A kind of cold heading steel high carbon hot rolled wire rod for 15.9 grade bolts and its manufacturing method
Through high C-Si-Mn-Cr chemical composition and online molten salt ultra-fast temperature control technology, the microstructure of tempered pearlite and tempered soxunite is formed, which solves the improvement of cold heading steel on the basis of high carbon steel The problem has achieved low-cost and efficient manufacturing of 15.9-level bolts.
Patent Information
- Application Number
- CN202411133214.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-19
AI Technical Summary
Existing cold heading steels are difficult to improve performance on the basis of cheaper high-carbon steels, especially in the manufacturing process of 15.9-level bolts, there are high material costs, abnormal tissue risks and processing brittle breakage risks, resulting in low material yield and efficiency.
High-carbon hot-rolled strips designed with high C-Si-Mn-Cr chemical composition are used to form microstructures of tempered pearlite and tempered cornula to avoid bainite through the ultra-fast temperature control technology of online molten salt The abnormal structure of martensite is combined with high-temperature rolling and roll slow cooling technology to regulate the strong plasticity of the strip.
It reduces material costs, improves manufacturing efficiency and material yield, avoids the risk of cracking caused by abnormal tissue, and achieves high strength and high plasticity matching, suitable for the manufacturing of 15.9-level bolts.
Smart Images

Figure CN118639124B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of hot-rolled cold-heading steel wire rods, and in particular relates to a high-carbon hot-rolled wire rod of cold-heading steel for 15.9-grade bolts and a manufacturing method thereof. Background Art
[0002] Cold heading steel has good cold forming properties and is widely used in various mechanical fasteners through cold processing. At present, cold heading steel at home and abroad is mainly 10.9 and 12.9 grade fasteners. As the automotive industry and mechanical equipment tend to develop towards complex environments such as high stress and high speed, more requirements are put forward for the performance improvement of cold heading steel. The demand for fastener steel such as 15.9 grade bolts with tensile strength ≥1500MPa and yield strength ratio ≥0.9 is becoming more and more urgent. At present, the performance improvement of cold heading steel is mainly developed from low-carbon alloying to medium-carbon alloying. However, due to the limitation of the cooling rate of the Stelmor air cooling line, it is difficult for cold heading steel with higher strength grades to develop into high-carbon steel with lower cost. It is often developed by adding a large number of elements to improve hardenability. The addition of a large number of elements to improve hardenability will also increase the risk of abnormal structures such as martensite, which in turn increases the risk of cracking of cold heading steel during processing. For example:
[0003] Patent CN115747678B discloses a high-strength bolt steel for wind power and a high-strength bolt for wind power. The steel adopts a medium C-Mn-Cr-Ni-Mo-VB-Ti-Al-Nb composition design, and is combined with low-temperature aging, austenite treatment, and salt bath isothermal quenching after pouring and forging to obtain a lower bainite mixed structure. However, on the one hand, a large amount of high hardenability elements such as Cr, Ni, Mo, B, Ti, and Nb are added. Although the strength grade is increased to 15.9, the material cost and hardenability are high, and abnormal structures are more likely to occur, which affects the yield rate. On the other hand, after the steel billet is rolled into a round bar, it is directly precisely forged into a bolt blank, rather than directly rolled into a wire rod with a smaller diameter. Although the problem of abnormal martensitic structure after the ingot is rolled and cooled by the existing Stelmor air cooling line is avoided, the manufacturing difficulty of small-size bolts is significantly increased. The bar blank is manufactured by multiple heat treatments, and the process is complicated and expensive, and it is impossible to reduce emissions and produce efficiently.
[0004] Patent CN114107822B discloses a 15.9 grade high strength bolt steel and its production method and heat treatment method, which adopts a medium C-Si-Mn-Cr-Mo-V-Nb-Ti-Al composition design, combines high temperature soaking, low temperature controlled rolling and controlled cooling, and low temperature spinning into a heat preservation cover for slow cooling to obtain a pearlite + ferrite + bainite structure, and also adds a large amount of high hardenability elements such as Cr, Mo, V, Nb, Ti, etc., with high material cost and hardenability. Although low temperature rolling spinning and heat preservation slow cooling are used to suppress The martensitic hard phase structure that is harmful to drawing is produced. However, on the one hand, the demand for low-temperature controlled rolling and controlled cooling increases the difficulty of controlled cooling, which makes the rolling mill load requirements higher and easily increases the wear of the rolling line. On the other hand, although the doping of bainite increases the strength of the matrix, bainite as a hard and brittle phase structure has high distortion and dislocation density, and the wire rod has insufficient plasticity and high brittleness, which can easily cause the wire rod to break brittlely during coiling, transportation and downstream uncoiling, resulting in a decrease in the yield or waste of raw materials, which in turn limits the manufacturing cost and efficiency of steel mills and downstream enterprises.
[0005] The technical difficulties and causes of the development of higher strength grade cold heading steel into lower cost high carbon steel are: the existing high carbon steel used for drawing manufacturing mainly improves the drawing performance by increasing the sorbite content in the organization, for example, in the fields of bridge cables, cords, tire bead wires, etc., the heat preservation or low-speed cooling process after spinning is combined to extend the incubation time of the wire rod in the sorbite phase region, so as to increase the sorbite content and reduce the risk of abnormal bainite or martensite organization. However, on the one hand, too low a cooling rate will cause the high-temperature wire rod after spinning to pass through the secondary cementite region for a long time, forming a higher level of network carbide, which hinders the continuity and uniformity of the matrix organization and seriously deteriorates the plastic toughness of the wire rod. The use value of carbon element is low and it is difficult to eliminate after heat treatment, which can easily cause The risk of wire breakage during drawing and cracking during cold heading. After increasing the cooling rate, the troostite content in the wire rod structure decreases and the network carbon cannot be effectively eliminated, which has limited improvement on the drawing and cold heading performance. On the other hand, the wire rod production efficiency is insufficient under long-term heat preservation treatment, and the minimum cooling capacity of heat preservation cooling is limited. The time for the wire rod to pass through the troostite phase region is still relatively short, which makes the interlamellar spacing of the troostite structure larger. Under continuous cooling, the wire rod is in a low-temperature state after the structure is incubated, and the structure stress and dislocation density are high. It is difficult to further improve the plasticity, and the degree of cold work hardening is improved. Increasing the ferrite content in the structure to regulate the plasticity will lead to a significant loss of wire rod strength, and the plasticity improvement is limited. After spheroidizing annealing, large drawing deformation is required to strengthen the wire rod, and the plasticity loss is large, which aggravates the risk of wire breakage during drawing and cracking during cold heading. Summary of the invention
[0006] The present invention aims to solve at least one of the above-mentioned technical problems to a certain extent. The present invention provides a high-carbon hot-rolled wire rod of cold heading steel for 15.9-grade bolts and a manufacturing method thereof, which can utilize high-carbon steel to reduce material costs, improve manufacturing efficiency and yield rate, avoid abnormal structures such as martensite, and achieve strength-plasticity matching of the wire rod. It is used in the field of cold heading manufacturing of fasteners such as 15.9-grade bolts, and is beneficial to reducing the risk of cracking of cold heading steel during the processing process.
[0007] The technical solution adopted by the present invention to solve its technical problem is:
[0008] A high-carbon hot-rolled wire rod of cold heading steel for 15.9-grade bolts, the chemical composition and mass percentage of the high-carbon hot-rolled wire rod comprising: C: 0.85%-0.88%, Si: 0.30%-0.45%, Mn: 0.45%-0.60%, Cr: 0.20%-0.40%, P≤0.015%, S≤0.015%, the remainder being Fe and unavoidable impurities, and the microstructure thereof comprising 67%-72% by volume of tempered pearlite, 24%-29% by volume of tempered troostite, and the remainder being a mixed structure consisting of ferrite and fused pearlite.
[0009] The chemical composition and mass percentage design basis of the above-mentioned cold heading steel high carbon wire rod include:
[0010] (1) Carbon: As the main added cheap strengthening element, C can play a role in solid solution strengthening to ensure the matrix strength and high hardenability of steel, but at the same time it increases the decarburization sensitivity and the risk of cementite distribution along the grain boundaries. If the C content is too high, the resulting tissue lamellae in the medium temperature range will be thicker, which will lead to slow spheroidization and softening of the tissue, which is not conducive to the control of the matrix structure. Therefore, based on material cost considerations, easy tissue control, ensuring the cold deformation performance of cold heading steel wire rod, and meeting the final performance level requirements of 15.9 grade bolts, the mass percentage of C is controlled to be 0.85%~0.88%.
[0011] (2) Silicon: Si is the main deoxidizing element in steel and can be dissolved in austenite as a solid solution hardening element, which helps to improve the strength. It can inhibit the grain coarsening in the early stage of online molten salt ultra-fast temperature control. However, excessive silicon will increase the sensitivity of non-metallic inclusions and surface decarburization, increase the deformation resistance of the wire rod, and is not conducive to cold heading and cold extrusion. Therefore, the mass percentage of Si is controlled to be 0.30%~0.45%.
[0012] (3) Manganese: Mn is often added to steel as a deoxidizer during the smelting process to expand the austenite phase. The solid-dissolved Mn element can improve the strength and hardenability of the steel. However, too high a Mn content will aggravate the segregation during the solidification process of the steel billet, reduce the activity of carbon and the diffusion rate of carbon, increase the overheating sensitivity of the steel and the difficulty of controlling the cooling structure. Too high a Mn content will also increase the material cost. Therefore, the mass percentage of Mn is controlled to be 0.45%~0.60%.
[0013] (4) Chromium: As a medium-strong carbide-forming element, Cr can significantly increase the hardenability of steel and strengthen the matrix. Through ultra-fast temperature control of online molten salt, fine dispersed carbide particles are precipitated, which plays a role in dispersion strengthening and improves the strength of the material. However, if the Cr content is too high, it will increase the temper brittleness tendency of steel and produce low-temperature structure, which is not conducive to structure control. Therefore, the mass percentage of Cr is controlled to be 0.20%~0.40%.
[0014] (5) Phosphorus and sulfur: P and S are impurity elements. The lower the better. Therefore, P is controlled to be ≤ 0.015% and S is ≤ 0.015%.
[0015] The high carbon hot rolled wire rod is designed with high C-Si-Mn-Cr chemical composition, with relatively low Cr content and no Mo, V, Nb, Ti, B and other high hardenability expensive elements, which greatly reduces the material cost of the wire rod. With the high carbon component system, the performance level of 15.9 grade bolts can be achieved after quenching and tempering. Compared with the existing 15.9 grade bolt steel, which is a mixed structure containing a small amount or a large amount of bainite in the hot rolled state, the microstructure of the high carbon hot rolled wire rod contains most of tempered pearlite and a small amount of tempered troostite. The interlamellar spacing of pearlite is larger than that of troostite, the plasticity is better than that of troostite, and the strength is higher than that of ferrite. After tempering and melting and transforming to spheroidized structure, tempered pearlite and fused pearlite are obtained, and the organizational stress and dislocation density are further reduced. The interlayer spacing is smaller than that of pearlite, the strength is better than that of pearlite, and the plasticity is higher than that of bainite. After tempering and transformation to spheroidized structure, tempered troostite is obtained, and the dislocation density is further reduced. Therefore, on the basis of not excessively losing the strength of pearlite and troostite, it can cooperate with the high-carbon solid solution strengthening effect to provide the matrix strength of carbon steel that does not belong to the bainite structure. At the same time, compared with the hard and brittle phase bainite and the troostite structure with higher dislocation density, it can utilize the moderate strength and plasticity of pearlite and troostite, and through the regulation of tissue proportion and tempering state, further effectively improve the plasticity of wire rod, avoid the fracture problems in the coiling, transportation and downstream uncoiling processes caused by abnormal structures such as bainite and martensite, improve the yield rate, improve the utilization rate of raw materials, and effectively reduce the cracking risk of cold heading steel during the processing process.
[0016] A small amount of ferrite is produced during the generation of troostite and pearlite and the transformation to tempered structure. The larger the lamellar spacing of tempered pearlite and tempered troostite, the higher the plasticity of the wire rod and the lower the strength. However, too large lamellar spacing is accompanied by an increase in the ferrite content and an increase in the difficulty of melting and spheroidization, which is not conducive to organizational control. In a preferred embodiment, the lamellar spacing of the tempered pearlite is 160~200nm, the lamellar spacing of the tempered troostite is 85~125nm, and the volume percentage of the ferrite is ≤3%.
[0017] In a preferred embodiment, the network carbide of the high carbon hot-rolled wire rod is level 0, which can eliminate the network carbon deterioration phase caused by excessive carbon elements, improve the use value of carbon elements, achieve better solid solution and precipitation strengthening effects, and avoid the adverse effects of network carbon on plastic toughness.
[0018] In a preferred embodiment, the diameter of the high carbon hot-rolled wire rod is 6.0~15.0mm, the tensile strength Rm is 1155~1200MPa, and the cross-sectional shrinkage rate Z is 40%~45%. Compared with the existing cold heading steel wire rod, it has higher strength and plasticity matching, and the wire rod has a smaller diameter. The wire rod plasticity can be further increased by spheroidizing annealing, and the risk of wire breakage during drawing and cold heading cracking can be reduced. After that, the performance level of 15.9 grade bolts can be achieved through tempering on the basis of high carbon component design. Compared with multiple heat treatment manufacturing of bar blanks, it can meet the emission reduction and efficient manufacturing of small-size bolts. Compared with the hot-rolled wire rod containing bainite structure, it can also avoid the adverse effects of hardness and brittleness on the wire rod yield.
[0019] A method for manufacturing a cold heading steel high carbon hot rolled wire rod for 15.9 grade bolts, the manufacturing method comprising:
[0020] According to the chemical composition of the high carbon hot rolled wire rod of cold heading steel for 15.9 grade bolts as described above, the wire rod is rolled to produce the wire rod. After the wire rod is spun into the wire rod at a spinning temperature of ≥955°C, the wire rod is subjected to online molten salt ultra-fast temperature control, so that the wire rod is cooled to the pearlite phase region at a cooling rate of ≥40°C / s for isothermal phase transformation, and the wire rod is controlled to form troostite and pearlite structures, while promoting the spheroidization and softening of the troostite structure and the melting and softening of the pearlite structure. Finally, it is slowly cooled by a roller to produce a high carbon hot rolled wire rod whose microstructure includes 67% to 72% by volume of tempered pearlite, 24% to 29% by volume of tempered troostite, and the rest is a mixed structure composed of ferrite and fused pearlite.
[0021] The above-mentioned manufacturing method selects a higher spinning temperature to avoid the risk of cementite precipitation caused by excessively low temperature of high carbon steel in the spinning stage, and at the same time to facilitate the subsequent online molten salt ultra-fast cooling to form a higher degree of supercooling, thereby forming a finer structure, and also to reduce the difficulty of the rolling process and improve the rolling speed and efficiency. Compared with the existing Stelmor insulation cooling process after low-temperature spinning, the above-mentioned manufacturing method adopts online molten salt ultra-fast temperature control directly after spinning. One of the purposes is to utilize the high heat exchange capacity of molten salt to make the austenitized high-temperature wire rod after spinning quickly pass through the precipitation temperature range of secondary cementite, thereby inhibiting the formation of network carbon. At the same time, compared with improving the air cooling intensity and cooling rate of the Stelmor cooling line, there is no problem of air volume difference between the windward side and the leeward side when the wire rod passes through the molten salt, which can avoid the risk of abnormal martensite or bainite structure caused by excessive cooling rate, and reduce the fluctuation of mechanical properties. The second is: quickly enter the pearlite phase region to form a higher degree of supercooling, so that the austenite phase changes to form a structure with finer interlamellar spacing, provide matrix strength, and a small amount of inevitable ferrite will not affect the strength and drawing performance of the wire rod. Finer troostite and pearlite structures are also conducive to rapid spheroidization and softening of the structure. Compared with the insulation cooling process, the wire rod can be kept at the same temperature as the molten salt, so that the wire rod can be subjected to high-temperature isothermal treatment in the pearlite phase region for a longer time, rather than continuous cooling. This makes the wire rod still in a high-temperature state after the troostite and pearlite are inoculated, which can further promote the rapid spheroidization and softening of the troostite structure to form tempered troostite, promote the melting of the pearlite structure and the transformation to the spheroidized structure to form tempered pearlite and fused pearlite, reduce the tissue stress caused by high-speed cooling, further reduce the dislocation density of troostite and pearlite, and quickly regulate the plasticity of the structure.
[0022] Since the wire rod is in a high temperature state after the online molten salt ultra-fast temperature control treatment, the slow cooling through the roller can continue the tempering regulation effect of the high temperature on the wire rod structure and further soften the wire rod structure. At the same time, compared with the continuous insulation cooling after spinning, the wire rod after the online molten salt ultra-fast temperature control can use higher wire rod cooling to speed up the processing rhythm and reduce the processing time of roller slow cooling, making the production and manufacturing of the wire rod more efficient, and finally achieving wire rod structure regulation and strength-plasticity matching.
[0023] In a preferred embodiment, during the rolling, the heating furnace temperature is controlled to be ≤1150°C before rolling, and the furnace time is 4 to 6 hours. A higher heating furnace temperature is selected to promote the homogenization of the billet composition, while avoiding the risk of burning and decarburization caused by excessive heating furnace temperature and excessive furnace time, so as to adapt to rapid high-temperature rolling.
[0024] Due to the use of higher spinning temperature and online molten salt ultra-fast temperature control, the limitation of low-temperature rolling on the manufacturing of cold heading steel wire rod can be broken during rolling. High-temperature rolling is used to increase the rolling speed and reduce the wear on the rolling line, so that elements such as carbon in the wire are more evenly distributed, and a larger initial rolling reduction is used to suppress excessive growth and coarsening of the original grains. In a preferred embodiment, high-temperature rolling is used during the rolling, and the initial rolling temperature is controlled to be 1095~1120℃, and the initial rolling reduction is 22%~32%.
[0025] In a preferred embodiment, during the rolling, the final rolling temperature is controlled to be ≥975°C, and the final rolling reduction is 26%~36%. At a higher final rolling temperature, low-temperature rolling is more stable, and the deformation resistance of the wire is smaller, which is convenient for obtaining a smaller diameter wire with a larger final rolling reduction on the rolling mill, thereby improving the dimensional stability of the wire rod, preventing cracking during the rolling process, reducing the rolling mill load, avoiding the imperfect recrystallization process and increased residual stress caused by the final rolling temperature being too low, and improving the toughness and plasticity of the wire.
[0026] In a preferred embodiment, the final rolling temperature is 975-995° C., and the spinning temperature is 955-970° C., which can avoid grain coarsening caused by excessively high final rolling temperature and spinning temperature, and is beneficial to further strengthening the matrix.
[0027] In a preferred embodiment, the molten salt temperature of the online molten salt ultra-fast temperature control is 555~585℃, and the processing time is 50~150s. The lower the molten salt temperature, the faster the wire rod cooling rate and the greater the supercooling degree, which is beneficial to the formation of a structure with finer interlamellar spacing, and increases the content of austenite transformed into troostite. Finer troostite is beneficial to rapid spheroidization and softening of the structure, and the proportion of tempered troostite in the structure increases, the interlamellar spacing of tempered pearlite becomes finer, the strength of the wire rod increases, and the plasticity decreases. However, if the molten salt temperature is too low, the troostite content increases, but it is not conducive to the melting of pearlite and the transformation to spheroidized structure, and even bainite structure will appear, which seriously deteriorates the plasticity of the wire rod. On the contrary, the higher the molten salt temperature, the greater the interlamellar spacing of tempered troostite and tempered pearlite, the proportion of tempered pearlite increases, the strength of the wire rod decreases, and the plasticity increases. However, if the molten salt temperature is too high, the structure is too coarse. , the proportion of tempered troostite decreases and the content of ferrite increases, which will affect the strength of the wire rod and is not conducive to inhibiting the network carbon; the longer the processing time, the more obvious the softening effect of the organization, the greater the proportion of fused pearlite, the higher the plasticity of the wire rod and the lower the strength, but the processing time is too long and the wire rod is too softened, which is not conducive to the strength, energy consumption, stable organization regulation and rapid production of the wire rod. On the contrary, the shorter the processing time, the greater the residual stress of the organization, the greater the dislocation density of the troostite and pearlite organizations, the plasticity of the wire rod cannot be improved, and it is easy to harden by drawing, which is not conducive to the efficient production and yield rate of 15.9 grade bolts. Therefore, the molten salt temperature and processing time of the online molten salt ultra-fast temperature control can be further controlled to inhibit the formation of network carbon. At the same time, the proportion of troostite and pearlite, the interlamellar spacing and the tempering state can be adjusted to promote rapid spheroidization and softening of the organization in a shorter time, and stably regulate the strength and plasticity matching of the matrix.
[0028] In a preferred embodiment, the molten salt circulation rate of the online molten salt ultra-fast temperature control is 540~640t / h, and the molten salt temperature rise is ≤8°C. A higher molten salt circulation rate is selected to control the molten salt temperature rise, thereby improving the temperature accuracy of the online molten salt ultra-fast cooling, thereby improving the stability of tissue regulation and avoiding abnormal tissue risks.
[0029] In a preferred embodiment, the roller slow cooling adopts the method of closing the heat preservation cover and controlling the wire rod to cool at a cooling rate of 0.7~1.0℃ / s. This can continue the high temperature state of the wire rod after the online molten salt ultra-fast temperature control treatment, promote further softening of the wire rod structure, and avoid roller accumulation caused by too low cooling rate of the wire rod, thereby affecting production efficiency.
[0030] In a preferred embodiment, the wire rod is slowly cooled to below 350°C on a roller and then coiled, so that a sufficient softening effect can be maintained in the roller slow cooling stage, thereby avoiding surface scratches caused by excessively high coiling temperature and excessively soft wire rod, and improving the surface quality and uniformity of the wire rod.
[0031] Compared with the prior art, the beneficial effects of the present invention are at least:
[0032] (1) In view of the current situation that the performance improvement of the existing upsetting steel is mainly developed from low-carbon alloying to medium-carbon strong hardenability alloying, which leads to the increase of material cost, risk of abnormal structures such as martensite, risk of brittle fracture during processing, and risk of cold upsetting cracking, the high carbon hot-rolled wire rod of the present invention adopts a high C-Si-Mn-Cr chemical composition design, with a relatively low Cr content and no Mo, V, Nb, Ti, B and other high hardenability expensive elements, so that the wire rod material cost is greatly reduced, and the microstructure does not contain bainite or martensite hard and brittle phase structure, and is mainly composed of tempered pearlite, a small amount of tempered troostite, and other The rest is ferrite and fused pearlite, which provide matrix strength with high carbon solid solution strengthening. The tempered state structure is used to regulate the softened matrix, and small-sized wire rods can be directly obtained to achieve strength-plasticity matching of the wire rods. The wire rod performance before further processing by downstream users can reach a tensile strength Rm of 1155~1200MPa and a cross-sectional shrinkage rate Z of 40%~45%. It effectively avoids the brittle fracture problems of coiling, transportation and uncoiling by downstream users caused by abnormal structures such as bainite and martensite, improves the yield rate, and is used in the manufacture of 15.9 grade bolts and other application fields, with good market application prospects.
[0033] (2) In view of the current situation that the existing manufacturing methods are limited by the cooling rate of the Stelmor air-cooling line, and it is difficult to develop cold-heading steel with higher strength grades into high-carbon steel with lower cost, the manufacturing method of the present invention adopts a high C-Si-Mn-Cr chemical composition design and combines it with online molten salt ultra-fast temperature control technology. On the one hand, it can quickly pass through the secondary cementite zone, eliminate the network carbon deterioration phase caused by excessive carbon elements, and improve the use value of carbon elements; on the other hand, it provides a higher degree of supercooling in combination with a higher spinning temperature to form a finer structure, and undergoes isothermal phase transformation in the pearlite phase region. Compared with direct insulation cooling after spinning, it can avoid abnormal structure and control the formation of troostite and pearlite structures in the wire rod. At the same time, it promotes the spheroidization and softening of the troostite structure and the melting and softening of the pearlite structure. Then, it promotes further softening of the wire rod structure through slow cooling on a roller, thereby realizing the regulation of the wire rod structure and strength and plasticity properties, successfully manufacturing high-carbon hot-rolled wire rod of cold-heading steel, and improving the manufacturing efficiency and yield rate of the wire rod, and has good industrial adaptability.
[0034] (3) In view of the problems of mill wear, reduced rolling speed, structural stress and production difficulty caused by low-temperature rolling and spinning, the manufacturing method of the present invention adopts a higher spinning temperature and online molten salt ultra-fast temperature control. During rolling, a higher heating furnace temperature can be used to promote the homogenization of the steel billet composition, breaking the limitation of low-temperature rolling on the manufacturing of cold heading steel wire rods, and high-temperature rolling is used to further increase the rolling speed, reduce the wear on the rolling line, and improve the structural stress and plasticity and toughness. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0036] Figure 1 is a metallographic structure diagram of Example 1 of the present invention;
[0037] Figure 2 is the metallographic structure diagram of Example 2 of the present invention;
[0038] Figure 3 It is the metallographic structure diagram of Example 3 of the present invention. DETAILED DESCRIPTION
[0039] The embodiments described below with reference to the accompanying drawings are exemplary and are only for illustration and do not limit the description of the features and characteristics of the present invention. They are intended to be used to explain the present invention and are sufficient to enable those skilled in the art to implement the present invention. They should not be construed as limiting the scope of the present invention, which is limited only by the appended claims. Embodiment 1:
[0040] A preferred embodiment of the manufacturing method of the cold heading steel high carbon hot rolled wire rod for 15.9 grade bolts of the present invention, the chemical composition and mass percentage of the high carbon hot rolled wire rod include: C: 0.88%, Si: 0.39%, Mn: 0.55%, Cr: 0.38%, P: 0.014%, S: 0.015%, and the rest are Fe and unavoidable impurities, and the manufacturing method thereof is manufactured according to the process flow of high temperature rolling → spinning → online molten salt ultra-fast temperature control → roller slow cooling → coiling, specifically:
[0041] The high temperature rolling is used to heat the steel billet with a specification of 220mm×220mm through a heating furnace to promote the homogenization of the steel billet composition and avoid the risk of burning and decarburization. After heating to a high-temperature steel billet with rollable plasticity, the steel billet coming out of the heating furnace is rolled into a wire with a diameter of 15mm through a rolling line. High temperature rolling is used to increase the rolling speed and reduce the wear on the rolling line, so that elements such as carbon in the wire are more evenly distributed, the dimensional stability of the wire rod is improved, and the residual stress is reduced. Specifically: before rolling, the heating furnace temperature is controlled to be 1140°C, the furnace time is 6h, the initial rolling temperature is controlled to be 1110°C, the initial rolling reduction is 22%, the final rolling temperature is 990°C, and the final rolling reduction is 26%.
[0042] The spinning process is used to convert the wire rod coming out of the rolling line into wire rods through a spinning mechanism. The wire rods are spread on the rollers and transported along the rollers to avoid the risk of cementite precipitation caused by excessively low temperatures of high carbon steel during the spinning stage, so that subsequent online molten salt ultra-fast cooling can form a higher degree of supercooling and further form a finer structure. Specifically, the spinning temperature is controlled to 965°C.
[0043] The online molten salt ultra-fast temperature control adopts a salt bath tank with molten salt inside. The wire rod after spinning is conveyed through the salt bath tank by rollers and quickly cooled to the molten salt temperature, so that the wire rod is cooled to the pearlite phase region at a cooling rate of 41°C / s for isothermal phase transformation, and quickly passes through the precipitation temperature range of secondary cementite, eliminates the network carbon deterioration phase caused by excessive carbon element, improves the use value of carbon element, forms a higher degree of supercooling, controls the wire rod to form troostite structure and pearlite structure, and promotes the spheroidization and softening of troostite structure, promotes the melting and softening of pearlite structure, reduces tissue stress and dislocation density, and takes into account both rapid production and tissue stability regulation. Specifically: the molten salt temperature is controlled to be 573°C, the processing time is 150s, the molten salt circulation volume is 600t / h, and the molten salt temperature rise is ≤8°C.
[0044] The roller slow cooling process adopts closing the heat preservation cover, and conveying the wire rod from the salt bath tank into the heat preservation cover by rollers for slow cooling treatment to promote further softening of the wire rod structure. Specifically, the wire rod is controlled to cool to 340°C at a cooling rate of 0.9°C / s; the coiling process is used to coil the wire rod into a coil through a coiling drum, and obtain a high-carbon hot-rolled wire rod product after packaging and storage. Its metallographic structure diagram is as follows Figure 1 shown.
[0045] Comparative Example 1:
[0046] A method for manufacturing wire rod, which differs from Example 1 in that the method is manufactured according to the process flow of low-temperature rolling → low-temperature spinning → Stelmor insulation and slow cooling. Specifically: the low-temperature rolling controls the temperature of the heating furnace to 1155°C, the furnace time is 6h, the initial rolling temperature is controlled to be 1010°C, the final rolling temperature is controlled to be 790°C, the spinning temperature of the low-temperature spinning is 760°C, the Stelmor insulation and slow cooling adopts the method of shutting down all fans and insulation covers, and conveying the wire rod with rollers. The wire rod completes phase change in the cover at a cooling rate of 0.9°C / s, and the finished wire rod is obtained after it comes off the line.
[0047] Comparative Example 2:
[0048] A method for manufacturing a wire rod, which differs from that of Example 1 in that the method is manufactured according to a process flow of low-temperature rolling → low-temperature wire drawing → Stelmor air cooling → insulation and slow cooling. Specifically: the low-temperature rolling controls the temperature of a heating furnace to 1160°C, the furnace time to 5.5h, the initial rolling temperature to 1035°C, the final rolling temperature to 860°C, the wire drawing temperature of the low-temperature wire drawing is 830°C, the Stelmor air cooling adopts opening 1~6# fans at 15%, so that the wire rod is cooled to 625°C at a cooling rate of 2.9°C / s, the insulation and slow cooling adopts closing all fans and insulation covers, so that the wire rod completes phase change in the cover at a cooling rate of 1°C / s, and the finished wire rod is obtained after coiling and rolling off the line.
[0049] Comparative Example 3:
[0050] A method for manufacturing a wire rod, which differs from that of Example 1 in that the method is manufactured according to a process flow of high-temperature rolling → spinning → Stelmor rapid cooling → roller slow cooling. Specifically: the Stelmor rapid cooling is performed by opening 1~7# fans at 70%, so that the wire rod is cooled to 610°C at a cooling rate of 7.5°C / s; the roller slow cooling is performed by closing all fans and insulation covers, so that the wire rod completes a phase change in the cover at a cooling rate of 0.8°C / s, and the finished wire rod is obtained after it comes off the line.
[0051] The wire rods obtained in the above-mentioned Example 1 and Comparative Examples 1 to 3 were subjected to organization and performance testing: the tensile test was conducted using "GB-T228.1-2021 Metal Material Tensile Test Part 1: Room Temperature Test Method" to obtain tensile strength and cross-sectional shrinkage, and the organization was tested according to the metal microstructure detection method of GB / T13298 standard. The comparative results obtained are shown in Table 1 below:
[0052] Table 1. Comparison of wire rod structure and properties by different manufacturing methods
[0053]
[0054] From the comparison results of Example 1 and Comparative Example 1, it can be seen that compared with the troostite + ferrite structure obtained by low-temperature controlled rolling and controlled cooling and heat preservation treatment after spinning, although the tensile strength is higher, the high-temperature wire rod after spinning passes through the secondary cementite interval for a longer time, forming a higher level of network carbide, which seriously deteriorates the plastic toughness of the wire rod and makes the rolling mill load requirement higher. The present invention, through the high C-Si-Mn-Cr chemical composition design and combined with the online molten salt ultra-fast temperature control technology, can quickly pass through the secondary cementite interval, eliminate the network carbon deterioration phase caused by excessive carbon element, provide a higher degree of supercooling with a higher spinning temperature, form a finer structure, control the wire rod to form troostite structure and pearlite structure, and at the same time promote the spheroidization and softening of the troostite structure and the melting and softening of the pearlite structure, and then promote the further softening of the wire rod structure through slow cooling on the roller, thereby realizing the regulation of the wire rod structure and strong plastic properties.
[0055] From the comparison results of Example 1 and Comparative Example 2, it can be seen that compared with low-temperature controlled rolling and controlled cooling and first fast and then slow cooling after spinning to obtain pearlite + ferrite + bainite structure, although the doping of bainite improves the strength of the matrix, it is easy to aggravate the wear of the rolling line. Bainite as a hard and brittle phase structure has high distortion and dislocation density, the wire rod has insufficient plasticity and high brittleness, which can easily cause brittle fracture of the wire rod during coiling, transportation and downstream uncoiling. The present invention does not contain bainite structure, can improve the manufacturing efficiency and yield rate of wire rod, and has good industrial adaptability.
[0056] From the comparison results of Example 1 and Comparative Example 3, it can be seen that compared with improving the air-cooling strength, which is easy to produce a martensitic hard phase structure that is harmful to drawing, the present invention does not contain a martensitic structure, and uses the tempered state structure to regulate the softened matrix, so that small-sized wire rods can be directly obtained, achieving strength and plasticity matching of the wire rod. Embodiment 2:
[0057] A preferred embodiment of the manufacturing method of the cold heading steel high carbon hot rolled wire rod for grade 15.9 bolts of the present invention, the chemical composition and mass percentage of the high carbon hot rolled wire rod include: C: 0.87%, Si: 0.45%, Mn: 0.6%, Cr: 0.28%, P: 0.012%, S: 0.013%, and the rest are Fe and unavoidable impurities, and the manufacturing method thereof is manufactured according to the process flow of high temperature rolling → wire laying → online molten salt ultra-fast temperature control → roller slow cooling → coiling, specifically:
[0058] The high temperature rolling is used to heat the steel billet with a specification of 220mm×220mm through a heating furnace to promote the homogenization of the steel billet composition and avoid the risk of burning and decarburization. After heating to a high-temperature steel billet with rollable plasticity, the steel billet coming out of the heating furnace is rolled into a wire with a diameter of 12mm through a rolling line. High temperature rolling is used to increase the rolling speed and reduce the wear on the rolling line, so that elements such as carbon in the wire are more evenly distributed, the dimensional stability of the wire rod is improved, and the residual stress is reduced. Specifically: before rolling, the heating furnace temperature is controlled to be 1150°C, the furnace time is 5.5h, the initial rolling temperature is controlled to be 1120°C, the initial rolling reduction is 26%, the final rolling temperature is 995°C, and the final rolling reduction is 28%.
[0059] The spinning process is used to convert the wire rod coming out of the rolling line into wire rods through a spinning mechanism. The wire rods are spread on the rollers and transported along the rollers to avoid the risk of cementite precipitation caused by excessively low temperatures of high carbon steel during the spinning stage, so that subsequent online molten salt ultra-fast cooling can form a higher degree of supercooling and further form a finer structure. Specifically, the spinning temperature is controlled to 970°C.
[0060] The online molten salt ultra-fast temperature control adopts a salt bath tank with molten salt inside. The wire rod after spinning is conveyed through the salt bath tank by rollers and quickly cooled to the molten salt temperature, so that the wire rod is cooled to the pearlite phase region at a cooling rate of 40°C / s for isothermal phase transformation, and quickly passes through the precipitation temperature range of secondary cementite, eliminates the network carbon deterioration phase caused by excessive carbon element, improves the use value of carbon element, forms a higher degree of supercooling, controls the wire rod to form troostite structure and pearlite structure, and promotes the spheroidization and softening of troostite structure, promotes the melting and softening of pearlite structure, reduces tissue stress and dislocation density, and takes into account both rapid production and tissue stability regulation. Specifically: the molten salt temperature is controlled to be 585°C, the processing time is 50s, the molten salt circulation volume is 540t / h, and the molten salt temperature rise is ≤8°C.
[0061] The roller slow cooling process adopts closing the heat preservation cover, and conveying the wire rod from the salt bath tank into the heat preservation cover by rollers for slow cooling treatment to promote further softening of the wire rod structure. Specifically, the wire rod is controlled to cool to 325°C at a cooling rate of 1°C / s; the coiling process is used to coil the wire rod into a coil through a coiling drum, and obtain a high-carbon hot-rolled wire rod product after packaging and storage. Its metallographic structure diagram is as follows Figure 2 shown.
[0062] Comparative Example 4:
[0063] A method for manufacturing a wire rod, which differs from that of Example 2 in that, before rolling, the heating furnace temperature is controlled to be 1130°C, the furnace time is 6 hours, the initial rolling temperature is controlled to be 1090°C, the final rolling temperature is 970°C, and the spinning temperature is 950°C. The online molten salt ultra-fast temperature control allows the wire rod to be cooled to the pearlite phase region at a cooling rate of 36°C / s for isothermal phase transformation, and the finished wire rod is obtained after it comes off the line.
[0064] Comparative Example 5:
[0065] A method for manufacturing a wire rod, which differs from that of Example 2 in that the online molten salt ultra-fast temperature control allows the wire rod to be cooled to the pearlite phase region at a cooling rate of 38°C / s for isothermal phase transformation, the molten salt temperature is 600°C, and the finished wire rod is obtained after going offline.
[0066] Comparative Example 6:
[0067] A method for manufacturing wire rod, which differs from Example 2 in that the online molten salt ultra-fast temperature control allows the wire rod to be cooled to the pearlite phase region at a cooling rate of 44°C / s for isothermal phase transformation, the molten salt temperature is 55°C, the molten salt circulation rate is 700t / h, and the finished wire rod is obtained after going offline. Embodiment 3:
[0068] A preferred embodiment of the manufacturing method of the cold heading steel high carbon hot rolled wire rod for grade 15.9 bolts of the present invention, the chemical composition and mass percentage of the high carbon hot rolled wire rod include: C: 0.85%, Si: 0.3%, Mn: 0.49%, Cr: 0.2%, P: 0.015%, S: 0.014%, and the rest are Fe and unavoidable impurities, and the manufacturing method thereof is manufactured according to the process flow of high temperature rolling → wire laying → online molten salt ultra-fast temperature control → roller slow cooling → coiling, specifically:
[0069] The high temperature rolling is used to heat the steel billet with a specification of 180mm×180mm through a heating furnace to promote the homogenization of the steel billet composition and avoid the risk of burning and decarburization. After heating to a high-temperature steel billet with rollable plasticity, the steel billet coming out of the heating furnace is rolled into a wire with a diameter of 6mm through a rolling line. High temperature rolling is used to increase the rolling speed and reduce the wear on the rolling line, so that elements such as carbon in the wire are more evenly distributed, the dimensional stability of the wire rod is improved, and the residual stress is reduced. Specifically: before rolling, the heating furnace temperature is controlled to be 1130°C, the furnace time is 4h, the initial rolling temperature is controlled to be 1095°C, the initial rolling reduction is 32%, the final rolling temperature is 975°C, and the final rolling reduction is 36%.
[0070] The spinning process is used to convert the wire rod coming out of the rolling line into wire rods through a spinning mechanism. The wire rods are spread on the rollers and transported along the rollers to avoid the risk of cementite precipitation caused by excessively low temperatures of high carbon steel during the spinning stage, so that subsequent online molten salt ultra-fast cooling can form a higher degree of supercooling and further form a finer structure. Specifically, the spinning temperature is controlled to 955°C.
[0071] The online molten salt ultra-fast temperature control adopts a salt bath tank with molten salt inside. The wire rod after spinning is conveyed through the salt bath tank by rollers and quickly cooled to the molten salt temperature, so that the wire rod is cooled to the pearlite phase region at a cooling rate of 43°C / s for isothermal phase transformation, and quickly passes through the precipitation temperature range of secondary cementite, eliminates the network carbon deterioration phase caused by excessive carbon element, improves the use value of carbon element, forms a higher degree of supercooling, controls the wire rod to form troostite structure and pearlite structure, and promotes the spheroidization and softening of troostite structure, promotes the melting and softening of pearlite structure, reduces tissue stress and dislocation density, and takes into account both rapid production and tissue stability regulation. Specifically: the molten salt temperature is controlled to be 555°C, the processing time is 120s, the molten salt circulation volume is 640t / h, and the molten salt temperature rise is ≤8°C.
[0072] The roller slow cooling process adopts closing the heat preservation cover, and conveying the wire rod from the salt bath tank into the heat preservation cover by rollers for slow cooling treatment to promote further softening of the wire rod structure. Specifically, the wire rod is controlled to cool to 332°C at a cooling rate of 0.7°C / s; the coiling process is used to coil the wire rod into a coil through a coiling drum, and obtain a high-carbon hot-rolled wire rod product after packaging and storage. Its metallographic structure diagram is as follows Figure 3 shown.
[0073] Comparative Example 7:
[0074] A method for manufacturing a wire rod, which differs from that of Example 3 in that the processing time of the online molten salt ultra-fast temperature control is 45 seconds, and the finished wire rod is obtained after going offline.
[0075] Comparative Example 8:
[0076] A method for manufacturing a wire rod, which differs from the manufacturing method of Example 3 in that the processing time of the online molten salt ultra-fast temperature control is 160s, and the finished wire rod is obtained after going offline. Embodiment 4:
[0077] A preferred embodiment of the manufacturing method of the cold heading steel high carbon hot rolled wire rod for 15.9 grade bolts of the present invention, the chemical composition and mass percentage of the high carbon hot rolled wire rod include: C: 0.86%, Si: 0.42%, Mn: 0.45%, Cr: 0.4%, P: 0.013%, S: 0.013%, and the rest are Fe and unavoidable impurities, and the manufacturing method thereof is manufactured according to the process flow of high temperature rolling → wire laying → online molten salt ultra-fast temperature control → roller slow cooling → coiling, specifically:
[0078] The high temperature rolling is used to heat the steel billet with a specification of 180mm×180mm through a heating furnace to promote the homogenization of the steel billet composition and avoid the risk of burning and decarburization. After heating to a high-temperature steel billet with rollable plasticity, the steel billet coming out of the heating furnace is rolled into a wire with a diameter of 8mm through a rolling line. High temperature rolling is used to increase the rolling speed and reduce the wear on the rolling line, so that elements such as carbon in the wire are more evenly distributed, the dimensional stability of the wire rod is improved, and the residual stress is reduced. Specifically: before rolling, the heating furnace temperature is controlled to be 1135°C, the furnace time is 5h, the initial rolling temperature is controlled to be 1105°C, the initial rolling reduction is 29%, the final rolling temperature is 980°C, and the final rolling reduction is 32%.
[0079] The spinning process is used to convert the wire rod coming out of the rolling line into wire rods through a spinning mechanism. The wire rods are spread on the rollers and transported along the rollers to avoid the risk of cementite precipitation caused by excessively low temperatures of high carbon steel during the spinning stage, so that subsequent online molten salt ultra-fast cooling can form a higher degree of supercooling, thereby forming a finer structure. Specifically, the spinning temperature is controlled to 960°C.
[0080] The online molten salt ultra-fast temperature control adopts a salt bath tank with molten salt inside. The wire rod after spinning is conveyed through the salt bath tank by rollers and quickly cooled to the molten salt temperature, so that the wire rod is cooled to the pearlite phase region at a cooling rate of 41°C / s for isothermal phase transformation, and quickly passes through the precipitation temperature range of secondary cementite, eliminates the network carbon deterioration phase caused by excessive carbon element, improves the use value of carbon element, forms a higher degree of supercooling, controls the wire rod to form troostite structure and pearlite structure, and promotes the spheroidization and softening of troostite structure, promotes the melting and softening of pearlite structure, reduces tissue stress and dislocation density, and takes into account both rapid production and tissue stability regulation. Specifically: the molten salt temperature is controlled to be 562°C, the processing time is 85s, the molten salt circulation volume is 620t / h, and the molten salt temperature rise is ≤8°C.
[0081] The roller slow cooling process adopts closing the insulation cover and conveying the wire rod coming out of the salt bath tank into the insulation cover by rollers for slow cooling treatment to promote further softening of the wire rod structure. Specifically: the wire rod is controlled to be cooled to 330°C at a cooling rate of 0.8°C / s; the coiling process is used to coil the wire rod into coils through the coiling drum, and the high carbon hot rolled wire rod finished product is obtained after packaging and storage.
[0082] Comparative Example 9:
[0083] A method for manufacturing a wire rod, which differs from Example 4 in that the method is manufactured according to a process flow of high-temperature rolling → spinning → online molten salt ultra-fast temperature control → air cooling → coiling. Specifically: the air cooling is performed by opening a heat preservation cover, and conveying the wire rod coming out of a salt bath tank into the heat preservation cover by a roller for air cooling. The wire rod is controlled to be cooled to 330°C at a cooling rate of 2°C / s, and a finished wire rod is obtained after it comes off the line.
[0084] The wire rods obtained in the above-mentioned Examples 2 to 4 and Comparative Examples 4 to 9 were subjected to organizational and performance tests: the tensile test was conducted according to GB-T 228.1-2021 Metallic Material Tensile Test Part 1: Room Temperature Test Method to obtain tensile strength and cross-sectional shrinkage, and the organizational test was conducted according to the metal microstructure detection method of GB / T13298 standard. The comparative results obtained are shown in Table 2 below:
[0085] Table 2. Comparison of the microstructure and properties of wire rods with different high carbon hot rolled wire rod compositions and manufacturing methods
[0086]
[0087] It can be seen from the results of Examples 1 to 4 that the present invention adopts a high C-Si-Mn-Cr chemical composition design, has a relatively low Cr content, and does not contain high hardenability precious elements such as Mo, V, Nb, Ti, and B, so that the cost of wire rod materials is greatly reduced, and the tensile strength Rm can reach 1155~1200MPa, and the cross-sectional shrinkage rate Z is 40%~45%, which effectively avoids the brittle fracture problems of coiling, transportation and uncoiling for downstream users caused by abnormal tissues such as bainite and martensite, improves the yield rate, and is used in the manufacture of 15.9 grade bolts and other application fields, and has good market application prospects.
[0088] It can be seen from the comparison results of Example 2 and Comparative Example 4 that a higher spinning temperature can be used to avoid the risk of cementite precipitation caused by excessively low temperature in the spinning stage of high carbon steel, and at the same time, it is convenient for the subsequent online ultra-fast molten salt cooling to form a higher degree of supercooling, thereby forming a finer structure, and also facilitating the reduction of the difficulty of the rolling process and the improvement of the rolling speed and efficiency; It can be seen from the comparison results of Example 2 and Comparative Example 5 that the higher the molten salt temperature, the larger the interlamellar spacing of tempered troostite and tempered pearlite, the greater the proportion of tempered pearlite, the lower the strength of the wire rod, and the higher the plasticity, but the molten salt temperature is. If the salt temperature is too high, the structure is too coarse, the proportion of tempered troostite decreases, and the ferrite content increases, which will affect the strength of the wire rod and is not conducive to inhibiting the carbon network; from the comparison results of Example 2 and Comparative Example 6, it can be seen that the lower the molten salt temperature, the faster the cooling rate of the wire rod and the greater the degree of supercooling, which is beneficial to the formation of a structure with finer interlamellar spacing, the proportion of tempered troostite in the structure increases, the interlamellar spacing of tempered pearlite becomes finer, the strength of the wire rod increases, and the plasticity decreases. However, if the molten salt temperature is too low, the troostite content increases, but it is not conducive to the melting of pearlite and the transformation to spheroidized structure, resulting in a decrease in the plasticity of the wire rod.
[0089] From the comparison results of Example 3 and Comparative Example 7, it can be seen that the shorter the treatment time, the greater the residual stress of the tissue, the greater the dislocation density of the troostite and pearlite tissues, and the plasticity of the wire rod cannot be improved; from the comparison results of Example 3 and Comparative Example 8, it can be seen that the longer the treatment time, the more obvious the tissue softening effect, the greater the proportion of fused pearlite, the higher the plasticity of the wire rod, and the lower the strength, but if the treatment time is too long, the wire rod will be too softened, which is not conducive to the strength, energy consumption, stable tissue regulation and rapid production of the wire rod; from the comparison results of Example 4 and Comparative Example 9, it can be seen that the use of roller slow cooling can continue the high temperature state of the wire rod after the online molten salt ultra-fast temperature control treatment, and promote further softening of the wire rod tissue.
[0090] The series of detailed descriptions listed above are only specific descriptions of feasible embodiments of the present invention, and they are not intended to limit the scope of protection of the present invention. For example, steel billets can be obtained by sequentially performing converter smelting, refining, and continuous casting processes on steelmaking raw materials. Any equivalent embodiments or changes that do not deviate from the technical spirit of the present invention should be included in the scope of protection of the present invention.
Claims
1. A 15.9 grade cold heading steel high carbon hot rolled wire rod for bolts, characterized in that: The chemical composition and mass percentage of the high carbon hot rolled wire rod include: C: 0.85% to 0.88%, Si: 0.30% to 0.45%, Mn: 0.45% to 0.60%, Cr: 0.20% to 0.40%, P≤0.015%, S≤0.015%, and the rest are Fe and unavoidable impurities, and its microstructure includes tempered pearlite accounting for 67% to 72% by volume, tempered troostite accounting for 24% to 29% by volume, and the rest is a mixed structure composed of ferrite and fused pearlite; The manufacturing method comprises: rolling and producing wire rods according to the chemical composition of the cold heading steel high carbon hot rolled wire rod for grade 15.9 bolts, spinning the wire rod into wire rod at a spinning temperature of ≥955°C, and then carrying out online molten salt ultra-fast temperature control, so that the wire rod is cooled to the pearlite phase region at a cooling rate of ≥40°C / s for isothermal phase transformation, controlling the wire rod to form troostite structure and pearlite structure, and promoting the spheroidization and softening of the troostite structure and the melting and softening of the pearlite structure, and finally slowly cooling through a roller to produce a high carbon hot rolled wire rod with a microstructure including a mixed structure composed of tempered pearlite, tempered troostite, ferrite and fused pearlite; the molten salt temperature of the online molten salt ultra-fast temperature control is 555-585°C, and the processing time is 50-150s.
2. The 15.9 grade cold heading steel high carbon hot rolled wire rod for bolts according to claim 1, characterized in that: The interlamellar spacing of the tempered pearlite is 160-200 nm, the interlamellar spacing of the tempered bainite is 85-125 nm, the volume percentage of the ferrite is ≤3%, and the network carbide of the high carbon hot-rolled wire rod is grade 0.
3. The 15.9 grade cold heading steel high carbon hot rolled wire rod for bolts according to claim 1 or 2, characterized in that: The high carbon hot-rolled wire rod has a diameter of 6.0-15.0 mm, a tensile strength of 1155-1200 MPa, and a cross-sectional shrinkage of 40%-45%.
4. A method for manufacturing a cold heading steel high carbon hot rolled wire rod for 15.9 grade bolts, characterized in that: The manufacturing method thereof comprises: The wire rod is produced by rolling the chemical composition of the high carbon hot-rolled wire rod of cold heading steel for grade 15.9 bolts according to claim 1. After the wire rod is spun into wire rod at a spinning temperature of ≥955°C, online molten salt ultra-fast temperature control is performed to cool the wire rod to the pearlite phase region at a cooling rate of ≥40°C / s for isothermal phase transformation, and the wire rod is controlled to form troostite and pearlite structures, while promoting the spheroidization and softening of the troostite structure and the melting and softening of the pearlite structure. Finally, it is slowly cooled by a roller to produce a high carbon hot-rolled wire rod whose microstructure includes 67% to 72% tempered pearlite by volume, 24% to 29% tempered troostite by volume, and the rest is a mixed structure composed of ferrite and fused pearlite; the molten salt temperature of the online molten salt ultra-fast temperature control is 555 to 585°C, and the processing time is 50 to 150s.
5. The method for manufacturing the cold heading steel high carbon hot rolled wire rod for 15.9 grade bolts according to claim 4, characterized in that: Before the rolling, the heating furnace temperature is controlled to be ≤1150°C, and the time in the furnace is 4-6 hours.
6. The method for manufacturing the cold heading steel high carbon hot rolled wire rod for 15.9 grade bolts according to claim 4, characterized in that: The rolling adopts high temperature rolling, the initial rolling temperature is controlled to be 1095-1120°C, the initial rolling reduction is 22%-32%, the final rolling temperature is ≥975°C, and the final rolling reduction is 26%-36%.
7. The method for manufacturing the cold heading steel high carbon hot rolled wire rod for 15.9 grade bolts according to claim 4, characterized in that: The molten salt circulation rate of the online molten salt ultra-fast temperature control is 540-640 t / h, and the molten salt temperature rise is ≤8°C.
8. The method for manufacturing the cold heading steel high carbon hot rolled wire rod for 15.9 grade bolts according to claim 4, characterized in that: Therefore, the roller slow cooling adopts the method of closing the heat preservation cover and controlling the wire rod to cool at a cooling rate of 0.7~1.0℃ / s.
9. The method for manufacturing the cold heading steel high carbon hot rolled wire rod for 15.9 grade bolts according to claim 8, characterized in that: The wire rod is slowly cooled on a roller conveyor to below 350°C and then coiled.