Photocuring 3D printing and bridging forming method for large-size and large-suspension-span ceramic parts
Through light-curing 3D printing and bridge molding technology, the collapse, deposition and shrinkage problems of traditional ceramic light-curing additive manufacturing in the preparation of large-size and large-suspension span ceramic parts have been solved, and efficient molding and mechanical performance improvement have been achieved.
Patent Information
- Application Number
- CN202410941786.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-09-27
AI Technical Summary
Traditional ceramic light-curing additive manufacturing technology has problems such as printing collapse, slurry deposition, curing shrinkage and limited molding size when preparing large-size and large-span ceramic parts. It is difficult to meet the requirements of modern industry for ceramic structure and function.
Using light-curing 3D printing and bridge molding methods, a high-solid content slurry is prepared by uniformly mixing micron-grade ceramic powder and photosensitive resin solvent, and using three-dimensional slicing software to cut large-sized parts into small-sized non-overhanging parts, and use light-curing and thermal Cross-linking and curing technology bridge molding, followed by high-temperature sintering and infiltration processes to fill defects and improve mechanical properties.
It effectively avoids the molding difficulties of large-size and large-span ceramic parts, reduces curing shrinkage deformation, achieves molding larger than the platform size, and improves the mechanical properties and stability of the parts.
Smart Images

Figure HDA0004944381390000012 
Figure HDA0004944381390000013 
Figure HDA0004944381390000011
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of additive manufacturing of ceramic materials, and in particular relates to a light-curing 3D printing and bridging molding method for large-size and large-span ceramic parts. Background Art
[0002] Structural and functional ceramic materials have been widely used and studied in the past two decades, becoming important materials for the development of aerospace, biomedicine, chips, new energy, nuclear power plants, military and other fields in the future. Traditional ceramic preparation processes can no longer meet the requirements of modern industrial applications for ceramic structure and function. However, the emergence of ceramic additive manufacturing technology has broken through the technical bottleneck of free manufacturing of ceramic materials with complex shapes, multiple pores, and curved surfaces, and achieved the structural goals that traditional processes cannot prepare. Ceramic photocuring additive manufacturing technology has become a relatively mature ceramic parts preparation process, mainly used for the preparation of ceramic materials with low refractive index such as silicon oxide, aluminum oxide, zirconium oxide, and hydroxyapatite. The prepared ceramic green body is formed into a ceramic part with a density of up to 99.98% after degreasing and high-temperature sintering. Therefore, it has attracted much attention from the ceramic material additive manufacturing industry. At the same time, with the upgrading and high-speed iteration of products, photocuring ceramic additive manufacturing also has some technical bottlenecks in structure and size.
[0003] The principle of ceramic photopolymerization additive manufacturing technology is to use ultraviolet laser to induce photoinitiator to generate free radicals to promote the curing of resin monomer into glassy polymer, thereby encapsulating ceramic powder in it to form ceramic green body. According to this principle, when preparing photosensitive ceramic resin slurry, long-term printing will cause ceramic particle deposition, which is not conducive to uniform curing and molding. This has a greater impact on large-size ceramic parts that require long-term printing. At the same time, the platform size of additive manufacturing molding is limited, which further limits the 3D printing of large-size ceramic parts. When the resin monomer forms a polymer during photocuring, it will produce curing shrinkage due to the reduction of atomic distance. Therefore, the larger the molding size, the greater the degree of photopolymerization shrinkage deformation and risk factor. In addition, ceramic structural parts with large overhang spans are prone to printing collapse during the printing process and cannot be prepared by 3D printing. In summary, there are many obstacles to large overhang spans and large-size parts, including printing collapse, slurry deposition, limited platform size, unstable process, curing shrinkage deformation and other problems. To this end, the present invention proposes a light-curing 3D printing and bridging molding method for large-sized and large-span ceramic parts, which can effectively avoid the above-mentioned size and structure limitations. Summary of the invention
[0004] The present invention provides a photocuring 3D printing and bridging molding method for large-sized and large-span ceramic parts, which can effectively solve the photocuring molding problems brought about by large-sized and large-span ceramic structural parts, and solve the shortcomings of printing collapse, slurry deposition, curing shrinkage, and limited molding size from the source of molding technology and structural design.
[0005] The present invention provides a light-curing 3D printing and bridging molding method for large-size and large-span ceramic parts, comprising the following steps:
[0006] Step 1: uniformly mixing micron-sized ceramic powder and photosensitive resin solvent to prepare a slurry with a high solid content;
[0007] Step 2: Use 3D slicing software to cut large-sized and large-overhang span parts into limited small-sized and non-overhang span parts; and form interfaces that can be bridged to each other at the cutting points;
[0008] Step 3: Using the photo-curing technology to prepare a small-sized and non-overhanging span part bridge matrix;
[0009] Step 4: Clean the uncured slurry on the surface of the ceramic green body formed by light-curing 3D printing under ultrasonic wave to prepare a bridging matrix;
[0010] Step 5: After the bridging interface and the bridged interface of the bridging substrate are evenly coated with slurry, they are matched according to the design accuracy and shape, and then the coated slurry is cured by in-situ photo-crosslinking;
[0011] Step 6: Place the photoinduced cross-linked cured ceramic parts into an electric furnace and perform secondary curing bridging at 170-250° C.;
[0012] Step 7: high-temperature sintering is performed on the ceramic green parts after photocuring 3D printing and bridging to achieve the purpose of preparing large-size and large-span parts;
[0013] Step 8: Perform infiltration and secondary sintering process on the pores and cracks in the bridge interface and matrix of the parts after high-temperature sintering to fill the defects and improve the mechanical properties.
[0014] Preferably, in step 1, the micron-sized ceramic powder comprises silicon oxide, aluminum oxide, zirconium oxide, and apatite; the size range of the micron-sized ceramic powder is 1 to 50 microns, and more preferably the size range of the micron-sized ceramic powder is 2 to 10 microns. More preferably, the surface of the micron-sized ceramic powder is modified by a dispersant, and the dispersant is any one or more of ammonium citrate, BYK series dispersants, active polymer dispersants, and polypropoxy quaternary ammonium salts, and the dispersant accounts for 2 to 5 wt% of the mass of the micron-sized ceramic powder.
[0015] Preferably, in step 1, the photosensitive resin solvent is a product obtained by uniformly mixing resin monomer, photoinitiator, oligomer and plasticizer in a magnetic stirrer. Wherein, the resin monomer is any one or more of dipropylene glycol diacrylate (DPGDA), 1,6-hexanediol diacrylate (HDDA), tripropylene glycol diacrylate (TPGDA) and trimethylolpropane triacrylate (TMPTA); the photoinitiator is any one or more of 1-hydroxycyclohexyl benzophenone (Irgacure184 / 819 / 1173), trimethylbenzoyl-diphenylphosphine oxide (TPO) and 2-hydroxy-2-methyl-1-phenyl-1-propanone, and the mass of the photoinitiator accounts for 0.5-3.5wt% of the total mass of the photosensitive resin solvent. It is further preferred that the mass of the photoinitiator accounts for 0.5-3.5wt% of the total mass of the photosensitive resin solvent. 0.5-1.5wt% of the total mass of the lipid solvent; the oligomer is any one or more of difunctional, tetrafunctional and hexafunctional aliphatic polyurethane acrylate and phenolic resin, and the ratio of the total mass of the oligomer to the total mass of the resin monomer is (0.1-3):(10-5), and the ratio of the total mass of the oligomer to the total mass of the resin monomer is further preferably (1-2):(9-7); the plasticizer is any one of 1,2-dibutyl phthalate and polyethylene glycol, and the ratio of the mass of the plasticizer to the total mass of the oligomer and the resin monomer is 1:(10-40), and the ratio of the mass of the plasticizer to the total mass of the oligomer and the resin monomer is further preferably 1:(20-30). The above ingredients are stirred at 40-60°C for 5-24 hours by a magnetic stirrer to obtain a uniformly stirred photosensitive resin solvent.
[0016] Preferably, in the step 1, the ball milling mixing time of the mixed micron-sized ceramic powder and the photosensitive resin solvent is 24 to 72 hours, and the stirring speed is 150 to 800 r / min.
[0017] Preferably, in step 2, the shapes of the interface surfaces that can be bridged to each other include planes, curved surfaces, frustums, prisms, pyramids and rectangular concave and convex surfaces.
[0018] Preferably, in step three, the photocuring molding technology is any one of a stereolithography molding process (Stereolithography, SL) of point / line / layer scanning molding and a digital light processing molding process (Digital light process, DLP) of layer-by-layer exposure molding.
[0019] Preferably, in step 4, the ultrasonic cleaning time is 1 to 15 minutes.
[0020] Preferably, in step five, the light source used for the in-situ photo-crosslinking and curing is an ultraviolet light source with a wavelength of 355 to 405 nm and a curing time of 0.5 to 10 minutes.
[0021] Preferably, in step six, the photoinduced cross-linked cured and bridged ceramic parts are placed in an electric furnace and subjected to secondary curing and bridging at 170-250°C. The heating rate is 0.1-20°C / min, the dwelling time is 1-30min, and the cooling rate is the furnace cooling rate or cooled to room temperature at a rate of 1-10°C / min.
[0022] Preferably, in step seven, the high temperature sintering molding process includes two steps of degreasing and high temperature sintering:
[0023] The debinding sintering program is set as follows: 25-150°C, heating at a rate of 0.1-2°C / min, and keeping warm for 0.5-2h; 150-300°C, heating at a rate of 0.1-1.5°C / min, and keeping warm for 0.5-2.5h; 300-550°C, heating at a rate of 0.1-1°C / min, and keeping warm for 0.5-3h; 550-1150°C, heating at a rate of 1-5°C / min, and keeping warm for 0.5-1h; 1150-25°C, cooling at a rate of 2-4°C / min; the pyrolysis atmosphere is any one of argon, nitrogen and helium;
[0024] The high-temperature sintering program is set as follows: 25-150°C, heating at a rate of 1-5°C / min, and keeping warm for 0.5-2h; 150-300°C, heating at a rate of 2-6°C / min, and keeping warm for 0.5-2.5h; 300-550°C, heating at a rate of 5-10°C / min, and keeping warm for 0.5-3h; 550-(1500-1700)°C, heating at a rate of 6-15°C / min, and keeping warm for 0.5-1h; (1500-1700)-25°C, cooling at a rate of 10-20°C / min; the pyrolysis atmosphere is any one of argon, nitrogen and helium.
[0025] Preferably, in step eight, the infiltration process is any one of a chemical vapor deposition process and a polymer impregnation pyrolysis process (PIP infiltration process).
[0026] Preferably, in step eight, the secondary sintering process is set as follows: heating from 25 to 800°C at a rate of 0.1 to 5°C / min, and keeping warm for 1 to 2 hours; heating from 800 to (1500 to 1700)°C at a rate of 2 to 10°C / min, and keeping warm for 0.5 to 2 hours; cooling from (1500 to 1700) to 25°C at a rate of 5 to 10°C / min; the pyrolysis atmosphere is any one of argon, nitrogen and helium.
[0027] Compared with the prior art, the present invention has the following functions:
[0028] The present invention proposes a bridging process of a ceramic part bridging matrix after limited cutting by photocuring 3D printing based on photosensitive slurry, and then photocrosslinking and thermal crosslinking curing are performed by cutting and designing a compatible bridge interface. The green body is 3D printed by preparing a high volume fraction of ceramic resin slurry to reduce the deformation caused by curing shrinkage; the ceramic part structure with large size and large suspended span is cut without suspended structure to obtain a limited number of small-sized parts, avoiding the collapse of suspended parts during printing; small-sized parts can be printed and formed at the same time, reducing the space size of large-sized suspended parts, effectively reducing the printing time and the particle deposition phenomenon of long-term printing, and can manufacture large parts larger than the size of the molding platform in a limited molding platform; the 3D printed model can reconstruct the original design model by bridging after modular cutting, and even reconstruct arbitrary regular graphics and structural parts; photocrosslinking and thermal crosslinking can control the relative position of the green body after bridging during the sintering process to maintain the original shape. Finally, the densification sintering is carried out by high-temperature sintering of the infiltration process and the growth of particle sintering necks to achieve the target strength design. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 It is a process flow chart of the light-curing 3D printing and bridge molding method for large-size and large-overhang span ceramic parts;
[0030] Figure 2 It is thermal cross-linking curing bridging temperature analysis;
[0031] Figure 3 It is a demonstration piece formed by light-curing 3D printing and bridging technology. DETAILED DESCRIPTION
[0032] In order to make the slurry preparation method, molding process, infiltration and sintering process of the present invention clearer and more specific, the following is a further detailed description of the light-curing 3D printing and bridging molding technology of large-size and large-span ceramic parts in combination with the accompanying drawings and embodiments. The specific embodiments described here are only used to explain the present invention, and are not all embodiments.
[0033] The following will be combined with the accompanying drawings and some specific embodiments to clearly and accurately describe the slurry preparation method, molding process and infiltration and sintering process of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by relevant technicians in this field without making any innovations are within the scope of protection of the present invention.
[0034] In the process of making large-sized and large-span ceramic parts, the 3D model is cut into non-overhanging structures and small-sized parts through slicing software, and a bridging interface is reserved to ensure the bridging accuracy; the high-solid content slurry is used to print the cut parts in batches through 3D printing technology to prepare ceramic bridging green bodies; the divided ceramic structure is reconstructed into a pre-designed model through UV cross-linking and thermal cross-linking bridging processes; large-sized and large-span ceramic parts are prepared through degreasing and high-temperature sintering processes, infiltration processes and secondary sintering processes.
[0035] The present invention provides a light-curing 3D printing and bridging molding method for large-sized and large-span ceramic parts, which can avoid preparation and molding problems such as particle deposition, printing collapse, limited molding size and curing shrinkage caused by long-term printing. The specific preparation steps are as follows:
[0036] S1: uniformly mixing micron-sized ceramic powder and photosensitive resin solvent to prepare a slurry with a high solid content;
[0037] After mixing in a ratio of (1-2) to (9-7) of the total mass of the oligomer to the total mass of the resin monomer, the mixture is then uniformly mixed with 0.5-1.5wt% of a photoinitiator and a plasticizer in a magnetic stirrer at 40-60°C for 6-12 hours to prepare a photosensitive resin solvent. The ratio of the mass of the plasticizer to the total mass of the oligomer and the resin monomer is 1:(20-30). Subsequently, a ceramic powder of 2-10 microns is surface-modified with 2-4wt% of a BYK dispersant, and then uniformly mixed with the photosensitive resin solvent in a ball mill for 24-72 hours at a rotation speed of 150-800r / min to obtain a ceramic resin slurry with a high solid content.
[0038] S2: Use 3D slicing software to cut large-sized and large-overhang span parts into limited small-sized and non-overhang span parts; and form bridging interfaces of planes, curved surfaces and / or convex and concave surfaces that can bridge each other at the cutting point, which is convenient for subsequent bridging processes and ensures bridging accuracy.
[0039] S3: Use stereolithography technology to prepare small-sized and non-overhanging span part bridge matrix;
[0040] Specifically, the bridging matrix is prepared in batches by stereolithography (SL) and digital light processing (DLP).
[0041] S4: The 3D printed ceramic green body is cleaned under ultrasonic waves for 1 to 15 minutes to remove the uncured slurry on the surface to prepare a bridging matrix.
[0042] S5: After the bridging interface and the bridged interface of the bridging substrate are evenly coated with the slurry, they are matched according to the design accuracy and shape, and then the coated slurry is cured by in-situ photo-crosslinking;
[0043] After applying a layer of resin slurry on the bridging interface of the ceramic green body available for bridging, the photosensitive resin slurry is in-situ photo-crosslinked and cured to ensure the bridging accuracy; the light source used for in-situ photo-crosslinking and curing is an ultraviolet light source with a wavelength of 355 to 405 nm, and the photocuring time is 1 to 5 minutes.
[0044] S6: Place the photoinduced cross-linked cured ceramic green parts into an electric furnace at 170-250°C for secondary curing bridging. The heating rate of the electric furnace is 0.1-20°C / min, the dwell time is 1-30min, the cooling rate is the furnace cooling rate or 1-10°C / min, and the bridging time is 1-5min.
[0045] S7: High-temperature sintering of the green ceramic parts after photocuring 3D printing and bridging to achieve the purpose of preparing large-size and large-span parts;
[0046] The high-temperature sintering molding process includes two steps: debinding and high-temperature sintering. The debinding sintering program is set as follows: 25-150℃, heating at a rate of 0.1-2℃ / min, and keeping warm for 0.5-2h; 150-300℃, heating at a rate of 0.1-1.5℃ / min, and keeping warm for 0.5-2.5h; 300-550℃, heating at a rate of 0.1-1℃ / min, and keeping warm for 0.5-3h; 550-1150℃, heating at a rate of 1-5℃ / min, and keeping warm for 0.5-1h; 1150-25℃, cooling at a rate of 2-4℃ / min; the pyrolysis atmosphere is any one of argon, nitrogen and helium. The high-temperature sintering program is set as follows: 25-150°C, heating at a rate of 1-5°C / min, and keeping warm for 0.5-2h; 150-300°C, heating at a rate of 2-6°C / min, and keeping warm for 0.5-2.5h; 300-550°C, heating at a rate of 5-10°C / min, and keeping warm for 0.5-3h; 550-(1500-1700)°C, heating at a rate of 6-15°C / min, and keeping warm for 0.5-1h; (1500-1700)-25°C, cooling at a rate of 10-20°C / min; the pyrolysis atmosphere is any one of argon, nitrogen and helium.
[0047] S8: Perform infiltration and secondary sintering process on the pores and cracks in the bridge interface and matrix of the parts after high-temperature sintering to fill the defects and improve the mechanical properties;
[0048] The infiltration process is a chemical vapor deposition process and a polymer impregnation cracking process (PIP infiltration process). After infiltration, a secondary sintering process is performed, and the program settings are as follows: 25-800°C at a rate of 0.1-5°C / min, and keep warm for 1-2 hours; 800-(1500-1700)°C at a rate of 2-10°C / min, and keep warm for 0.5-2 hours; (1500-1700)-25°C at a rate of 5-10°C / min; the pyrolysis atmosphere is any one of argon, nitrogen and helium.
[0049] The present invention provides a light-curing 3D printing and bridging molding method for large-size and large-span ceramic parts. The entire preparation process is as follows: Figure 1 shown.
[0050] The present invention is described in detail below in conjunction with specific embodiments.
[0051] Example 1
[0052] S1: Preparation of ceramic resin slurry with high solid content: 100g of 1,6-hexanediol diacrylate (HDDA), 40g of trimethylolpropane triacrylate (TMPTA), 20g of tetrafunctional aliphatic polyurethane acrylate (Chengdu Sicheng New Materials Co., Ltd.), 1.7g of trimethylbenzoyl-diphenylphosphine oxide (TPO) and 6g of polyethylene glycol plasticizer (molecular weight 200) were uniformly mixed in a magnetic stirrer for 8h to prepare a photosensitive resin solvent. Subsequently, 850g of 5-micron alumina ceramic powder was surface-modified with 25.5g of BYK dispersant and uniformly mixed with the photosensitive resin solvent in a ball mill for 72h at a ball mill speed of 400r / min to obtain a ceramic resin slurry with high solid content.
[0053] S2: 3D model cutting processing: Using the 3D slicing software Materialise Magics 21.0, ceramic structure models with large sizes and large suspended spans are cut and curved bridging interfaces are reserved for bridging.
[0054] S3: Stereolithography 3D printing: Batch preparation of bridging substrates using a stereolithography device (SL).
[0055] S4: Ultrasonic cleaning of the ceramic green body: The bridging base green body after 3D printing is cleaned in an ultrasonic environment for 10 min.
[0056] S5: Photocuring the bridging substrate: After applying a layer of photosensitive resin slurry on the bridging interface of the ceramic green body that can be bridged, the photosensitive resin slurry is cured by in-situ photocrosslinking for 2 minutes.
[0057] S6: Thermal curing of bridging matrix: The ceramic green body with in-situ photo-crosslinking and bridging is placed in an electric furnace at 190° C. for 2 minutes for secondary curing and bridging.
[0058] S7: High temperature sintering: Debind and sinter the bridged ceramic parts at high temperature. The debinding and sintering program is set as follows: 25-150℃ at a rate of 0.5℃ / min, keep warm for 1h; 150-300℃ at a rate of 0.3℃ / min, keep warm for 1h; 300-550℃ at a rate of 0.2℃ / min, keep warm for 2h; 550-1150℃ at a rate of 1.5℃ / min, keep warm for 0.6h; 1150-25℃ at a rate of 3℃ / min; argon is the pyrolysis atmosphere. The high-temperature sintering program was set as follows: heating from 25 to 150 °C at a rate of 2 °C / min, and keeping warm for 0.6 h; heating from 150 to 300 °C at a rate of 3 °C / min, and keeping warm for 1 h; heating from 300 to 550 °C at a rate of 8 °C / min, and keeping warm for 0.6 h; heating from 550 to (1500 to 1700) °C at a rate of 10 °C / min, and keeping warm for 0.5 h; cooling from (1500 to 1700) to 25 °C at a rate of 15 °C / min; the pyrolysis atmosphere was argon.
[0059] S8: Infiltration process and secondary sintering: Select the polymer impregnation cracking process (PIP infiltration process) to infiltrate the ceramic parts after high-temperature sintering. After the infiltration is completed, the secondary sintering process is carried out, and the program settings are as follows: 25-800℃ at a rate of 2℃ / min, keep warm for 1h; 800-(1500-1700)℃ at a rate of 5℃ / min, keep warm for 1h; (1500-1700)-25℃ at a rate of 8℃ / min; argon gas is used as the pyrolysis atmosphere.
[0060] Figure 2 This is a thermogravimetric analysis of the high solid content slurry in Example 1; thermal crosslinking and curing mainly occurs between 120 and 170°C; exothermic peaks appear throughout the process, indicating that the resin monomer releases heat due to bond breaking during the curing process.
[0061] Figure 3 It is a ceramic green body formed by a stereolithography printer. After bridging, degreasing, high-temperature sintering, infiltration and secondary sintering processes, the final product display of large-span ceramic structural parts is obtained. The parts have excellent structural functionality and no obvious defects are formed.
[0062] The above embodiments are only an illustration of the technical solution of the invention and do not limit it. For scientific research or technical personnel in this field, without changing the technical solution and preparation principle of the present application, the optimization and improvement made should belong to the protection scope of the present application.
[0063] Example 2
[0064] S1: Preparation of ceramic resin slurry with high solid content: 180g of 1,6-hexanediol diacrylate (HDDA), 20g of tetrafunctional aliphatic polyurethane acrylate, 3.8g of trimethylbenzoyl-diphenylphosphine oxide (TPO) and 8g of polyethylene glycol plasticizer (molecular weight 200) were uniformly mixed in a magnetic stirrer for 10 hours to prepare a photosensitive resin solvent. Subsequently, 850g of 5-micron alumina ceramic powder was surface-modified with 34g of BYK dispersant and uniformly mixed with the photosensitive resin solvent in a ball mill for 48 hours at a speed of 600r / min to obtain a ceramic resin slurry with high solid content.
[0065] S2: 3D model cutting processing: Using the 3D slicing software Materialise Magics 21.0, ceramic structure models with large sizes and large suspended spans are cut and a planar bridging interface is reserved for bridging.
[0066] S3: Stereolithography 3D printing: Batch preparation of bridging substrates using a stereolithography device (SL).
[0067] S4: Ultrasonic cleaning of the ceramic green body: The bridging base green body after 3D printing is cleaned in an ultrasonic environment for 10 min.
[0068] S5: Photocuring the bridging substrate: After applying a layer of photosensitive resin slurry on the bridging interface of the ceramic green body available for bridging, the photosensitive resin slurry is cured by in-situ photocrosslinking for 2 minutes.
[0069] S6: Thermal curing of bridging matrix: The ceramic green body with in-situ photo-crosslinking and curing bridge is placed in an electric furnace at 220° C. for 2 minutes for secondary curing and bridging.
[0070] S7: High temperature sintering: Debind and high temperature sinter the bridged ceramic parts. The debinding and sintering program is set as follows: 25-150℃ at a rate of 1℃ / min, keep warm for 1.5h; 150-300℃ at a rate of 0.5℃ / min, keep warm for 1.5h; 300-550℃ at a rate of 0.2℃ / min, keep warm for 2h; 550-1150℃ at a rate of 2℃ / min, keep warm for 1h; 1150-25℃ at a rate of 3℃ / min; argon gas is used as the pyrolysis atmosphere. The high-temperature sintering program was set as follows: heating from 25 to 150 °C at a rate of 1 °C / min, and keeping warm for 0.5 h; heating from 150 to 300 °C at a rate of 2 °C / min, and keeping warm for 1.5 h; heating from 300 to 550 °C at a rate of 5 °C / min, and keeping warm for 1 h; heating from 550 to (1500 to 1700) °C at a rate of 8 °C / min, and keeping warm for 0.5 h; cooling from (1500 to 1700) to 25 °C at a rate of 10 °C / min; the pyrolysis atmosphere was argon.
[0071] S8: Infiltration process and secondary sintering: Select the polymer impregnation cracking process (PIP infiltration process) to infiltrate the ceramic parts after high-temperature sintering. After the infiltration is completed, the secondary sintering process is carried out, and the program settings are as follows: 25-800℃ at a rate of 3℃ / min, keep warm for 1.5h; 800-(1500-1700)℃ at a rate of 8℃ / min, keep warm for 1h; (1500-1700)-25℃ at a rate of 10℃ / min; the pyrolysis atmosphere is argon.
[0072] Example 3
[0073] S1: Preparation of ceramic resin slurry with high solid content: 100g of 1,6-hexanediol diacrylate (HDDA), 40g of trimethylolpropane triacrylate (TMPTA), 40g of tetrafunctional aliphatic polyurethane acrylate, 1.0g of trimethylbenzoyl-diphenylphosphine oxide (TPO) and 8g of polyethylene glycol plasticizer (molecular weight 200) were uniformly mixed in a magnetic stirrer for 6 hours to prepare a photosensitive resin solvent. Subsequently, 850g of 5-micron alumina ceramic powder was surface-modified with 17g of BYK dispersant and uniformly mixed with the photosensitive resin solvent in a ball mill for 56 hours at a speed of 800r / min to obtain a ceramic resin slurry with high solid content.
[0074] S2: 3D model cutting processing: Using the 3D slicing software Materialise Magics 21.0, ceramic structure models with large sizes and large suspended spans are cut and a planar bridging interface is reserved for bridging.
[0075] S3: Stereolithography 3D printing: Batch preparation of bridging substrates using a stereolithography device (SL).
[0076] S4: Ultrasonic cleaning of the ceramic green body: The bridging base green body after 3D printing is cleaned in an ultrasonic environment for 15 min.
[0077] S5: Photocuring the bridging substrate: After applying a layer of photosensitive resin slurry on the bridging interface of the ceramic green body available for bridging, the photosensitive resin slurry is cured by in-situ photocrosslinking for 2 minutes.
[0078] S6: Thermal curing of bridging matrix: The ceramic green body with in-situ photo-crosslinking and curing bridge is placed in an electric furnace at 170° C. for 5 minutes for secondary curing and bridging.
[0079] S7: High temperature sintering: Debind and high temperature sinter the bridged ceramic parts. The debinding and sintering program is set as follows: 25-150℃ at a rate of 0.5℃ / min, keep warm for 1h; 150-300℃ at a rate of 0.2℃ / min, keep warm for 1h; 300-550℃ at a rate of 0.5℃ / min, keep warm for 1.5h; 550-1150℃ at a rate of 2℃ / min, keep warm for 0.5h; 1150-25℃ at a rate of 2℃ / min; argon gas is used as the pyrolysis atmosphere. The high-temperature sintering program was set as follows: heating from 25 to 150 °C at a rate of 2 °C / min, and keeping warm for 1 h; heating from 150 to 300 °C at a rate of 4 °C / min, and keeping warm for 1.5 h; heating from 300 to 550 °C at a rate of 10 °C / min, and keeping warm for 1 h; heating from 550 to (1500 to 1700) °C at a rate of 10 °C / min, and keeping warm for 1 h; cooling from (1500 to 1700) to 25 °C at a rate of 10 °C / min; the pyrolysis atmosphere was argon.
[0080] S8: Infiltration process and secondary sintering: Select the polymer impregnation cracking process (PIP infiltration process) to infiltrate the ceramic parts after high-temperature sintering. After the infiltration is completed, the secondary sintering process is carried out, and the program settings are as follows: 25-800℃ at a rate of 1℃ / min, keep warm for 1h; 800-(1500-1700)℃ at a rate of 3℃ / min, keep warm for 1h; (1500-1700)-25℃ at a rate of 5℃ / min; the pyrolysis atmosphere is argon.
Claims
1. A method for photocuring 3D printing and bridging molding of large-sized and large-span ceramic parts, characterized in that: The following steps are involved: Step 1: uniformly mixing micron-sized ceramic powder and photosensitive resin solvent to prepare a slurry with a high solid content; Step 2: Use 3D slicing software to cut large-sized and large-overhang span parts into limited small-sized and non-overhang span parts; and form interfaces that can be bridged to each other at the cutting points; Step 3: Using the photo-curing technology to prepare a small-sized and non-overhanging span part bridge matrix; Step 4: Clean the uncured slurry on the surface of the ceramic green body formed by light-curing 3D printing under ultrasonic wave to prepare a bridging matrix; Step 5: After the bridging interface and the bridged interface of the bridging substrate are evenly coated with slurry, they are matched according to the design accuracy and shape, and then the coated slurry is cured by in-situ photo-crosslinking; Step 6: Place the photoinduced cross-linked cured ceramic parts into an electric furnace and perform secondary curing bridging at 170-250° C.; Step 7: high-temperature sintering is performed on the ceramic green parts after photocuring 3D printing and bridging to achieve the purpose of preparing large-size and large-span parts; Step 8: Perform infiltration and secondary sintering process on the pores and cracks in the bridge interface and matrix of the parts after high-temperature sintering to fill the defects and improve the mechanical properties.
2. A method for photocuring 3D printing and bridging molding of large-sized and large-span ceramic parts according to claim 1, characterized in that: In the step 1, the micron-sized ceramic powder includes silicon oxide, aluminum oxide, zirconium oxide, and apatite; the size range of the micron-sized ceramic powder is 1 to 50 microns; the surface of the micron-sized ceramic powder is modified by a dispersant, and the dispersant is any one or more of ammonium citrate, BYK series dispersants, active polymer dispersants, and polypropoxy quaternary ammonium salts, and the dispersant accounts for 2 to 5 wt% of the mass of the micron-sized ceramic powder.
3. A method for photocuring 3D printing and bridging molding of large-sized and large-span ceramic parts according to claim 1, characterized in that: In the step 1, the photosensitive resin solvent is a product obtained by uniformly mixing a resin monomer, a photoinitiator, an oligomer and a plasticizer in a magnetic stirrer; wherein the resin monomer is any one or more of dipropylene glycol diacrylate, 1,6-hexanediol diacrylate, tripropylene glycol diacrylate and trimethylolpropane triacrylate; the photoinitiator is any one or more of 1-hydroxycyclohexyl benzophenone, trimethylbenzoyl-diphenylphosphine oxide and 2-hydroxy-2-methyl-1-phenyl-1-propanone, and the mass of the photoinitiator accounts for 10% of the photosensitive resin solvent. The oligomer is any one or more of difunctional, tetrafunctional and hexafunctional aliphatic polyurethane acrylate and phenolic resin, and the ratio of the total mass of the oligomer to the total mass of the resin monomer is (0.1-3):(10-5); the plasticizer is any one of 1,2-dibutyl phthalate and polyethylene glycol, and the ratio of the mass of the plasticizer to the total mass of the oligomer and the resin monomer is 1:(10-40); the above ingredients are stirred at 40-60° C. for 5-24 hours by a magnetic stirrer to obtain a uniformly stirred photosensitive resin solvent; The ball milling mixing time of the mixed micron-sized ceramic powder and the photosensitive resin solvent is 24 to 72 hours, and the stirring speed is 150 to 800 r / min.
4. A method for photocuring 3D printing and bridging molding of large-sized and large-span ceramic parts according to claim 1, characterized in that: In the step 2, the shapes of the interface surfaces that can be bridged to each other include planes, curved surfaces, prisms, prisms, pyramids and rectangular concave and convex surfaces.
5. The method of photocuring 3D printing and bridging molding for large-size and large-span ceramic parts according to claim 1, characterized in that: In the step three, the photo-curing molding technology is any one of the stereolithography molding process of point / line / layer scanning molding and the digital light processing technology molding process of layer-by-layer exposure molding.
6. The method of photocuring 3D printing and bridging molding for large-size and large-span ceramic parts according to claim 1, characterized in that: In the step 4, the ultrasonic cleaning time is 1 to 15 minutes.
7. A method for photocuring 3D printing and bridging molding of large-sized and large-span ceramic parts according to claim 1, characterized in that: In the step 5, the light source used for the in-situ photo-crosslinking and curing is an ultraviolet light source with a wavelength of 355 to 405 nm and a curing time of 0.5 to 10 minutes.
8. The method of photocuring 3D printing and bridging molding for large-size and large-span ceramic parts according to claim 1, characterized in that: In the step six, the ceramic parts with light-induced cross-linking and curing bridges are placed in an electric furnace and subjected to secondary curing and bridging at 170-250°C. The heating rate is 0.1-20°C / min, the dwell time is 1-30min, and the cooling rate is the furnace cooling rate or cooled to room temperature at a rate of 1-10°C / min.
9. The method of photocuring 3D printing and bridging molding for large-size and large-span ceramic parts according to claim 1, characterized in that: In step seven, the high temperature sintering molding process includes two steps of degreasing and high temperature sintering: The debinding sintering program is set as follows: 25-150°C, heating at a rate of 0.1-2°C / min, and keeping warm for 0.5-2h; 150-300°C, heating at a rate of 0.1-1.5°C / min, and keeping warm for 0.5-2.5h; 300-550°C, heating at a rate of 0.1-1°C / min, and keeping warm for 0.5-3h; 550-1150°C, heating at a rate of 1-5°C / min, and keeping warm for 0.5-1h; 1150-25°C, cooling at a rate of 2-4°C / min; the pyrolysis atmosphere is any one of argon, nitrogen and helium; The high-temperature sintering program is set as follows: 25-150°C, heating at a rate of 1-5°C / min, and keeping warm for 0.5-2h; 150-300°C, heating at a rate of 2-6°C / min, and keeping warm for 0.5-2.5h; 300-550°C, heating at a rate of 5-10°C / min, and keeping warm for 0.5-3h; 550-(1500-1700)°C, heating at a rate of 6-15°C / min, and keeping warm for 0.5-1h; (1500-1700)-25°C, cooling at a rate of 10-20°C / min; the pyrolysis atmosphere is any one of argon, nitrogen and helium.
10. The method of photocuring 3D printing and bridging molding for large-size and large-span ceramic parts according to claim 1, characterized in that: The infiltration process is any one of a chemical vapor deposition process and a polymer impregnation cracking process; the secondary sintering process program is set as follows: heating from 25 to 800°C at a rate of 0.1 to 5°C / min, and keeping warm for 1 to 2 hours; heating from 800 to (1500 to 1700)°C at a rate of 2 to 10°C / min, and keeping warm for 0.5 to 2 hours; cooling from (1500 to 1700) to 25°C at a rate of 5 to 10°C / min; the pyrolysis atmosphere is any one of argon, nitrogen and helium.
Citation Information
Cited By
Modular photocuring 3D ceramic printing method
CN119427495A
A modular method for light-curing 3D printing ceramics
CN119427495B
Method for preparing ceramic material through cooperation and modularization of photocuring 3D printing and traditional ceramic processing technology
CN119430884A
A modular method for preparing ceramic materials by combining photocuring 3D printing with traditional ceramic processing technology
CN119430884B