A method for preparing a solid-state lithium-ion battery

Through improved solid-state lithium-ion battery preparation methods, including magnetic field modification and ultrasonic welding technology, the interface properties of electrolytes and electrode materials are solved, and the battery conductivity, lithium ion migration and cycle life are improved, achieving more efficient Electrochemical properties and stability.

CN117996211BActive Publication Date: 2024-11-22HUNAN TAIHE NEW ENERGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410184724.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-19
Publication Date
2024-11-22
Estimated Expiration
2044-02-19

AI Technical Summary

Technical Problem

In the preparation technology of solid-state lithium-ion batteries, the uniformity of the electrolyte, the composite method of the electrode material and the interface properties are insufficient, resulting in poor solid-solid interface contact performance, affecting the transmission of lithium ions and charge transfer, and thus affecting the charging and discharging performance of the battery and Cycle life.

Method used

Adopting improved preparation methods, including preparing composite positive electrode and negative electrode slurry, using magnetic field modified electrode materials, selecting appropriate binders and conductive polymers, and stacking the positive electrode, solid electrolyte and negative electrodes in turn through ultrasonic welding to optimize interface properties. and contact performance.

Benefits of technology

It improves the conductivity, lithium ion migration, energy density and power density, extends the cycle life of the battery, reduces the resistance and internal resistance of the electrode, and enhances the mechanical strength and stability of the electrode.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004705443640000071
    Figure BDA0004705443640000071
  • Figure BDA0004705443640000072
    Figure BDA0004705443640000072
  • Figure BDA0004705443640000081
    Figure BDA0004705443640000081
Patent Text Reader

Abstract

The invention provides a method for preparing a solid-state lithium-ion battery. The solid-state lithium-ion battery comprises a positive electrode sheet, a negative electrode sheet and a solid electrolyte. The positive electrode material is mixed with a binder solution, a positive electrode active substance and a conductive polymer in proportion to prepare a composite positive electrode slurry, which is coated on an aluminum foil to obtain an electrode sheet. The negative electrode active substance and the aqueous binder of the invention are mixed to obtain a negative electrode slurry, which is coated on the negative electrode sheets on both sides of the copper foil. The positive electrode sheet and the negative electrode sheet are then treated with a magnetic field respectively, and the magnetic field process parameters are controlled, which not only effectively changes the surface structure and chemical properties of the sheet and improves the compatibility with the solid electrolyte, but also makes the conductive particles in the electrode sheet evenly arranged, reduces the agglomeration phenomenon, improves the conductivity of the electrode sheet, and is beneficial to the electrochemical stability of the battery. The solid-state lithium-ion battery of the invention has good electrochemical performance and stability, and can improve the energy density and cycle life of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of lithium ion solid-state batteries, and in particular to a method for preparing a solid-state lithium ion battery. Background Art

[0002] With the growing demand for energy storage, solid-state lithium-ion batteries are lithium-ion batteries that use solid electrolytes instead of traditional liquid electrolytes. Due to their advantages such as high energy density, long life, fast charging and high safety, solid-state lithium-ion batteries have become an important development direction for the next generation of lithium-ion battery technology. Solid-state lithium-ion batteries use solid electrolytes instead of traditional liquid electrolytes, and have the advantages of high safety, high energy density and long cycle life. However, the preparation technology of solid-state lithium-ion batteries still has certain challenges, such as the preparation of solid electrolytes and the preparation of composite electrodes.

[0003] There are still some challenges and problems in the existing solid-state lithium-ion battery preparation technology. At present, there are still some problems in the preparation technology of solid-state lithium-ion batteries, such as the uniformity of the electrolyte, the composite mode of the electrode material and the interface properties, etc. The solid-solid interface contact performance between the solid electrolyte and the electrode is poor, resulting in a large interface impedance between the positive and negative electrodes of the solid-state battery, which will affect the transmission of lithium ions and the transfer of charges, thereby affecting the battery's charge and discharge performance; these problems may lead to unstable battery performance and reduced cycle life. Therefore, it is necessary to research and develop new preparation technologies to solve these problems and improve the performance and stability of solid-state lithium-ion batteries. Summary of the invention

[0004] In view of this, the present invention proposes a method for preparing a solid-state lithium-ion battery to solve the above problems.

[0005] The technical solution of the present invention is implemented as follows: A method for preparing a solid-state lithium-ion battery: the solid-state lithium-ion battery comprises a positive electrode sheet, a negative electrode sheet, and a solid electrolyte, and the solid-state lithium-ion preparation method comprises the following steps:

[0006] (1) The method for preparing the positive electrode material comprises the following steps:

[0007] Step S1, preparing composite positive electrode slurry: mixing a binder solution with a positive electrode active material and a conductive polymer, stirring evenly, drying, grinding to a particle size of 5-15 μm, adding a solvent to adjust the viscosity of the slurry, and dispersing to obtain a slurry;

[0008] Step S2, coating and drying: coating the prepared positive electrode slurry evenly on the aluminum foil, and then drying and shearing to obtain a positive electrode sheet;

[0009] (2) The method for preparing the negative electrode material comprises the following steps:

[0010] Step S3, preparing negative electrode slurry: crushing the negative electrode active material, grinding to obtain a powder with a particle size of 5-15 μm, adding an aqueous binder, the mass volume ratio of the powder to the aqueous binder is 100:1.5-3 g / mL, mixing and stirring for 5-25 minutes to obtain a negative electrode slurry;

[0011] Step S4, coating and drying: coating the negative electrode slurry on both sides of the copper foil, drying, rolling, and shearing to obtain a negative electrode sheet;

[0012] (3) Modification step: taking the positive electrode sheet and the negative electrode sheet obtained above and placing them in a magnetic field respectively, controlling the magnetic field strength to 200-400 GS and the magnetic field action time to 10-30 min, to obtain the modified positive electrode sheet and the negative electrode sheet;

[0013] (4) preparing a solid electrolyte sheet: crushing the solid electrolyte into powder with a particle size of less than 5 μm, mixing, granulating, and pressing to obtain a solid electrolyte sheet, wherein the thickness of the solid electrolyte sheet is controlled to be 5-30 μm and set aside;

[0014] (5) Preparing a solid-state lithium-ion battery: stacking the modified positive electrode sheet, solid electrolyte sheet, and negative electrode sheet in sequence, welding and packaging them by ultrasonic welding to obtain the solid-state lithium-ion battery.

[0015] Furthermore, in step S1, the binder solution is prepared by dissolving the binder in a solvent, with the mass volume ratio of the binder to the solvent being 12-25:30 g / mL to form a binder solution, wherein the binder is polyvinylidene fluoride or polytetrafluoroethylene, and the solvent is N-methylpyrrolidone or acetone.

[0016] Furthermore, in step S1, the positive electrode active material is any one or a combination of lithium cobalt oxide, lithium iron phosphate, lithium manganese oxide, nickel-cobalt-manganese ternary material, lithium-manganese-rich material or sulfur-containing material.

[0017] Furthermore, in step S1, the conductive polymer is one or a combination of polyacetylene, polythiophene, polypyrrole, polyaniline, polyaniline, polyphenylene vinylene or polydiacetylene.

[0018] Furthermore, the solvent in step S1 is polyvinyl alcohol or polyvinyl ketone.

[0019] Furthermore, the mass volume ratio of the positive electrode active material, the conductive agent polymer and the binder solution is 60-80:5-20:1-5 g / mL.

[0020] Furthermore, the negative electrode active material in step S3 is any one or a combination of artificial graphite, natural graphite, soft carbon, hard carbon, carbon fiber, silicon alloy, lithium titanate or tin alloy.

[0021] Furthermore, the aqueous binder in step S3 is sodium carboxymethyl cellulose, polyacrylic acid, and pullulan in a volume ratio of (5-15):(1-3):(0.2-0.8), and the viscosity range is 500-800 mPa·s.

[0022] Furthermore, the solid electrolyte is one of lithium lanthanum zirconium oxide, lithium lanthanum titanium oxide, lithium phosphorus sulfur chlorine, lithium germanium phosphorus sulfur, lithium phosphorus oxygen nitrogen, and lithium chloride.

[0023] Furthermore, the frequency of the ultrasonic welding in (5) is 80-150 kHz, and the ultrasonic amplitude is ≤3 μm.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] The solid-state lithium-ion battery of the present invention adopts a solid electrolyte instead of a traditional liquid electrolyte. From the test results, it can be seen that the conductivity is 1.32-1.42mS / cm, the lithium ion migration number is ≥0.90, the 100-cycle capacity retention rate is 95.6-97.5%, and the 200-cycle capacity retention rate is 91.4-94.5%, indicating that the solid-state lithium-ion battery of the present invention has better conductivity and high lithium ion migration. By selecting the raw materials and formula of the positive electrode sheet, the overall conductivity of the electrode can be improved, the resistance of the electrode can be reduced, and the aqueous binder of the present invention is used to prepare the negative electrode sheet, so that the electrode material can be better Adhere to the current collector to improve the mechanical strength and stability of the electrode, and solve the problem of electrode material expansion. Use magnetic field treatment on the electrode plate to improve the electrochemical activity of the electrode plate surface, increase the contact area and electron transmission efficiency between the active material and the current collector, thereby reducing internal resistance and increasing the energy density and power density of the battery. It can also better orient and arrange the conductive particles in the electrode plate, reduce the agglomeration of conductive particles, and improve the conductivity of the electrode plate; use ultrasonic welding to stack and weld the positive electrode plate, solid electrolyte plate, and negative electrode plate in sequence to optimize contact performance and improve interface properties. DETAILED DESCRIPTION

[0026] In order to better understand the technical content of the present invention, specific embodiments are provided below to further illustrate the present invention.

[0027] Unless otherwise specified, the experimental methods used in the embodiments of the present invention are all conventional methods.

[0028] Unless otherwise specified, the materials, reagents, etc. used in the embodiments of the present invention can be obtained from commercial sources.

[0029] Example 1

[0030] A method for preparing a solid-state lithium-ion battery: the solid-state lithium-ion battery comprises a positive electrode sheet, a negative electrode sheet, and a solid electrolyte, and the solid-state lithium-ion preparation method comprises the following steps:

[0031] (1) The method for preparing the positive electrode material comprises the following steps:

[0032] Step S1, preparing a composite positive electrode slurry: mixing a binder solution with a positive electrode active material and a conductive polymer, wherein the mass volume ratio of the positive electrode active material, the conductive agent polymer and the binder solution is 60:5:1 g / mL, stirring evenly, drying, grinding the particles to a particle size of 5 μm, adding a solvent to adjust the viscosity of the slurry, and dispersing to obtain a slurry; the binder solution is prepared by dissolving a binder in polyvinyl alcohol, wherein the mass volume ratio of the binder to the polyvinyl alcohol is 12:30 g / mL to form a binder solution, wherein the binder is polyvinylidene fluoride, and the positive electrode active material is lithium cobalt oxide; the conductive polymer is polyacetylene,

[0033] Step S2, coating and drying: coating the prepared positive electrode slurry evenly on the aluminum foil, and then drying and shearing to obtain a positive electrode sheet;

[0034] (2) The method for preparing the negative electrode material comprises the following steps:

[0035] Step S3, preparing negative electrode slurry: crushing the negative electrode active material, grinding to obtain a powder with a particle size of 5 μm, adding an aqueous binder, the mass volume ratio of the powder to the aqueous binder g / mL is 100:1.5, mixing and stirring for 5 minutes, and obtaining a negative electrode slurry; the negative electrode active material is artificial graphite; the aqueous binder is sodium carboxymethyl cellulose, polyacrylic acid, and pullulan in a volume ratio of 5:1:0.2, and the viscosity range is 500 mPa·s;

[0036] Step S4, coating and drying: coating the negative electrode slurry on both sides of the copper foil, drying, rolling, and shearing to obtain a negative electrode sheet;

[0037] (3) Modification step: taking the positive electrode sheet and the negative electrode sheet obtained above and placing them in a magnetic field respectively, controlling the magnetic field intensity to 200 GS and the magnetic field action time to 10 min, to obtain the modified positive electrode sheet and the negative electrode sheet;

[0038] (4) preparing a solid electrolyte sheet: crushing the solid electrolyte lithium lanthanum zirconium oxide into a powder with a particle size of less than 5 μm, mixing, granulating, and pressing to obtain a solid electrolyte sheet, controlling the thickness of the solid electrolyte sheet to be 5 μm, and setting aside;

[0039] (5) Preparation of solid-state lithium-ion battery: stacking the modified positive electrode sheet, solid electrolyte sheet and negative electrode sheet in sequence, and encapsulating them by ultrasonic welding, wherein the frequency of ultrasonic welding is 80 kHz and the ultrasonic amplitude is ≤3 μm, to obtain the solid-state lithium-ion battery.

[0040] Example 2

[0041] A method for preparing a solid-state lithium-ion battery: the solid-state lithium-ion battery comprises a positive electrode sheet, a negative electrode sheet, and a solid electrolyte, and the solid-state lithium-ion preparation method comprises the following steps:

[0042] (1) The method for preparing the positive electrode material comprises the following steps:

[0043] Step S1, preparing a composite positive electrode slurry: mixing a binder solution with a positive electrode active material and a conductive polymer, wherein the mass volume ratio of the positive electrode active material, the conductive agent polymer and the binder solution is 80:20:5 g / mL, stirring evenly, drying, grinding to a particle size of 15 μm, adding a solvent to adjust the viscosity of the slurry, and dispersing to obtain a slurry; the binder solution is prepared by dissolving a binder in polyvinyl ketone, wherein the mass volume ratio of the binder to the polyvinyl ketone is 25:30 g / mL to form a binder solution, wherein the binder is polytetrafluoroethylene, the solvent is acetone, the positive electrode active material is lithium iron phosphate, and the conductive polymer is polythiophene;

[0044] Step S2, coating and drying: coating the prepared positive electrode slurry evenly on the aluminum foil, and then drying and shearing to obtain a positive electrode sheet;

[0045] (2) The method for preparing the negative electrode material comprises the following steps:

[0046] Step S3, preparing negative electrode slurry: crushing the negative electrode active material, grinding to obtain a powder with a particle size of 15 μm, adding an aqueous binder, the mass volume ratio of the powder to the aqueous binder g / mL is 100:3, mixing and stirring for 25 minutes, and obtaining a negative electrode slurry; the negative electrode active material is silicon alloy; the aqueous binder is sodium carboxymethyl cellulose, polyacrylic acid, and pullulan in a volume ratio of 15:3:0.8, and the viscosity range is 800 mPa·s;

[0047] Step S4, coating and drying: coating the negative electrode slurry on both sides of the copper foil, drying, rolling, and shearing to obtain a negative electrode sheet;

[0048] (3) Modification step: taking the positive electrode sheet and the negative electrode sheet obtained above and placing them in a magnetic field respectively, controlling the magnetic field intensity to 400 GS and the magnetic field action time to 30 min, to obtain the modified positive electrode sheet and the negative electrode sheet;

[0049] (4) preparing a solid electrolyte sheet: crushing the solid electrolyte lithium phosphorus sulfur chlorine into powder with a particle size of less than 5 μm, mixing, granulating and pressing to obtain a solid electrolyte sheet, controlling the thickness of the solid electrolyte sheet to 30 μm, and setting aside;

[0050] (5) Preparation of solid-state lithium-ion battery: stacking the modified positive electrode sheet, solid electrolyte sheet and negative electrode sheet in sequence, and encapsulating them by ultrasonic welding, wherein the frequency of ultrasonic welding is 150 kHz and the ultrasonic amplitude is ≤3 μm, to obtain the solid-state lithium-ion battery.

[0051] Example 3

[0052] A method for preparing a solid-state lithium-ion battery: the solid-state lithium-ion battery comprises a positive electrode sheet, a negative electrode sheet, and a solid electrolyte, and the solid-state lithium-ion preparation method comprises the following steps:

[0053] (1) The method for preparing the positive electrode material comprises the following steps:

[0054] Step S1, preparing a composite positive electrode slurry: mixing a binder solution with a positive electrode active material and a conductive polymer, wherein the mass volume ratio of the positive electrode active material, the conductive agent polymer and the binder solution is 70:12:2 g / mL, stirring evenly, drying, grinding the particles to a particle size of 10 μm, adding a solvent to adjust the viscosity of the slurry, and dispersing to obtain a slurry; the binder solution is prepared by dissolving a binder in polyvinyl ketone, wherein the mass volume ratio of the binder to the polyvinyl ketone is 20:30 g / mL to form a binder solution, wherein the binder is polytetrafluoroethylene, the solvent is N-methylpyrrolidone, the positive electrode active material is a nickel-cobalt-manganese ternary material NCM811; and the conductive polymer is polyaniline;

[0055] Step S2, coating and drying: coating the prepared positive electrode slurry evenly on the aluminum foil, and then drying and shearing to obtain a positive electrode sheet;

[0056] (2) The method for preparing the negative electrode material comprises the following steps:

[0057] Step S3, preparing negative electrode slurry: crushing the negative electrode active material, grinding to obtain a powder with a particle size of 10 μm, adding an aqueous binder, the mass volume ratio of the powder to the aqueous binder g / mL is 100:2.2, mixing and stirring for 15 minutes, and obtaining a negative electrode slurry; the negative electrode active material is lithium titanate; the aqueous binder is sodium carboxymethyl cellulose, polyacrylic acid, and pullulan in a volume ratio of 10:2:0.5, and the viscosity range is 700 mPa·s;

[0058] Step S4, coating and drying: coating the negative electrode slurry on both sides of the copper foil, drying, rolling, and shearing to obtain a negative electrode sheet;

[0059] (3) Modification step: taking the positive electrode sheet and the negative electrode sheet obtained above and placing them in a magnetic field respectively, controlling the magnetic field intensity to 300 GS and the magnetic field action time to 20 min, to obtain the modified positive electrode sheet and the negative electrode sheet;

[0060] (4) preparing a solid electrolyte sheet: crushing solid electrolyte lithium chloride into powder with a particle size of less than 5 μm, mixing, granulating, and pressing to obtain a solid electrolyte sheet, wherein the thickness of the solid electrolyte sheet is controlled to be 18 μm and set aside;

[0061] (5) Preparation of solid-state lithium-ion battery: stacking the modified positive electrode sheet, solid electrolyte sheet and negative electrode sheet in sequence, and encapsulating them by ultrasonic welding, wherein the frequency of ultrasonic welding is 120 kHz and the ultrasonic amplitude is ≤3 μm, to obtain the solid-state lithium-ion battery.

[0062] Comparative Example 1

[0063] The difference between this comparative example and Example 3 is that in step S1, the mass volume ratio of the positive electrode active material, the conductive agent polymer and the binder solution is 40:25:9 g / mL.

[0064] Comparative Example 2

[0065] The difference between this comparative example and Example 3 is that the pullulan in the aqueous binder is replaced by an equal amount of guardo gum.

[0066] Comparative Example 3

[0067] The difference between this comparative example and Example 3 is that the positive electrode plate and the negative electrode plate are not modified by a magnetic field.

[0068] Comparative Example 4

[0069] The difference between this comparative example and Example 3 is that the solid electrolyte powder and N-methylpyrrolidone are mixed at a mass volume ratio of g / mL of 12-25:50 to form an electrolyte slurry, which is then coated on the positive electrode sheet and the negative electrode sheet.

[0070] 1. Electrochemical performance test

[0071] 1. Conductivity test: The solid-state lithium-ion batteries of Examples 1-3 and Comparative Examples 1-4 were tested by AC impedance. The samples were polished into small discs with a thickness of about 1 mm, and the diameter and thickness of the samples were measured. Silver paste was evenly applied to the surfaces of both sides of the samples, and silver wire was glued on them. The samples were placed in an air furnace and calcined at 400° C. for 30 min to remove organic matter in the silver paste and obtain a uniform current collector layer. The test frequency range was 20 Hz-1 MHz, and the disturbance voltage was 5 mV. The impedance spectrum obtained by the test was fitted and analyzed to obtain the resistance (R) of the material, and then the conductivity was obtained. The formula is as follows:

[0072] σ=L / RS

[0073] Where: σ--conductivity (S·cm); L disc thickness (cm); S disc area (cm 2 ).

[0074] 2. Test of lithium ion migration number: put the battery into the test system, perform AC impedance test, obtain the initial interface resistance R between the electrolyte and the electrode, apply a polarization voltage of 3.0V to both ends of the battery, polarize for 2 hours, and then perform AC impedance test to obtain the interface resistance R after polarization, and calculate the lithium ion migration number by the formula. The formula is:

[0075]

[0076] Where, tLi + is the migration number of lithium ions, I S is the current after polarization stabilization, I 0 is the initial current,

[0077] ΔV is the applied polarization voltage, R 0 is the initial interface resistance, R S is the interfacial resistance after polarization.

[0078] The test results are shown in Table 1:

[0079]

[0080]

[0081] 3. Charge and discharge cycle test: The solid-state lithium-ion batteries prepared in the above Examples 1-3 and Comparative Examples 1-4 were discharged at a constant current of 0.2C to a specified termination voltage at an ambient temperature of 20±5°C, and then charged at a constant current of 0.2C to the termination voltage, and then switched to constant voltage charging (the charging termination current is generally 0.02C). The performance indicators such as the initial efficiency, 100-cycle capacity retention rate, and 200-cycle capacity retention rate were recorded, and their changes were observed. The test results are as follows:

[0082] First efficiency (%) 100 cycles capacity retention rate (%) 200 cycles capacity retention rate (%) Example 1 95 95.6 92.5 Example 2 93 94.1 91.4 Example 3 97 97.5 94.5 Comparative Example 1 91 90.2 87.3 Comparative Example 2 90 88.4 81.5 Comparative Example 3 87 81.6 72.4 Comparative Example 4 89 84.2 78.1

[0083] From the above results, it can be seen that the solid-state lithium-ion battery of the present invention has good electrochemical properties and stability, and can improve the energy density and cycle life of the battery; from the comparison of Example 1, it can be seen that the positive electrode active material, the conductive agent polymer and the binder solution can achieve a relatively stable charge and discharge performance at a certain ratio; in Example 2, a better aqueous binder is selected to prepare the negative electrode plate, which has a strong bonding force and elasticity, inhibits the expansion of the negative electrode plate, ensures the stability of the negative electrode plate during the cycle, provides an effective transmission channel for the conduction of lithium ions during the charge and discharge cycle, realizes the effective transfer of lithium ions, and improves the high rate performance and cycle stability performance of the negative electrode plate.

[0084] Comparative Example 3 shows that the present invention performs magnetic field modification on the positive electrode and the negative electrode, effectively changes their surface structure and chemical properties, and improves the compatibility with the solid electrolyte; at the same time, the magnetic field treatment can reduce the impedance of the electrode material in the high frequency region, form a faster charge transfer channel, which is beneficial to the electrochemical stability of the battery, effectively improves the polarization phenomenon of the positive electrode material, reduces the internal resistance of the battery, and improves the energy efficiency and power performance of the battery.

[0085] From the comparison of comparative example 4, it can be seen that the present invention uses ultrasonic welding to stack the electrolyte powder on the positive electrode sheet, the solid electrolyte sheet, and the negative electrode sheet in sequence, effectively reducing the resistance and interface impedance at the connection, thereby improving the energy density and performance of the battery, achieving more uniform contact between the solid electrolyte and the electrode sheet, reducing the non-uniformity of the interface impedance, and allowing the battery to stably cycle 200 times while maintaining a high capacity retention rate.

[0086] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a solid-state lithium-ion battery, Features: The solid-state lithium-ion battery comprises a positive electrode sheet, a negative electrode sheet, and a solid electrolyte. The solid-state lithium-ion preparation method comprises the following steps: (1) The method for preparing the positive electrode sheet comprises the following steps: Step S1, preparing a composite positive electrode slurry: mixing a binder solution with a positive electrode active material and a conductive polymer, stirring evenly, drying, grinding to a particle size of 5-15 μm, adding a solvent to adjust the viscosity of the slurry, and dispersing to obtain a slurry; the mass volume ratio of the positive electrode active material, the conductive agent polymer and the binder solution is 60-80:5-20:1-5 g / mL; Step S2, coating and drying: coating the prepared positive electrode slurry evenly on the aluminum foil, and then drying and shearing to obtain a positive electrode sheet; (2) The method for preparing the negative electrode sheet comprises the following steps: Step S3, preparing negative electrode slurry: crushing the negative electrode active material, grinding to obtain a powder with a particle size of 5-15 μm, adding an aqueous binder, the mass volume ratio of the powder to the aqueous binder is 100:1.5-3 g / mL, mixing and stirring for 5-25 minutes to obtain a negative electrode slurry; the aqueous binder is sodium carboxymethyl cellulose, polyacrylic acid, and pullulan in a volume ratio of (5-15):(1-3):(0.2-0.8), and the viscosity range is 500-800 mPa·s; Step S4, coating and drying: coating the negative electrode slurry on both sides of the copper foil, drying, rolling, and shearing to obtain a negative electrode sheet; (3) Modification step: taking the positive electrode sheet and the negative electrode sheet obtained above and placing them in a magnetic field respectively, controlling the magnetic field strength to 200-400 GS and the magnetic field action time to 10-30 min, to obtain the modified positive electrode sheet and the negative electrode sheet; (4) preparing a solid electrolyte sheet: crushing the solid electrolyte into powder with a particle size of less than 5 μm, mixing, granulating, and pressing to obtain a solid electrolyte sheet, wherein the thickness of the solid electrolyte sheet is controlled to be 5-30 μm and set aside; (5) Preparation of solid-state lithium-ion battery: stacking the modified positive electrode sheet, solid electrolyte sheet and negative electrode sheet in sequence, and encapsulating them by ultrasonic welding, wherein the frequency of ultrasonic welding is 80-150 kHz and the ultrasonic amplitude is ≤3 μm, to obtain the solid-state lithium-ion battery.

2. A method for preparing a solid-state lithium-ion battery as claimed in claim 1, Features: In step S1, the binder solution is prepared by dissolving the binder in a solvent, wherein the mass volume ratio of the binder to the solvent is 12-25:30 g / mL to form a binder solution, wherein the binder is polyvinylidene fluoride or polytetrafluoroethylene, and the solvent is N-methylpyrrolidone or acetone.

3. A method for preparing a solid-state lithium-ion battery as claimed in claim 1, Features: In step S1, the positive electrode active material is any one or a combination of lithium cobalt oxide, lithium iron phosphate, lithium manganese oxide, nickel-cobalt-manganese ternary material, lithium-manganese-rich material or sulfur-containing material.

4. A method for preparing a solid-state lithium-ion battery as claimed in claim 1, Features: In the step S1, the conductive polymer is one or a combination of polyacetylene, polythiophene, polypyrrole, polyaniline, polyaniline, polyphenylene vinylene or polybisyne.

5. A method for preparing a solid-state lithium-ion battery as claimed in claim 1, Features: The solvent in step S1 is polyvinyl alcohol or polyvinyl ketone.

6. A method for preparing a solid-state lithium-ion battery as claimed in claim 1, Features: In step S3, the negative electrode active material is any one or a combination of artificial graphite, natural graphite, soft carbon, hard carbon, carbon fiber, silicon alloy, lithium titanate or tin alloy.

7. A method for preparing a solid-state lithium-ion battery according to claim 1, Features: The solid electrolyte is one of lithium lanthanum zirconium oxide, lithium lanthanum titanium oxide, lithium phosphorus sulfur chlorine, lithium germanium phosphorus sulfur, lithium phosphorus oxygen nitrogen, and lithium chloride.