with stirring at 125° C. under a nitrogen atmosphere overnight, then removing toluene from the reactant by rotary evaporation under reduced pressure to obtain a crude product, diluting it with 80 g of dichloromethane, and then washing it with 500 g of a saturated sodium bicarbonate aqueous solution and 300 g of water, respectively, collecting the organic phase and drying it with anhydrous magnesium sulfate overnight to obtain a pretreated initiator;

[0125] Step 3, 5 g of 3-(2,3-epoxypropoxy)propyltrimethoxysilane, 6 g of the pre-treated initiator prepared in step 2, 0.2 g of triethylamine and 30 g of dichloromethane were mixed, and stirred at 40° C. for 2 h under a nitrogen atmosphere to obtain a grafting initiator;

[0126] Step 4, 20 g of triethoxysilane, 5 g of water and 9 g of anhydrous ethanol were stirred and mixed for 2 h, and after the mixture was allowed to stand to clarify, 0.2 g of 10 wt % hydrochloric acid was added under stirring, and the mixture was left at room temperature overnight to obtain pretreated triethoxysilane;

[0127] Step 5: 40 g of aliphatic polyurethane acrylate, 10 g of 1,6-hexanediol dimethacrylate, 0.8 g of pretreated triethoxysilane and 0.8 g of the grafting initiator prepared in step 3 are mixed and stirred until a uniform solution is formed, and then maintained in vacuum at 50° C. for 10 min to remove bubbles formed during the stirring process, thereby obtaining a UV-curable nanoimprint material.

[0128] The method of using the UV-curable nanoimprint material is the same as that in Example 1.

[0129] Test Example 1

[0130] Thermal stability test

[0131] The embossed product prepared by the present invention was subjected to thermogravimetric analysis to test its thermal stability, and the temperature at which the sample lost 10 wt% and the temperature at which the sample lost 50 wt% were statistically analyzed. The test results are shown in Table 1.

[0132] Table 1 Thermal stability test results

[0133]

[0134] Test Example 2

[0135] Mechanical properties

[0136] The tensile properties of the embossed product prepared by the present invention were tested in accordance with the requirements of GB / T 1040.3-2006 "Determination of tensile properties of plastics Part 3: Test conditions for films and sheets". The sample length was 150 mm, the width was 20 mm, a 4-type dumbbell-shaped specimen was used, and the tensile rate was 50 mm / min. Test conditions: room temperature, 5 samples per group, and the average value was taken.

[0137] The test results are shown in Table 2.

[0138] Table 2 Mechanical properties test results

[0139] Experimental protocol Tensile strength(MPa) Elongation at break (%) Example 1 18.2 32.4 Example 2 17.3 31.0 Example 3 16.5 28.7 Example 4 19.8 26.5 Comparative Example 1 15.7 31.6 Comparative Example 2 15.9 33.5 Comparative Example 3 16.1 31.1 Comparative Example 4 17.3 30.5 Comparative Example 5 14.2 33.8

[0140] From the test data of Table 1 and Table 2, it can be seen that the thermal stability and tensile strength of the embossed product prepared in Example 4 of the present invention are the best, and the slightly lower elongation at break can reduce the deformation of the embossed product. The possible reason for the comparison between the embodiment and the comparative example is that compared with p-toluenesulfonic acid, 5-amino-2-chlorotoluene-5-sulfonic acid in the present invention is a compound containing amino groups and chlorine atoms, and these functional groups can provide reactive centers to promote the polymerization reaction of the material. Compared with p-toluenesulfonic acid, 5-amino-2-chlorotoluene-5-sulfonic acid may be more likely to participate in the reaction, thereby enhancing the degree of polymerization and crosslinking density of the material.

[0141] In Example 4 of the present invention, 2-[4-(2-hydroxy-2-methyl-1-oxypropyl)phenoxy]acetic acid and 2-hydroxy-1-[4-(2-hydroxypropyloxy)phenyl]-2-methylprop-1-one are used to prepare UV-curable nanoimprint materials, compared with only using 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone, as initiators to participate in the polymerization reaction. Compared with 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone, these two compounds may have higher initiator activity, can more effectively initiate the polymerization reaction of the material, and promote the formation of a cross-linked structure. A tighter cross-linked network is formed, and the mechanical properties and thermal stability of the material are improved.

[0142] Compared with 3-(2,3-epoxypropoxy)propyltrimethoxysilane, the 3-glycidyloxypropyltriethoxysilane has a glycidyloxy functional group, which may undergo a condensation reaction with the carbonyl compound in the organic matrix to form a strong chemical bond, thereby enhancing the compatibility of the interface. In contrast, the epoxy group in 3-(2,3-epoxypropoxy)propyltrimethoxysilane may undergo an epoxy ring-opening reaction with the carbonyl compound in the matrix, and the resulting functional group may have a relatively weak chemical bond with the matrix. Therefore, the use of 3-glycidyloxypropyltriethoxysilane may be better compatible with the matrix and improve the interfacial properties of the material. A cross-linked structure is formed. This cross-linked structure can enhance the mechanical properties, thermal stability and tensile strength of the material.

[0143] Compared with 1,6-hexanediol dimethacrylate, the use of octadecyl methacrylate contains a long-chain aliphatic structure, which may increase the intermolecular crosslinking points of the material and inhibit the thermal motion of the molecules, thereby improving the thermal stability of the material. In contrast, the hexanediol structure in the 1,6-hexanediol dimethacrylate molecule is shorter, has fewer intermolecular crosslinking points, and has relatively low thermal stability. Therefore, the use of octadecyl methacrylate may help improve the thermal stability of the material. The long-chain aliphatic structure in the octadecyl methacrylate molecule may provide more crosslinking points, enhance the network structure of the material, and thus improve the tensile strength of the material. In contrast, the hexanediol structure in the 1,6-hexanediol dimethacrylate molecule is shorter, has fewer crosslinking points, and has relatively low tensile strength. Therefore, the use of octadecyl methacrylate may be able to enhance the mechanical properties of the material.

Claims

1. A process for manufacturing a UV-curable nanoimprint material, characterized in that: The manufacturing process is as follows, in parts by weight: Step 1, dissolving 8-12 parts of 4-methylaminopyridine and 8-12 parts of a sulfonic acid compound in 80-120 parts of toluene at 60-80° C., then stirring and mixing for 1-3 hours, cooling to room temperature, and vacuum filtering and drying to obtain a powder; Step 2, adding 20-30 parts of initiator, 8-13 parts of thioglycolic acid and 0.5-0.8 parts of the powder prepared in step 1 to 80-120 parts of toluene, refluxing and stirring at 110-130° C. under a nitrogen atmosphere overnight, then removing toluene from the reactant by rotary evaporation under reduced pressure to obtain a crude product, diluting it with 70-90 parts of dichloromethane, and then washing it with 400-600 parts of a saturated sodium bicarbonate aqueous solution and 200-400 parts of water, respectively, collecting the organic phase and drying it with anhydrous magnesium sulfate overnight to obtain a pretreated initiator; Step 3, 4 to 6 parts of the silane compound, 5 to 7 parts of the pre-treated initiator prepared in step 2, 0.1 to 0.3 parts of triethylamine and 25 to 35 parts of dichloromethane are mixed, and stirred at 30 to 50° C. for 1 to 3 hours under a nitrogen atmosphere to obtain a grafting initiator; Step 4, 18 to 22 parts of triethoxysilane, 4 to 6 parts of water and 8 to 10 parts of anhydrous ethanol are stirred and mixed for 1 to 3 hours, and after the mixture is allowed to stand for clarification, 0.1 to 0.3 parts of 5 to 20 wt % hydrochloric acid are added under stirring, and the mixture is left at room temperature overnight to obtain pretreated triethoxysilane; Step 5, 35-45 parts of aliphatic polyurethane acrylate, 8-12 parts of lipid compounds, 0.7-0.9 parts of pretreated triethoxysilane and 0.7-0.9 parts of the grafting initiator prepared in step 3 are mixed and stirred until a uniform solution is formed, and then maintained in a vacuum at 40-60° C. for 5-15 minutes to remove bubbles formed during the stirring process, thereby obtaining a UV-curable nanoimprint material; The initiators are 2-[4-(2-hydroxy-2-methyl-1-oxypropyl)phenoxy]acetic acid and 2-hydroxy-1-[4-(2-hydroxypropyloxy)phenyl]-2-methylpropan-1-one; The sulfonic acid compound is 5-amino-2-chlorotoluene-5-sulfonic acid; The silane compound is 3-glycidyloxypropyltriethoxysilane; The lipid compound is octadecyl methacrylate.

2. A UV-curable nanoimprint material, characterized in that: The method is prepared by the manufacturing process as claimed in claim 1.

3. An application of the UV-curable nanoimprint material as claimed in claim 2, characterized in that: The applications are as follows: S1, prepare the imprinting mold and substrate; S2, coating the UV-curable nanoimprint material on the surface of the imprinting part of the imprinting mold at an ambient temperature of 18-25° C.; S3, using ultraviolet irradiation to perform primary curing on the surface of the imprinting part of the imprinting mold, with an irradiation dose of 800-1200 mJ to fix the imprinting material; S4. After heating at 90-110° C., the substrate is imprinted using an imprinting mold, and then the substrate is exposed and cured using ultraviolet rays with an irradiation dose of 1000-2000 mJ to obtain an imprinted product.