A solid electrolyte membrane, a preparation method thereof and a solid-state battery
By stacking the second film layer on the upper and lower surfaces of the first film layer of the solid electrolyte membrane and performing hot pressing composite, adjusting the particle size ratio and binder content, the problems of high porosity and low ionic conductivity of the solid electrolyte membrane are solved. , improves the performance and stability of solid-state batteries.
Patent Information
- Application Number
- CN202410895972.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-07-05
AI Technical Summary
The solid electrolyte membrane prepared by the existing dry film forming process has high porosity and low ionic conductivity, which leads to poor battery performance and prone to lithium-ion short circuits.
Using a double-layer structure, the solid electrolyte membrane is used to stack the second membrane layer on the upper and lower surfaces of the first membrane layer and perform hot pressing composite to adjust the particle size ratio and binder content, reduce the surface porosity, improve the ionic conductivity and Tensile strength.
The surface porosity and thickness of the solid electrolyte membrane are significantly reduced, its ionic conductivity and tensile strength are improved, the charging and discharging performance of solid-state batteries is improved, and the occurrence of lithium-ion short circuits is reduced.
Smart Images

Figure CN118431552B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of secondary batteries, and in particular to a solid electrolyte membrane, a preparation method thereof, and a solid-state battery. Background Art
[0002] There are two main methods for preparing inorganic all-solid-state electrolyte membranes: wet coating process and dry film forming process. Among them, the wet coating process is to stir and disperse the inorganic solid electrolyte material, binder and organic solvent at high speed to prepare a uniform slurry for coating. This process is simple and feasible, and the technology is relatively mature, but most inorganic solid electrolytes are unstable to water, oxygen and organic solvents, which leads to the deterioration of solid electrolyte materials and the ion conductivity cannot meet the requirements. The dry film forming process can avoid the use of solvents. It mainly fiberizes the solid electrolyte powder and binder, and constructs a network-like skeleton through the fibers of the binder to support the solid electrolyte powder, and then rolls it into a film.
[0003] However, the solid electrolyte membranes currently produced by dry film forming rollers often have many holes on the surface, the solid electrolyte membrane cannot be thinned, the solid electrolyte membrane is prone to cracking, or the ion conductivity is low. Using a solid electrolyte membrane with many holes on the surface to assemble a battery will cause contact failure between the positive and negative electrodes and the solid electrolyte membrane interface, resulting in poor battery performance and even lithium short circuit. If the thickness of the solid electrolyte membrane is too thick, it will affect the energy density of the battery and reduce battery performance. Summary of the invention
[0004] Based on the above-mentioned deficiencies, the present application provides a solid electrolyte membrane, a preparation method thereof and a solid-state battery to improve the problems of high surface porosity and poor ion conductivity of the solid electrolyte membrane in the related art.
[0005] This application is implemented as follows:
[0006] In a first aspect, an example of the present application provides a solid electrolyte membrane, comprising a first membrane layer and a second membrane layer hot-pressed and composited on the upper and lower surfaces of the first membrane layer; the raw material of the first membrane layer comprises first solid electrolyte particles, the raw material of the second membrane layer comprises second solid electrolyte particles, the ratio of D50 of the second solid electrolyte particles to D50 of the first solid electrolyte particles is 1:2~20, and the ratio of D50 to D90 of the first solid electrolyte particles is 1:1.25~5, and the ratio of D50 to D90 of the second solid electrolyte particles is 1:1~1.1.
[0007] In the above implementation process, the solid electrolyte membrane includes a first membrane layer and a second membrane layer hot-pressed and composited on the upper and lower surfaces of the first membrane layer, and the raw material of the second membrane layer includes second solid electrolyte particles, and the ratio of D50 (D50 refers to the particle size corresponding to when the cumulative particle size distribution percentage of a sample reaches 50%, and its physical meaning is that particles with a particle size larger than it account for 50%, and particles with a particle size smaller than it also account for 50%) of the second solid electrolyte particles to D50 of the first solid electrolyte particles is 1:2~20, and the ratio of D50 to D90 (D90 It refers to the particle size corresponding to when the cumulative particle size distribution percentage of a sample reaches 90%. Its physical meaning is that particles with a smaller size than it also account for 90%, and particles with a larger size than it account for 10%) is 1:1.25~5. The ratio of D50 to D90 of the second solid electrolyte particles is 1:1~1.1, which can reduce the surface porosity of the solid electrolyte membrane (surface porosity refers to the percentage of surface pore area), improve the ionic conductivity and tensile strength of the solid electrolyte membrane, and when applied to solid-state batteries, can improve the charge and discharge performance of solid-state batteries.
[0008] In combination with the first aspect, in an optional embodiment of the present application, the D50 of the second solid electrolyte particles is 0.5-1 μm; the D50 of the first solid electrolyte particles is 2-8 μm.
[0009] In the above implementation process, the D50 of the second solid electrolyte particles in the second film layer located in the outer layer is 0.5~1 μm, and the D50 of the first solid electrolyte particles in the first film layer located in the inner layer is 2~8 μm. The outer layer and the inner layer are combined and, after hot pressing and compounding, a solid electrolyte membrane with lower porosity, higher ionic conductivity and good tensile strength can be obtained. When applied to solid-state batteries, the charging and discharging performance of the battery can be improved.
[0010] In combination with the first aspect, in an optional embodiment of the present application, the D50 of the first solid electrolyte particle is 5-8 μm. In combination with the first aspect, in an optional embodiment of the present application, the D90 of the first solid electrolyte particle is 5-10 μm.
[0011] In the above implementation process, the D50 of the first solid electrolyte particles in the first film layer is 2~8 μm, and the D90 is 5~10 μm. When the first film layer and the second film layer are subjected to composite hot pressing, it can be beneficial to the thinning of the solid electrolyte membrane. During hot pressing thinning, the probability of forming holes and cracks can be reduced, the surface porosity of the solid electrolyte membrane can be reduced, and the tensile strength can be improved.
[0012] In combination with the first aspect, in an optional embodiment of the present application, D90 of the second solid electrolyte particles is 0.5~1 μm.
[0013] In the above implementation process, the D50 of the second solid electrolyte particles in the second film layer is 0.5~1 μm, and the D90 is 0.5~1 μm. The second solid electrolyte particles in the second film layer are uniform fine particles. When the first film layer and the second film layer are compositely hot-pressed, the surface porosity of the solid electrolyte membrane can be reduced, and the surface smoothness of the solid electrolyte membrane can be improved. When applied to batteries, the interface contact between the solid electrolyte membrane and the positive and negative electrodes can be improved, and the problems of battery overcharging and short circuit can be improved.
[0014] In combination with the first aspect, in an optional embodiment of the present application, the thickness ratio of the second film layer to the first film layer is 1:2~6.
[0015] In the above implementation process, the thickness ratio of the second film layer to the first film layer is 1:2-6, which can further reduce the surface porosity of the solid electrolyte membrane and improve the surface smoothness of the solid electrolyte membrane.
[0016] In combination with the first aspect, in an optional embodiment of the present application, the materials of the first solid electrolyte particles and the second solid electrolyte particles are independently selected from one or more of a sulfide solid electrolyte, a halide solid electrolyte or an oxide solid electrolyte; or, the materials of the first solid electrolyte particles and the second solid electrolyte particles are both selected from a sulfide solid electrolyte.
[0017] In combination with the first aspect, in an optional embodiment of the present application, the first film layer further includes a first binder, and the second film layer further includes a second binder. In terms of mass percentage, the first film layer includes 0.2% to 10% of the first binder and 90% to 99.8% of the first solid electrolyte particles. And / or, in terms of mass percentage, the second film layer includes 0.2% to 10% of the second binder and 90% to 99.8% of the second solid electrolyte particles.
[0018] In the above implementation process, the content of the solid electrolyte particles in the first film layer and the second film layer is 90%~99.8%, which can improve the ionic conductivity of the solid electrolyte membrane and improve the charging and discharging performance of the battery when applied to the battery.
[0019] In combination with the first aspect, in an optional embodiment of the present application, the first film layer includes, by weight percentage, 0.2% to 5% of a first binder and 95% to 99.8% of first solid electrolyte particles; and / or, by weight percentage, the second film layer includes, by weight percentage, 0.2% to 5% of a second binder and 95% to 99.8% of second solid electrolyte particles.
[0020] In the above implementation process, the content of the solid electrolyte particles in the first membrane layer and the second membrane layer is 95% to 99.8%, which enables the solid electrolyte membrane to have a lower surface porosity and a higher ionic conductivity.
[0021] In combination with the first aspect, in an optional embodiment of the present application, the first binder and the second binder are independently selected from one or more of polytetrafluoroethylene, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polyethylene oxide, polypropylene or polyacrylonitrile.
[0022] In the above implementation process, polytetrafluoroethylene, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polyethylene oxide, polypropylene or polyacrylonitrile is used as a binder, which is easy to form a film and can improve the stability of the all-solid electrolyte membrane.
[0023] In a second aspect, an example of the present application provides a method for preparing the solid electrolyte membrane provided in the first aspect, comprising:
[0024] The second film layer is stacked on the upper and lower surfaces of the first film layer and hot pressed.
[0025] In the above implementation process, the second film layer containing the second solid electrolyte particles is stacked on the upper and lower surfaces of the first film layer containing the first solid electrolyte particles, and then the stacked film layers are hot pressed to make the first film layer and the second film layer composite, so that a solid electrolyte membrane with a three-layer composite structure can be obtained. Since the ratio of D50 of the second solid electrolyte particles to D50 of the first solid electrolyte particles is 1:2~20, and the ratio of D50 to D90 of the first solid electrolyte particles is 1:1.25~5, and the ratio of D50 to D90 of the second solid electrolyte particles is 1:1~1.1, when the first film layer and the second film layer are hot pressed and composited, the thickness and surface porosity of the solid electrolyte membrane can be reduced, and the ionic conductivity and tensile strength of the solid electrolyte membrane can be improved. When the prepared solid electrolyte membrane is applied to a solid-state battery, the charging and discharging performance of the solid-state battery can be improved.
[0026] In combination with the second aspect, in an optional embodiment of the present application, the hot pressing method includes multi-axis hot rolling, the rolling temperature is 80~150°C, the rolling speed is 1~100 rpm, and the horizontal and vertical calendering pressure is 5~30 t.
[0027] In the above implementation process, when the stacked first membrane layer and the second membrane layer are subjected to multi-axis hot rolling, the rolling temperature is 80~150°C, the rolling speed is 1~100 rpm, and the horizontal and vertical calendering pressures are 5~30 t, which can reduce the thickness of the solid electrolyte membrane, reduce the surface porosity of the solid electrolyte membrane, and improve the tensile strength of the solid electrolyte membrane.
[0028] In conjunction with the second aspect, in an optional embodiment of the present application, the method for preparing the first film layer and the second film layer includes:
[0029] The first raw material for forming the first film layer and the second raw material for forming the second film layer are mixed to obtain a first mixed material and a second mixed material; the first mixed material and the second mixed material are subjected to pre-insulation treatment, fiberization treatment and hot rolling treatment in sequence to obtain a first film layer and a second film layer respectively.
[0030] In the above implementation process, when preparing the first membrane layer or the second membrane layer, the raw materials are mixed, and then pre-insulation treatment and fiberization treatment are performed. The fibers can be used to support and fix the solid electrolyte particles, and then hot rolling treatment is performed to obtain a membrane layer of a certain thickness.
[0031] In combination with the second aspect, in an optional embodiment of the present application, the temperature of the pre-insulation treatment is 50-150° C., and the insulation time is 1-10 h.
[0032] In the above implementation process, the mixture is heated to 50-150°C and pre-insulated for 1-10 hours, which can facilitate the fiberization of the binder, fix and support the solid electrolyte particles, reduce the surface porosity of the solid electrolyte membrane, and improve the tensile strength of the solid electrolyte membrane.
[0033] In combination with the second aspect, in an optional embodiment of the present application, the temperature of the pre-insulation treatment is 120-150°C.
[0034] In the above implementation process, the mixture is heated to 120-150°C for pre-insulation, which can further reduce the surface porosity of the subsequently prepared solid electrolyte membrane and improve the tensile strength.
[0035] In combination with the second aspect, in an optional embodiment of the present application, the fiberization treatment method is selected from one or more of scraper stirring, ball milling or screw extrusion, with a rotation speed of 1000~3000 rpm and a time of 1~2 h.
[0036] In the above implementation process, the pre-insulated mixture is treated at a speed of 1000~3000 rpm for 1~2 h by scraper stirring, ball milling or spiral extrusion, which can cause the binder to fiberize, fix and support the solid electrolyte particles, improve the stability of the solid electrolyte membrane, reduce the surface porosity of the solid electrolyte membrane and increase the tensile strength.
[0037] In combination with the second aspect, in an optional implementation manner of the present application, the rotation speed is 1000~3000 rpm.
[0038] In the above implementation process, the pre-insulated mixture is treated at a rotation speed of 2000~3000 rpm for 1~2 h by scraper stirring, ball milling or spiral extrusion, which can further reduce the surface porosity of the solid electrolyte membrane and improve the tensile strength.
[0039] In a third aspect, an example of the present application provides a solid-state battery, comprising the solid-state electrolyte membrane provided in the first aspect.
[0040] In the above-mentioned implementation process, the solid-state battery provided in the embodiment of the present application includes the solid-state electrolyte membrane provided in the first aspect. The solid-state electrolyte membrane has a low thickness and a low surface porosity, has good surface flatness and smoothness, good tensile strength and a high ionic conductivity, and can improve the electrical properties of the solid-state battery such as charging and discharging. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the embodiments are briefly introduced below.
[0042] Figure 1 A schematic cross-sectional view of a solid electrolyte membrane provided as an example of this application;
[0043] Figure 2 A schematic diagram of the process flow of preparing a solid electrolyte membrane provided for the example of this application;
[0044] Figure 3 A schematic diagram of detecting a solid electrolyte membrane provided in an embodiment of the present application;
[0045] Figure 4 An optical photograph of the solid electrolyte membrane provided in Example 1 of the present application;
[0046] Figure 5 An optical photograph of the solid electrolyte membrane provided in Example 4 of the present application;
[0047] Figure 6 Optical photograph of the solid electrolyte membrane provided for Comparative Example 1 of the present application;
[0048] Figure 7 An optical photograph of a solid electrolyte membrane provided for Comparative Example 2 of the present application;
[0049] Figure 8 It is a comparison diagram of the optical photographs of Example 1 and Comparative Example 2 of the present application;
[0050] Fig. 9 The impedance spectrum of the solid electrolyte membrane provided in Example 1 of the present application;
[0051] Fig.10It is a charge and discharge performance curve diagram of a solid-state battery assembled with the solid electrolyte membrane provided in Example 1 and Comparative Example 2.
[0052] Icon: 100 - solid electrolyte membrane; 101 - first membrane layer; 1011 - first solid electrolyte particle; 102 - second membrane layer; 1021 - second solid electrolyte particle.
[0053] 10 - first hot pressing roller; 20 - second hot pressing roller; 30 - third hot pressing roller; 40 - guide roller; 50 - light board; 60 - fill light; 70 - CCD optical microscope. DETAILED DESCRIPTION
[0054] The embodiments of the present application will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. In the examples, if specific conditions are not specified, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0055] There are two main preparation processes for inorganic all-solid-state electrolyte membranes: wet coating process and dry film forming process.
[0056] In the wet coating process, since most inorganic solid electrolytes are unstable to water, oxygen and organic solvents, the solid electrolyte material may deteriorate easily, resulting in low ionic conductivity of the prepared solid electrolyte membrane, which cannot meet the requirements.
[0057] However, the solid electrolyte membranes currently produced by dry film forming rollers often have many holes on the surface (high surface porosity), the solid electrolyte membrane cannot be thinned, the solid electrolyte membrane is prone to cracking, and the ion conductivity is low. If a solid electrolyte membrane with many holes on the surface is used to assemble a battery, the contact between the positive and negative electrodes and the solid electrolyte membrane interface will fail, resulting in poor battery performance and even lithium short circuit. If the thickness of the solid electrolyte membrane is too thick, it will affect the energy density of the battery and reduce battery performance.
[0058] Therefore, the present application provides a solid electrolyte membrane and a method for preparing the same, which can improve the problems of high surface porosity, inability to thin, easy cracking and low ion conductivity of the dry solid electrolyte membrane to a certain extent. In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be described clearly and completely in conjunction with the accompanying drawings.
[0059] See also Figure 1The present application example provides a solid electrolyte membrane 100, including a first membrane layer 101 and a second membrane layer 102 hot-pressed and composited on the upper and lower surfaces of the first membrane layer 101; the raw material of the first membrane layer 101 includes first solid electrolyte particles 1011, the raw material of the second membrane layer 102 includes second solid electrolyte particles 1021, the ratio of D50 of the second solid electrolyte particles 1021 to the D50 of the first solid electrolyte particles 1011 is 1:2~20, and the ratio of D50 to D90 of the first solid electrolyte particles 1011 is 1:1.25~5, and the ratio of D50 to D90 of the second solid electrolyte particles 1021 is 1:1~1.1.
[0060] The method for preparing the solid electrolyte membrane 100 includes:
[0061] S1. Stack the second film layer 102 on the upper and lower surfaces of the first film layer 101 and perform heat pressing.
[0062] The stacked first film layer 101 and the second film layer 102 are hot pressed to obtain a three-layer composite structure solid electrolyte membrane 100. Among them, the ratio of D50 of the second solid electrolyte particles 1021 in the second film layer 102 located in the outer layer to the D50 of the first solid electrolyte particles 1011 in the first film layer 101 located in the inner layer is 1:2~20, and the ratio of D50 to D90 of the first solid electrolyte particles 1011 is 1:1.25~5, and the ratio of D50 to D90 of the second solid electrolyte particles 1021 is 1:1~1.1. When hot pressing composite, it is not only conducive to thinning the diaphragm solid electrolyte membrane 100 to obtain a thinner solid electrolyte membrane 100, but also can reduce the surface porosity of the solid electrolyte membrane 100, and improve the ionic conductivity and tensile strength of the solid electrolyte membrane 100.
[0063] The ratio of D50 to D90 of the first solid electrolyte particles 1011 in the first film layer 101 located in the inner layer is 1:1.25~5. The first solid electrolyte particles 1011 are relatively non-uniform large-size particles. When hot-pressing is performed in conjunction with the second film layer 102, they can promote the thinning of the solid electrolyte membrane 100 and reduce the probability of holes and tears in the solid electrolyte membrane 100 during thinning and hot pressing.
[0064] The ratio of D50 to D90 of the second solid electrolyte particles 1021 in the second membrane layer 102 located in the outer layer is 1:1~1.1. The second solid electrolyte particles 1021 are relatively uniform small particles. When combined with the first membrane layer 101 for hot pressing, they can reduce the surface porosity of the solid electrolyte membrane 100 and improve the flatness and smoothness of the solid electrolyte membrane 100.
[0065] In some possible embodiments, the ratio of D50 of the second solid electrolyte particles 1021 to D50 of the first solid electrolyte particles 1011 can be 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, 1:11, 1:12, 1:13, 1:14, 1:15, 1:16, 1:17, 1:18, 1:19 or 1:20, or a range between any two of them.
[0066] If the D50 of the second solid electrolyte particle 1021 is too large, the ratio of the D50 of the second solid electrolyte particle 1021 to the D50 of the first solid electrolyte particle 1011 is greater than 1:2-20, which will affect the strength of the solid electrolyte membrane 100 and increase the surface porosity of the solid electrolyte membrane 100. If the D50 of the first solid electrolyte particle 1011 is too large, the ratio of the D50 of the second solid electrolyte particle 1021 to the D50 of the first solid electrolyte particle 1011 is less than 1:2-20, which will affect the thinning property and strength of the solid electrolyte membrane 100.
[0067] In some possible embodiments, the ratio of D50 to D90 of the first solid electrolyte particles 1011 can be 1:1.25, 1:1.3, 1:1.35, 1:1.4, 1:1.45, 1:1.5, 1:1.55, 1:1.6, 1:1.65, 1:1.7, 1:1.75, 1:1.8, 1:1.85, 1:1.9, 1:1.95, 1:2, 1:2.5, 1:3, 1:3.5, 1:4, 1:4.5 or 1:5, or a range between any two of them.
[0068] If the ratio of D50 to D90 of the first solid electrolyte particles 1011 is less than 1:5, the particle size non-uniformity of the first solid electrolyte particles 1011 is relatively large, which will increase the surface porosity of the solid electrolyte membrane 100 and affect the strength of the solid electrolyte membrane 100. If the ratio of D50 to D90 of the first solid electrolyte particles 1011 is greater than 1:2.5, the particle size non-uniformity of the first solid electrolyte particles 1011 is relatively small, which is not conducive to the thinning of the solid electrolyte membrane 100 during hot pressing, and is likely to cause defects such as cracking of the solid electrolyte membrane 100. When applied to solid-state batteries, it will affect the energy density, charge and discharge performance of the solid-state batteries.
[0069] In some possible embodiments, the ratio of D50 to D90 of the second solid electrolyte particles 1021 may be 1:1, 1:1.01, 1:1.02, 1:1.03, 1:1.04, 1:1.05, 1:1.06, 1:1.07, 1:1.08, 1:1.09, 1:1 or a range between any two of them.
[0070] If the ratio of D50 to D90 of the second solid electrolyte particles 1021 is less than 1:1.1, the particle size non-uniformity of the second solid electrolyte particles 1021 increases, which will increase the surface porosity of the solid electrolyte membrane 100 .
[0071] In some possible embodiments, the D50 of the first solid electrolyte particles 1011 may be 2-8 μm.
[0072] Illustratively, D50 of the first solid electrolyte particles 1011 may be in a range between one or any two of 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm, 5.5 μm, 6 μm, 6.5 μm, 7 μm, 7.5 μm or 8 μm.
[0073] Furthermore, in some possible embodiments, the D50 of the first solid electrolyte particles 1011 may be 5-8 μm.
[0074] In some possible embodiments, the D90 of the first solid electrolyte particles 1011 may be 5-10 μm.
[0075] Illustratively, D90 of the first solid electrolyte particles 1011 may be in the range of one or any two of 5 μm, 5.5 μm, 6 μm, 6.5 μm, 7 μm, 7.5 μm, 8 μm, 8.5 μm, 9 μm, 9.5 μm or 10 μm.
[0076] Exemplarily, the first solid electrolyte particles 1011 have a D50 of 2 μm and a D90 of 5 μm.
[0077] Exemplarily, the first solid electrolyte particles 1011 have a D50 of 2 μm and a D90 of 10 μm.
[0078] Exemplarily, the first solid electrolyte particles 1011 have a D50 of 5 μm and a D90 of 8 μm.
[0079] Exemplarily, the first solid electrolyte particles 1011 have a D50 of 8 μm and a D90 of 10 μm.
[0080] In some possible embodiments, the D50 of the second solid electrolyte particles 1021 may be 0.5-1 μm.
[0081] Illustratively, the D50 of the second solid electrolyte particles 1021 may be in the range of one or between any two of 0.5 μm, 0.55 μm, 0.6 μm, 0.65 μm, 0.7 μm, 0.75 μm, 0.8 μm, 0.85 μm, 0.9 μm, 0.95 μm or 1 μm.
[0082] For example, the D50 of the first solid electrolyte particle 1011 may be 5 μm, and the D50 of the second solid electrolyte particle 1021 may be 0.8 μm.
[0083] For example, the D50 of the first solid electrolyte particle 1011 may be 2 μm, and the D50 of the second solid electrolyte particle 1021 may be 0.5 μm.
[0084] In some possible embodiments, the D90 of the second solid electrolyte particles 1021 may be 0.5-1 μm.
[0085] Illustratively, the D90 of the second solid electrolyte particles 1021 may be in the range of one or between any two of 0.5 μm, 0.55 μm, 0.6 μm, 0.65 μm, 0.7 μm, 0.75 μm, 0.8 μm, 0.85 μm, 0.9 μm, 0.95 μm or 1 μm.
[0086] For example, the D50 of the second solid electrolyte particles 1021 may be 0.8 μm, and the D90 may be 0.85 μm.
[0087] For example, the second solid electrolyte particles 1021 may have a D50 of 0.5 μm and a D90 of 0.5 μm.
[0088] For example, the second solid electrolyte particles 1021 may have a D50 of 1 μm and a D90 of 1 μm.
[0089] Exemplarily, in the solid electrolyte membrane 100 , the first solid electrolyte particles 1011 in the first membrane layer 101 have a D50 of 5 μm and a D90 of 8 μm; the second solid electrolyte particles 1021 in the second membrane layer 102 have a D50 of 0.8 μm and a D90 of 0.85 μm.
[0090] Furthermore, the present application example also provides a method for preparing the first film layer 101 and the second film layer 102, comprising:
[0091] S01. Preparation of the first film layer 101:
[0092] The first raw materials for forming the first film layer 101 are mixed to obtain a first mixed material; the first mixed material is sequentially subjected to a pre-heat-insulating treatment, a fiberizing treatment and a hot rolling treatment to obtain the first film layer 101 .
[0093] In some possible embodiments, the first raw material includes first solid electrolyte particles 1011 and a first binder.
[0094] The first raw material containing the first solid electrolyte particles 1011 and the first binder is mixed evenly, and then pre-heat-insulated and fiberized to fiberize the binder and bond the first solid electrolyte particles 1011 to the fiber skeleton. After hot rolling, a first film layer 101 with a certain thickness and flatness can be obtained.
[0095] In some possible embodiments, the first solid electrolyte particles 1011 may be selected from at least one of a sulfide solid electrolyte, a halide solid electrolyte, or an oxide solid electrolyte.
[0096] In some possible embodiments, the material of the sulfide solid electrolyte particles may be selected from one or more of a sulfur perovskite sulfide electrolyte, a LISICON sulfide electrolyte, a NASICON sulfide electrolyte, a garnet sulfide electrolyte, lithium sulfide or sodium sulfide.
[0097] Exemplarily, the halide solid electrolyte particles can be selected from lithium fluoride, potassium fluoride, Li2ZrCl6, Li3InCl6 or Li 1.75 ZrCl 4.75 O 0.5 One or more of .
[0098] Exemplarily, the oxide solid electrolyte particles may be selected from one or more of lithium lanthanum zirconium oxide, lithium lanthanum titanium oxide, lithium aluminum titanium phosphate, or lithium aluminum germanium phosphate.
[0099] In some possible embodiments, the binder may be selected from one or more of polytetrafluoroethylene, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polyethylene oxide, polypropylene or polyacrylonitrile.
[0100] Exemplarily, the binder may be selected from polytetrafluoroethylene.
[0101] Using polytetrafluoroethylene as a binder, polytetrafluoroethylene is easy to fiberize, which can reduce the amount of polytetrafluoroethylene used and improve the ionic conductivity of the solid electrolyte membrane.
[0102] Furthermore, in some possible embodiments, the first raw material includes 0.2% to 10% of the first binder and 90% to 99.8% of the first solid electrolyte particles 1011 in terms of mass percentage.
[0103] Illustratively, in the first raw material, the mass percentage of the first solid electrolyte particles 1011 can be 90%, 90.5%, 91%, 91.5%, 92%, 92.5%, 93%, 93.5%, 94%, 94.5%, 95%, 95.5%, 96%, 96.5%, 97%, 97.5%, 98%, 98.5%, 99%, 99.5% or 99.8%, or a range between any two of them.
[0104] Exemplarily, in the first raw material, the mass percentage of the first binder can be 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, 9.5% or 10% or a range between any two of them.
[0105] Exemplarily, based on mass percentage, the first raw material includes 98% of sulfide solid electrolyte particles and 2% of polytetrafluoroethylene binder.
[0106] Exemplarily, the first raw material includes 90% of sulfide solid electrolyte particles and 10% of polytetrafluoroethylene binder by mass percentage.
[0107] Furthermore, in some possible embodiments, the first raw material includes 95% to 99.8% of first solid electrolyte particles and 0.2% to 0.5% of a first binder in terms of mass percentage.
[0108] In some possible embodiments, the method of pre-insulating the first mixed material includes: the pre-insulating temperature is 50-150° C., and the insulation time is 1-10 h.
[0109] Exemplarily, the pre-insulation temperature may be 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, 125°C, 130°C, 135°C, 140°C, 145°C or 150°C, or a range between any two thereof.
[0110] Exemplarily, the pre-insulation time can be one of 1 h, 2 h, 3 h, 4 h, 5 h, 6 h, 7 h, 8 h, 9 h or 10 h, or a range between any two of them.
[0111] Furthermore, in some possible embodiments, the pre-insulation temperature may be 120-150°C.
[0112] In some possible embodiments, the fiberization treatment method is selected from one or more of scraper stirring, ball milling or screw extrusion.
[0113] Furthermore, in some possible embodiments, during the fiberization treatment, the rotation speed can be selected from 1000 to 3000 rpm, and the time is 1 to 2 h.
[0114] For example, the rotation speed during the fiberization process may be one of 1000 rpm, 1100 rpm, 1200 rpm, 1500 rpm, 1700 rpm, 2000 rpm, 2100 rpm, 2200 rpm, 2500 rpm or 3000 rpm, or a range between any two of them.
[0115] Furthermore, in some possible embodiments, the rotation speed during the fiberization process may be 2000-3000 rpm.
[0116] S02. Preparation of the second film layer 102:
[0117] The second raw materials for forming the second film layer 102 are mixed to obtain a second mixed material; the second mixed material is sequentially subjected to a pre-heat-insulating treatment, a fiberizing treatment and a hot rolling treatment to obtain the second film layer 102 .
[0118] The second raw material includes second solid electrolyte particles 1021 and a second binder.
[0119] The selection range of the second adhesive is the same as that of the first adhesive, and will not be described in detail here.
[0120] The method of pre-insulating, fiberizing and hot rolling the second mixture can refer to the method of pre-insulating, fiberizing and hot rolling the first mixture when preparing the first film layer 101, and will not be repeated here.
[0121] In some possible embodiments, the ratio of the thickness of the second film layer 102 to the thickness of the first film layer 101 may be 1:2-6.
[0122] Exemplarily, the ratio of the thickness of the second film layer 102 to the thickness of the first film layer 101 may be 1:2, 1:2.5, 1:3, 1:3.5, 1:4, 1:4.5, 1:5, 1:5.5 or 1:6 or a range between any two of them.
[0123] Furthermore, the thickness ratio of the second film layer 102 to the first film layer 101 may be 1:3.
[0124] Furthermore, in some possible embodiments, the thickness of the second film layer 102 may be 5-15 μm, and the thickness of the first film layer 101 may be 15-50 μm.
[0125] In some possible embodiments, in step S1, the second film layer 102 is stacked on the upper and lower surfaces of the first film layer 101 and hot pressed, including:
[0126] The second film layer 102, the first film layer 101 and the second film layer 102 are stacked together in sequence, and then subjected to multi-axis hot rolling, the rolling temperature is 80-150°C, the rolling machine speed is 1-100 rpm, and the horizontal and vertical calendering pressures are 5-30t.
[0127] Furthermore, the present application example also provides a solid electrolyte membrane preparation device: comprising a first hot pressing roller 10, and second hot pressing rollers 20 are arranged above and below the first hot pressing roller 10. A third hot pressing roller 30 is arranged at the rear end of the first hot pressing roller 10.
[0128] See also Figure 2 The first hot pressing roller 10 is used to hot press the first mixed material to obtain the first film layer 101, and the upper and lower second hot pressing rollers 20 are used to hot press the second mixed material separately to obtain two layers of second film layers 102. The first film layer 101 is transported to the third hot pressing roller 30 via the guide roller 40, and the upper second film layer 102 and the lower second film layer 102 are transported to the third hot pressing roller 30 via the corresponding guide rollers 40 respectively. The third hot pressing roller 30 hot presses the composite film layers stacked in the order of the second film layer 102, the first film layer 101 and the second film layer 102.
[0129] Furthermore, the present application example also provides a detection device for a solid electrolyte membrane, see Figure 3 , including two light plates 50, the two light plates 50 are arranged at an interval, used to support the solid electrolyte membrane 100, and the area to be detected of the solid electrolyte membrane 100 is suspended in the gap between the two light plates 50. A fill light 60 is arranged below the gap between the two light plates 50, used to fill light to the area to be detected of the solid electrolyte membrane 100. A CCD optical microscope 70 is arranged above the gap between the two light plates 50, used to collect photos of the area to be detected of the solid electrolyte membrane 100.
[0130] Furthermore, the present application example also provides a method for detecting a solid electrolyte membrane, comprising:
[0131] The solid electrolyte membrane 100 is placed on the light plate 50, and the solid electrolyte membrane 100 is illuminated by the fill light 60 at the bottom. The solid electrolyte membrane 100 is photographed by the CCD optical microscope 70 arranged on the top, and the porosity and pore size distribution of the photographs are statistically analyzed to realize the quality evaluation of the solid electrolyte membrane 100.
[0132] The present application example also provides a solid-state battery, including the solid-state electrolyte membrane 100 provided in the present application example.
[0133] Furthermore, in some possible embodiments, the solid-state battery further includes a positive electrode sheet and a negative electrode sheet, and the solid electrolyte membrane 100 is located between the positive electrode sheet and the negative electrode sheet.
[0134] The solid electrolyte membrane 100 provided in the embodiment of the present application has the characteristics of low surface porosity, small thickness, high ionic conductivity, good tensile strength and smooth surface. When applied to solid-state batteries, it can have good interface contact with the positive and negative electrodes of the solid-state battery, and can improve the energy density and charge and discharge performance of the solid-state battery, and reduce the probability of lithium plating short circuit in the solid-state battery.
[0135] The solid electrolyte membrane 100 of the present application is further described in detail below in conjunction with embodiments.
[0136] Example 1
[0137] Embodiment 1 provides a solid electrolyte membrane 100, and the preparation method thereof is as follows:
[0138] (1) Preparation of the first film layer 101:
[0139] First, 20 g of the sulfide first solid electrolyte particles 1011 (Li6PS5Cl, D50=5 μm, D90=8 μm, and the ratio of D50 to D90 is 1:1.6) are placed in a scraper stirring tank, and 0.41 g of polytetrafluoroethylene binder (the mass ratio of the first solid electrolyte particles 1011 to the binder is 98:2) is weighed and placed in a scraper stirring tank, and mixed at a speed of 200 rpm for 1 h to obtain a first mixture.
[0140] Then, the first mixed material was placed in a vacuum oven and pre-heated at 150° C. for 1 h to obtain a first pre-heated mixed material.
[0141] The first pre-insulated mixture was placed in a scraper stirring tank for fiberization at a stirring speed of 3000 rpm for 2 h to obtain a first fiberized mixture.
[0142] The first fiberized mixture was placed on a roller press to form a film. The rolling temperature was 100° C., the speed of the roller press was 25 rpm, and the pressure was 5 t, thereby obtaining a first film layer 101 with a thickness of 75 μm.
[0143] (2) Preparation of the second film layer 102:
[0144] The preparation method of the second film layer 102 is similar to the preparation method of the first film layer 101, except that:
[0145] The second solid electrolyte particles 1021 are: Li6PS5Cl, D50=0.8 μm, D90=0.8 μm (the ratio of D50 to D90 is 1:1). The thickness of the second film layer 102 is 25 μm.
[0146] (3) Hot pressing:
[0147] The second membrane layer 102, the first membrane layer 101 and the second membrane layer 102 are stacked in sequence (the thickness ratio of the second membrane layer 102: the first membrane layer 101: the second membrane layer 102 is 1:3:1), and hot rolling is performed. The rolling temperature is 100 μm, the rolling machine speed is 25 rpm, and the pressure is 8 t to obtain a solid electrolyte membrane 100 with a thickness of 100 μm.
[0148] Example 2
[0149] Example 2 provides a solid electrolyte membrane 100, which is different from Example 1 in that the mass ratio of solid electrolyte particles to binder is 90:10, the stirring speed during fiberization treatment is 3000 rpm, and the time is 3 h.
[0150] Example 3
[0151] Embodiment 3 provides a solid electrolyte membrane 100 , which is different from Embodiment 1 in that the pre-heating temperature is 100° C.
[0152] Example 4
[0153] Embodiment 4 provides a solid electrolyte membrane 100, which is different from Embodiment 1 in that:
[0154] The thickness ratio of the second film layer 102 : the first film layer 101 : the second film layer 102 is 1:10:1.
[0155] Example 5
[0156] Embodiment 5 provides a solid electrolyte membrane 100, which is different from Embodiment 1 in that:
[0157] The first solid electrolyte particle 1011 is Li6PS5Cl, D50=10 μm, D90=12.5 μm (the ratio of D50 to D90 is 1:1.25); the second solid electrolyte particle 1021 is Li6PS5Cl, D50=1 μm, D90=1 μm (the ratio of D50 to D90 is 1:1).
[0158] Example 6
[0159] Embodiment 6 provides a solid electrolyte membrane 100, which is different from Embodiment 1 in that:
[0160] During the fiberization treatment, the stirring speed was 1000 rpm.
[0161] Comparative Example 1
[0162] Comparative Example 1 provides a solid electrolyte membrane, which is different from Example 1 in that:
[0163] Without performing step (1) and step (3), the second membrane layer 102 is a solid electrolyte membrane 100 obtained according to the method of step (2). The thickness of the solid electrolyte membrane 100 is 100 μm.
[0164] Comparative Example 2
[0165] Comparative Example 2 provides a solid electrolyte membrane, which differs from Example 1 in that: Step (2) and Step (3) are not performed, and the first membrane layer 101 obtained by the method of Step (1) is a solid electrolyte membrane 100, and the thickness of the solid electrolyte membrane 100 is 100 μm.
[0166] Comparative Example 3
[0167] Comparative Example 3 provides a solid electrolyte membrane, which differs from Example 1 in that the raw material for preparing the first membrane layer 101 and the raw material for preparing the second membrane layer 102 are mixed, and pre-insulation treatment, fiberization treatment and rolling treatment are performed in sequence to obtain a single-layer solid electrolyte membrane.
[0168] Comparative Example 4
[0169] Comparative Example 4 provides a solid electrolyte membrane, which is different from Example 1 in that:
[0170] In step (3), the first membrane layer 101, the second membrane layer 102 and the first membrane layer 101 are stacked in sequence and hot rolled at a rolling temperature of 100°C, a rolling machine speed of 25 rpm and a pressure of 8t to obtain a solid electrolyte membrane 100 with a thickness of 100 μm.
[0171] Test Example 1
[0172] The surface porosity test of the solid electrolyte membranes provided in Examples 1-6 and Comparative Examples 1-4 was performed, and the test method included: placing the solid electrolyte membrane 100 on the light board 50, irradiating the solid electrolyte membrane 100 through the fill light 60 at the bottom, and collecting photos of the solid electrolyte membrane 100 through the CCD optical microscope 70 configured at the top. The porosity of the collected photos was statistically analyzed, and the statistical results are shown in Table 1. The optical photos of the solid electrolyte membranes provided in Example 1, Example 4, Comparative Example 1 and Comparative Example 2 are shown in Table 1. Figure 4-Figure 8 shown.
[0173] Table 1 Performance test table
[0174]
[0175] Test Example 2
[0176] The electrical performance of the solid electrolyte membranes provided in Examples 1-6 and Comparative Examples 1-4 was tested, and the testing method was as follows:
[0177] The solid electrolyte membrane was placed in the mold battery, and a pressure of 300 MPa was applied and maintained at this pressure. The interface impedance value was tested at room temperature, and the ionic conductivity was calculated. The test results are shown in Table 1. The electrochemical performance of the solid-state battery assembled using the mold was tested. The positive electrode sheet, solid electrolyte membrane sheet, and negative electrode sheet were placed in the mold battery in turn, and a pressure of 500 MPa was applied and maintained at this pressure. The charge and discharge performance was tested. The test results are shown in Table 1.
[0178] The impedance spectrum of Example 1 is as follows Fig. 9 As shown, the charge and discharge test curves of the solid-state batteries assembled with the solid electrolyte membranes of Example 1 and Comparative Example 2 are as follows Fig.10 shown.
[0179] Result analysis:
[0180] Figure 4 In the embodiment 1, the surface of the solid electrolyte membrane is flat and smooth, with almost no holes; Figure 5 In the solid electrolyte membrane provided in Example 4, the thickness ratio of the second membrane layer to the first membrane layer is 1:10, and the surface of the obtained solid electrolyte membrane has a large number of large particle protrusions (for example Figure 5 The part enclosed by the dotted line in the middle), the surface is smooth but the flatness is poor. Figure 4 and Figure 5 It can be seen that in the embodiment of the present application, the thickness ratio of the second film layer to the first film layer is 1:2-6, which can further improve the surface flatness and smoothness of the solid electrolyte membrane.
[0181] Figure 6 In the solid electrolyte membrane provided in Comparative Example 1, all the solid electrolyte particles are relatively uniform small particles, and a large number of strip-shaped cracks (e.g. Figure 6 The part enclosed by the dotted circle); Figure 7 In the solid electrolyte membrane provided in Comparative Example 2, all the solid electrolyte particles are relatively large particles with relatively uneven distribution, and a large number of holes (e.g. Figure 7 The part enclosed by the dotted line). Figure 8 By comparing Example 1 and Comparative Example 2, it can be seen that the solid electrolyte membrane prepared according to the preparation method provided in the example of the present application has a lower surface porosity and a higher surface smoothness.
[0182] In Table 1, by comparing Examples 1-6 and Comparative Examples 1-4, it can be seen that the solid electrolyte membrane prepared by the preparation method provided by the examples of the present application has a lower thickness, a lower surface porosity (lower percentage of surface pore area), a higher ionic conductivity and a higher tensile strength.
[0183] Combining Example 1 with Example 2, it can be seen that the mass ratio of the solid electrolyte particles to the binder in Example 1 is 98:2, and the mass ratio of the solid electrolyte particles to the binder in Example 2 is 90:10. The ionic conductivity of the solid electrolyte membrane obtained in Example 1 is higher than the ionic conductivity of the solid electrolyte membrane obtained in Example 2, indicating that the raw materials for forming the first film layer or the second film layer include 0.2% to 10% of the binder and 90% to 99.8% of the solid electrolyte particles in terms of mass percentage, which can improve the ionic conductivity of the solid electrolyte membrane and improve the discharge specific capacity of the solid-state battery without substantially affecting the surface porosity.
[0184] Combining Example 1 with Example 3, it can be seen that the pre-insulation temperature in Example 1 is 150°C, and the pre-insulation temperature in Example 3 is 100°C. The surface porosity of the solid electrolyte membrane obtained in Example 1 is much lower than the surface porosity of the solid electrolyte membrane obtained in Example 3, indicating that pre-insulation at a temperature of 120~150°C in the embodiments of the present application can further reduce the surface porosity of the solid electrolyte membrane and improve the discharge specific capacity of the solid-state battery.
[0185] Combining Example 1 with Example 4, it can be seen that the thickness ratio of the second film layer to the first film layer in Example 1 is 1:3, and the thickness ratio of the second film layer to the first film layer in Example 4 is 1:10. The surface porosity of the solid electrolyte membrane obtained in Example 1 is lower than the surface porosity of the solid electrolyte membrane obtained in Example 5, indicating that in the embodiments of the present application, the thickness ratio of the second film layer to the first film layer is 1:2~6, which can further reduce the surface porosity of the solid electrolyte membrane and improve the discharge specific capacity of the solid-state battery.
[0186] Combining Example 1 with Example 5, it can be seen that the first solid electrolyte particles in Example 1 have D50=5 μm and D90=8 μm, and the first solid electrolyte particles in Example 5 have D50=10 μm and D90=12.5 μm. The ionic conductivity and discharge specific capacity of the solid electrolyte membrane provided in Example 1 are higher than the ionic conductivity and discharge specific capacity of the solid electrolyte membrane provided in Example 5, indicating that in the embodiments of the present application, the D50 of the second solid electrolyte particles is 0.5~1 μm and D90 is 0.5~1 μm, and the D50 of the first solid electrolyte particles is 2~8 μm and D90 is 5~10 μm, which can further improve the ionic conductivity of the solid electrolyte membrane and the discharge specific capacity of the solid-state battery.
[0187] Combining Example 1 with Example 6, it can be seen that the stirring speed during the fiberization treatment in Example 1 is 3000 rpm, and the stirring speed during the fiberization treatment in Example 6 is 1000 rpm. The surface porosity of the solid electrolyte membrane provided in Example 1 is lower than the surface porosity of the solid electrolyte membrane provided in Example 6, indicating that the fiberization treatment in the embodiment of the present application is performed at a speed of 2000~3000 rpm, which can further reduce the surface porosity of the solid electrolyte membrane, improve the ionic conductivity, and improve the discharge specific capacity of the solid-state battery.
[0188] Combining Example 1 with Comparative Examples 1-2, it can be seen that in Example 1, the three-layer composite solid electrolyte membrane prepared by stacking the second film layer, the first film layer and the second film layer in order and then hot pressing has lower surface porosity and higher tensile strength, which can improve the discharge specific capacity of the solid-state battery.
[0189] Fig.10 In the test, the solid-state battery prepared according to the solid electrolyte membrane provided in Example 1 can be charged and discharged normally, while the solid-state battery prepared according to the solid electrolyte membrane provided in Comparative Example 2 short-circuited during the charge and discharge test.
[0190] Combining Example 1 with Comparative Examples 3-4, it can be seen that in Comparative Example 3, the raw material for preparing the first film layer 101 and the raw material for preparing the second film layer 102 are mixed, and pre-insulation treatment, fiberization treatment and rolling treatment are carried out in sequence to obtain a solid electrolyte membrane with a single-layer structure, which will increase the surface porosity of the solid electrolyte membrane and reduce the discharge specific capacity of the solid-state battery; in Comparative Example 4, the first film layer 101, the second film layer 102 and the first film layer 101 are stacked in sequence and hot rolled, and the obtained solid electrolyte membrane has a higher surface porosity, and a short circuit occurs during the charge and discharge performance test.
[0191] In summary, according to the preparation method provided in the embodiment of the present application, the second film layer is stacked on the upper and lower surfaces of the first film layer, and hot pressed, wherein the ratio of D50 of the second solid electrolyte particles in the second film layer to the D50 of the first solid electrolyte particles in the first film layer is 1:2~20, and the ratio of D50 to D90 of the first solid electrolyte particles is 1:1.25~5, and the ratio of D50 to D90 of the second solid electrolyte particles is 1:1~1.1, which can reduce the surface porosity of the prepared solid electrolyte membrane, improve ionic conductivity and tensile strength. When applied to solid-state batteries, it can improve the charge and discharge performance of solid-state batteries.
[0192] The above description is only the preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.
Claims
1. A solid electrolyte membrane, characterized in that: The invention comprises a first film layer and a second film layer which is hot-pressed and composited to the upper and lower surfaces of the first film layer; the raw material of the first film layer comprises first solid electrolyte particles, the raw material of the second film layer comprises second solid electrolyte particles, the ratio of D50 of the second solid electrolyte particles to D50 of the first solid electrolyte particles is 1:6.25-20, the ratio of D50 to D90 of the first solid electrolyte particles is 1:1.25-5, and the ratio of D50 to D90 of the second solid electrolyte particles is 1:1-1.1; the D50 of the second solid electrolyte particles is 0.5-1 μm; the D50 of the first solid electrolyte particles is 2-8 μm.
2. The solid electrolyte membrane according to claim 1, characterized in that The D50 of the first solid electrolyte particles is 5-8 μm.
3. The solid electrolyte membrane according to claim 1, characterized in that The D90 of the first solid electrolyte particles is 5-10 μm.
4. The solid electrolyte membrane according to claim 1, characterized in that The D90 of the second solid electrolyte particles is 0.5-1 μm.
5. The solid electrolyte membrane according to claim 1, characterized in that The thickness ratio of the second film layer to the first film layer is 1:2-6.
6. The solid electrolyte membrane according to claim 1, characterized in that The first solid electrolyte particles and the second solid electrolyte particles are independently selected from one or more of sulfide solid electrolyte particles, halide solid electrolyte particles or oxide solid electrolyte particles; Alternatively, the first solid electrolyte particles and the second solid electrolyte particles are both selected from sulfide solid electrolyte particles.
7. The solid electrolyte membrane according to claim 1, characterized in that The first film layer further comprises a first adhesive, and the second film layer further comprises a second adhesive; Calculated by mass percentage, the first film layer includes 0.2% to 10% of the first binder and 90% to 99.8% of the first solid electrolyte particles; And / or, in terms of mass percentage, the second film layer includes 0.2% to 10% of the second binder and 90% to 99.8% of the second solid electrolyte particles.
8. The solid electrolyte membrane according to claim 7, characterized in that Calculated by mass percentage, the first film layer includes 0.2% to 5% of the first binder and 95% to 99.8% of the first solid electrolyte particles; And / or, in terms of mass percentage, the second film layer includes 0.2% to 5% of the second binder and 95% to 99.8% of the second solid electrolyte particles.
9. The solid electrolyte membrane according to claim 7, characterized in that: The first binder and the second binder are independently selected from one or more of polytetrafluoroethylene, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polyethylene oxide, polypropylene or polyacrylonitrile.
10. A method for preparing a solid electrolyte membrane according to any one of claims 1 to 9, characterized in that: include: The second film layer is stacked on the upper and lower surfaces of the first film layer and hot pressed.
11. The preparation method according to claim 10, characterized in that The hot pressing method includes multi-axis hot rolling pressing, the rolling temperature is 80-150°C, the rolling speed is 1-100 rpm, and the pressure is 5-30 t.
12. The preparation method according to claim 10, characterized in that: The preparation method of the first film layer and the second film layer comprises: The first raw material for forming the first film layer and the second raw material for forming the second film layer are mixed to obtain a first mixture and a second mixture; the first mixture and the second mixture are subjected to pre-insulation treatment, fiberization treatment and hot rolling treatment in sequence to obtain the first film layer and the second film layer respectively.
13. The preparation method according to claim 12, characterized in that The pre-heat preservation treatment is performed at a temperature of 50-150° C. and a heat preservation time of 1-10 h.
14. The preparation method according to claim 13, characterized in that The temperature of the pre-insulation treatment is 120-150°C.
15. The preparation method according to claim 12, characterized in that: The fiberization treatment method is selected from one or more of scraper stirring, ball milling or screw extrusion, with a rotation speed of 1000-3000 rpm and a time of 1-2 h.
16. The preparation method according to claim 15, characterized in that The rotation speed is 2000~3000 rpm.
17. A solid-state battery, characterized in that: A solid electrolyte membrane comprising the solid electrolyte membrane according to any one of claims 1 to 9.
Citation Information
Patent Citations
Preparation and processing method of solid electrolyte membrane
CN112421114A
Composite solid electrolyte membrane and preparation method and application thereof
CN116505063A
Solid-state electrolyte membrane and application thereof in solid-state lithium-sulfur battery
CN117613363A