A special synergistic additive for recycling polyethylene modified asphalt system and its synthesis method and application
By synthesizing a synergistic additive for recycling polyethylene modified asphalt system, the recovery of polyethylene modification was solved by using the amination reaction and click reaction of compounds such as calcium p-aminobenzoate, thioacetaldehyde and oleic acid chloride. The high-temperature stability, low-temperature ductility and poor flame retardant performance of the asphalt system have achieved significant performance improvement.
Patent Information
- Application Number
- CN202410409082.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-07
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-04-07
AI Technical Summary
The existing recovered polyethylene modified asphalt system has poor high-temperature stability, low-temperature ductility and flame retardant properties. Due to the poor compatibility between asphalt and recovered polyethylene, it is difficult to improve its basic performance and flame retardant properties at the same time.
A special synergistic additive for recycling polyethylene modified asphalt system is used. Its molecular structure can be synthesized through the amination reaction and click reaction of compounds such as calcium para-aminobenzoate, thioacetaldehyde and oleic acid chloride, and can be mixed without first In the case of polyethylene and additive granulation, it is directly added to the asphalt system to improve the interface compatibility and cross-linking performance of recovered polyethylene and asphalt, and improve its high-temperature stability, low-temperature ductility and flame retardant properties.
The high-temperature stability, low-temperature ductility and flame retardant properties of the recovered polyethylene modified asphalt system are significantly improved, and the molecular structure of the additive is stable, avoiding the weakening or disappearance of synergistic effects, achieving excellent modification effect.
Smart Images

Figure CN118420646B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a special synergistic auxiliary agent for recycling polyethylene modified asphalt system and a synthesis method and application thereof, belonging to the technical field of preparation and chemical processing of organic polymer compounds. Background Art
[0002] With the rapid development of my country's transportation industry, road transportation is constantly developing towards a trend of large traffic volume, axle load, and high degree of channelization. However, the poor high-temperature stability of ordinary asphalt and its brittle fracture at low temperatures seriously affect the service life of asphalt pavement. Recycled polyethylene, as one of the effective modifiers in asphalt pavement, can improve the performance of asphalt pavement. And this technology can greatly alleviate the pollution of polyethylene waste to the environment. Therefore, the construction of recycled polyethylene modified asphalt pavement is of great significance to the sustainable development of my country's economic environment. In addition, asphalt and recycled polyethylene are flammable and release a large amount of smoke and harmful gases when burning, especially when a fire occurs in a tunnel, due to its narrow and long space, the temperature can quickly reach 800 ℃ when a fire occurs in the tunnel, often causing dangerous situations such as high heat and thick smoke, thereby threatening the escape of personnel and affecting the fire fighting route. Therefore, the flame retardant problem of recycled polyethylene modified asphalt system also has important practical significance.
[0003] Due to the difference in molecular structure between asphalt and recycled polyethylene, their compatibility is poor, which limits the basic properties of recycled polyethylene modified asphalt system, such as penetration and ductility. In addition, the research and development of asphalt and recycled polyethylene flame retardant system is mostly focused on modifying the two materials separately. There are few reports on methods that can change the basic properties of recycled polyethylene modified asphalt system and its flame retardant properties without modifying the two materials separately, especially special additives. Summary of the invention
[0004] In order to solve the technical problems existing in the prior art, the present invention provides a special synergistic additive for a recycled polyethylene modified asphalt system, a synthesis method thereof and an application thereof, which has the function of improving the high temperature stability, low temperature ductility, rigidity and flame retardancy of the recycled polyethylene modified asphalt system. Most importantly, during the use of the additive, there is no need to first mix polyethylene with the additive for granulation, and the additive can be directly added to the recycled polyethylene asphalt system to obtain an excellent modification effect, which is of great significance to the field of recycled plastic modified asphalt systems.
[0005] To achieve the above purpose, the technical solution adopted by the present invention is a special synergistic additive for recycling polyethylene modified asphalt system, and its molecular structure is as follows:
[0006] .
[0007] A method for synthesizing a special synergistic additive for recycling polyethylene modified asphalt system is carried out according to the following steps:
[0008] a. Add 16.5 g of p-aminobenzoic acid to 28.6 g of oleoyl chloride and stir at 30 °C for 12 h. Filter the obtained white solid and wash it with 200 mL of acetone, then with 80 °C deionized water until the pH is 4-5. Dry it in an oven at 80 °C to constant weight to obtain intermediate 1.
[0009] b. Disperse 19.4 g of intermediate 1 in 200 mL of deionized water, add 18.5 g of calcium hydroxide to the system, control the system temperature at 90 °C and stir to react for 12 h. After the reaction, use hydrochloric acid to remove excess calcium hydroxide in the system until the pH of the system is 7, then wash with 500 mL of deionized water, filter, and dry in an oven at 80 °C to constant weight to obtain intermediate 2;
[0010] c. Place 2 g of mercaptoacetaldehyde in 100 mL of dimethyl sulfoxide, heat the system to 60 °C and stir until the solid is completely dissolved, then add 10.2 g of intermediate 2 and 0.3 g of catalyst tetrabutylammonium hexafluorophosphate and continue stirring and reacting at 60 °C for 6 h. After the reaction is completed, filter and wash the solid product with 80 °C dimethyl sulfoxide until it is neutral, then wash it with 200 mL of acetone and 500 mL of 80 °C deionized water in sequence, and place it in an oven at 80 °C for 24 h to obtain the synergistic additive.
[0011] The invention discloses an application of a special synergistic auxiliary agent for recycling polyethylene modified asphalt system. The synergistic auxiliary agent is applied in recycling polyethylene modified asphalt system.
[0012] Preferably, the base asphalt is heated to 195°C, and 10% of the mass of the base asphalt recycled polyethylene and 1%-3% of the mass of the base asphalt above-mentioned recycled polyethylene modified asphalt system special synergist are evenly added, and a high-speed modified asphalt emulsifying shearing machine is used to stir at 2500 r / min for 30 min and then shear at 6000 r / min for 60 min.
[0013] Preferably, the dosage of the special synergistic additive for the recycled polyethylene modified asphalt system is 2% of the mass of the recycled polyethylene modified asphalt system.
[0014] Compared with the prior art, the present invention has the following technical effects.
[0015] 1. Based on the strategy of auxiliary agent molecular structure design, the present invention combines the elements required for the recycled polyethylene modified asphalt system, such as recycled polyethylene toughening, asphalt cross-linking modification, recycled polyethylene and asphalt interface compatibility modification, system flame retardancy, etc., using p-aminobenzoic acid calcium salt, mercaptoacetaldehyde, and oleoyl chloride with a long carbon chain through amination reaction, click reaction, etc. to obtain a special synergistic auxiliary agent for the recycled polyethylene modified asphalt system. The auxiliary agent has a stable chemical structure and can remain stable during the system processing and construction process to avoid the weakening or disappearance of the synergistic effect.
[0016] 2. The calcium salt of p-aminobenzoic acid in the molecular chain of the additive can be used as a nucleating agent for recycled polyethylene. By improving the crystal structure of recycled polyethylene and promoting the transformation of large spherulites to microcrystals, recycled polyethylene with stronger rigidity can be obtained, providing conditions for improving the temperature stability and low-temperature ductility of the recycled polyethylene modified asphalt system.
[0017] 3. The aldehyde group in the molecular chain of the additive can act as a cross-linking agent for asphalt and react with the aromatic compounds in asphalt to promote the increase of its local viscosity, thereby fully cross-linking with asphalt during the processing to form a spatial network structure and further improve its high-temperature performance.
[0018] 4. The additive molecule contains a large amount of sulfur and nitrogen elements, which can play a S / N synergistic flame retardant effect. The long carbon chain of oleyl chloride provides a carbon source for the flame retardant system, further promoting the rapid carbonization during the combustion process of the system, thereby obtaining a recycled polyethylene modified asphalt system with good flame retardant properties.
[0019] 5. The long carbon chain on the additive molecular chain greatly reduces the polarity of the additive molecular structure, greatly improves the interfacial compatibility between the additive and recycled polyethylene or asphalt, and promotes the uniform dispersion of the additive in the system, providing conditions for further improving the physical properties and flame retardant properties of the system.
[0020] 6. During the use of this additive, there is no need to mix polyethylene and the additive and granulate them first. It can obtain excellent modification effect by directly adding it into the recycled polyethylene asphalt system, which is of great significance to the field of recycled plastic modified asphalt system. DETAILED DESCRIPTION
[0021] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0022] Example 1, 16.5 g of p-aminobenzoic acid (CAS: 150-13-0) was added to 28.6 g of oleoyl chloride (CAS: 112-77-6) and stirred at 30 ° C for 12 h. The obtained white solid was filtered and washed with 200 mL of acetone, then washed with 80 ° C deionized water until the pH was 4-5, and dried in an oven at 80 ° C to constant weight to obtain intermediate 1; 19.4 g of product 1 was dispersed in 200 mL of deionized water, 18.5 g of calcium hydroxide (CAS: 1305-62-0) was added to the system, and the system temperature was controlled at 90 ° C for 12 h. After the reaction, hydrochloric acid was used to remove excess calcium hydroxide in the system until the pH of the system was 7, and then 500 mL of deionized water was used to wash, filter, and dry in an oven at 80 ° C to constant weight to obtain intermediate 2; 2 g of mercaptoacetaldehyde (CAS: 4124-63-4) was placed at 100 mL of dimethyl sulfoxide, the system was heated to 60 °C and stirred until the solid was completely dissolved, then 10.2 g of product 2 and 0.03 g of catalyst tetrabutylammonium hexafluorophosphate (CAS: 3109-63-5) were added and stirred at 60 °C for 6 h. After the reaction was completed, the solid product was filtered and washed to neutrality with 80 °C dimethyl sulfoxide, then washed with 200 mL of acetone and 500 mL of 80 °C deionized water in sequence, and then placed in an 80 °C oven for 24 h to obtain a special synergist for recycling polyethylene modified asphalt system.
[0023] 500 g of base asphalt was heated to 195 °C, 50 g of recycled polyethylene and 10 g of the above-mentioned recycled polyethylene modified asphalt system special synergist were uniformly added, and a high-speed modified asphalt emulsifier shearing machine was used to stir at 2500 r / min for 30 min and then sheared at 6000 r / min for 60 min. The prepared system was prepared into standard samples according to SH / T 0821-2010 "Determination of Combustion Performance of Asphalt-Oxygen Index Method" and JTG-E20-2011 "Test Procedure for Asphalt and Asphalt Mixtures in Highway Engineering". The limiting oxygen index (LOI) value was determined by the method described in SH / T 0821-2010, and the penetration, softening point and ductility were determined by the method described in JTG-E20-2011. Each sample was tested 5 times in parallel and the average value was taken as the final data of its performance index. The test data are shown in Table 1.
[0024] Example 2: This example is basically the same as Example 1, except that the mass of the added synergistic additive for the recycled polyethylene modified asphalt system is 5 g (1% of the mass of the base asphalt). The test data is shown in Table 1.
[0025] Example 3: This example is basically the same as Example 1, except that the mass of the added synergistic additive for the recycled polyethylene modified asphalt system is 15 g (3% of the mass of the base asphalt). The test data is shown in Table 1.
[0026] In comparative example 1, 500 g of base asphalt was heated to 195 °C, stirred at 2500 r / min for 30 min using a high-speed modified asphalt emulsifying shearing machine, and then sheared at 6000 r / min for 60 min. The prepared system was tested for LOI value, needle penetration, softening point and ductility according to the method described in Example 1. Each sample was tested 5 times in parallel and the average value was taken as the final data of its performance index. The test data are shown in Table 1.
[0027] In comparative example 2, 500 g of base asphalt was heated to 195 °C, 50 g of recycled polyethylene was uniformly added, and a high-speed modified asphalt emulsifying shearing machine was used to stir at 2500 r / min for 30 min and then sheared at 6000 r / min for 60 min. The prepared system was measured for its LOI value, needle penetration, softening point and ductility according to the method described in Example 1. Each sample was tested 5 times in parallel and the average value was taken as the final data of its performance index. The test data are shown in Table 1.
[0028] Comparative Example 3: 500 g of recycled polyethylene and 100 g of the above-mentioned synergistic additive for the recycled polyethylene modified asphalt system are extruded and granulated using a conventional twin-screw extruder. 500 g of the base asphalt is heated to 195 ° C, 60 g of the mixed system of the above-mentioned recycled polyethylene and additives is evenly added, and a high-speed modified asphalt emulsifying shearing machine is used to stir at 2500 r / min for 30 min and then shear at 6000 r / min for 60 min. The prepared system is measured for its LOI value, needle penetration, softening point and ductility according to the method described in Example 1. Each sample is subjected to 5 parallel tests and the average value is taken as the final data of its performance index. The test data are shown in Table 1.
[0029] Comparative Example 4: 500 g of base asphalt was heated to 195 °C, 50 g of recycled polyethylene and 10 g of oleyl chloride were uniformly added, and a high-speed modified asphalt emulsifying shearing machine was used to stir at 2500 r / min for 30 min and then sheared at 6000 r / min for 60 min. The prepared system was measured for its LOI value, needle penetration, softening point and ductility according to the method described in Example 1. Each sample was tested 5 times in parallel and the average value was taken as the final data of its performance index. The test data are shown in Table 1.
[0030] In comparative example 5, 500 g of base asphalt was heated to 195 °C, 50 g of recycled polyethylene and 10 g of p-aminobenzoic acid were uniformly added, and a high-speed modified asphalt emulsifying shearing machine was used to stir at 2500 r / min for 30 min and then sheared at 6000 r / min for 60 min. The prepared system was measured for its LOI value, needle penetration, softening point and ductility according to the method described in Example 1. Each sample was tested 5 times in parallel and the average value was taken as the final data of its performance index. The test data are shown in Table 1.
[0031] In comparative example 6, 500 g of base asphalt was heated to 195 °C, 50 g of recycled polyethylene and 10 g of calcium hydroxide were uniformly added, and a high-speed modified asphalt emulsifying shearing machine was used to stir at 2500 r / min for 30 min and then sheared at 6000 r / min for 60 min. The prepared system was measured for its LOI value, needle penetration, softening point and ductility according to the method described in Example 1. Each sample was tested 5 times in parallel and the average value was taken as the final data of its performance index. The test data are shown in Table 1.
[0032] In comparative example 7, 500 g of base asphalt was heated to 195 °C, 50 g of recycled polyethylene and 10 g of mercaptoacetaldehyde were uniformly added, and a high-speed modified asphalt emulsifying shearing machine was used to stir at 2500 r / min for 30 min and then sheared at 6000 r / min for 60 min. The prepared system was measured for its LOI value, needle penetration, softening point and ductility according to the method described in Example 1. Each sample was subjected to 5 parallel tests and the average value was taken as the final data of its performance index. The test data are shown in Table 1.
[0033] In comparative example 8, 500 g of base asphalt was heated to 195 °C, 50 g of recycled polyethylene and 10 g of intermediate 1 were uniformly added, and a high-speed modified asphalt emulsifying shearing machine was used to stir at 2500 r / min for 30 min and then sheared at 6000 r / min for 60 min. The prepared system was measured for its LOI value, needle penetration, softening point and ductility according to the method described in Example 1. Each sample was subjected to 5 parallel tests and the average value was taken as the final data of its performance index. The test data are shown in Table 1.
[0034] In comparative example 9, 500 g of base asphalt was heated to 195 °C, 50 g of recycled polyethylene and 10 g of intermediate 2 were uniformly added, and a high-speed modified asphalt emulsifying shearing machine was used to stir at 2500 r / min for 30 min and then sheared at 6000 r / min for 60 min. The prepared system was measured for its LOI value, needle penetration, softening point and ductility according to the method described in Example 1. Each sample was subjected to 5 parallel tests and the average value was taken as the final data of its performance index. The test data are shown in Table 1.
[0035] In comparative example 10, 500 g of base asphalt was heated to 195 °C, and 50 g of recycled polyethylene and 28.6 g of oleyl chloride, 16.5 g of p-aminobenzoic acid, 18.5 g of calcium hydroxide, 2 g of mercaptoacetaldehyde, and 0.03 g of catalyst tetrabutylammonium hexafluorophosphate were evenly added. After simple physical mixing in a high-speed mixer (mixing speed 3000 rpm, mixing time 1 min), 10 g of the mixture was stirred at 2500 r / min for 30 min and sheared at 6000 r / min for 60 min using a high-speed modified asphalt emulsifying shearing machine. The obtained system was measured for its LOI value, needle penetration, softening point and ductility according to the method described in Example 1. Each sample was subjected to 5 parallel tests and the average value was taken as the final data of its performance index. The test data are shown in Table 1.
[0036] Table 1 Test data of various examples and comparative examples
[0037] sample Needle penetration (25 ℃) / 0.1mm Softening point / ℃ Elongation (15 ℃) / cm LOI Example 1 35.4 71.3 58.9 29.3 Example 2 38.9 67.3 62.3 24.5 Example 3 41.7 63.5 67.6 26.2 Comparative Example 1 68.2 49.5 135.6 19.2 Comparative Example 2 57.9 54.7 112.7 18.7 Comparative Example 3 52.4 56.4 110.2 20.3 Comparative Example 4 57.8 54.7 111.9 18.7 Comparative Example 5 57.8 54.8 112 18.5 Comparative Example 6 57.9 54.7 112.4 18.7 Comparative Example 7 45.7 58.3 105.4 18.6 Comparative Example 8 51.8 57.9 107.8 18.5 Comparative Example 9 45.8 58.5 105.7 18.6 Comparative Example 10 45.7 58.2 105.3 20.8
[0038] According to the experimental results in Table 1, compared with Comparative Example 1 of the pure matrix asphalt system and Comparative Example 2 in which the special synergistic aid for the recycled polyethylene modified asphalt system prepared by the present invention is not added, the LOI value and softening point of the samples of the special synergistic aid for the recycled polyethylene modified asphalt system prepared by the present invention are significantly improved in Examples 1-3, among which Example 1 with an addition amount of 2% of the mass of the matrix asphalt is the best. This shows that the special synergistic aid for the recycled polyethylene modified asphalt system synthesized by the present invention has the effect of significantly improving the flame retardant properties and high temperature resistance of the recycled polyethylene modified asphalt system. In addition, the needle penetration and ductility of the samples of the special synergistic aid for the recycled polyethylene modified asphalt system prepared by the present invention in Examples 1-3 are significantly reduced, among which Example 1 with an addition amount of 2% of the mass of the matrix asphalt is the best. This shows that the special synergistic aid for the recycled polyethylene modified asphalt system synthesized by the present invention can significantly improve the temperature stability and low-temperature ductility of the recycled polyethylene modified asphalt system. However, adding too much or too little synergistic additives for recycled polyethylene modified asphalt systems will have an adverse effect on the LOI value, softening point, penetration and elongation of the recycled polyethylene modified asphalt system.
[0039] Comparative Example 3 is a special synergistic additive for the recycled polyethylene modified asphalt system prepared by the present invention, which is first mixed with the recycled polyethylene and then mixed with the base asphalt. The results show that compared with Comparative Example 1-2 and Example 1-3, since it first reacts with the recycled polyethylene, it cannot be evenly dispersed into the base asphalt during the later mixing process with the base asphalt, and then synergizes with the base asphalt and the recycled polyethylene at the same time. Therefore, its effect on improving the softening point of the recycled polyethylene modified asphalt system and reducing the needle penetration and ductility is particularly limited. Only because of the synergistic flame retardant effect of nitrogen and sulfur in the system, its LOI is slightly improved.
[0040] The synergistic additive for the recycled polyethylene modified asphalt system prepared by the present invention is synthesized by chemical reaction, and a recycled polyethylene modified asphalt system with excellent flame retardancy, high temperature resistance, temperature stability and low temperature ductility can be obtained. However, Comparative Examples 4-10 are only single raw materials, intermediate products or simple mixing of raw materials, and a complete chemical reaction is not achieved, so the above synergistic effect cannot be fully exerted.
[0041] Among them, since comparative examples 4-9 lack a flame retardant system in the system, the LOI remains basically unchanged compared with comparative examples 1 and 2. Comparative example 10 has a slightly improved LO1 value due to the presence of nitrogen and sulfur elements, but there is still a very large gap compared with the chemically combined special synergistic additives.
[0042] In addition, since Comparative Examples 4-6 are only single raw materials, and these raw materials cannot act alone in the recycled polyethylene modified asphalt system, there is almost no effect on the improvement of its softening point and the reduction of needle penetration and ductility. However, when mercaptoacetaldehyde is added to the system in Comparative Example 7, due to its reaction with aromatic compounds in the asphalt matrix, it brings a slightly better effect than Comparative Examples 4-6. The intermediate 1 added in Comparative Example 8 only obtains good compatibility in the recycled polyethylene modified asphalt system due to its long carbon chain, so its performance is slightly improved compared to Comparative Examples 4-6, or even worse than Comparative Example 7. The intermediate 2 added in Comparative Example 9 has the effect of recycling polyethylene nucleating agent, so the improvement of the softening point of the recycled polyethylene modified asphalt system and the reduction of needle penetration and ductility bring a slightly better effect than Comparative Examples 4-6, but it is basically the same as Comparative Example 7, which also shows from another angle that the aldehyde group reacts with it during the asphalt processing process to contribute greatly to the improvement of the performance of the asphalt system. Finally, Comparative Example 10 only plays a certain role in nitrogen-sulfur synergistic flame retardancy due to the lack of complete chemical reaction. However, due to the presence of aldehyde groups, it has a certain effect of improving the softening point and needle penetration of the recycled polyethylene modified asphalt system and reducing the ductility. The effect is better than that of Comparative Examples 4-6 and Comparative Examples 8-9, but is basically the same as that of Comparative Example 7.
[0043] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principle of the present invention should be included in the scope of the present invention.
Claims
1. A synergistic additive for recycling polyethylene modified asphalt system, characterized in that: Its molecular structure is as follows: 。 2. The method for synthesizing a special synergistic aid for recycling polyethylene modified asphalt system according to claim 1, characterized in that: Follow the steps below, a. Add 16.5 g of p-aminobenzoic acid to 28.6 g of oleoyl chloride and stir at 30 °C for 12 h. Filter the obtained white solid and wash it with 200 mL of acetone, then with 80 °C deionized water until the pH is 4-5. Dry it in an oven at 80 °C to constant weight to obtain intermediate 1. b. Disperse 19.4 g of intermediate 1 in 200 mL of deionized water, add 18.5 g of calcium hydroxide to the system, control the system temperature at 90 °C and stir to react for 12 h. After the reaction, use hydrochloric acid to remove excess calcium hydroxide in the system until the pH of the system is 7, then wash with 500 mL of deionized water, filter, and dry in an oven at 80 °C to constant weight to obtain intermediate 2; c. Place 2 g of mercaptoacetaldehyde in 100 mL of dimethyl sulfoxide, heat the system to 60 °C and stir until the solid is completely dissolved, then add 10.2 g of intermediate 2 and 0.3 g of catalyst tetrabutylammonium hexafluorophosphate and continue to stir and react at 60 °C for 6 h. After the reaction is completed, filter and wash the solid product with 80 °C dimethyl sulfoxide until it is neutral, then wash it with 200 mL of acetone and 500 mL of 80 °C deionized water in turn, and place it in an oven at 80 °C for 24 h to obtain the synergistic additive.
3. The use of a special synergistic additive for recycling polyethylene modified asphalt system as claimed in claim 1, characterized in that: The synergistic additive is used in the recycled polyethylene modified asphalt system.
4. The use of a special synergistic additive for recycling polyethylene modified asphalt system according to claim 3, characterized in that: The base asphalt was heated to 195 °C, and 10% of the mass of the base asphalt was recycled polyethylene and 1%-3% of the mass of the base asphalt was added evenly. A high-speed modified asphalt emulsifying shearing machine was used to stir at 2500 r / min for 30 min and then sheared at 6000 r / min for 60 min.
5. The use of a special synergistic aid for recycling polyethylene modified asphalt system according to claim 4, characterized in that: The dosage of the above-mentioned synergistic additive for the recycled polyethylene modified asphalt system is 2% of the mass of the recycled polyethylene modified asphalt system.
Citation Information
Patent Citations
Vegetable oil-based hydrophilic polymer aqueous dispersion as well as preparation method and application thereof
CN113354769A
Amphiphilic low-molecular-weight organic oil gelling agent for offshore oil spill treatment and preparation method thereof
CN115322115A
Novel compound and organic nanotube gel including the same
JP2021084877A