Low friction composite reinforcing filler for fluororesin and preparation method thereof
By using low-friction composite reinforced filler in fluororesin, using the combination of porous adsorbent and solid lubricant, the frictional performance problem of fluororesin under high temperature and dry friction conditions is solved, and better lubricating and wear resistance are achieved. .
Patent Information
- Application Number
- CN202411088312.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-09
AI Technical Summary
Fluororesin has a high friction coefficient and a large wear rate under high temperature and dry friction conditions, and the friction coefficient increases with time during continuous friction, which limits its application.
Using the preparation method of low friction composite reinforced filler, the coupling agent solution is applied to the porous adsorbent and solid lubricant and dried, then mixed, and then left to stand in a high-temperature negative pressure environment, freeze-drying and crushing into particles to form lubricating grease. Micro-particle filler filled in porous adsorbent pores, combined with solid lubricant to provide friction reduction effect.
The friction performance of fluororesin materials under high temperature conditions is significantly improved, and good lubricating performance is maintained through the release of solid lubricants and greases, reducing friction coefficient and wear rate.
Smart Images

Figure CN118652508B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a low-friction composite reinforced filler for fluororesin and a preparation method thereof, belonging to the field of lubricating fillers. Background Art
[0002] The rapid development of high-end technical equipment has put forward higher requirements on the wear resistance of polymer materials, especially the wear resistance under high pressure and high temperature special working conditions. Resin-based materials have attracted much attention due to their light weight and high strength. Among them, fluororesin has become a common material in the field of self-lubricating wear-resistant materials because of its good self-lubrication, wear resistance and corrosion resistance.
[0003] However, fluororesins have poor wear resistance and high friction coefficient under certain working conditions, which limits their development. Specifically, they have the following characteristics: 1. The friction coefficient is large and the wear rate is high under high temperature environment; 2. When friction is continuous, the friction coefficient increases rapidly over time; 3. The friction coefficient is large during dry friction. Summary of the invention
[0004] In order to overcome the deficiencies of the prior art, the present invention provides a low-friction composite reinforced filler for fluororesin and a preparation method thereof. When the filler is applied to fluororesin, the fluororesin can have better lubricity under dry friction conditions and high temperature conditions.
[0005] The technical solution adopted by the present invention to solve its technical problem is:
[0006] In a first aspect, the present application provides a method for preparing a low-friction composite reinforcing filler for a fluororesin, comprising the following steps:
[0007] Applying a coupling agent solution on a porous adsorbent and a solid lubricant respectively and drying the solution to obtain a modified porous adsorbent and a modified solid lubricant;
[0008] Adding the modified porous adsorbent to the grease heated to melt and mixing to obtain a first mixed system;
[0009] placing the first mixed system in an environment with a temperature above the dropping point of the grease and allowing it to stand at negative pressure;
[0010] Taking out the first mixed system and adding the modified solid lubricant to mix, to obtain a second mixed system;
[0011] The second mixed system is frozen, dried, and crushed into particles to obtain the low-friction composite reinforcing filler for fluororesin.
[0012] The method provided in the present application prepares grease and wear-resistant fillers (solid lubricants, etc.) into micro-particle fillers with self-lubricating properties through vacuum adsorption and freeze-drying. The grease is filled in the pores of the porous adsorbent. Applying the micro-particle filler to fluororesin can improve the wear resistance of the fluororesin material.
[0013] Furthermore, the raw materials include, by mass, 20 to 45 parts of the porous adsorbent, 40 to 50 parts of the solid lubricant, 10 to 22 parts of the grease, and 5 to 8 parts of the coupling agent (the solute in the coupling agent solution).
[0014] The use of this raw material ratio in the preparation method can ensure that most of the grease is filled into the porous adsorbent, and a small amount of grease on the surface of the porous adsorbent enhances the adhesion of the solid lubricant on the porous adsorbent to a certain extent; the solid lubricant partially enters the porous adsorbent and partially adheres to the surface of the porous adsorbent. After being applied to the fluororesin, in the early stage of wear, the solid lubricant first provides a friction reduction effect. When further wear occurs, the solid lubricant on the surface of the porous adsorbent falls off to replace the wear of the fluororesin. When friction continues to generate heat, the grease in the porous adsorbent melts and releases, continuing to make the fluororesin have good lubrication properties.
[0015] Furthermore, the dropping point of the lubricating grease is 200° C. to 250° C., and the temperature resistance is above 550° C. The lubricating grease meeting this requirement is not easy to lose during preparation, and can play a lubricating role in time during continuous friction.
[0016] Furthermore, the freezing requirement in the freeze-drying is -40°C for 12 hours.
[0017] Freeze drying can reduce the moisture content in the reinforcing filler while keeping the pore structure of the porous material intact. In addition, the vacuum environment during the freeze drying process is conducive to keeping the grease in the pores, reducing the grease loss rate.
[0018] Furthermore, the first mixed system is placed in an environment with a temperature above the dropping point of the grease and left to stand under negative pressure for 6 hours.
[0019] Furthermore, the solid lubricant is selected from at least one of graphite, molybdenum disulfide, black phosphorus, boron nitride, boron carbide, graphene, and tungsten disulfide.
[0020] Furthermore, the coupling agent solution comprises at least one component selected from KH550, KH560, a titanate coupling agent, and aminoethylaminopropyltrimethoxysilane.
[0021] Furthermore, the porous adsorbent is selected from porous silica microspheres, molecular sieves or porous polyimide, and the pore size is 2 μm to 5 μm.
[0022] Molecular sieves are composed of crystalline silicates or aluminosilicates. Silicates, aluminosilicates, silicon dioxide, polyimide, etc. can be used as wear-resistant fillers. When they are made into porous forms, they can not only play the role of wear-resistant fillers, but also serve as carriers of grease. Pores of 2μm~5μm are conducive to the adsorption of molten grease in a vacuum, and are not easy to cause grease loss, which solves the problem that it is difficult to add grease to the resin system in traditional methods; and this pore size range is conducive to the release of molten grease under high temperature or repeated friction.
[0023] Furthermore, after being crushed into particles, the particles need to be sieved through a 40-mesh sieve.
[0024] In a second aspect, the present application provides a low-friction composite reinforced filler for fluororesin, which is made by the preparation method of the low-friction composite reinforced filler for fluororesin described in the first aspect.
[0025] The low-friction composite reinforcing filler for fluororesin comprises the porous adsorbent, the grease, and the solid lubricant. The grease is filled in the pores of the porous adsorbent. The porous adsorbent and the solid lubricant are provided with a coupling agent. A part of the solid lubricant is located in the pores of the porous adsorbent, and a part of the solid lubricant is attached to the porous adsorbent.
[0026] The beneficial effects of the present invention are as follows: the present invention utilizes the storage function of the porous adsorbent to melt the grease and absorb it into the pores to form a tiny grease storage unit, and combines the solid lubricant to be adsorbed on the interface of the grease storage unit to form a high-temperature self-lubricating composite filler with grease inside and solid outside. The filler has good high temperature resistance and lubrication performance, can effectively improve the friction performance of fluororesin materials under high temperature conditions, relies on solid lubricants to provide friction reduction effects in the early stage of wear, and with the friction heat generation and the transfer of solid lubricants, the stored grease is released, thereby maintaining good friction performance.
[0027] Other features and advantages of the present application will be described in the following description, and partly become apparent from the description, or understood by practicing the present application. The purpose and other advantages of the present application can be realized and obtained by the structures particularly pointed out in the written description and the drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 It is a schematic diagram of the structure of a low-friction composite reinforcing filler for fluororesin provided in an embodiment of the present application.
[0029] Figure 2 This is a physical picture of a low-friction composite reinforcing filler for fluororesin provided in Example 1 of the present application.
[0030] Figure 3This is an electron microscope image of a low-friction composite reinforcing filler for fluororesin provided in Example 1 of the present application.
[0031] Figure 4 This is a physical picture of the polytetrafluoroethylene composite material mixed with the filler prepared in Example 1.
[0032] Figure 5 This is a thermogravimetric analysis diagram of the polytetrafluoroethylene composite material doped with the filler prepared in Example 1.
[0033] Figure 6 It is a graph showing the lubrication performance test results of the polytetrafluoroethylene composite materials corresponding to each embodiment and comparative example.
[0034] Figure numerals: 1. porous adsorbent; 11. pores; 2. solid lubricant; 3. grease. DETAILED DESCRIPTION
[0035] The embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and cannot be understood as limiting the present invention.
[0036] The disclosure below provides many different embodiments or examples to implement different structures of the present invention. In order to simplify the disclosure of the present invention, the parts and settings of specific examples are described below. Of course, they are only examples, and the purpose is not to limit the present invention. In addition, the present invention can repeat reference numbers and / or reference letters in different examples, and this repetition is for the purpose of simplification and clarity, which itself does not indicate the relationship between the various embodiments and / or settings discussed.
[0037] It is difficult to add grease to the fluororesin system to improve the lubrication performance of the fluororesin under dry friction conditions. The fluororesin in the prior art has poor wear performance under high temperature conditions; the reason why the friction coefficient rises rapidly during continuous friction may also be due to local high heat caused by friction.
[0038] In order to improve the above problems, the present invention provides a method for preparing a low-friction composite reinforced filler for fluororesin, comprising the following steps:
[0039] S1: applying a coupling agent solution to a porous adsorbent and a solid lubricant respectively and drying them to obtain a modified porous adsorbent and a modified solid lubricant.
[0040] S2: adding the modified porous adsorbent into the grease heated to melt and mixing to obtain a first mixed system.
[0041] S3: The first mixed system is placed in a temperature higher than the dropping point of the grease and allowed to stand under negative pressure.
[0042] S4: taking out the first mixed system and adding the modified solid lubricant to mix, so as to obtain a second mixed system.
[0043] S5: freeze-drying the second mixed system and crushing it into particles to obtain a low-friction composite reinforcing filler for fluororesin.
[0044] This method can solve the problem that it is difficult to add grease to the fluororesin system in the prior art. It is simple to operate, low in cost and high in efficiency. The filler particles prepared by this method have high practical value. After adding them to the fluororesin material, the friction performance under dry friction conditions can be effectively improved.
[0045] By mass, the raw materials include 20 to 45 parts of porous adsorbent, 40 to 50 parts of solid lubricant, 10 to 22 parts of grease, and 5 to 8 parts of coupling agent.
[0046] In step S1, the coupling agent solution is applied to the porous adsorbent and the solid lubricant by air jet treatment. In step S3, the coupling agent solution can be treated in a vacuum oven for 6 hours. In step S5, the coupling agent solution can be treated in a freeze drying oven for 12 hours at a trap temperature of -40°C. In step S5, the particles can be crushed into particles by a high-speed crusher. Preferably, the particles are crushed and passed through a 40-mesh sieve.
[0047] The low friction composite reinforcing filler for fluororesin prepared by this method has similar Figure 1 The structure shown includes a porous adsorbent 1, a grease 3, and a solid lubricant 2. The grease 3 is filled in the pores 11 of the porous adsorbent 1. The porous adsorbent 1 and the solid lubricant 2 have a coupling agent (the content is low, not shown in the figure). A portion of the solid lubricant 2 is located in the pores 11 of the porous adsorbent 1, and a portion of the solid lubricant 2 is attached to the porous adsorbent 1.
[0048] Among them, the porous adsorbent is selected from porous silica microspheres, molecular sieves or porous polyimides, and the pore size is 2μm~5μm. The solid lubricant is selected from at least one of graphite, molybdenum disulfide, black phosphorus, boron nitride, boron carbide, graphene, and tungsten disulfide. These materials can be used alone in self-lubricating resins as wear-resistant fillers. The components of molecular sieves are crystalline silicates or aluminosilicates, and silicates, aluminosilicates, silicon dioxide, polyimides, etc. can originally be used as wear-resistant fillers. In the embodiment of the present application, grease and wear-resistant fillers are prepared into micro-particle fillers with self-lubricating properties by vacuum adsorption and freeze drying, and then the particle fillers are used as reinforcing phases to improve the wear resistance of the resin material. The prepared filler can effectively reduce the friction coefficient and wear rate of fluororesin composite materials in an oil-free lubrication environment, and can be used in oil-free lubrication conditions.
[0049] Example 1
[0050] In this example, graphite is used as a solid lubricant to prepare a low-friction composite reinforced filler for fluororesin. The raw materials include the following components in percentage by mass: 30% porous silica microspheres with a pore size of 3 μm (Fanrui VR 01, Note: the materials repeated in the following examples and comparative examples are from the same source), 50% graphite (Xiens), 5% titanate coupling agent (Guangzhou Kehua JC-SJH58), and 15% 568°C high-temperature grease (BKD bearing grease).
[0051] The preparation process is as follows:
[0052] 1. Prepare 0.5g of titanate coupling agent into a 5% ethanol-water (ethanol: water = 9:1) solution for later use.
[0053] 2. Place 3 g of porous silica microspheres in a stirring container with a solvent injection port, start stirring and spray 3.75 g of the coupling agent solution prepared in step 1 on the surface of the microspheres. After spraying, pour out and place in a 60°C oven for 4 hours to dry for use.
[0054] 3. Place 5 g of graphite in a stirring container with a solvent injection port, start stirring and spray the remaining 6.25 g of the coupling agent solution prepared in step 1 on the graphite surface. After spraying, pour it out and place it in a 60°C oven for 4 hours to dry for use.
[0055] 4. Place 1.5g of high-temperature grease with a temperature resistance of 568℃ in a 250℃ oven and wait for it to completely melt and turn into liquid state. Keep it warm for later use.
[0056] 5. Pour the porous silica microspheres modified in step 2 into the liquid high-temperature grease prepared in step 4 and stir thoroughly.
[0057] 6. Place the mixture of porous silica microspheres and high temperature grease prepared in step 5 in a vacuum oven at 250°C and maintain vacuum for 6 hours.
[0058] 7. After step 6 is completed, add the graphite prepared in step 3 to the lubricating oil system and stir it thoroughly. After cooling, place it in a freeze drying oven and dry it for 12 hours.
[0059] 8. Pour the dried material from step 7 into a high-speed crusher and crush it, then pour it out for later use. Figure 2 shown.
[0060] 9. Pass the crushed material prepared in step 8 through a 40-mesh sieve to obtain a low-friction composite reinforcing filler for fluororesin. Figure 3 As shown, it can be seen that almost all porous adsorbents ( Figure 3The larger balls have solid lubricants ( Figure 3 The smaller ball in the figure), and the position indicated by the arrow shows that the porous adsorbent is completely wrapped by the solid lubricant.
[0061] Example 2
[0062] In this example, molybdenum disulfide is used as a solid lubricant to prepare a low-friction composite reinforced filler for fluororesin. The raw materials include the following components in terms of mass percentage: 45% of 5μm pore size molecular sieve (McLean ZSM-5), 40% of molybdenum disulfide, 5% of aminoethylaminopropyltrimethoxysilane, and 10% of 568°C high-temperature grease.
[0063] This embodiment provides a method for preparing the composite reinforced filler, comprising the following steps:
[0064] 1. Prepare 0.5 g of aminoethylaminopropyltrimethoxysilane into a 5% ethanol-water solution for later use.
[0065] 2. Place 4.5 g of molecular sieve with a pore size of 5 μm in a stirring container with a solvent injection port, start stirring and spray 5.29 g of the coupling agent solution prepared in step 1 on the surface of the microspheres. After spraying, pour it out and place it in a 60°C oven for 4 hours to dry for use.
[0066] 3. Place 4 g of molybdenum disulfide in a stirring container with a solvent injection port, start stirring and spray the remaining 4.71 g of the coupling agent solution prepared in step 1 on the graphite surface. After spraying, pour it out and place it in a 60°C oven for 4 hours to dry for use.
[0067] 4. Place 1g of high-temperature grease with a temperature resistance of 568℃ in a 250℃ oven and wait for it to completely melt and turn into liquid state. Keep it warm for later use.
[0068] 5. Pour the modified molecular sieve in step 2 into the liquid high-temperature grease prepared in step 4 and stir thoroughly.
[0069] 6. Place the mixture of molecular sieve and high temperature grease prepared in step 5 in a vacuum oven at 250°C and maintain vacuum for 6 hours.
[0070] 7. After step 6 is completed, add the molybdenum disulfide prepared in step 3 to the lubricating oil system and stir it thoroughly. After cooling, place it in a freeze drying oven and dry it for 12 hours.
[0071] 8. Pour the dried material from step 7 into a high-speed crusher and crush it for later use.
[0072] 9. Pass the crushed material prepared in step 8 through a 40-mesh sieve to obtain a low-friction composite reinforcing filler for fluororesin.
[0073] Example 3
[0074] In this example, porous polyimide is used as a porous adsorbent to prepare a low-friction composite reinforced filler for fluororesin. The raw materials include the following components in terms of mass percentage: 20% polyimide (DuPont SP-1) with a pore size of 2 μm, 50% boron nitride, 8% KH550, and 22% 568°C high-temperature grease.
[0075] This embodiment provides a method for preparing the composite reinforced filler, comprising the following steps:
[0076] 1. Prepare 0.8g KH550 into 5% ethanol-water solution for later use.
[0077] 2. Place 2 g of polyimide powder with a pore size of 3 μm in a stirring container with a solvent injection port, start stirring and spray 4.57 g of the coupling agent solution prepared in step 1 on the surface of the microspheres. After spraying, pour it out and place it in a 60°C oven for 4 hours to dry for use.
[0078] 3. Place 5g of boron nitride in a stirring container with a solvent injection port, start stirring and spray the remaining 11.43g of the coupling agent solution prepared in step 1 on the surface of the boron nitride. After spraying, pour it out and place it in a 60℃ oven for 4 hours to dry for use.
[0079] 4. Place 2.2g of high-temperature grease with a temperature resistance of 568℃ in a 250℃ oven and wait for it to completely melt and turn into liquid state. Keep it warm for later use.
[0080] 5. Pour the modified polyimide powder in step 2 into the liquid high-temperature grease prepared in step 4 and stir thoroughly.
[0081] 6. Place the mixture of polyimide and high temperature grease prepared in step 5 in a vacuum oven at 250°C and maintain vacuum for 6 hours.
[0082] 7. After step 6 is completed, add the boron nitride prepared in step 3 to the lubricating oil system and stir it thoroughly. After cooling, place it in a freeze drying oven and dry it for 12 hours.
[0083] 8. Pour the dried material from step 7 into a high-speed crusher and crush it for later use.
[0084] 9. Pass the crushed material prepared in step 8 through a 40-mesh sieve to obtain a low-friction composite reinforcing filler for fluororesin.
[0085] Comparative Example 1
[0086] According to mass percentage, the raw materials include the following components: 45% of porous silica microspheres with a pore size of 3 μm, 50% of graphite, and 5% of titanate coupling agent.
[0087] The preparation process is as follows:
[0088] 1. Prepare 0.5g of titanate coupling agent into 5% ethanol aqueous solution for later use.
[0089] 2. Place 4.5 g of porous silica microspheres in a stirring container with a solvent injection port, start stirring and spray 4.74 g of the coupling agent solution prepared in step 1 on the surface of the microspheres. After spraying, pour out and place in a 60°C oven for 4 hours to dry for use.
[0090] 3. Place 5 g of graphite in a stirring container with a solvent injection port, start stirring and spray the remaining 5.26 g of the coupling agent solution prepared in step 1 on the graphite surface. After spraying, pour it out and place it in a 60°C oven for 4 hours to dry for use.
[0091] 4. The materials prepared in steps 2 and 3 are fully mixed to obtain the filler of comparative example 1.
[0092] Example 4
[0093] In terms of mass percentage, the raw materials include the following components: 32% porous silica microspheres with a pore size of 3 μm, 40% graphite, 5% titanate coupling agent, and 23% 568°C high-temperature grease.
[0094] The preparation process is as follows:
[0095] 1. Prepare 0.5g of titanate coupling agent into 5% ethanol aqueous solution for later use.
[0096] 2. Place 3.2 g of porous silica microspheres in a stirring container with a solvent injection port, start stirring and spray 4.44 g of the coupling agent solution prepared in step 1 on the surface of the microspheres. After spraying, pour out and place in a 60°C oven for 4 hours to dry for use.
[0097] 3. Place 4 g of graphite in a stirring container with a solvent injection port, start stirring and spray 5.56 g of the coupling agent solution prepared in step 1 on the graphite surface. After spraying, pour it out and place it in a 60°C oven for 4 hours to dry for use.
[0098] 4. Place 2.3g of high-temperature grease with a temperature resistance of 568℃ in a 250℃ oven and wait for it to completely melt and turn into liquid state. Keep it warm for later use.
[0099] 5. Pour the porous silica microspheres modified in step 2 into the liquid high-temperature grease prepared in step 4 and stir thoroughly.
[0100] 6. Place the mixture of porous silica microspheres and high temperature grease prepared in step 5 in a vacuum oven at 250°C and maintain vacuum for 6 hours.
[0101] 7. After step 6 is completed, add the graphite prepared in step 3 to the lubricating oil system and stir it thoroughly. After cooling, place it in a freeze drying oven and dry it for 12 hours.
[0102] 8. Pour the dried material obtained in step 7 into a high-speed crusher, crush it, and pour it out for later use, thereby obtaining a low-friction composite reinforcing filler for fluororesin.
[0103] Example 5
[0104] In terms of mass percentage, the raw materials include the following components: 20% porous silica microspheres with a pore size of 3 μm, 60% graphite, 5% titanate coupling agent, and 15% 568°C high-temperature grease.
[0105] The preparation process is as follows:
[0106] 1. Prepare 0.5g of titanate coupling agent into 5% ethanol aqueous solution for later use.
[0107] 2. Place 2 g of porous silica microspheres in a stirring container with a solvent injection port, start stirring and spray 2.5 g of the coupling agent solution prepared in step 1 on the surface of the microspheres. After spraying, pour out and place in a 60°C oven for 4 hours to dry for use.
[0108] 3. Place 6 g of graphite in a stirring container with a solvent injection port, start stirring and spray the remaining 7.5 g of the coupling agent solution prepared in step 1 on the graphite surface. After spraying, pour it out and place it in a 60°C oven for 4 hours to dry for use.
[0109] 4. Place 1.5g of high-temperature grease with a temperature resistance of 568℃ in a 250℃ oven and wait for it to completely melt and turn into liquid state. Keep it warm for later use.
[0110] 5. Pour the porous silica microspheres modified in step 2 into the liquid high-temperature grease prepared in step 4 and stir thoroughly.
[0111] 6. Place the mixture of porous silica microspheres and high-temperature grease prepared in step 5 in a vacuum oven at 250°C and maintain vacuum for 6 hours.
[0112] 7. After step 6 is completed, add the graphite prepared in step 3 to the lubricating oil system and stir it thoroughly. After cooling, place it in a freeze drying oven and dry it for 12 hours.
[0113] 8. Pour the dried material from step 7 into a high-speed crusher and crush it for later use.
[0114] 9. Pass the crushed material prepared in step 8 through a 40-mesh sieve to obtain a low-friction composite reinforcing filler for fluororesin.
[0115] The fillers prepared in the examples and comparative examples were added to polytetrafluoroethylene resin to modify the composite material, and the steps were as follows:
[0116] (1) Weigh 80 parts of polytetrafluoroethylene (Sanaifu FR014-4, this application is not limited to this brand) and 20 parts of filler, dry each component at 80°C for 24 hours, shake and mix evenly, and sieve to obtain a powder for use.
[0117] (2) Pour the powder into a cylindrical mold and press it at a pressure of 100 MPa for 30 minutes. After demolding, place the molded material in a sintering furnace for sintering. The sintering temperature is raised from room temperature to 220°C at 150°C / h and then kept at this temperature for 30 minutes. Then, the temperature is raised to 375°C at 60°C / h and kept at this temperature for 2 hours. After the sintering is completed, the temperature is lowered to 220°C at -40°C / h, kept at this temperature for 2 hours, and then naturally cooled to obtain a polytetrafluoroethylene composite material. Among them, the polytetrafluoroethylene composite material sample obtained by adding the filler in Example 1 is as follows: Figure 4 shown.
[0118] The thermogravimetric analysis of the polytetrafluoroethylene composite material obtained by adding the filler in Example 1 was performed. The results are as follows: Figure 5 As shown in the figure, it can be seen from the thermal weight loss that the oil does not have a serious weight loss at 500°C and has good thermal stability.
[0119] The performance of each polytetrafluoroethylene composite material sample was tested and evaluated. The lubrication performance was measured by a reciprocating friction and wear tester, where the load was 10N, the linear speed was 36mm / s, and the test time was 60 minutes; the wear rate was measured by a white light interferometer; and the compression strength was tested by a universal testing machine. The results are as follows Figure 6 And as shown in Table 1.
[0120] Table 1
[0121] Example 1 Example 2 Example 3 Comparative Example 1 Example 4 Example 5 Visual inspection of packing size Smaller Smaller Smaller Smaller Larger Basically powdery Coefficient of Friction (COF) 0.057 0.063 0.059 0.156 0.104 0.127 <![CDATA[Wear rate / x10 -5 mm 3 / N.m]]> 4.71 4.92 4.79 9.69 8.43 7.52 25% deformation compression strength / MPa 12.9 12.5 12.1 13.1 11.9 12.6
[0122] Figure 6 In the graph, the curve value corresponds to the vertical axis on the right; the bar graph value corresponds to the vertical axis on the left. Figure 6As can be seen from Table 1, no high-temperature grease was added to Comparative Example 1, and the friction coefficient and wear rate were higher than those of Example 1 (specifically, the polytetrafluoroethylene composite material mixed with fillers in Example 1, for ease of description, the corresponding examples are directly used below), indicating that the grease stored in the pores can effectively reduce friction. More high-temperature grease was added to Example 4, and the friction coefficient and wear rate were also higher than those of Example 1. The main reason is that the grease content increased, the viscosity increased, the grease was not only filled in the pores, but also a large amount of grease was attached to the surface of the porous adsorbent, and the filler was difficult to disperse, resulting in uneven dispersion of the filler in the material. More solid lubricants were added to Example 5, and the friction coefficient and wear rate were higher than those of Example 1. The reason may be that the filler was not filled with enough grease, and the combination of the solid lubricant and the porous adsorbent was not strong enough, resulting in more fine powder in the filler, which was easily peeled off during the friction process. In general, each embodiment achieved a better lubrication effect than Comparative Example 1, proving that the filler prepared in the embodiment of the present application can effectively reduce the friction of the fluororesin system and has good temperature resistance.
[0123] In the description of this specification, the description with reference to the terms "one embodiment", "certain embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials, or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials, or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0124] The above is a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several improvements and modifications without departing from the principle of the present invention. These improvements and modifications are also considered to be within the scope of protection of the present invention.
Claims
1. A method for preparing a low-friction composite reinforcing filler for fluororesin, It is characterized in that The following steps are involved: Applying a coupling agent solution on a porous adsorbent and a solid lubricant respectively and drying the solution to obtain a modified porous adsorbent and a modified solid lubricant; Adding the modified porous adsorbent to the grease heated to melt and mixing to obtain a first mixed system; placing the first mixed system in an environment with a temperature above the dropping point of the grease and allowing it to stand at negative pressure; Taking out the first mixed system and adding the modified solid lubricant to mix, to obtain a second mixed system; The second mixed system is freeze-dried and crushed into particles to obtain the low-friction composite reinforcing filler for fluororesin.
2. The method for preparing the low-friction composite reinforcing filler for fluororesin according to claim 1, It is characterized in that The raw materials include, by mass, 20 to 45 parts of the porous adsorbent, 40 to 50 parts of the solid lubricant, 10 to 22 parts of the grease, and 5 to 8 parts of the coupling agent.
3. The method for preparing the low-friction composite reinforcing filler for fluororesin according to claim 1, It is characterized in that The dropping point of the grease is 200°C to 250°C and the temperature resistance is above 550°C.
4. The method for preparing a low-friction composite reinforcing filler for fluororesin according to claim 1, It is characterized in that The freezing requirement in the freeze drying is -40°C for 12 hours.
5. The method for preparing the low-friction composite reinforcing filler for fluororesin according to claim 1, It is characterized in that The negative pressure standing time is 6 hours.
6. The method for preparing a low-friction composite reinforcing filler for fluororesin according to claim 1, It is characterized in that The solid lubricant is selected from at least one of graphite, molybdenum disulfide, black phosphorus, boron nitride, boron carbide, graphene, and tungsten disulfide.
7. The method for preparing a low-friction composite reinforcing filler for fluororesin according to claim 1, It is characterized in that The coupling agent solution comprises at least one component selected from KH550, KH560, a titanate coupling agent, and aminoethylaminopropyltrimethoxysilane.
8. The method for preparing a low-friction composite reinforcing filler for fluororesin according to claim 1, It is characterized in that The porous adsorbent is selected from porous silica microspheres, molecular sieves or porous polyimide, and has a pore size of 2 μm to 5 μm.
9. The method for preparing a low-friction composite reinforcing filler for fluororesin according to claim 1, It is characterized in that After being crushed into particles, the particles need to be screened through a 40-mesh sieve.
10. A low friction composite reinforcing filler for fluororesin, It is characterized in that The low-friction composite reinforcing filler for fluororesin is prepared by the preparation method of any one of claims 1 to 9.
Citation Information
Patent Citations
Porous oil-containing polyimide composite material for ultrasonic motor and preparation method thereof
CN104893288A
Porous high-aluminum zinc-based oil bearing material
CN105400979A
Porous polymer composite material, blended lubricating oil, porous oil-containing self-lubricating composite material and preparation method and application thereof
CN118325166A