A method for preparing a polyolefin-based lithium battery separator with high thermal stability
By using a three-layer structure design of glass fiber polyolefin composite temperature-resistant support layer and graphene polyolefin composite conductive layer in lithium battery separator, combined with silane-modified glass fiber powder and reduced graphene oxide, the thermal stability of the polyolefin separator is solved. The problem of poor performance has achieved a lithium battery separator with high thermal stability and excellent conductivity.
Patent Information
- Application Number
- CN202410463885.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-17
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-04-17
AI Technical Summary
Poor thermal stability of polyolefin separators at high temperatures affects the safety of lithium batteries and is difficult to meet the requirements of high-power systems.
Using glass fiber polyolefin composite temperature-resistant support layer and graphene polyolefin composite conductive layer, a three-layer polyolefin-based lithium battery separator with meltblown technology was prepared, and using silane-modified glass fiber powder and reduced graphene oxide to improve the separator. Thermal stability and conductivity are used to avoid damage to the web structure by hot-rolled composites.
It significantly reduces the thermal shrinkage rate of the diaphragm, improves thermal stability and mechanical properties, and also has excellent electrical conductivity, avoids the risk of inorganic materials falling off and coating falling off, and ensures the performance stability of the diaphragm.
Smart Images

Figure BDA0004796633860000071
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polyolefin separators, and in particular relates to a method for preparing a polyolefin-based lithium battery separator with high thermal stability. Background Art
[0002] Lithium battery separator is a very important component of lithium battery. It can isolate the positive and negative electrodes and prevent internal short circuit of the battery, improve the efficiency and safety performance of the battery, and is an indispensable component of lithium battery. Lithium battery separator is generally made of polyolefin (PP) film, polyethylene (PE) film and other materials, but when the external temperature reaches or exceeds the melting point of the separator, the separator itself will shrink or melt over a large area, resulting in thermal runaway or short circuit inside the battery. Therefore, reducing the thermal shrinkage rate of the separator at high temperature is the key to improving battery safety. Lithium battery separator must have excellent electrolyte wettability, heat resistance, mechanical strength, high porous structure and ionic conductivity. Due to the high porosity and large specific surface area of non-woven fabrics, many non-woven-based separators have been used in lithium batteries.
[0003] Pure polyolefin separators have limited conductivity and thermal stability, and poor stability at high temperatures, which seriously affects the safety of the battery. It is difficult to meet the requirements of high-power systems, and its thermodynamic stability needs to be further improved. Inorganic ultrafine powder coating or composite modified polymer is one of the effective methods to improve the thermal stability of the separator. Using inorganic powders with high heat resistance, conductivity and mechanical strength as modifiers can improve the mechanical strength of the separator and reduce the thermal shrinkage of the separator.
[0004] The patent with application number CN201810585774.3 discloses a composite diaphragm for lithium batteries and its preparation method. A non-woven fabric made of melt-blown PP fibers is used as a substrate layer. LCP polymer solution is sprayed on both sides of the substrate layer to form a double-layer electrospun layer. The melt-blown polypropylene (PP) non-woven fabric plays a mechanical support role, and the liquid crystal polymer (LCP) electrospun layer plays a role in regulating the surface pore structure of the diaphragm, enhancing heat resistance and dimensional stability. Finally, PVDF is sprayed on the surface to form an effective closed-cell temperature and increase the adhesion with the positive and negative electrodes. The prepared diaphragm has enhanced mechanical properties and a certain heat resistance, but LCP has excellent electrical insulation properties, which is not conducive to the conductive properties of the diaphragm. Summary of the invention
[0005] The object of the present invention is to provide a method for preparing a polyolefin-based lithium battery separator with high thermal stability, so as to solve the problem that the polyolefin separator has poor thermal stability during use.
[0006] The purpose of the present invention can be achieved through the following technical solutions:
[0007] (1) Preparing a glass fiber polyolefin composite heat-resistant support layer: mixing glass fiber powder modified raw materials according to a ratio, and melt-blowing to form a polyolefin-based non-woven fiber membrane to obtain a glass fiber polyolefin composite heat-resistant support layer, wherein the glass fiber powder modified raw materials are polyolefin resin chips, vinyl silane and glass fiber powder;
[0008] (2) preparing a graphene polyolefin composite conductive layer: mixing reduced graphene oxide and polyolefin raw materials according to a proportion, and preparing the graphene polyolefin composite conductive layer by melt-blowing, wherein the reduced graphene oxide and polyolefin raw materials are reduced graphene oxide, polyolefin resin chips, and a compatibilizer;
[0009] (3) Preparation of polyolefin-based lithium battery separator: A glass fiber polyolefin composite heat-resistant support layer is used as the middle layer, and the upper and lower layers are graphene polyolefin composite conductive layers. After hydroentanglement and drying, a polyolefin-based lithium battery separator is obtained.
[0010] Furthermore, the glass fiber powder is 0.7-1 μm, and too large a particle size is not conducive to uniform dispersion.
[0011] Furthermore, the polyolefin resin slice is at least one of a polyethylene resin slice and a polypropylene resin slice.
[0012] Furthermore, the vinyl silane is one of vinyl silanes such as vinyl triethoxy silane, vinyl trimethoxy silane and vinyl tri(β-methoxyethoxy) silane.
[0013] Furthermore, the preparation steps of the glass fiber polyolefin composite heat-resistant support layer are:
[0014] The glass fiber powder and vinyl silane solution are mixed in a mass ratio of 1:5-1:10, the mass concentration of the vinyl silane solution is 3%-5%, and the mixture is heated and impregnated for 1-6 hours. The mixture is filtered, washed, and dried to obtain the modified glass fiber powder. The polyolefin resin slices and the modified glass fiber powder are melt-extruded through a screw machine, the modified glass fiber powder is 5%-10% of the mass of the polyolefin resin slices, and the glass fiber polyolefin composite heat-resistant support layer is obtained through continuous spinning, drawing, and laying. The gram weight is 5-20g / m 2 , layer thickness is 10-20μm, pore size is 1-3μm, and porosity is 60%-80%.
[0015] Furthermore, the electrical conductivity of the reduced graphene oxide is ≥100 S / cm, and compared with graphene and graphene oxide, the reduced graphene oxide has good heat resistance, electrical conductivity and hydrophilicity.
[0016] Furthermore, the compatibilizer is at least one of PE-g-ST, PP-g-ST, ABS-g-MAH, PE-g-MAH, and PP-g-MAH, and the compatibilizer grafted with maleic anhydride can improve the compatibility between the inorganic filler and the organic resin.
[0017] Furthermore, the graphene polyolefin composite conductive layer is prepared by the following steps:
[0018] The polyolefin resin slices are added to the screw machine and heated to melt, the reduced graphene oxide and the compatibilizer are mixed and added to the screw machine, stirred for 3-6 hours and then extruded, the reduced graphene oxide is 5-10% of the mass of the polyolefin slices, and the amount of the compatibilizer added is 3-4 times the mass of the reduced graphene oxide. After continuous spinning, drawing and laying, a graphene polyolefin composite conductive layer is obtained, with a gram weight of 10-20g / m 2 , layer thickness is 15-25μm, pore size is 0.5-2μm, and porosity is 45%-65%.
[0019] Furthermore, the process parameters of the spunlace composite are:
[0020] The water needle pressure is 70×10 5 Pa-150×10 5 Pa, the distance between the water needle plate and the net curtain is 1-2cm. Low and medium pressure water spunlace is used to effectively entangle and laminate the three layers of materials without destroying the fiber net structure.
[0021] Furthermore, the index parameters of the polyolefin-based lithium battery separator are:
[0022] The diaphragm weight is 30-65g / m 2 , thickness is 40-70μm, pore size is 0.2-0.4μm, and porosity is 30%-60%.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] 1. The present invention utilizes silane to modify glass fiber powder, thereby increasing the affinity between glass fiber powder and polyolefin, improving interface bonding, and the modified glass fiber powder and polyolefin composite improve the thermal stability and mechanical strength of the diaphragm, thereby realizing resource utilization of glass fiber powder and reducing raw material costs;
[0025] 2. The present invention utilizes a compatibilizer to combine reduced graphene oxide and polyolefin resin, and the reduced graphene oxide is evenly dispersed at the interface of the polyolefin matrix, thereby enhancing the interfacial interaction and giving the polyolefin-based diaphragm excellent thermal and electrical conductivity.
[0026] 3. The present invention obtains a polyolefin-based lithium battery separator by preparing a non-woven fabric by melt-blowing a mixture of inorganic materials and polyolefin raw materials, thereby avoiding the shedding of inorganic materials and ensuring the performance stability of the separator.
[0027] 4. The present invention prepares a three-layer polyolefin-based lithium battery separator through a spunlace process, which effectively avoids the damage of the fiber web structure in the separator by hot rolling and composite, and makes the porosity of the separator meet the performance requirements. The three-layer structure ensures that the separator has good mechanical properties and conductive properties while having excellent thermal stability. DETAILED DESCRIPTION
[0028] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] Example 1
[0030] This embodiment provides a method for preparing a polyolefin-based lithium battery separator with high thermal stability, comprising the following steps:
[0031] Step 1: Prepare glass fiber polyolefin composite heat-resistant support layer:
[0032] A solvent with a water-alcohol volume ratio of 1:2 was prepared, vinyl triethoxysilane was added to the solvent for hydrolysis, the mass proportion of vinyl triethoxysilane in the solution was 5%, and a vinyl triethoxysilane solution was obtained after the hydrolysis was completed, 0.7 μm glass fiber powder was added to the vinyl triethoxysilane solution at a mass proportion of 10%, heated to 70°C for 6 hours of impregnation treatment, filtered, washed and dried to obtain modified glass fiber powder, polypropylene resin chips and modified glass fiber powder were mixed according to a ratio and added to a screw machine, the modified glass fiber powder was 5% of the mass of the polyolefin resin chips, and a glass fiber polypropylene composite heat-resistant support layer was obtained after melt extrusion spinning and hot air drawing and laying. The laying weight was controlled to be 20 g / m 2, The thickness is 20μm, the pore size is 1-2μm, and the porosity is 68%.
[0033] Step 2: Preparation of graphene polyolefin composite conductive layer:
[0034] The polypropylene resin slices were added into the screw machine and heated to melt. 5% of the reduced graphene oxide and 15% of the PP-g-MAH compatibilizer of the polyolefin resin slices were mixed and added into the screw machine. After mixing and stirring for 3 hours, the microporous graphene polyolefin composite conductive layer was obtained by hot air drawing and laying. The weight of the laid net was controlled to be 10g / m 2 , thickness is 15μm, pore size is 1-2μm, and porosity is 63%.
[0035] Step 3: Preparation of polyolefin-based lithium battery separator:
[0036] The glass fiber polyolefin composite heat-resistant support layer and the graphene polyolefin composite conductive layer are hydroentangled and composited according to the three-layer structure of conductive layer, support layer and conductive layer, and dried to remove moisture to obtain a polyolefin-based lithium battery separator with a gram weight of 41g / m 2 , thickness is 43μm, pore size is 0.3-0.4μm, and porosity is 58%. The thermal shrinkage and electrical conductivity of the diaphragm were tested, and the specific data are shown in Table 1.
[0037] Example 2
[0038] The other steps are the same as those in Example 1. In step 2, the amount of reduced graphene oxide added is added according to different mass ratios of 8% and 10% of the mass of the polyolefin resin slice. Correspondingly, the amount of PP-g-MAH compatibilizer added is 3 times the mass of graphene oxide. The obtained graphene polyolefin composite conductive layer is used to prepare a diaphragm, and the thermal shrinkage and conductivity of the diaphragm are tested. The specific data are shown in Table 1.
[0039] Example 3
[0040] The other steps are the same as those in Example 1. In step 1, the modified glass fiber powder is added and mixed in different mass ratios of 8% and 10% of the mass of the polyolefin resin slices. The obtained glass fiber polypropylene composite heat-resistant support layer is used to prepare a diaphragm. The thermal shrinkage rate and conductive properties of the diaphragm are tested. The specific data are shown in Table 1.
[0041] Comparative Example 1
[0042] Using micron polypropylene fibers, polypropylene non-woven fabrics were made through the existing melt-blown technology. The thickness of the polypropylene non-woven fabric was 43 μm. Its thermal shrinkage and electrical conductivity were tested. The specific data are shown in Table 1.
[0043] Comparative Example 2
[0044] The polypropylene powder was melt-extruded at high temperature, stretched and pressed into sheets, and cooled to form a 30μm thick polypropylene diaphragm substrate. Polyvinylidene fluoride and ceramic powder were evenly stirred in N-methylpyrrolidone at a ratio of 1:19 to form a slurry. The prepared slurry was applied to the upper and lower layers of the diaphragm substrate with a coating machine to form a 13μm coating. After drying, a ceramic diaphragm was formed. The thermal shrinkage and conductivity of the diaphragm were tested. The specific data are shown in Table 1.
[0045] Comparative Example 3
[0046] The polypropylene powder was melt-extruded at high temperature, stretched and pressed into sheets, and cooled to form a 30 μm thick polypropylene diaphragm substrate. Reduced graphene oxide and polyvinylidene fluoride were added to N-methylpyrrolidone in a mass ratio of 1:1 and stirred evenly. The dispersion was obtained after ultrasonic treatment. The dispersion was filtered and placed on the upper and lower layers of the diaphragm substrate to form a 13 μm coating. After drying, a graphene diaphragm was formed. The thermal shrinkage and conductivity of the diaphragm were tested. The specific data are shown in Table 1.
[0047] Comparative Example 4
[0048] The present comparative example is compared with Example 1, except that silane is not added to modify the glass fiber powder, and 0.7 μm glass fiber powder is directly added to the polypropylene resin slices and mixed with the mixture, and then added to the screw machine. The glass fiber powder is 5% of the mass of the polyolefin resin slices, and a glass fiber polypropylene composite heat-resistant support layer is obtained. The other steps are the same as those in Example 1. The thermal shrinkage rate and the conductive performance of the diaphragm are tested. The specific data are shown in Table 1.
[0049] Comparative Example 5
[0050] Compared with Example 1, in this comparative example, no compatibilizer is added. The reduced graphene oxide and the polyolefin resin slices are directly mixed in the same mass ratio as in Example 1 and then added to the screw machine to obtain a microporous graphene polyolefin composite conductive layer. The other steps are the same as in Example 1. The thermal shrinkage and conductivity of the diaphragm are tested. The specific data are shown in Table 1.
[0051] Comparative Example 6
[0052] The other steps are the same as in Example 1. A different multilayer structure composite process is used to hot-press the glass fiber polyolefin composite heat-resistant support layer and the graphene polyolefin composite conductive layer according to the three-layer structure of the conductive layer, the support layer and the conductive layer to obtain a polyolefin-based lithium battery separator. The gram weight of the separator is controlled to be 41 g / m 2 , thickness is 43μm, and performance testing is carried out according to the standard of battery diaphragm performance test. The pore size of the diaphragm is 0.15-0.2μm, the porosity is 28%, and the specific data of the thermal shrinkage rate and conductive performance of the diaphragm are shown in Table 1.
[0053] The performance of the diaphragms prepared in Examples 1-3 of the present invention and Comparative Examples 1-6 was tested according to the standard for battery diaphragm performance testing. The results are shown in Table 1.
[0054] The thermal shrinkage test method is: place the sample in a 120°C oven for heat treatment for 60 minutes, and then measure the change in the diaphragm area before and after the heat treatment.
[0055] Table 1
[0056]
[0057] As can be seen from Table 1, Examples 1-3 detect the thermal shrinkage and ionic conductivity of the prepared diaphragms by changing the addition amount of modified glass fiber powder and reduced graphene oxide. The results show that modified glass fiber powder and reduced graphene oxide as raw materials for melt-blown non-woven fabrics can greatly reduce the thermal shrinkage of polyolefin-based diaphragms, improve thermal stability, and enable them to have good ionic conductivity; Comparative Example 1 is a pure polypropylene non-woven fabric diaphragm without adding other materials, which has poor thermal stability and low ionic conductivity.
[0058] In the research on improving the thermal stability of the diaphragm, ceramics and graphene are often used as diaphragm modification materials. The widely used process is to prepare coated diaphragms. Comparative Examples 2 and 3 are diaphragms prepared by ceramic coating and graphene coating respectively. Both ceramic coating and graphene coating can reduce thermal shrinkage and increase ionic conductivity. However, as can be seen from Table 1, the improvement is smaller than that in Example 1, and there is a risk of the coating falling off.
[0059] In Comparative Example 4, glass fiber powder and polypropylene are directly mixed, and in Comparative Example 5, reduced graphene oxide and polypropylene are directly mixed. The affinity of the glass fiber powder without silane modification and the polypropylene resin is reduced, and the compatibility of reduced graphene oxide in the polypropylene resin without adding a compatibilizer is reduced, resulting in a significant reduction in the dispersibility of the two materials in the polypropylene resin, and the presence of agglomeration. As can be seen from Table 1, the thermal stability and electrochemical properties of Comparative Examples 4 and 5 are reduced to varying degrees compared with Example 1.
[0060] Compared with implementation 1, comparative example 6 changes the composite process of the three-layer structure and adopts hot pressing composite. Compared with the hydroentanglement process, hot pressing composite will cause the pore size of the diaphragm to become smaller, the porosity to decrease, and the ionic conductivity to decrease, which affects the electrochemical properties of the diaphragm.
[0061] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0062] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a polyolefin-based lithium battery separator with high thermal stability, characterized in that: The following steps are involved: (1) Preparing a glass fiber polyolefin composite heat-resistant support layer: glass fiber powder modified raw materials are mixed according to a ratio, and melt-blown to form a polyolefin-based non-woven fiber membrane to obtain a polyolefin composite heat-resistant support layer, wherein the glass fiber powder modified raw materials are polyolefin resin chips, vinyl silane and glass fiber powder; glass fiber powder and vinyl silane solution are mixed according to a mass ratio of 1:5-1:10, and the mass concentration of the vinyl silane solution is 3%-5%, and heated and impregnated for 1-6 hours, filtered, washed and dried to obtain modified glass fiber powder, polyolefin resin chips and modified glass fiber powder are melt-extruded through a screw machine, and the modified glass fiber powder is 5%-10% of the mass of the polyolefin resin chips, and continuously spun, stretched and laid to obtain a glass fiber polyolefin composite heat-resistant support layer; (2) Preparing a graphene polyolefin composite conductive layer: reducing graphene oxide and polyolefin raw materials are mixed in proportion, and melt-blown to form a graphene polyolefin composite conductive layer, wherein the reduced graphene oxide and polyolefin raw materials are reduced graphene oxide, polyolefin resin slices and a compatibilizer; adding the polyolefin resin slices to a screw machine and heating them until they are melted, mixing the reduced graphene oxide and the compatibilizer, and adding them to the screw machine, stirring for 3-6 hours and then extruding, wherein the reduced graphene oxide is 5%-10% of the mass of the polyolefin slices, and the amount of the compatibilizer added is 3-4 times the mass of the graphene oxide, and the graphene polyolefin composite conductive layer is obtained by continuous spinning, drawing and web laying; (3) Preparation of polyolefin-based lithium battery separator: A glass fiber polyolefin composite heat-resistant support layer is used as the middle layer, and the upper and lower layers are graphene polyolefin composite conductive layers. After hydroentanglement and drying, a polyolefin-based lithium battery separator is obtained.
2. The method for preparing a polyolefin-based lithium battery separator with high thermal stability according to claim 1, characterized in that: The particle size of the glass fiber powder is 0.7-1 μm.
3. The method for preparing a polyolefin-based lithium battery separator with high thermal stability according to claim 1, characterized in that: The polyolefin resin chips are at least one of polyethylene resin chips and polypropylene resin chips.
4. The method for preparing a polyolefin-based lithium battery separator with high thermal stability according to claim 1, characterized in that: The vinyl silane is one of vinyl triethoxy silane, vinyl trimethoxy silane and vinyl tri(β-methoxyethoxy) silane.
5. The method for preparing a polyolefin-based lithium battery separator with high thermal stability according to claim 1, characterized in that: The weight of the glass fiber polyolefin composite heat-resistant support layer is 5-20 g / m 2 The layer thickness is 10-20μm, the pore size is 1-3μm, and the porosity is 60%-80%.
6. The method for preparing a polyolefin-based lithium battery separator with high thermal stability according to claim 1, characterized in that: The electrical conductivity of the reduced graphene oxide is ≥100 S / cm.
7. The method for preparing a polyolefin-based lithium battery separator with high thermal stability according to claim 1, characterized in that: The compatibilizer is at least one of PE-g-ST, PP-g-ST, ABS-g-MAH, PE-g-MAH, and PP-g-MAH.
8. The method for preparing a polyolefin-based lithium battery separator with high thermal stability according to claim 1, characterized in that: The weight of the graphene polyolefin composite conductive layer is 10-20 g / m 2 The layer thickness is 15-25μm, the pore size is 0.5-2μm, and the porosity is 45%-65%.
9. The method for preparing a polyolefin-based lithium battery separator with high thermal stability according to claim 1, characterized in that: The process parameters of the spunlace composite are: The water needle pressure is 70×10 5 Pa-150×10 5 Pa, the distance between the water needle plate and the supporting net curtain is 1-2cm.
10. The method for preparing a polyolefin-based lithium battery separator with high thermal stability according to claim 1, characterized in that: The index parameters of the polyolefin-based lithium battery separator are: The diaphragm weight is 30-65g / m 2 , thickness is 40-70μm, pore size is 0.2-0.4μm, and porosity is 30%-60%.