Negative electrode material and preparation method thereof and lithium ion battery

By using Raman surface sweep test in lithium-ion batteries, the silicon-based-graphite negative electrode material was solved by combining plasma modification and uniform dispersion technology, the existing silicon-based-graphite materials were insufficient in the synergistic effect of lithium-ion batteries. The problem has improved the yield and performance stability of the battery.

CN118658985BActive Publication Date: 2024-11-22BTR NEW MATERIAL GRP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411132627.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-22
Estimated Expiration
2044-08-19

AI Technical Summary

Technical Problem

The existing silicon-based-graphite anode materials cannot effectively play a synergistic role in lithium-ion batteries, resulting in low battery yield and unstable performance. The introduction of silicon-based materials increases the difficulty of the battery process, making it easy for a decrease in battery yield.

Method used

Through Raman surface sweep test, it was determined that the morphological difference between particles in the negative electrode material was low. The modified silicon-based material was treated with plasma modification, and it was evenly dispersed with the graphite material, and bonded with an appropriate amount of adhesive precursor. A negative electrode material that meets specific peak strength ratios and other characteristics is produced.

Benefits of technology

It improves the batch yield and performance stability of lithium-ion batteries, reduces the gas production during the aging process and the production of gas in high-temperature storage, and enhances the consistency and efficiency of the batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118658985B_ABST
    Figure CN118658985B_ABST
Patent Text Reader

Abstract

The present application belongs to the technical field of negative electrode materials for lithium-ion batteries, and discloses a negative electrode material and a preparation method thereof and a lithium-ion battery. The negative electrode material comprises a silicon-based material and a graphite-based material. The negative electrode material is subjected to a Raman surface scan test, and 200 groups of spectra are randomly selected. The 500 cm ‑1 ‑520cm ‑1 The number of spectra with peaks at 500 cm is set to n. ‑1 ‑520cm ‑1 In the spectrum with peaks at: 1345cm ‑1 ‑1355cm ‑1 The peak intensities at I A1 , I A2 , … , I An , 1570cm ‑1 ‑1610cm ‑1 The peak intensities at I´ A1 , I ´ A2 , … , I´ An The negative electrode material satisfies the relationship: #imgabs0#, #imgabs1#. The negative electrode material prepared according to the embodiment of the present application has low morphological differences between particles and high concentration. The battery batch yield made using the negative electrode material is high and the batch is stable.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of negative electrode materials for lithium-ion batteries, and more specifically, to a negative electrode material and a preparation method thereof, and a lithium-ion battery. Background Art

[0002] The negative electrode material is one of the most critical materials in lithium-ion batteries. The existing commonly used negative electrode materials are usually ordinary carbon materials, and their capacity has reached its limit. If you want to continue to increase the capacity, you need to introduce other types of negative electrode materials. Silicon-based negative electrode materials have high specific capacity and have been industrialized, but their large volume expansion limits large-scale applications. At present, the application of silicon-based negative electrode materials is still used in combination with graphite, and the addition ratio is not high. In order to give full play to the advantages of silicon-based-graphite negative electrode materials and avoid disadvantages at the same time, it is necessary to consider the matching and composite methods of graphite and silicon-based materials.

[0003] At present, silicon-based-graphite negative electrode materials are mainly a simple mixture of silicon-based materials and graphite, which cannot bring into play the synergistic effect of the two. Silicon-based materials only enter the graphite system as simple additives and cannot effectively exert their advantageous performance. A good composite method can synergistically bring out the advantages of graphite and silicon-based materials while hiding the disadvantages. For example, the addition of silicon-based materials can make up for the insufficient capacity of graphite, and the introduction of graphite can buffer the expansion of silicon-based materials and extend the cycle life. However, the introduction of silicon-based materials will increase the difficulty of the battery process and easily lead to a decrease in battery yield.

[0004] Based on this, providing a silicon-based-graphite negative electrode material so that the produced battery has high yield and stable performance is an urgent problem to be solved. Summary of the invention

[0005] According to one aspect of the present application, a negative electrode material is provided, the negative electrode material comprises a silicon-based material and a graphite-based material, and a Raman surface scan test is performed on the negative electrode material, 200 groups of spectra are randomly selected, 500 cm -1 -520cm -1 The number of spectra with peaks at 500 cm is set to n. -1 -520cm -1 In the spectrum with peaks at: 1345cm -1 -1355cm -1 The peak intensities at I A1 , I A2 , … , I An , 1570cm -1 -1610cm -1 The peak intensities at I´A1 , I´ A2 , … , I´ An ; The negative electrode material satisfies the relationship:

[0006]

[0007] in, .

[0008] According to one embodiment of the present application, the negative electrode material satisfies the relationship:

[0009] .

[0010] According to one embodiment of the present application, the negative electrode material satisfies the relationship:

[0011] .

[0012] According to one embodiment of the present application, the negative electrode material includes at least one of the following features:

[0013] a. Specific surface area <3.0 m 2 / g; b. Water content by mass <0.5%; c. Volume distribution of particle size D10>1.0μm; d. Based on the mass of the negative electrode material as 100wt%, the carbon content is 5wt%~95wt%, and the silicon content is 5wt%~95%; e. The gas production of the battery made of the negative electrode material during aging is <0.01mL / Ah; f. The gas production of the battery made of the negative electrode material during aging after being stored at 60℃ for 15 days is <0.1mL / Ah; g. 500cm in the Raman spectrum -1 -520cm -1 The ratio of the number of spectra with peaks to the number of spectra without peaks is 0.05-40.

[0014] According to one embodiment of the present application, the negative electrode material includes at least one of the following features:

[0015] a. Silicon-based materials include at least one of amorphous silicon, crystalline silicon, silicon oxide and silicate; b. Graphite-based materials include at least one of natural graphite, artificial graphite, expanded graphite and graphite oxide; c. The negative electrode material includes a carbon material, and the carbon material includes at least one of amorphous carbon and graphitized carbon.

[0016] According to another aspect of the present application, a method for preparing a negative electrode material is provided, comprising: a first step of preparing a modified silicon-based material: taking a silicon-based material having a surface coated with a carbon layer, introducing a non-polymerizing gas to perform plasma modification treatment on the surface of the silicon-based material under vacuum to a pressure less than 0.1 MPa, wherein the temperature of the plasma modification treatment is 30°C to 180°C, the time of the plasma modification treatment is 10s-150s, the median particle size of the particles of the silicon-based material is 2μm to 20μm, and a modified silicon-based material is obtained; a second step of preparing a suspension containing a silicon-based material and graphite: uniformly dispersing the modified silicon-based material in a dispersant, gradually adding graphite particles, stirring and dispersing to obtain a suspension containing a silicon-based material and graphite, wherein the D50 of the graphite particles is 6μm-20μm; a third step of preparing a negative electrode material: mixing a suspension containing a silicon-based material and graphite with a binder precursor having a mass ratio of 0.01%-3% relative to the suspension, separating the solvent and drying to obtain the negative electrode material.

[0017] According to one embodiment of the present application, the first step includes at least one of the following parameters: a. the pressure range of the plasma modification treatment is 50Pa~150Pa; b. the non-polymerizing gas includes at least one of hydrogen, argon, helium, nitrogen, krypton, and neon; c. the silicon-based material includes at least one of amorphous silicon, crystalline silicon, silicon oxide and silicate.

[0018] According to one embodiment of the present application, the second step includes at least one of the following parameters:

[0019] a. The graphite particles include at least one of natural graphite, artificial graphite, expanded graphite and graphite oxide; b. The dispersant includes one or a mixture of two or more of deionized water, ethanol, propanol, isopropanol, propane, DFM (N,N-dimethylformamide), and acetone; c. The mass content of silicon particles in the suspension containing silicon-based material and graphite is 5wt%~95wt%; d. The mass content of graphite in the suspension containing silicon-based material and graphite is 5wt%~95wt%.

[0020] According to one embodiment of the present application, the third step includes at least one of the following parameters:

[0021] a. The adhesive precursor contains at least one of amino, carboxyl, cyano and hydroxyl functional groups; b. The number average molecular weight of the adhesive precursor is 2000-1000000; c. The viscosity of the adhesive precursor at a solid content of 3% is 1000mPa·s-100000mPa·s.

[0022] According to another aspect of the present application, a lithium-ion battery is provided, comprising the negative electrode material of any of the foregoing embodiments or the negative electrode material prepared according to the preparation method of any of the foregoing embodiments.

[0023] The negative electrode material prepared according to the embodiment of the present application has low morphology difference between particles and high concentration. The battery batch yield made by using the negative electrode material is high and the batch is stable. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] By reading the detailed description below with reference to the accompanying drawings, the above and other purposes, features and advantages of the exemplary embodiments of the present application will become easy to understand. In the accompanying drawings, several embodiments of the present application are shown in an exemplary and non-limiting manner, and the same or corresponding reference numerals represent the same or corresponding parts, wherein:

[0025] Figure 1 shows a schematic diagram of a battery in a discharged state;

[0026] Figure 2 A schematic diagram showing the steps of a method for preparing a negative electrode material;

[0027] Figure 3 A schematic diagram of the Raman spectrum of the negative electrode material of Example 1 is shown. DETAILED DESCRIPTION

[0028] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present application.

[0029] It should be understood that the terms "include" and "comprising" used in the specification and claims of the present application indicate the presence of described features, wholes, steps, operations, elements and / or components, but do not exclude the presence or addition of one or more other features, wholes, steps, operations, elements, components and / or collections thereof.

[0030] It should also be understood that the terms used in this application specification are only for the purpose of describing specific embodiments and are not intended to limit the present application. As used in this application specification and claims, unless the context clearly indicates otherwise, the singular forms of "a", "an" and "the" are intended to include plural forms. It should also be further understood that the term "and / or" used in this application specification and claims refers to any combination of one or more of the associated listed items and all possible combinations, and includes these combinations.

[0031] As used in this specification and claims, the term "if" can be interpreted as "when" or "upon" or "in response to determining" or "in response to detecting," depending on the context. Similarly, the phrases "if it is determined" or "if [described condition or event] is detected" can be interpreted as meaning "upon determination" or "in response to determining" or "upon detection of [described condition or event]" or "in response to detecting [described condition or event]," depending on the context.

[0032] The specific implementation methods of the present application are described in detail below in conjunction with the accompanying drawings. Unless otherwise specified, the materials, reagents and equipment used in the examples of the present application are all obtained from conventional commercial channels.

[0033] An embodiment of the present application provides a secondary battery (such as a lithium-ion battery, a sodium-ion battery, etc.), comprising a housing, an electrode assembly, and an electrolyte / electrolyte. The electrode assembly and the electrolyte / electrolyte are both located in the housing.

[0034] The outer shell may be a packaging bag encapsulated by an encapsulation film (such as an aluminum-plastic film), such as a soft-pack battery. In other embodiments, the secondary battery may also be a steel-shell battery, an aluminum-shell battery, or the like.

[0035] Figure 1 A schematic diagram of a battery in a discharge state, i.e., during operation, is shown. As shown in the figure, the electrode assembly includes a positive electrode sheet 110, a negative electrode sheet 120, and a separator 130, and the separator is disposed between the positive electrode sheet and the negative electrode sheet. The electrode assembly can be a laminated structure, which is formed by alternately stacking the positive electrode sheet, the separator, and the negative electrode sheet in sequence. In other embodiments, the electrode assembly can also be a winding structure, which is formed by stacking the positive electrode sheet, the separator, and the negative electrode sheet in sequence and then winding them.

[0036] Positive electrode

[0037] The positive electrode sheet 110 includes a positive electrode current collector 111 and a positive electrode active layer 112 disposed on at least one surface of the positive electrode current collector. The positive electrode current collector may be made of aluminum foil or nickel foil, or may be any composite current collector disclosed in the prior art, such as but not limited to the current collector formed by combining the aforementioned conductive foil and a polymer substrate. The positive electrode active layer contains a positive electrode active material, and the positive electrode active material includes a compound that reversibly embeds and deintercalates metal ions. In some embodiments, the positive electrode active material may include a lithium transition metal composite oxide, a sodium transition metal composite oxide, and the like. The lithium transition metal composite oxide contains lithium and at least one element selected from cobalt, manganese and nickel. In some embodiments, the positive electrode active material may include but is not limited to lithium cobalt oxide (LiCoO2), lithium nickel manganese cobalt ternary material (NCM), lithium manganese oxide (LiMn2O4), lithium nickel manganese oxide (LiNi 0.5 Mn 1.5O4) or at least one of lithium iron phosphate (LiFePO4).

[0038] Negative plate

[0039] The negative electrode sheet 120 includes a negative electrode current collector 121 and a negative electrode active material layer 122 disposed on at least one surface of the negative electrode current collector. The negative electrode current collector may be at least one of copper foil, nickel foil, stainless steel foil, titanium foil or carbon-based current collector, or may be any composite current collector disclosed in the prior art, such as but not limited to a current collector formed by combining the aforementioned conductive foil and a polymer substrate. The negative electrode active material layer includes a negative electrode material.

[0040] During battery operation, that is, when the battery is in a discharge state, metal ions 140 (eg, lithium ions) in the negative electrode are released from the lattice of the negative electrode material, pass through the separator 130 through the electrolyte / electrolyte, and are embedded in the lattice of the positive electrode material.

[0041] Conversely, when the battery is charged by applying an external circuit, the oxidation of the positive electrode material causes the metal ions (such as lithium ions) in the positive electrode to escape from the lattice of the positive electrode material, pass through the isolation membrane through the electrolyte / electrolyte, and move to the negative electrode; at the same time, the negative electrode material undergoes a reduction reaction, causing the metal ions to be embedded in the lattice of the negative electrode material.

[0042] As metal ions move back and forth between the positive and negative electrodes, the battery can be discharged and charged thousands of times.

[0043] The performance of the negative electrode material containing silicon-based materials and graphite is mainly affected by the performance of graphite and silicon-based materials. There is interference and synergy between silicon-based materials and graphite. Only by giving full play to the positive synergy between silicon-based materials and graphite as much as possible and suppressing their negative interference, can the negative electrode material containing silicon-based materials and graphite exert good electrochemical performance.

[0044] The present application provides a negative electrode material, which includes a silicon-based material and a graphite-based material. The negative electrode material is subjected to a Raman surface scan test, and 200 groups of spectra are randomly selected, 500 cm -1 -520cm -1 The number of spectra with peaks at 500 cm is set to n. -1 -520cm -1 In the spectrum with peaks at: 1345cm -1 -1355cm -1 The peak intensities at I A1 , I A2 , … , I An , 1570cm -1-1610cm -1 The peak intensities at I´ A1 , I´ A2 , … , I´ An ; The negative electrode material satisfies the relationship:

[0045] in, .

[0046] Batteries prepared with negative electrode materials containing silicon-based materials and graphite are prone to fluctuations in capacity and first effect. The inventors speculate that this is related to the large differences in the particle surface morphology of the negative electrode materials. After a large number of experimental studies and verifications, the inventors found that by limiting the degree of difference in particle morphology in negative electrode materials containing silicon-based materials and graphite-like materials to a certain range, the yield of lithium-ion batteries can be effectively improved. Raman surface scanning can characterize the surface characteristics of negative electrode materials. Therefore, in the embodiments of the present application, Raman surface scanning can be used to determine / characterize the differences in particle surface morphology of negative electrode materials containing silicon-based materials and graphite-like materials, thereby providing negative electrode materials that can produce batteries with high yield and stable performance.

[0047] In the Raman scan spectrum, 500 cm -1 -520cm -1 The peak at 500cm can be used to characterize the resonance vibration peak between Si-Si atoms. Its peak intensity and shape can reflect the crystal structure and impurity content of the active substance in the silicon-based material. -1 -520cm -1 The peak at 1345cm indicates that the negative electrode material contains silicon-based materials within the Raman scan range. -1 -1355cm -1 The peak at 1570cm (also called D peak) reflects the disordered structure of the carbon material (amorphous carbon material). -1 -1610cm -1 The peak at (also called G peak) corresponds to the plane vibration mode of graphite and represents the SP 2 bond (planar structure), reflecting the ordered structure of the carbon material (i.e., graphitized carbon material). The K value in the above relationship refers to the ratio of the peak intensity of the D peak to the peak intensity of the G peak detected in the spectrum of the silicon-based material in the negative electrode material. D / I G The above relationship represents the variance of the ratio of the peak intensity of the D peak to the peak intensity of the G peak in the spectrum of the silicon-based material. The difference from the average value (e.g., variance) is used to measure the morphological differences between particles in the negative electrode material. The smaller the variance, the closer the morphology between particles. The battery produced with this negative electrode material has a higher yield and more stable performance.

[0048] Specifically, in the Raman scan spectrum, at 500 cm -1 -520cm -1 When the peak intensity of the spectrum with a peak at satisfies the numerical range of the above relationship, the morphological difference between the particles of the negative electrode material is low, the concentration is high, and the batch yield of the manufactured battery is high and the batch is stable. The higher the morphological concentration between the particles, the higher the consistency of the reaction degree between the surface of the negative electrode material particles and the electrolyte after the battery is made, that is, the closer the thickness and composition of the solid electrolyte interface (SEI) layer generated on the surface of different negative electrode material particles during the battery formation and capacity separation process, the smaller the difference, the more concentrated the capacity and efficiency of the battery made of the negative electrode material, the higher the battery consistency, that is, the higher the battery yield.

[0049] When the value of the above relationship is greater than 0.8, it means that the morphology concentration between particles in the negative electrode material is low, the morphology is diverse and dispersed, and the SEI content, morphology, and thickness generated during the formation and capacity separation process are different, resulting in large fluctuations in the capacity and efficiency of the battery made of the negative electrode material and low battery yield.

[0050] Furthermore, in some embodiments, when the above relationship is less than 0.01, more steps and costs need to be added, which is not conducive to the industrialization of negative electrode material products and the embodiment of commercial value.

[0051] In some embodiments, the negative electrode material satisfies the relationship: . This relationship can be further used to characterize the surface morphology concentration between particles in the negative electrode material from another perspective. This relationship represents the average deviation of the ratio of the peak intensity of the D peak to the G peak in the spectrum of each silicon-based material relative to the average value K, that is, the absolute deviation of the mean. When the concentration satisfies the range of the above relationship, the morphology concentration between particles in the negative electrode material is high, and the produced batteries have good consistency and high yield. When the absolute value of the concentration is greater than 0.3, it means that the surface morphology between particles in the negative electrode material is relatively dispersed and diverse, and the SEI content, morphology, and thickness generated during the formation and capacity separation process are different, resulting in large fluctuations in the battery capacity and efficiency, and low battery yield.

[0052] In some embodiments, the specific surface area of ​​the negative electrode material is less than 3.0 m 2 / g, which can be 2.9m 2 / g, 2.8m 2 / g, 2.7m 2 / g, 2.6m 2 / g, 2.5m 2 / g, 2.4m 2 / g, 2.3m 2 / g, 2.0m 2 / g, 1.5m 2 / g, 1.0 m 2 / g, etc., and of course, other values ​​within the above range are also possible. When the specific surface area falls within the above range, it means that the surface morphology of the negative electrode material is concentrated, not dispersed or messy, and the SEI content, morphology, and thickness generated during the formation and capacity separation process are uniform, so that the capacity and efficiency of the battery fluctuate little and the battery yield is high.

[0053] In some embodiments, the water content of the negative electrode material is less than 0.5%, and can be 0.49%, 0.48%, 0.47%, 0.46%, 0.45%, 0.40%, 0.35%, 0.30%, 0.25%, 0.20%, 0.15%, 0.10%, etc., and can also be other values ​​within the above range. When the water content falls within the above range, it means that the surface morphology of the negative electrode material is concentrated, not scattered or messy, and the SEI content, morphology, and thickness generated during the formation and volume separation process are uniform, so that the capacity and efficiency of the battery fluctuate little, and the battery yield is high.

[0054] In some embodiments, the volume distribution D10 of the particle size in the negative electrode material is greater than 1.0 μm, and can be 1.1 μm, 1.2 μm, 1.3 μm, 1.4 μm, 1.5 μm, 1.6 μm, 1.7 μm, 1.8 μm, 1.9 μm, 2.0 μm, etc., and can also be other values ​​within the above range. When the volume distribution D10 falls within the above range, it means that the surface morphology of the negative electrode material is concentrated, not dispersed or messy, and the SEI content, morphology, and thickness generated during the formation and volume separation process are uniform, so that the capacity and efficiency of the battery fluctuate little, and the battery yield is high.

[0055] In some embodiments, based on the mass of the negative electrode material as 100wt%, the carbon content is 5wt%~95wt%, and the silicon content is 5wt%~95%. Exemplarily, the carbon content can be 5wt%, 10wt%, 15wt%, 20wt%, 25wt%, 30wt%, 35wt%, 40wt%, 45wt%, 50wt%, 60wt%, 70wt%, 80wt%, 90wt%, 95wt%, etc., and of course, it can also be other values ​​within the above range. Similarly, exemplary, the silicon content can be 95wt%, 90wt%, 85wt%, 80wt%, 75wt%, 70wt%, 65wt%, 60wt%, 55wt%, 50wt%, 40wt%, 30wt%, 20wt%, 10wt%, 5wt%, etc., and of course, it can also be other values ​​within the above range.

[0056] In some embodiments, the gas production of batteries made of negative electrode materials during aging is less than 0.01 mL / Ah, and exemplary values ​​may be 0.009 mL / Ah, 0.008 mL / Ah, 0.007 mL / Ah, 0.006 mL / Ah, 0.005 mL / Ah, 0.004 mL / Ah, 0.003 mL / Ah, 0.002 mL / Ah, 0.001 mL / Ah, etc., and of course other values ​​within the above range may also be possible.

[0057] In some embodiments, after a battery made of a negative electrode material is stored at 60°C for 15 days, the gas production during the process is less than 0.1 mL / Ah. Exemplary values ​​may be 0.09 mL / Ah, 0.08 mL / Ah, 0.07 mL / Ah, 0.06 mL / Ah, 0.05 mL / Ah, 0.04 mL / Ah, 0.03 mL / Ah, 0.02 mL / Ah, 0.01 mL / Ah, etc., and of course other values ​​within the above range may also be possible.

[0058] In some embodiments, the Raman spectrum of the negative electrode material is 500 cm -1 -520cm -1 The ratio of the number of spectra with peaks to the number of spectra without peaks is 0.05-40, and can be 0.05, 0.1, 0.5, 1, 5, 10, 15, 20, 25, 30, 35, 40, etc., and can be other values ​​within the above range. The ratio of the number of spectra with peaks to the number of spectra without peaks can characterize the proportion of silicon in the product from another perspective.

[0059] In some embodiments, the silicon-based material in the negative electrode material may include at least one of amorphous silicon, crystalline silicon, silicon oxide, and silicate.

[0060] In some embodiments, the silicon-based material includes silicon oxide, the silicon oxide includes silicon element and oxygen element, and the atomic ratio of the silicon element to the oxygen element is 0~2, and does not include 0.

[0061] In some embodiments, the silicon-based material includes silicon oxide, and the chemical formula of silicon oxide is SiOx, where 0<x≤2. Specifically, SiOx can be SiO 0.5 、SiO 0.7 、SiO 0.9 、SiO、SiO 1.2 、SiO 1.5 、SiO 1.8 、SiO 1.9 Etc., no limitation is made here.

[0062] Silicon oxide can be expressed by the general formula SiOx (0<x≤2). It can be a material formed by silicon dispersed in SiO2; it can also be a material with a tetrahedral structural unit, in which the silicon atom is located at the center of the tetrahedral structural unit, and the oxygen atoms and / or silicon atoms are located at the four vertices of the tetrahedral structural unit.

[0063] In some embodiments, the graphite material in the negative electrode material may include at least one of natural graphite, artificial graphite, expanded graphite, and oxidized graphite.

[0064] In some embodiments, the negative electrode material includes a carbon material, and the carbon material includes at least one of amorphous carbon and graphitized carbon.

[0065] The negative electrode material provided in the embodiment of the present application is a composite material comprising a silicon-based material and a graphite-like material, and its specific composite form can be diverse, for example, it can be a silicon-based material and a graphite-like material composited into a core, and the surface of the core has a carbon coating layer; it can also be a silicon-based material and a graphite-like material dispersed with each other, and the surfaces of the two have carbon coating layers respectively. This good composite method can synergistically bring out the advantages of silicon-based materials and graphite-like materials. The battery prepared using this negative electrode material has a high yield and good stability.

[0066] Figure 2 A schematic diagram showing exemplary steps of a method for preparing negative electrode materials according to some embodiments of the present application is shown.

[0067] As shown in the figure, the preparation method of the negative electrode material includes: a first step S1, preparing a modified silicon-based material: taking a silicon-oxygen raw material with a carbon layer coated on the surface, and introducing a non-polymerizing gas to perform plasma modification on the surface of the silicon-oxygen raw material under vacuum to a pressure less than 0.1MPa, wherein the temperature of the plasma modification treatment is 30°C~180°C, the time of the plasma modification treatment is 10s-150s, and the median particle size of the silicon-based material is 2μm~20μm, thereby obtaining a modified silicon-based material; a second step S2, preparing a suspension containing silicon-based material and graphite: uniformly dispersing the modified silicon-based material in a dispersant, gradually adding graphite particles, stirring and dispersing to obtain a suspension containing silicon-based material and graphite, wherein the D50 of the graphite particles is 6μm-20μm; a third step S3, preparing a negative electrode material: mixing a suspension containing silicon-based material and graphite with a binder precursor having a mass ratio of 0.01%-3% relative to the suspension, separating the solvent and drying to obtain a negative electrode material.

[0068] Specifically, in the first step, 200-1000 g of silicon-oxygen raw material with a surface coated with a carbon layer is placed in a low-temperature plasma device, and after evacuating to a pressure less than 0.1 MPa, a non-polymerizing gas is introduced to perform plasma modification treatment on the surface of the silicon-oxygen raw material particles.

[0069] Placing the silicon-oxygen raw material in a plasma device for modification can adjust the surface morphology of the silicon-oxygen raw material. After plasma modification, the carbon layer on the surface of the silicon-oxygen raw material particles is evenly wrapped on its surface, while controlling the deposition speed and thickness of the carbon layer on the surface of graphite and silicon-oxygen raw materials, and adjusting the morphology concentration between particles.

[0070] In some embodiments, the silicon-oxygen raw material includes silicon oxide SiOy, wherein 0<y≤2, and silicon oxide is a silicon-oxygen composite, comprising oxygen atoms and silicon atoms, and the molar ratio of oxygen atoms to silicon atoms is 0 to 2 and does not include 0. It can be Si, SiO 0.2 、SiO 0.5 、SiO 0.8 、SiO、SiO 1.2 、SiO 1.5 、SiO 1.8 Or a substance composed of two or more of SiO2, etc., or a compound with the chemical formula SiOy, y can of course also be other values ​​within the above range, and this application does not limit it here.

[0071] The modification results are related to temperature, pressure, time, etc.

[0072] In some embodiments, the pressure range of the plasma modification treatment in the first step is 50Pa~150Pa, and exemplary values ​​may be 50Pa, 60Pa, 70Pa, 80Pa, 90Pa, 100Pa, 110Pa, 120Pa, 130Pa, 140Pa, 150Pa, etc., and of course other values ​​within the above range may also be possible.

[0073] In some embodiments, the time of the plasma modification treatment in the first step is 10s-150s, and exemplary values ​​may be 10s, 20s, 30s, 40s, 50s, 60s, 70s, 80s, 90s, 100s, 110s, 120s, 130s, 140s, 150s, etc., and of course other values ​​within the above range may also be possible.

[0074] In some embodiments, the non-polymerizable gas in the first step includes at least one of hydrogen, argon, helium, nitrogen, krypton, and neon. The non-polymerizable gas refers to a gas that cannot undergo polymerization reaction by itself.

[0075] In some embodiments, the silicon-based material includes at least one of amorphous silicon, crystalline silicon, silicon oxide, and silicate.

[0076] In some embodiments, the median particle size of the silicon-based material is 2 μm to 20 μm, and exemplary values ​​may be 2 μm, 4 μm, 6 μm, 8 μm, 10 μm, 12 μm, 14 μm, 16 μm, 18 μm, 20 μm, etc., and other values ​​within the above range are also possible.

[0077] Specifically, in the second step, the modified silicon-based material obtained in the first step is uniformly dispersed in a dispersant, and then graphite particles are gradually added, and after stirring and dispersing at a rotation speed of 300-1000 rpm for 1h-4h, a suspension containing silicon-based material and graphite is obtained.

[0078] The dispersant includes one of deionized water, ethanol, propanol, isopropanol, propane, DFM, and acetone, or a mixture of two or more thereof.

[0079] The graphite particles include at least one of natural graphite, artificial graphite, expanded graphite and oxidized graphite. The Dv50 of the graphite particles is 6μm-20μm, and can be 6μm, 8μm, 10μm, 12μm, 14μm, 16μm, 18μm, 20μm, etc., and can also be other values ​​within the above range. The mass content of silicon particles in the suspension containing silicon-based materials and graphite is 5wt%~95wt%. The mass content of graphite in the suspension containing silicon-based materials and graphite is 5wt%~95wt%.

[0080] The modified silicon-based material is first dispersed in a solution using a liquid phase dispersion method, and then graphite particles are added continuously in batches, which helps to evenly disperse the silicon-based material and graphite particles and further prevent particle agglomeration.

[0081] Specifically, in the third step, the suspension containing the silicon-based material and graphite is transferred to a three-necked flask, 0.01%-3% of a binder precursor is added, and the rotation speed of the stirring paddle is set at 50 rpm-300 rpm.

[0082] The adhesive precursor contains at least one of amino, carboxyl, cyano and hydroxyl functional groups. The number average molecular weight of the adhesive precursor is 2000-1000000. The adhesive precursor has a viscosity of 1000 Pa·s-100000 mPa·s when the solid content is 3%.

[0083] After the suspension containing silicon-based material and graphite is evenly mixed with the binder precursor, start heating and keep stirring during heating. When the temperature reaches 50℃-120℃, turn on the vacuum pump and keep the vacuum degree in the three-necked flask below 0.5MPa. After reacting for 4h-12h, start condensation reflux to separate the solvent in the mixed solution after the reaction, and then place the remaining material in the three-necked flask in a vacuum oven and dry it below 80℃ to obtain the negative electrode material.

[0084] A small amount of binder precursor is first added to the mixed suspension containing silicon-based materials and graphite, and then dried. On the one hand, this can prevent the silicon-based materials and graphite from agglomerating again during the slurry preparation process, which would lead to uneven distribution of components. On the other hand, secondary adjustments can be made to the surfaces of the silicon-based materials and graphite to further improve the concentration of their morphology and improve the yield of battery production.

[0085] Optionally or additionally, in some embodiments, the negative electrode material obtained in the above steps can be dispersed and sieved by a vibration chamber (VC) high-efficiency mixer.

[0086] The negative electrode material prepared according to the preparation method of the embodiment of the present application can be applied to lithium-ion batteries. It is a composite material of silicon and graphite, and its good composite method can synergistically bring out the advantages of graphite and silicon.

[0087] According to another aspect of the present application, a lithium-ion battery is provided, comprising the aforementioned negative electrode material or the negative electrode material prepared according to the aforementioned preparation method.

[0088] Example 1

[0089] Step 1: Take 50g of silicon oxide particles (core SiO, surface with carbon coating) (D50 = 6μm) (commercially available) and place them in the material chamber of the low-temperature plasma equipment, evacuate to an internal pressure of 80Pa, heat to 130℃, and heat at 10cm 3 Hydrogen was introduced at a rate of / min, and after treating for 60s, the temperature began to drop to 25°C, and the sample was taken out to obtain modified silicon oxide particles.

[0090] Step 2: Take 50g of modified silica particles (D50=6μm) and put them into 200g of isopropanol solvent, disperse them at 200rpm for 1h, then add 450g of graphite particles (commercially available) and continue to stir and disperse for 1h to obtain silica-graphite suspension. The mass content of silicon particles in the suspension is 10wt%, and the mass content of graphite is 90wt%.

[0091] Step 3: Transfer the silicon-graphite suspension to a three-necked flask, add 1% (mass ratio relative to the total amount of silicon and graphite) of polyacrylic acid with a number average molecular weight of 2000-1000000, i.e., polyacrylic acid precursor, and set the speed of the stirring paddle to 100rpm. Turn on the heating, and when the temperature reaches 80°C, turn on the vacuum pump, maintain the vacuum degree at 0.1MPa for 6h, start condensation reflux, separate the solvent in the solution, and then place the remaining material in a vacuum oven at below 80°C to dry to obtain the negative electrode material.

[0092] Finally, the negative electrode material is broken up and sieved by a VC high-efficiency mixer to obtain a negative electrode material in a powder state.

[0093] Figure 3 A schematic diagram of the Raman spectrum of the negative electrode material of Example 1 is shown.

[0094] like Figure 3 As shown in the spectrum, the 500-520cm -1 The spectrum with peaks at 1345-1355cm -1 Peak intensity I A1 , I A2 , … , I An , 1570-1610cm -1 Peak intensity I´ A1 , I´ A2 , … , I´ An , bring it into the relational expression for calculation.

[0095] Example 2

[0096] The preparation process of the negative electrode material is basically the same as that of Example 1.

[0097] The difference is that the modification temperature of the silicon oxide particles is 50°C and the modification time is 120s.

[0098] Example 3

[0099] The preparation process of the negative electrode material is basically the same as that of Example 1.

[0100] The difference is that the modification temperature of the silicon oxide particles is 50°C and the amount of the adhesive precursor is 3%.

[0101] Example 4

[0102] The preparation process of the negative electrode material is basically the same as that of Example 1.

[0103] The difference is that the modification time of the silicon oxide particles is 140s and the amount of the adhesive precursor is 3%.

[0104] Example 5

[0105] The preparation process of the negative electrode material is basically the same as that of Example 1.

[0106] The difference is that the pressure in step 1 is 50 Pa, and the amount of the adhesive precursor in step 3 is 0.01%.

[0107] Example 6

[0108] The preparation process of the negative electrode material is basically the same as that of Example 1.

[0109] The difference is that the pressure in step 1 is 150 Pa, and the amount of the adhesive precursor in step 3 is 1%.

[0110] Example 7

[0111] The preparation process of the negative electrode material is basically the same as that of Example 1.

[0112] The difference is that the amount of adhesive precursor used is 0.01%.

[0113] Example 8

[0114] The preparation process of the negative electrode material is basically the same as that of Example 1.

[0115] The difference is that the D50 of the silicon oxide particles is 18 μm.

[0116] Example 9

[0117] The preparation process of the negative electrode material is basically the same as that of Example 1.

[0118] The difference is that the graphite particles have a D50 of 18 μm.

[0119] Example 10

[0120] The preparation process of the negative electrode material is basically the same as that of Example 1.

[0121] The difference is that the mass content of silicon particles in the suspension is 30wt%, and the mass content of graphite is 70wt%.

[0122] Embodiment 11

[0123] The preparation process of the negative electrode material is basically the same as that of Example 1.

[0124] The difference is that the D50 of the silicon oxide particles is 9 μm.

[0125] Comparative Example 1

[0126] The preparation process of the negative electrode material is basically the same as that of Example 1.

[0127] The differences are: the modification time of the silicon oxide particles is 300 s, the amount of the binder precursor is 4%, and the temperature in the three-necked flask is 100°C.

[0128] Comparative Example 2

[0129] The preparation process of the negative electrode material is basically the same as that of Example 1.

[0130] The difference is that the pressure in step 1 is 0.18 MPa.

[0131] Comparative Example 3

[0132] The preparation process of the negative electrode material is basically the same as that of Example 1.

[0133] The difference is that the modification temperature of the silicon oxide particles is 20°C.

[0134] Comparative Example 4

[0135] The preparation process of the negative electrode material is basically the same as that of Example 1.

[0136] The difference is that the modification temperature of the silicon oxide particles is 250°C.

[0137] Comparative Example 5

[0138] The preparation process of the negative electrode material is basically the same as that of Example 1.

[0139] The difference is that the modification time of the silicon oxide particles is 5s.

[0140] Comparative Example 6

[0141] The preparation process of the negative electrode material is basically the same as that of Example 1.

[0142] The difference is that the modification time of the silicon oxide particles is 200s.

[0143] Comparative Example 7

[0144] The preparation process of the negative electrode material is basically the same as that of Example 1.

[0145] The difference is that the D50 of the silicon oxide particles is 21 μm.

[0146] Comparative Example 8

[0147] The preparation process of the negative electrode material is basically the same as that of Example 1.

[0148] The difference is that the D50 of the silicon oxide particles is 1.5 μm.

[0149] Comparative Example 9

[0150] The preparation process of the negative electrode material is basically the same as that of Example 1.

[0151] The difference is that the graphite particles have a D50 of 25 μm.

[0152] Comparative Example 10

[0153] The preparation process of the negative electrode material is basically the same as that of Example 1.

[0154] The difference is that the graphite particles have a D50 of 5 μm.

[0155] Comparative Example 11

[0156] The preparation process of the negative electrode material is basically the same as that of Example 1.

[0157] The difference is that the mass content of silicon particles in the suspension is 4wt%, and the mass content of graphite is 96wt%.

[0158] Comparative Example 12

[0159] The preparation process of the negative electrode material is basically the same as that of Example 1.

[0160] The difference is that the mass content of silicon particles in the suspension is 96wt%, and the mass content of graphite is 4wt%.

[0161] The negative electrode materials of Examples 1 to 11 and Comparative Examples 1 to 12 were subjected to Raman surface scanning tests, 200 spectra were randomly selected, and the spectra values ​​that met the conditions were substituted into the relationship: , the calculated value is A, also called variance.

[0162] , the calculated value is B, also known as the absolute deviation.

[0163] The test specific surface area is C, the test moisture content is D, the volume distribution of particle size is D10, the carbon content and silicon content in the negative electrode material, the gas production during the aging process of the battery made of the negative electrode material, the gas production during high-temperature storage, and the battery yield E.

[0164] The test method is as follows:

[0165] 1. Raman surface scanning test method

[0166] The Raman spectrum of the powder was tested using the In Via micro-confocal Raman spectrometer from Renishaw of Japan. The test parameters are: laser wavelength 532nm, test range 120μm×120μm, step length 4μm. The raw data was processed using the software that comes with the instrument. The processing process is to remove fluorescence, remove baseline, mark peaks, fit, and then obtain the peak intensity of each peak. In particular, the baseline removal is based on the standard that the processed baseline is near 0. The other processing steps all use the initial parameters of the software. According to the above test method, 961 tests are required, that is, 961 sets of data are obtained, from which 200 sets of data are randomly selected for analysis. 500cm -1 -520cm -1 The method for determining whether there is a peak in the spectrum is that when the peak intensity in this range is higher than 100, it is considered to be a peak.

[0167] 2. Specific surface area test method

[0168] The gas adsorption BET method is used to determine the specific surface area of ​​the negative electrode material. The American Micrometer TriStar3000&3020 specific surface area and pore size analyzer is used to test the specific surface area of ​​the powder sample. First, take an empty tube of the specific surface tube after high-temperature drying, weigh M1, load a certain amount of sample (accounting for 1 / 2~2 / 3 of the volume of the tube), and degas at 300℃ for one hour. After cooling, weigh the tube weight M2, and the sample mass is M2-M1. Enter the sample mass into the computer and install the test. The instrument automatically completes the test, reads the data and records the test results. It should be noted that the sample is heated to 300℃ and purged with nitrogen for 1h and then cooled to room temperature. N2 purging is still required during the cooling process.

[0169] 3. Moisture content test method

[0170] The moisture content is determined according to the Karl Fischer method. The test is performed using a Mettler-Toledo coulometric titrator. ① Sample dosage: 0.5g to 1.0g. ② Sample processing: Take a clean sample bottle and place it on the analytical balance to zero, then add the sample to the sample bottle, record the sample weight, seal it with a special aluminum foil, and cover it with a plastic cover. ③ Sample testing: Place the sealed sample bottle into the card furnace of the moisture meter and heat it at 200°C to turn the moisture in the sample into water vapor, which is carried into the moisture meter analysis cell by the dry carrier gas for testing. ④ Record results: Read the data and record the test results, and the test results are accurate to 0.001%.

[0171] 4. Particle size test method

[0172] The test was conducted using a Malvern 3000 laser particle size analyzer. ① Instrument parameter settings: pump speed 2400r / min -2500r / min; ultrasonic power 20%; timed ultrasound 1 minute 10 seconds; refractive index 2.42, absorbance 1. ② Sample processing: Add 2mL of anhydrous ethanol to a 50mL beaker, stir to moisten, then add pure water to about 3 / 4 of the volume (about 40mL), stir evenly, scrape off the floating objects on the surface, ultrasonicate for 1min before testing, and take 0.5g of the test sample. ③ Sample testing: Stir the sample evenly and quickly pour it into the test beaker. At this time, the shading degree should be between 8% and 12%. Start ultrasound, and click on the sample test after 10s to get the test result.

[0173] 5. Calculation method of battery yield after capacity division

[0174] The negative electrode sheet is prepared according to the formula of negative electrode material: binder: conductive agent = 95.1:3.4:1.5. The positive electrode uses high nickel NMC products (hereinafter referred to as NMC), and the positive electrode sheet is prepared according to the formula of NMC: binder: conductive agent = 96.6:1.4:2.0. Then the positive and negative electrode sheets are wound into soft-pack batteries (55 mm long, 40 mm wide, and 6.5 mm thick). The battery cells undergo aging, liquid injection, formation, and capacity division to form soft-pack batteries. The battery design parameters are: positive electrode compaction 3.4g / cc, negative electrode compaction 1.65g / cc, negative electrode surface density 200g / m 2 , the N / P ratio is designed to be 8.2%. Each batch of batteries is made of 100 pieces, and the capacity of each battery is compared with the design capacity. When -0.5%≤(actual capacity-design capacity) / design capacity≤0.5% and the battery has a neat appearance, no cracks, no deformation, no leakage, etc., it is judged as a qualified product. Yield = number of qualified batteries / total number of batteries.

[0175] 6. Carbon content test method

[0176] The carbon content is tested by infrared carbon and sulfur analyzer, instrument name and model: German Bruker G4ICARUSHF. Test method: weigh a certain amount of sample into a ceramic crucible, add flux, enter a high-frequency furnace, pass high-purity oxygen to burn to generate carbon dioxide and sulfur dioxide, and directly measure the carbon and sulfur content in the gas through an infrared detector.

[0177] 7. Silicon content test method

[0178] The silicon content is tested by burning method. Test instrument: weigh 1.0000g to 1.2000g of sample (calculated as m0) into a corundum crucible, accurate to 0.1mg, and weigh 2 parallel samples for each sample. Place the sample in a muffle furnace for heat treatment, weigh the weight of the product after heat treatment as m1, and calculate the silicon content using the following formula.

[0179]

[0180] Muffle furnace model: Sigma (Shanghai) High Temperature Electric Furnace Co., Ltd., model: SGM110 / 14A. Heat treatment conditions: starting from room temperature, rising to 400°C in 30 minutes, and staying at 400°C for 60 minutes, then rising to 900°C in 60 minutes, and staying at 900°C for 120 minutes, and then rising to 1100°C in 30 minutes, and staying at 1100°C for 480 minutes, and then cooling to room temperature.

[0181] 8. Gas production test during battery aging

[0182] The negative electrode sheet was prepared according to the formula of negative electrode material: binder: conductive agent = 95.1:3.4:1.5. The positive electrode used high nickel NMC products (hereinafter referred to as NMC), and the positive electrode sheet was prepared according to the formula of NMC: binder: conductive agent = 96.6:1.4:2.0. Then the positive and negative electrode sheets were wound into soft-pack batteries (55 mm long, 40 mm wide, and 6.5 mm thick). After the battery was aged, the weight of the test battery was m1, and the battery was placed in the gas production equipment to test the mass m2. The buoyancy F = (m1-m2) g generated by the gas in the battery was calculated. According to the Archimedean principle F = ρgV, V was calculated to be the total gas production of the battery, and then converted to the gas production per ampere-hour G = V / Q, where V is the total gas production of the battery and Q is the capacity of the battery.

[0183] 9. Gas production test during high temperature storage

[0184] The negative electrode sheet is prepared according to the formula of negative electrode material: binder: conductive agent = 95.1:3.4:1.5. The positive electrode uses high nickel NMC products (hereinafter referred to as NMC), and the positive electrode sheet is prepared according to the formula of NMC: binder: conductive agent = 96.6:1.4:2.0. Then the positive and negative electrode sheets are wound into soft-pack batteries (55 mm long, 40 mm wide, and 6.5 mm thick). The battery cells undergo aging, liquid injection, formation, and capacity division to form soft-pack batteries. The battery design parameters are: positive electrode compaction 3.4g / cc, negative electrode compaction 1.65g / cc, negative electrode surface density 200g / m 2 , the N / P ratio is designed to be 8.2%. The gas production G1 of the cell after capacity division was tested, and then it was charged to 100% SOC at a rate of 0.5C, stored in a 60℃ constant temperature box for 15 days, cooled to room temperature, and the gas production G2 was tested again. The gas production G' during battery storage is G2-G1.

[0185] The weight of the test battery is m1. The battery is placed in a gas production device with a test mass of m2. The buoyancy generated by the gas in the battery is calculated as F=(m1-m2)g. According to the Archimedean principle F=ρgV, V is calculated to be the total gas production of the battery, and then converted into the gas production per ampere-hour G=V / Q, where V is the total gas production of the battery and Q is the capacity of the battery.

[0186] Table 1 shows the preparation process parameters of various embodiments and comparative examples.

[0187] Table 1

[0188]

[0189] Table 2 shows the test results of various embodiments and comparative examples.

[0190] Table 2

[0191]

[0192] According to the results shown in Table 2, by controlling the variance A value, that is, the silicon-containing spectrum The difference from the average value (variance) can control the morphological differences between particles in the negative electrode material. When the variance is smaller, it means that the particle morphology is closer. The battery produced by this negative electrode material has a higher yield and more stable performance.

[0193] Compared with Example 1, Example 2 has a lower modification temperature but a longer modification time, which can well adjust the surface morphology of the silicon oxide particles, with a high morphology concentration between particles and a smaller A value.

[0194] In Example 3, compared with Example 1, the modification temperature is lowered, so the modification treatment has less effect on the surface morphology of the silicon oxide particles, and the content of the binder precursor is relatively high, so the morphology concentration between the particles is smaller and the A value is larger.

[0195] Compared with Example 1, Example 4 has a longer modification time, so the modification treatment can fully adjust the surface morphology of the silicon oxide particles, but the content of the binder precursor is relatively high, so the morphology concentration between the particles is slightly higher and the A value is slightly larger.

[0196] Compared with Example 1, the modification time of Comparative Example 1 is too long, and the content of the binder precursor is too high. Therefore, the morphology between the particles is dispersed and not concentrated, the A value is very large, and the SEI content, morphology, and thickness generated during the formation and capacity separation process are different, resulting in large fluctuations in the capacity and efficiency of the battery made of the negative electrode material, and low battery yield.

[0197] The negative electrode material prepared according to the embodiments of the present application has low morphology differences between particles and high concentration. The battery batch yield made using the negative electrode material is high and the batch is stable.

[0198] Although multiple embodiments of the present application have been shown and described herein, it is obvious to those skilled in the art that such embodiments are provided only by way of example. Those skilled in the art can think of many changes, modifications and alternatives without departing from the thought and spirit of the present application. It should be understood that in the process of practicing the present application, various alternatives to the embodiments of the present application described herein can be adopted. The attached claims are intended to limit the scope of protection of the present application, and therefore cover equivalents or alternatives within the scope of these claims.

Claims

1. A negative electrode material, comprising a silicon-based material and a graphite-based material, characterized in that: The negative electrode material was tested by Raman scanning, and 200 groups of spectra were randomly selected. 500cm in the atlas -1 -520cm -1 The number of spectra with peaks at is set to n, 500cm -1 -520cm -1 In the spectrum with peaks at: 1345cm -1 -1355cm -1 The peak intensities at A1 , I A2 ,…,I An , 1570cm -1 -1610cm -1 The peak intensities at I′ are A1 , I′ A2 ,…,I′ An ; The negative electrode material satisfies the relationship: in, as well as The negative electrode material also satisfies the relationship: 0<(|I A1 / I′ A1 -K|+|I A2 / I′ A2 -K|+…+|I An / I′ An -K|) / n≤0.3。 2. The negative electrode material according to claim 1, characterized in that The negative electrode material satisfies the relationship: 。 3. The negative electrode material according to any one of claims 1 or 2, characterized in that The negative electrode material includes at least one of the following features: a. Specific surface area <3.0m 2 / g; b. Water content by mass < 0.5%; c. Volume distribution of particle size D10>1.0μm; d. Based on the mass of the negative electrode material being 100wt%, the carbon content is 5wt% to 95wt%, and the silicon content is 5wt% to 95%; e. The gas production of the battery made of the negative electrode material during aging is less than 0.01 mL / Ah; f. After the battery made of the negative electrode material is stored at 60°C for 15 days, the gas production during the process is less than 0.1mL / Ah; g. 500cm in Raman spectrum -1 -520cm -1 The ratio of the number of spectra with peaks to the number of spectra without peaks is 0.05-40.

4. The negative electrode material according to any one of claims 1 or 2, characterized in that The negative electrode material includes at least one of the following features: a. The silicon-based material comprises at least one of amorphous silicon, crystalline silicon, silicon oxide and silicate; b. The graphite material comprises at least one of natural graphite, artificial graphite, expanded graphite and oxidized graphite; c. The negative electrode material includes a carbon material, and the carbon material includes at least one of amorphous carbon and graphitized carbon.

5. A method for preparing a negative electrode material according to any one of claims 1 to 4, characterized in that: include: The first step is to prepare a modified silicon-based material: a silicon-based material with a carbon layer on its surface is taken, and a non-polymerizing gas is introduced into the surface of the silicon-based material for plasma modification treatment under the condition of evacuating to a pressure of 50Pa-150Pa, wherein the temperature of the plasma modification treatment is 30°C-180°C, and the time of the plasma modification treatment is 10s-150s, to obtain a modified silicon-based material; The second step is to prepare a suspension containing silicon-based materials and graphite: the modified silicon-based material is uniformly dispersed in a dispersant, graphite particles are gradually added, and the suspension containing silicon-based materials and graphite is obtained by stirring and dispersing, wherein the median particle size of the silicon-based material particles is 2 μm to 20 μm, and the D50 of the graphite particles is 6 μm to 20 μm; wherein the mass content of silicon particles in the suspension containing silicon-based materials and graphite is 5 wt% to 95 wt%, and the mass content of graphite in the suspension containing silicon-based materials and graphite is 5 wt% to 95 wt%; The third step is to prepare the negative electrode material: the suspension containing the silicon-based material and graphite is mixed with a binder precursor having a mass ratio of 0.01% to 3% relative to the suspension, and the solvent is separated and then dried to obtain the negative electrode material.

6. The preparation method according to claim 5, characterized in that: The first step includes at least one of the following parameters: a. The non-polymerizable gas comprises at least one of hydrogen, argon, helium, nitrogen, krypton and neon; b. The silicon-based material includes at least one of amorphous silicon, crystalline silicon, silicon oxide and silicate.

7. The preparation method according to claim 5, characterized in that: The second step includes at least one of the following parameters: a. The graphite particles include at least one of natural graphite, artificial graphite, expanded graphite and graphite oxide; b. The dispersant comprises one or a mixture of two or more of deionized water, ethanol, propanol, isopropanol, propane, DFM, and acetone.

8. The preparation method according to claim 5, characterized in that: The third step includes at least one of the following parameters: a. The adhesive precursor comprises at least one of an amino group, a carboxyl group, a cyano group, and a hydroxyl functional group; b. The number average molecular weight of the adhesive precursor is 2000-1000000; c. The adhesive precursor has a viscosity of 1000 mPa·s-100000 mPa·s when the solid content is 3%.

9. A lithium ion battery, characterized in that: The lithium-ion battery comprises the negative electrode material according to any one of claims 1 to 4 or the negative electrode material prepared by the preparation method according to any one of claims 5 to 8.