Antibacterial outer catheter for tampon and preparation method thereof
By acidizing and oxidizing treatment and modification treatment on the outer surface of the tampon, antibacterial liquid is prepared in combination with modified nanotitanium dioxide and polyurethane acrylate and other materials to form an antibacterial coating, the problem of insufficient antibacterial properties on the inner and outer surfaces of the catheter is solved, and the problem of insufficient antibacterial properties on the inner and outer surfaces of the catheter is realized Long-lasting antibacterial and lubricating properties reduce the risk of infection and inconvenience of use.
Patent Information
- Application Number
- CN202410602487.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-15
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-05-15
AI Technical Summary
The existing tampon outer catheter lacks antibacterial properties, resulting in the risk of bacterial growth and infection. The existing antibacterial coating sprayed on the outside of the outer catheter cannot guarantee the internal antibacteriality and is inconvenient to use.
By acidizing and oxidizing treatment and thiolation modification on the surface of the outer catheter, antibacterial liquid is prepared by combining modified nanotitanium dioxide and polyurethane acrylate and other materials, impregnating and ultraviolet curing to form an antibacterial coating to ensure that both the inner and outer surfaces of the catheter are antibacterial and lubricating. sex.
It realizes the long-lasting antibacterial and lubricating properties of the inner and outer surfaces of the catheter, reduces the risk of bacterial growth, improves the convenience of use and antibacterial effect.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of tampons, and in particular relates to an antibacterial outer catheter for a tampon and a preparation method thereof. Background Art
[0002] Tampons, also known as sanitary plugs, can be inserted into the vagina to absorb menstrual blood. Tampons are a cotton cylinder, mainly made of cotton, synthetic fibers or a mixture of these two materials, with diameters ranging from 1 cm to 1.9 cm, with a cotton thread (drawstring) attached to the end. The degree of arc at the tip of the tampon varies from brand to brand, allowing users to choose according to their own usage habits.
[0003] Conventional tampons usually include two inner and outer tubes. The outer tube is generally used to store the tampon, and the inner tube is generally used to push it. However, the outer tube is basically made of plastic, which does not have antibacterial properties. Many women think that tampons and plastic tube walls are not hygienic enough, and they are worried that bacteria will be introduced into the uterus and cause infection, increasing the chance of infection and even causing toxic shock syndrome.
[0004] In the prior art, some technicians have improved the lubricity and antibacterial properties of the outer catheter of tampons by coating the outer catheter with antibacterial lubricants. For example, Chinese patent CN107693837A discloses the preparation and application of an antibacterial lubricant for the outer tube of tampons, and its technical scheme is: antibacterial metal oxides, a small amount of rare earth mineral elements and a chelating agent are mixed in a certain proportion, and then gradually added dropwise to an oily system under stirring conditions to form a stable water-in-oil system; reacting in a reactor at 120-170°C for 30-120 minutes, cooling, and centrifugation to remove sediments to obtain a lubricant with antibacterial effects; the antibacterial lubricant is sprayed on the outer tube of the tampon to facilitate catheter implantation and has an antibacterial effect, effectively overcoming the skin allergy problem of the currently commonly used organic antibacterial agents and the precipitation and discoloration problem caused by inorganic silver ion antibacterial agents. The outer tube microorganisms are removed, and its lubricity is improved. It has a strong antibacterial function, has no irritation or allergy to the human body, is safe and environmentally friendly; especially when used as a lubricant for the outer tube of tampons, it can effectively overcome the current concerns about excessive microorganisms in the outer tube of tampons. Although the tampon outer tube lubricant has good antibacterial properties and has no irritation to the human body, it is sprayed on the outer wall of the outer catheter after all, and there is still residue when it is inserted. Due to the presence of the lubricant, when the hand is stained with the lubricant, it is easy to slide, and it is also inconvenient to use. At the same time, it is only coated on the outside of the outer catheter, and the antibacterial properties of the inner side of the catheter cannot be guaranteed. Therefore, it needs further improvement. Summary of the invention
[0005] In view of the deficiencies in the prior art, the object of the present invention is to provide an antibacterial outer catheter for a tampon and a preparation method thereof. The antibacterial outer catheter is coated with an antibacterial coating on the surface of the outer catheter so that both the inner and outer surfaces of the outer catheter have antibacterial properties and antibacterial durability. During storage, bacteria will not colonize on the surface of the tampon. At the same time, it also has a certain lubricity and has good application prospects.
[0006] To achieve the above object, the present invention provides the following technical solutions:
[0007] A method for preparing an antibacterial catheter for a tampon comprises the following steps:
[0008] S1. Pretreatment of the outer catheter of the tampon: Add KMnO 4 / HNO 3 dipping in the mixed solution, washing and drying after the dipping is completed to obtain a pretreated tampon outer catheter;
[0009] S2. Modification of the outer conduit of the tampon: adding the pretreated outer conduit of the tampon in step S1 into the γ-mercaptopropyltrimethoxysilane solution, stirring the solution, washing and drying the solution after the treatment, and obtaining a modified outer conduit of the tampon;
[0010] S3, preparation of antibacterial liquid: under light-proof conditions, polyurethane acrylate, isopropyl alcohol, polyvinyl pyrrolidone, and polyacrylamide are added to a reaction kettle, and after stirring evenly, modified nano-titanium dioxide and benzophenone are added, and stirring is continued for 5-10 minutes to obtain the antibacterial liquid;
[0011] S4, preparation of antibacterial catheter: adding the modified tampon outer catheter in step S2 into the antibacterial liquid for dipping, drying after dipping, then UV curing, then washing and drying, to obtain the antibacterial outer catheter for tampon.
[0012] Preferably, the immersion temperature in step S1 is 30-40°C and the time is 3-4h; the KMnO 4 / HNO 3 The mixed solution was prepared as follows: 5-10 g of 20% HNO 3 Add 25-40g of 10% KMnO 4 Add to aqueous solution and stir evenly to obtain.
[0013] In the present invention, the surface of the outer catheter is subjected to an acidification and oxidation treatment to increase the active reaction sites on the surface of the outer catheter, which is beneficial to improving the adhesion between the antibacterial liquid and the outer catheter.
[0014] Preferably, the stirring treatment temperature in step S2 is 50-60°C and the time is 2-3h; the preparation method of the γ-mercaptopropyltrimethoxysilane solution is as follows: add 5-10g of γ-mercaptopropyltrimethoxysilane solution to 100g of 80% ethanol solution by mass and stir for 30-40min.
[0015] In the present invention, the outer conduit is modified by γ-mercaptopropyltrimethoxysilane, so that mercapto groups are introduced into the surface of the outer conduit, which is beneficial to improve the bonding force between the outer conduit and the modified nano-titanium dioxide.
[0016] Preferably, the preparation method of the modified nano titanium dioxide in step S3 is as follows:
[0017] (a) adding nano titanium dioxide to an ethanol aqueous solution, then adding 3-chloropropyltriethoxysilane, stirring to react, filtering, washing, and drying after the reaction is completed to obtain pretreated nano titanium dioxide;
[0018] (b) adding the pretreated nano-titanium dioxide in step (a) to DMF, followed by adding 5-guanidine valeric acid, and reacting at a constant temperature under a nitrogen atmosphere, adding triethylamine during the reaction to maintain the pH at 7, and centrifuging, filtering, washing, and drying after the reaction to obtain a solid product;
[0019] (c) adding the solid product in step (b) to a 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride solution, stirring and activating, adding 4-amino-3-fluoroallyl benzoate and N-hydroxysuccinimide, heating to react, filtering, washing, drying and grinding after the reaction is completed, to obtain the modified nano titanium dioxide.
[0020] Preferably, the mass fraction of ethanol in the ethanol aqueous solution in step (a) is 50-60%; the mass ratio of the nano-titanium dioxide, ethanol aqueous solution and 3-chloropropyltriethoxysilane is 100:800-1000:10-20; the temperature of the stirring reaction is 60-70°C and the time is 3-5h.
[0021] Preferably, in step (b), the mass ratio of the pretreated nano-titanium dioxide, DMF, and 5-guanidine valeric acid is 100:1000-1500:7-13; the temperature of the isothermal reaction is 110-120° C., and the time is 6-9 hours.
[0022] Preferably, the mass fraction of the 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride solution in step (c) is 10-15%; the mass ratio of the solid product, 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride solution, 4-amino-3-fluoroallyl benzoate, and N-hydroxysuccinimide is 100:1000-1500:9-15:60-90; the temperature of the heating reaction is 80-90°C, and the time is 4-6h.
[0023] In the present invention, the prepared antibacterial liquid uses nano titanium dioxide as a raw material. Titanium dioxide itself has good antibacterial properties. By modifying it, not only the antibacterial properties of the nano titanium dioxide are improved, but also the bonding strength between it and the outer catheter is improved, making the antibacterial liquid less likely to fall off, thereby improving the long-lasting antibacterial properties of the outer catheter of the tampon.
[0024] Preferably, in step S3, the mass ratio of polyurethane acrylate, isopropyl alcohol, polyvinyl pyrrolidone, polyacrylamide, modified nano titanium dioxide and benzophenone is 50-60:40-50:5-10:5-10:10-20:0.3-0.6; the stirring temperature is 30-40° C. and the stirring time is 20-30 min.
[0025] More preferably, in step S3, the mass ratio of polyurethane acrylate, isopropyl alcohol, polyvinyl pyrrolidone, polyacrylamide, modified nano-titanium dioxide and benzophenone is 55-60:45-50:8-10:7-10:15-20:0.4-0.6; the stirring temperature is 35-40° C. and the stirring time is 20-25 min.
[0026] Preferably, the drying temperature in step S4 is 80-90°C and the drying time is 30-40 minutes; the UV curing process is: the UV irradiation intensity is 100-200 mW / cm 2 , time is 1-2min.
[0027] More preferably, the drying temperature in step S4 is 85-90°C and the drying time is 30-35 min; the UV curing process is: the UV irradiation intensity is 150-200 mW / cm 2 , time is 1-2min.
[0028] The present invention also protects an antibacterial outer catheter for tampons prepared by the method.
[0029] Compared with the prior art, the present invention has the following beneficial effects:
[0030] (1) The antibacterial outer catheter for tampons provided by the present invention is first subjected to chemical oxidation in acidic potassium permanganate to improve the reaction activity of its surface, and then the pretreated outer catheter of the tampon is thiol-modified to facilitate the next step of the reaction; then polyurethane acrylate, isopropyl alcohol, polyvinyl pyrrolidone, polyacrylamide, modified nano-titanium dioxide, and benzophenone are mixed to prepare an antibacterial liquid, and then the modified outer catheter of the tampon is immersed in the antibacterial liquid to make the antibacterial liquid adhere to the inner and outer surfaces of the outer catheter, and through drying and ultraviolet irradiation, on the one hand, the antibacterial coating can be firmly attached to the outer catheter after curing, and on the other hand, the thiol group on the modified outer catheter of the tampon can react with the double bond on the modified nano-titanium dioxide, so that the nano-titanium dioxide is more firmly combined with the outer catheter and is not easy to fall off, thereby improving the durable antibacterial property of the outer catheter of the tampon.
[0031] (2) The antibacterial outer catheter for tampons provided by the present invention is added with a modified antibacterial liquid. Nano titanium dioxide is used as a raw material. 3-chloropropyltriethoxysilane is first reacted with titanium dioxide. The silane water corner is then grafted with the nano titanium dioxide to improve the dispersibility of the nano titanium dioxide. At the same time, a chloropropyl group is introduced on the surface of the titanium dioxide, which is beneficial to the next step of the reaction. Then, the pretreated nano titanium dioxide is reacted with 5-guanidine valeric acid to introduce guanidine and carboxyl groups on the surface of the nano titanium dioxide. The guanidine group has good antibacterial properties and can further improve the antibacterial properties of the nano titanium dioxide. The introduction of the guanidine group on the surface of the titanium dioxide by chemical bonding improves the Its antibacterial persistence, and the introduced carboxyl group is also conducive to the next reaction; finally, the solid product is reacted with 4-amino-3-fluoroallyl benzoate, and through the amidation reaction of the carboxyl group and the amino group, 4-amino-3-fluoroallyl benzoate is introduced into the nano-titanium dioxide through a chemical bond. The fluorine-containing group in 4-amino-3-fluoroallyl benzoate can improve the lubricity of the antibacterial liquid, so that the outer catheter has better lubricity, and the double bond it contains can also react with the thiol group on the outer catheter under ultraviolet light, thereby improving the binding force between the outer catheter and the modified nano-titanium dioxide, and making the outer catheter have a longer-lasting antibacterial property. DETAILED DESCRIPTION
[0032] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] The polyurethane acrylate was purchased from Kangdis Chemical (Hubei) Co., Ltd.; the nano titanium dioxide was purchased from Qinghe Chaotai Metal Materials Co., Ltd., with a particle size of 300-500 nm.
[0034] Example 1
[0035] A method for preparing an antibacterial outer catheter for a tampon, characterized in that it comprises the following steps:
[0036] S1. Pretreatment of the outer catheter of the tampon: Add KMnO 4 / HNO 3 The mixture was immersed in the solution at 35°C for 3.5 hours, and washed and dried after the immersion to obtain the pretreated tampon outer catheter. 4 / HNO 3 The mixed solution was prepared as follows: 10 g of 20% HNO 3 Add 40g of KMnO with a mass concentration of 10% 4 In aqueous solution, stir evenly to obtain;
[0037] S2. Modification of the outer catheter of the tampon: add the pretreated outer catheter of the tampon in step S1 into the γ-mercaptopropyltrimethoxysilane solution, stir and treat at 55° C. for 2.5 hours, wash with deionized water after the treatment, and dry at 80° C. for 4 hours to obtain a modified outer catheter of the tampon, wherein the preparation method of the γ-mercaptopropyltrimethoxysilane solution is as follows: add 10g of the γ-mercaptopropyltrimethoxysilane solution into 100g of an ethanol solution with a mass fraction of 80%, and stir for 40 minutes to obtain;
[0038] S3, preparation of antibacterial liquid: under light-proof conditions, 55g of polyurethane acrylate, 45g of isopropanol, 7g of polyvinyl pyrrolidone, and 8g of polyacrylamide were added to a reaction kettle, stirred at 35°C for 25min, and then 15g of modified nano-titanium dioxide and 0.5g of benzophenone were added, and stirring was continued for 8min to obtain the antibacterial liquid;
[0039] S4. Preparation of antibacterial outer catheter: Add the modified tampon outer catheter in step S2 into the antibacterial solution, immerse at 45°C for 1.5 hours, dry at 80°C for 4 hours, and then irradiate at an ultraviolet radiation intensity of 150 mW / cm 2 The resulting mixture was cured under ultraviolet light for 2 minutes, then washed with deionized water, and dried at 90° C. for 3 hours to obtain the antibacterial outer catheter for tampons.
[0040] Wherein, the preparation method of the modified nano titanium dioxide in step S3 is as follows:
[0041] (a) adding 100 g of nano-titanium dioxide to 900 g of 50% ethanol aqueous solution, then adding 15 g of 3-chloropropyltriethoxysilane, stirring and reacting at 65° C. for 4 h, filtering, washing and drying after the reaction is completed to obtain pretreated nano-titanium dioxide;
[0042] (b) adding 100 g of the pretreated nano-titanium dioxide in step (a) to 1300 g of DMF, followed by adding 10 g of 5-guanidine valeric acid, and reacting at 115° C. for 8 h under a nitrogen atmosphere, adding triethylamine during the reaction to maintain the pH at 7, and after the reaction is completed, centrifuging, filtering, washing, and drying to obtain a solid product;
[0043] (c) adding 100 g of the solid product in step (b) to 1300 g of a 10% by mass solution of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride, stirring and activating at 40° C. for 1 h, adding 12 g of 4-amino-3-fluoroallyl benzoate and 80 g of N-hydroxysuccinimide, reacting at 85° C. for 5 h, filtering, washing, drying and grinding after the reaction is completed to obtain the modified nano titanium dioxide.
[0044] Example 2
[0045] A method for preparing an antibacterial outer catheter for a tampon, characterized in that it comprises the following steps:
[0046] S1. Pretreatment of the outer catheter of the tampon: Add KMnO 4 / HNO 3 The mixture was immersed in the solution at 35°C for 3.5 hours, and washed and dried after the immersion to obtain the pretreated tampon outer catheter. 4 / HNO 3 The mixed solution was prepared as follows: 10 g of 20% HNO 3 Add 40g of KMnO with a mass concentration of 10% 4 In aqueous solution, stir evenly to obtain;
[0047] S2. Modification of the outer catheter of the tampon: add the pretreated outer catheter of the tampon in step S1 into the γ-mercaptopropyltrimethoxysilane solution, stir and treat at 55° C. for 2.5 hours, wash with deionized water after the treatment, and dry at 80° C. for 4 hours to obtain a modified outer catheter of the tampon, wherein the preparation method of the γ-mercaptopropyltrimethoxysilane solution is as follows: add 10g of the γ-mercaptopropyltrimethoxysilane solution into 100g of an ethanol solution with a mass fraction of 80%, and stir for 40 minutes to obtain;
[0048] S3, preparation of antibacterial liquid: under light-proof conditions, 55g of polyurethane acrylate, 45g of isopropanol, 8g of polyvinyl pyrrolidone, and 7g of polyacrylamide were added to a reaction kettle, stirred at 35°C for 25min, and then 15g of modified nano-titanium dioxide and 0.4g of benzophenone were added, and stirring was continued for 7min to obtain the antibacterial liquid;
[0049] S4. Preparation of antibacterial outer catheter: Add the modified tampon outer catheter in step S2 into the antibacterial solution, immerse at 45°C for 1.5 hours, dry at 80°C for 4 hours, and then irradiate at an ultraviolet radiation intensity of 150 mW / cm 2 The resulting mixture was cured under ultraviolet light for 1 minute, then washed with deionized water, and dried at 90° C. for 3 hours to obtain the antibacterial outer catheter for tampons.
[0050] Wherein, the preparation method of the modified nano titanium dioxide in step S3 is as follows:
[0051] (a) adding 100 g of nano-titanium dioxide to 900 g of 60% ethanol aqueous solution, then adding 15 g of 3-chloropropyltriethoxysilane, stirring and reacting at 65° C. for 4 h, filtering, washing and drying after the reaction is completed to obtain pretreated nano-titanium dioxide;
[0052] (b) adding 100 g of the pretreated nano-titanium dioxide in step (a) to 1300 g of DMF, followed by adding 10 g of 5-guanidine valeric acid, and reacting at 115° C. for 7 h under a nitrogen atmosphere, adding triethylamine during the reaction to maintain the pH at 7, and after the reaction is completed, centrifuging, filtering, washing, and drying to obtain a solid product;
[0053] (c) 100 g of the solid product in step (b) is added to 1300 g of a 15% by mass solution of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride, and after stirring and activating at 40° C. for 1 h, 12 g of 4-amino-3-fluoroallyl benzoate and 70 g of N-hydroxysuccinimide are added, and the mixture is reacted at 85° C. for 5 h. After the reaction is completed, the mixture is filtered, washed, dried, and ground to obtain the modified nano titanium dioxide.
[0054] Example 3
[0055] A method for preparing an antibacterial outer catheter for a tampon, characterized in that it comprises the following steps:
[0056] S1. Pretreatment of the outer catheter of the tampon: Add KMnO 4 / HNO 3 The mixture was immersed in the solution at 30°C for 4 hours, and washed and dried after the immersion to obtain the pretreated tampon outer catheter. 4 / HNO 3 The mixed solution was prepared as follows: 10 g of 20% HNO 3 Add 40g of KMnO with a mass concentration of 10% 4 In aqueous solution, stir evenly to obtain;
[0057] S2. Modification of the outer catheter of the tampon: add the pretreated outer catheter of the tampon in step S1 into the γ-mercaptopropyltrimethoxysilane solution, stir and treat at 50° C. for 3 hours, wash with deionized water after the treatment, and dry at 80° C. for 4 hours to obtain a modified outer catheter of the tampon, wherein the preparation method of the γ-mercaptopropyltrimethoxysilane solution is as follows: add 10g of the γ-mercaptopropyltrimethoxysilane solution into 100g of an ethanol solution with a mass fraction of 80%, and stir for 40 minutes to obtain;
[0058] S3, preparation of antibacterial liquid: under light-proof conditions, add 50g of polyurethane acrylate, 40g of isopropanol, 5g of polyvinyl pyrrolidone, and 5g of polyacrylamide into a reaction kettle, stir at 30°C for 30min, then add 10g of modified nano-titanium dioxide and 0.3g of benzophenone, and continue stirring for 5min to obtain the antibacterial liquid;
[0059] S4, preparation of antibacterial outer catheter: add the modified tampon outer catheter in step S2 into the antibacterial liquid, immerse at 40°C for 2 hours, dry at 80°C for 4 hours after immersion, and then irradiate with ultraviolet radiation at an intensity of 100 mW / cm 2 The resulting mixture was cured under ultraviolet light for 2 minutes, then washed with deionized water, and dried at 90° C. for 3 hours to obtain the antibacterial outer catheter for tampons.
[0060] Wherein, the preparation method of the modified nano titanium dioxide in step S3 is as follows:
[0061] (a) adding 100 g of nano-titanium dioxide to 800 g of 50% ethanol aqueous solution, then adding 10 g of 3-chloropropyltriethoxysilane, stirring and reacting at 60° C. for 5 h, filtering, washing and drying after the reaction is completed to obtain pretreated nano-titanium dioxide;
[0062] (b) adding 100 g of the pretreated nano-titanium dioxide in step (a) to 1000 g of DMF, followed by adding 7 g of 5-guanidine valeric acid, and reacting at 110° C. for 9 h under a nitrogen atmosphere, adding triethylamine during the reaction to maintain the pH at 7, and after the reaction is completed, centrifuging, filtering, washing, and drying to obtain a solid product;
[0063] (c) adding 100 g of the solid product in step (b) to 1000 g of a 15% by mass solution of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride, stirring and activating at 40° C. for 1 h, adding 9 g of 4-amino-3-fluoroallyl benzoate and 60 g of N-hydroxysuccinimide, reacting at 80° C. for 6 h, filtering, washing, drying and grinding after the reaction is completed, to obtain the modified nano titanium dioxide.
[0064] Example 4
[0065] A method for preparing an antibacterial outer catheter for a tampon, characterized in that it comprises the following steps:
[0066] S1. Pretreatment of the outer catheter of the tampon: Add KMnO 4 / HNO 3 The mixture was immersed in the solution at 40°C for 3 hours, and washed and dried after the immersion to obtain the pretreated tampon outer catheter. 4 / HNO 3 The mixed solution was prepared as follows: 10 g of 20% HNO 3 Add 40g of KMnO with a mass concentration of 10% 4 In aqueous solution, stir evenly to obtain;
[0067] S2. Modification of the outer catheter of the tampon: add the pretreated outer catheter of the tampon in step S1 into the γ-mercaptopropyltrimethoxysilane solution, stir and treat at 60° C. for 2 hours, wash with deionized water after the treatment, and dry at 80° C. for 4 hours to obtain a modified outer catheter of the tampon, wherein the preparation method of the γ-mercaptopropyltrimethoxysilane solution is as follows: add 10g of the γ-mercaptopropyltrimethoxysilane solution into 100g of an ethanol solution with a mass fraction of 80%, and stir for 40 minutes to obtain;
[0068] S3, preparation of antibacterial liquid: under light-proof conditions, add 60g of polyurethane acrylate, 50g of isopropanol, 10g of polyvinyl pyrrolidone, and 10g of polyacrylamide into a reaction kettle, stir at 40°C for 20min, then add 20g of modified nano-titanium dioxide and 0.6g of benzophenone, and continue stirring for 5min to obtain the antibacterial liquid;
[0069] S4. Preparation of antibacterial outer catheter: Add the modified tampon outer catheter in step S2 into the antibacterial solution, immerse at 50°C for 1 hour, dry at 80°C for 4 hours, and then irradiate with ultraviolet light at an intensity of 200 mW / cm 2 The resulting mixture was cured under ultraviolet light for 1 minute, then washed with deionized water, and dried at 90° C. for 3 hours to obtain the antibacterial outer catheter for tampons.
[0070] Wherein, the preparation method of the modified nano titanium dioxide in step S3 is as follows:
[0071] (a) adding 100 g of nano-titanium dioxide to 1000 g of 60% ethanol aqueous solution, then adding 20 g of 3-chloropropyltriethoxysilane, stirring and reacting at 70° C. for 3 h, filtering, washing and drying after the reaction is completed to obtain pretreated nano-titanium dioxide;
[0072] (b) adding 100 g of the pretreated nano-titanium dioxide in step (a) to 1500 g of DMF, followed by adding 13 g of 5-guanidine valeric acid, and reacting at 120° C. for 6 h under a nitrogen atmosphere, adding triethylamine during the reaction to maintain the pH at 7, and after the reaction is completed, centrifuging, filtering, washing, and drying to obtain a solid product;
[0073] (c) adding 100 g of the solid product in step (b) to 1500 g of a 10% by mass solution of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride, stirring and activating at 40° C. for 1 h, adding 15 g of 4-amino-3-fluoroallyl benzoate and 90 g of N-hydroxysuccinimide, reacting at 90° C. for 4 h, filtering, washing, drying and grinding after the reaction is completed to obtain the modified nano titanium dioxide.
[0074] Comparative Example 1
[0075] A method for preparing an antibacterial outer catheter for a tampon, characterized in that it comprises the following steps:
[0076] S1. Pretreatment of the outer catheter of the tampon: Add KMnO 4 / HNO 3 The mixture was immersed in the solution at 35°C for 3.5 hours, and washed and dried after the immersion to obtain the pretreated tampon outer catheter. 4 / HNO 3 The mixed solution was prepared as follows: 10 g of 20% HNO 3 Add 40g of KMnO with a mass concentration of 10% 4 In aqueous solution, stir evenly to obtain;
[0077] S2. Modification of the outer catheter of the tampon: add the pretreated outer catheter of the tampon in step S1 into the γ-mercaptopropyltrimethoxysilane solution, stir and treat at 55° C. for 2.5 hours, wash with deionized water after the treatment, and dry at 80° C. for 4 hours to obtain a modified outer catheter of the tampon, wherein the preparation method of the γ-mercaptopropyltrimethoxysilane solution is as follows: add 10g of the γ-mercaptopropyltrimethoxysilane solution into 100g of an ethanol solution with a mass fraction of 80%, and stir for 40 minutes to obtain;
[0078] S3, preparation of antibacterial liquid: under light-proof conditions, 55g of polyurethane acrylate, 45g of isopropyl alcohol, 7g of polyvinyl pyrrolidone, and 8g of polyacrylamide were added to a reaction kettle, stirred at 35°C for 25min, and then 15g of nano-titanium dioxide and 0.5g of benzophenone were added, and stirring was continued for 8min to obtain the antibacterial liquid;
[0079] S4. Preparation of antibacterial outer catheter: Add the modified tampon outer catheter in step S2 into the antibacterial solution, immerse at 45°C for 1.5 hours, dry at 80°C for 4 hours, and then irradiate at an ultraviolet radiation intensity of 150 mW / cm 2 The resulting mixture was cured under ultraviolet light for 2 minutes, then washed with deionized water, and dried at 90° C. for 3 hours to obtain the antibacterial outer catheter for tampons.
[0080] Comparative Example 2
[0081] A method for preparing an antibacterial outer catheter for a tampon, characterized in that it comprises the following steps:
[0082] S1. Pretreatment of the outer catheter of the tampon: Add KMnO 4 / HNO 3 The mixture was immersed in the solution at 35°C for 3.5 hours, and washed and dried after the immersion to obtain the pretreated tampon outer catheter. 4 / HNO 3 The mixed solution was prepared as follows: 10 g of 20% HNO 3 Add 40g of KMnO with a mass concentration of 10% 4 In aqueous solution, stir evenly to obtain;
[0083] S2. Modification of the outer catheter of the tampon: add the pretreated outer catheter of the tampon in step S1 into the γ-mercaptopropyltrimethoxysilane solution, stir and treat at 55° C. for 2.5 hours, wash with deionized water after the treatment, and dry at 80° C. for 4 hours to obtain a modified outer catheter of the tampon, wherein the preparation method of the γ-mercaptopropyltrimethoxysilane solution is as follows: add 10g of the γ-mercaptopropyltrimethoxysilane solution into 100g of an ethanol solution with a mass fraction of 80%, and stir for 40 minutes to obtain;
[0084] S3, preparation of antibacterial liquid: under light-proof conditions, 55g of polyurethane acrylate, 45g of isopropanol, 7g of polyvinyl pyrrolidone, and 8g of polyacrylamide were added to a reaction kettle, stirred at 35°C for 25min, and then 15g of modified nano-titanium dioxide and 0.5g of benzophenone were added, and stirring was continued for 8min to obtain the antibacterial liquid;
[0085] S4. Preparation of antibacterial outer catheter: Add the modified tampon outer catheter in step S2 into the antibacterial solution, immerse at 45°C for 1.5 hours, dry at 80°C for 4 hours, and then irradiate at an ultraviolet radiation intensity of 150 mW / cm 2 The resulting mixture was cured under ultraviolet light for 2 minutes, then washed with deionized water, and dried at 90° C. for 3 hours to obtain the antibacterial outer catheter for tampons.
[0086] Wherein, the preparation method of the modified nano titanium dioxide in step S3 is as follows:
[0087] (a) adding 100 g of nano-titanium dioxide to 900 g of 50% ethanol aqueous solution, then adding 15 g of 3-chloropropyltriethoxysilane, stirring and reacting at 65° C. for 4 h, filtering, washing and drying after the reaction is completed to obtain pretreated nano-titanium dioxide;
[0088] (b) adding 100 g of the pretreated nano-titanium dioxide in step (a) to 1300 g of DMF, followed by adding 10 g of 5-guanidine valeric acid, and reacting at 115° C. for 8 h under a nitrogen atmosphere. During the reaction, triethylamine was added to maintain the pH at 7. After the reaction was completed, the mixture was centrifuged, filtered, washed, dried, and ground to obtain the modified nano-titanium dioxide.
[0089] The tampons prepared in Examples 1-4 and Comparative Examples 1-2 were tested for performance using an antibacterial outer catheter. Referring to Standard YY0325-2016 and Technical Specifications for Disinfection, the antibacterial ring test method was used to test the antibacterial properties of the above products. Staphylococcus aureus (ATCC25923) and Escherichia coli (ATCC25922) were used as test strains. The incubator temperature was 40°C, the humidity was 60%, and the culture cycles were 1d, 3d, and 5d. The specific test data are shown in Table 1:
[0090] Table 1
[0091] 1d antibacterial ring diameter / mm 3d antibacterial ring diameter / mm 5d antibacterial ring diameter / mm Example 1 26.4 22.9 21.5 Example 2 25.8 22.6 20.4 Example 3 24.7 21.4 19.6 Example 4 26.2 22.1 20.8 Comparative Example 1 23.8 19.2 16.6 Comparative Example 2 25.9 21.7 20.3
[0092] It can be seen from the data in Table 1 that the antibacterial outer catheter for tampons prepared by the present invention has good antibacterial and antimicrobial effects. Compared with comparative examples 1-2, it has good antibacterial effects and long antibacterial time, and has good application prospects.
[0093] The antibacterial outer catheter of the tampon prepared in Example 1 and Comparative Examples 1-2 was subjected to an antibacterial durability test and a friction coefficient test. The specific method of the antibacterial durability test is: the sample is placed in a sodium chloride solution with a mass fraction of 5% for 6 hours, and then rinsed in a medical alcohol with a mass fraction of 75% for 1 hour, repeated 30 times, and the antibacterial ring experiment is performed again, and the test cycle is 1 day; the friction coefficient test: the outer catheter of the tampon is soaked in water for 30 seconds, and then fixed on the groove plate, and water is injected into the water tank until the sample is completely immersed therein, and a 200g standard slider is gently placed above the sample, and the slider is dragged by the sensor connecting rod to move at a speed of 100mm / min, and the dynamic friction coefficient is measured. The specific test data are shown in Table 2:
[0094] Table 2
[0095] Example 1 Comparative Example 1 Comparative Example 2 1d antibacterial ring diameter / mm 24.8 18.1 19.8 Friction coefficient 0.16 0.34 0.35
[0096] It can be seen from the data in Table 2 that after rinsing, the antibacterial rings of Comparative Examples 1 and 2 decreased significantly, and the antibacterial effect decreased significantly, indicating that the adhesion between the antibacterial liquid and the catheter was less, and the antibacterial property decreased after rinsing. After 30 rinses, the antibacterial ring of the antibacterial outer catheter for tampons prepared in Example 1 only decreased slightly, and it had good antibacterial durability. At the same time, according to the data of the friction coefficient, it can be seen that the antibacterial outer catheter for tampons prepared by the present invention has a lower friction coefficient, which can reduce discomfort during use and has good application prospects.
[0097] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing an antibacterial outer catheter for a tampon, characterized in that: The following steps are involved: S1. Pretreatment of the outer catheter of the tampon: adding the outer catheter of the tampon to a KMnO4 / HNO3 mixed solution for dipping, washing and drying after the dipping is completed to obtain a pretreated outer catheter of the tampon; S2. Modification of the outer conduit of the tampon: adding the pretreated outer conduit of the tampon in step S1 into the γ-mercaptopropyltrimethoxysilane solution, stirring the solution, washing and drying the solution after the treatment, and obtaining a modified outer conduit of the tampon; S3, preparation of antibacterial liquid: under light-proof conditions, polyurethane acrylate, isopropyl alcohol, polyvinyl pyrrolidone, and polyacrylamide are added to a reaction kettle, and after stirring evenly, modified nano-titanium dioxide and benzophenone are added, and stirring is continued for 5-10 minutes to obtain the antibacterial liquid; S4, preparation of an antibacterial outer catheter: adding the modified tampon outer catheter in step S2 into an antibacterial liquid for dipping, drying after dipping, then UV curing, then washing and drying, to obtain the antibacterial outer catheter for the tampon; Wherein, the preparation method of the modified nano titanium dioxide in step S3 is as follows: (a) adding nano titanium dioxide to an ethanol aqueous solution, then adding 3-chloropropyltriethoxysilane, stirring to react, filtering, washing, and drying after the reaction is completed to obtain pretreated nano titanium dioxide; (b) adding the pretreated nano-titanium dioxide in step (a) to DMF, followed by adding 5-guanidine valeric acid, and reacting at a constant temperature under a nitrogen atmosphere, adding triethylamine during the reaction to maintain the pH at 7, and centrifuging, filtering, washing, and drying after the reaction to obtain a solid product; (c) adding the solid product in step (b) to a 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride solution, stirring and activating, adding 4-amino-3-fluoroallyl benzoate and N-hydroxysuccinimide, heating to react, filtering, washing, drying and grinding after the reaction is completed, to obtain the modified nano titanium dioxide.
2. The preparation method according to claim 1, characterized in that: The immersion temperature in step S1 is 30-40°C and the time is 3-4h; the preparation method of the KMnO4 / HNO3 mixed solution is as follows: add 5-10g of HNO3 with a mass fraction of 20% to 25-40g of KMnO4 aqueous solution with a mass concentration of 10%, stir evenly, and obtain.
3. The preparation method according to claim 1, characterized in that: The stirring treatment temperature in step S2 is 50-60°C and the time is 2-3h; the preparation method of the γ-mercaptopropyltrimethoxysilane solution is as follows: add 5-10g of γ-mercaptopropyltrimethoxysilane solution to 100g of 80% ethanol solution by mass and stir for 30-40min.
4. The preparation method according to claim 1, characterized in that: The mass fraction of ethanol in the ethanol aqueous solution in step (a) is 50-60%; the mass ratio of the nano-titanium dioxide, the ethanol aqueous solution and 3-chloropropyltriethoxysilane is 100:800-1000:10-20; the temperature of the stirring reaction is 60-70°C and the time is 3-5h.
5. The preparation method according to claim 1, characterized in that: The mass ratio of the pretreated nano-titanium dioxide, DMF and 5-guanidine valeric acid in step (b) is 100:1000-1500:7-13; the temperature of the isothermal reaction is 110-120° C. and the time is 6-9 hours.
6. The preparation method according to claim 1, characterized in that: The mass fraction of the 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride solution in step (c) is 10-15%; the mass ratio of the solid product, 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride solution, 4-amino-3-fluoroallyl benzoate, and N-hydroxysuccinimide is 100:1000-1500:9-15:60-90; the temperature of the heating reaction is 80-90°C and the time is 4-6h.
7. The preparation method according to claim 1, characterized in that: In step S3, the mass ratio of polyurethane acrylate, isopropyl alcohol, polyvinyl pyrrolidone, polyacrylamide, modified nano titanium dioxide and benzophenone is 50-60:40-50:5-10:5-10:10-20:0.3-0.6; the stirring temperature is 30-40° C. and the stirring time is 20-30 min.
8. The preparation method according to claim 1, characterized in that: The drying temperature in step S4 is 80-90°C and the drying time is 30-40 minutes; the UV curing process is: the UV radiation intensity is 100-200 mW / cm 2 , time is 1-2min.
9. An antibacterial outer catheter for tampon prepared by the method according to any one of claims 1 to 8.
Citation Information
Patent Citations
Application and preparation of antibacterial lubricant for tampon outer tubes
CN107693837A
Preparation method of antibacterial wear-resistant hydrophilic coating for medical catheter
CN116966352A