High-surface-quality low-yield-ratio hot-rolled steel plate for automobile and manufacturing method thereof

Through low Si composition design and wet sandblasting descaling process, combined with RH+LF double smelting and air cooling+ultra-fast cooling process, the problems of poor surface quality and high production cost of traditional hot-rolled steel plates are solved, and high tensile strength is obtained and low yield ratio automotive hot-rolled steel plates, suitable for high-strength automotive parts.

CN118703884AInactive Publication Date: 2024-09-27ANGANG STEEL CO LTD

Patent Information

Application Number
CN202410844526.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-09-27
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

It is difficult to produce hot-rolled steel plates with high surface quality and low yield ratio at low cost with existing technology. The high Si content in traditional methods leads to poor surface quality, high production costs, and the yield ratio does not meet the requirements of automotive parts.

Method used

It adopts low Si composition design, cooperates with wet sandblasting and descaling process, and forms ferrite, martensite and bainite structures through RH+LF double smelting process, constant speed rolling and air cooling + ultra-fast cooling mode. structure, control the chemical composition and process parameters, and obtain a low yield ratio steel plate with a tensile strength higher than 650MPa.

Benefits of technology

It achieves high surface quality, tensile strength and plasticity matching of the steel plate, reduces production costs, and is suitable for the manufacturing of high-strength automobile wheel parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004915339190000063
    Figure BDA0004915339190000063
  • Figure BDA0004915339190000062
    Figure BDA0004915339190000062
  • Figure BDA0004915339190000071
    Figure BDA0004915339190000071
Patent Text Reader

Abstract

The invention relates to a high-surface-quality low-yield-ratio hot-rolled steel plate for an automobile and a manufacturing method of the high-surface-quality low-yield-ratio hot-rolled steel plate. The steel plate comprises the following chemical components: 0.05%-0.08% of C, 0.05%-0.10% of Si, 0.8%-1.0% of Mn, 0.030%-0.050% of P, less than or equal to 0.003% of S, 0.03%-0.05% of Al, less than or equal to 0.30% of Cr, 0.010%-0.020% of Nb and the balance of Fe and impurities. The low-Si component design is adopted, the wet-type sand blasting descaling process is matched, and the surface quality of the finished steel plate is good; through reasonable component design and matching of smelting and hot rolling process parameters, the low-yield-ratio steel plate with the tensile strength higher than 650 MPa is obtained, and the steel plate has good strength and plasticity matching and is low in production cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of steel rolling, and in particular to a hot-rolled steel plate with high surface quality and low yield ratio for automobiles and a manufacturing method thereof. Background Art

[0002] With the rapid development of the automobile industry, the performance requirements for steel materials used to manufacture automobile parts are increasing. For example, the production process of automobile wheels, which are an important part of automobiles, has been greatly improved in recent years. The use of new processes such as spinning has prompted more personalized requirements for steel materials. Not only are steel materials required to have high strength, but they are also required to have good forming properties and surface quality to meet the requirements of cold forming, electrophoresis, appearance, etc.

[0003] Traditional low-alloy high-strength steel has a high yield ratio, which is prone to cracking and springback during stamping; hot-rolled dual-phase steel with a low yield ratio has poor surface quality and high production cost, which affects the product's application range. Therefore, it is necessary to develop a low yield ratio hot-rolled steel plate with good surface quality for automobiles.

[0004] The Chinese patent application with publication number CN108504958A discloses "a 690MPa grade hot-rolled thick gauge low yield ratio automobile wheel spoke steel and its preparation method". The steel plate adopts C-Si-Mn-Cr-Nb-Ti composition system, wherein Si content is ≤0.2%, Cr content is 0.15-0.25%, Nb content is 0.02-0.04%, Ti content is 0.01-0.03%, and the steel plate adopts ultra-fast cooling + air cooling + layer cooling cooling after rolling. The room temperature structure obtained is composed of a large amount of ferrite, a small amount of martensite and pearlite; the tensile strength of the finished steel plate in the embodiment can reach 690MPa, the yield ratio is greater than 0.71, and the elongation is higher than 23%. The steel plate prepared by this method has high tensile strength and elongation matching, and the yield ratio is lower than that of ordinary low-alloy high-strength steel, but its cooling process is more complicated and the production cost is high.

[0005] The Chinese patent application with publication number CN107746931A discloses "a hot-rolled dual-phase steel plate for automobile wheels and its manufacturing method", which adopts a C-Si-Mn-Cr-P component system, wherein the Si content is 0.1-0.25%, the Cr content is 0.50-0.60%, and the P content is 0.035-0.070%. After the steel plate is finished rolled, a three-stage cooling mode is adopted to obtain a 600MPa-grade hot-rolled dual-phase steel plate with good comprehensive performance. The Si content in the chemical composition of the steel plate is high, the surface quality of the steel plate is poor, and the high content of Cr in the steel plate leads to high cost.

[0006] A Chinese patent application with publication number CN108467996A discloses "a ferrite / martensite hot-rolled dual-phase steel for wheel spokes and a method for manufacturing the same". The steel plate adopts a C-Si-Mn-Cr-Mo component system, wherein the Si content is 0.4-0.6%, the Cr content is 0.30-0.40%, and the Mo content is 0.1-0.2%. After heating, the continuous casting billet is rolled, cooled, pickled, and oiled to finally obtain a 600MPa grade hot-rolled pickled dual-phase steel plate. The hot-rolled pickled dual-phase steel manufactured by this method contains a large amount of Si, Cr, and Mn elements, resulting in a high production cost and a surface quality that is difficult to meet the requirements of high-end wheel steel.

[0007] The Chinese patent application with publication number CN101279330A discloses a method for manufacturing a hot-rolled dual-phase steel plate with a tensile strength of 700 MPa. The main chemical components are as follows: 0.03% to 0.08% C, 0.50% to 0.70% Si, 1.00% to 1.60% Mn, 0% to 0.60% Cr, 0% to 0.40% Mo, 0.02% to 0.05% Nb, and the balance is Fe. The thickness specification is 3.0 to 4.0 mm, and the steel plate has a polygonal ferrite and martensite dual-phase structure with a small amount of granular bainite. The tensile strength of the steel plate is 700 MPa. The steel plate adopts a C-Si-Mn-Cr-Mo-Nb component system, has a high Si content (reaching 0.50-0.70%), and has a poor surface quality. At the same time, the addition of Mo element greatly increases the production cost. Summary of the invention

[0008] The present invention provides a hot-rolled steel plate with high surface quality and low yield ratio for automobiles and a manufacturing method thereof. The steel plate adopts a low Si component design and cooperates with a wet sandblasting descaling process, so that the surface quality of the finished steel plate is good. Through reasonable component design and coordination of smelting and hot rolling process parameters, a low yield ratio steel plate with a tensile strength higher than 650 MPa is obtained. The steel plate has good strength and plasticity matching and low production cost.

[0009] In order to achieve the above object, the present invention adopts the following technical solutions:

[0010] A hot-rolled steel plate with high surface quality and low yield strength ratio for automobiles. The chemical composition of the steel plate is calculated by mass percentage as follows: C: 0.05%-0.08%, Si: 0.05%-0.10%, Mn: 0.8%-1.0%, P: 0.030%-0.050%, S≤0.003%, Al: 0.03%-0.05%, Cr≤0.30%, Nb: 0.010%-0.020%, and the balance is Fe and unavoidable impurities.

[0011] Furthermore, the structure of the steel plate consists of ferrite, martensite and bainite, wherein the volume fraction of ferrite is 80% to 90%, the volume fraction of martensite is 10% to 17%, and the volume fraction of bainite is 0 to 3%; the grain size of ferrite is <4μm, and the banded structure grade is ≤1.5.

[0012] Furthermore, the steel plate has a tensile strength of 650-700 MPa, a yield strength ratio of 0.55-0.58, an elongation of ≥28.0%, and an n value of ≥0.20.

[0013] A method for manufacturing a hot-rolled steel plate with high surface quality and low yield strength ratio for automobiles comprises the following steps:

[0014] (1) Smelting and continuous casting: Refining adopts RH+LF double process, and the smelting end point is controlled to be [H]≤0.0002%, [O]≤0.0015%; calcium treatment is carried out in the refining process, and the amount of silicon calcium wire is fed>2.2m / ton of steel; electromagnetic stirring and soft pressure are used in the continuous casting process;

[0015] (2) Heating: The heating temperature is 1150-1180°C and the soaking time is 100-130 min;

[0016] (3) Rolling, cooling and coiling: The rolling reduction ratio of the steel plate in the non-recrystallization zone is greater than 90%, the final rolling temperature is 800-840°C, constant speed rolling is adopted, and the steel throwing speed is 4-8 m / s; after the final rolling, the cooling mode of air cooling + ultra-fast cooling is adopted, and the air cooling to 630°C-660°C is followed by ultra-fast cooling, and the cooling rate is greater than 100°C / s; the steel plate is cooled to below 180°C, then coiled and air cooled to room temperature;

[0017] (4) Wet sandblasting descaling: After the steel coil is cooled to room temperature, it is unrolled and wet sandblasting descaling is performed. The steel plate travel speed is 15-25 m / min, the steel sand hardness is HRC>60, and the speed of the sandblasting motor is 2100-2300 rpm.

[0018] Furthermore, the thickness of the ingot is 200-230 mm, and the thickness of the finished steel plate is 4-10 mm.

[0019] Furthermore, the surface roughness Ra of the finished steel plate is 1.5-2.5 μm, and the surface cleanliness Sa is ≤3.0.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] 1) The low Si component design is adopted, and the wet sandblasting descaling process is used. The surface quality of the finished steel plate is good, without defects such as iron oxide stripes, color difference and cracks. The surface roughness Ra of the steel plate is 1.5-1.8μm, and the surface cleanliness Sa is lower than level 3.0;

[0022] 2) Through reasonable composition design, as well as smelting and hot rolling process parameter coordination, a low yield ratio steel plate with a tensile strength higher than 650MPa is obtained; the steel plate has good strength and plasticity matching, low production cost, and various indicators are superior to similar products. It is particularly suitable for manufacturing high-strength automobile wheels and other parts with complex shapes and high surface quality requirements. DETAILED DESCRIPTION

[0023] The chemical composition (by mass percentage) of the hot-rolled steel plate with high surface quality and low yield strength ratio for automobiles described in the present invention is C: 0.05%-0.08%, Si: 0.05%-0.10%, Mn: 0.8%-1.0%, P: 0.030%-0.050%, S≤0.003%, Al: 0.03%-0.05%, Cr≤0.30%, Nb: 0.010%-0.020%, and the balance is Fe and unavoidable impurities.

[0024] The reasons for selecting each chemical component and its content (main role) are as follows:

[0025] C: The main function of carbon is to form the required amount of martensite and ensure the strength of steel. Too high a C content will affect the welding performance of the steel plate, while too low a C content is not conducive to obtaining a martensite structure. Therefore, the C content in the present invention is controlled at 0.05% to 0.08%.

[0026] Si: Silicon can expand the two-phase region, which is conducive to promoting the transformation of austenite to ferrite, and is the main element to ensure the percentage of ferrite. However, if the Si content is too high, a large number of iron oxide scale defects will appear on the surface of the steel plate, which is difficult to meet the use requirements of automotive parts. The steel plate of the present invention adopts a low Si component system, and the Si content is controlled at 0.050% to 0.10%.

[0027] Mn: Manganese is a typical austenite stabilizing element, which can significantly improve the hardenability of steel, and play a role in solid solution strengthening and refining ferrite grains, and can significantly delay pearlite transformation and bainite transformation. However, if the Mn content is too high, it will delay the precipitation of ferrite while delaying the pearlite transformation, and it is easy to cause banded structure in the steel plate. Therefore, the present invention controls the Mn content in the steel to be 0.80% to 1.0%.

[0028] P: Phosphorus can significantly change the morphology of martensite islands, making them smaller and more evenly distributed. P can also increase the formation temperature of the α phase and expand the temperature range of the α phase. However, excessive addition of P will deteriorate the workability of the steel plate, so the phosphorus content in the steel is controlled to be 0.030% to 0.050% in the present invention.

[0029] S: Sulfur forms sulfide inclusions such as MnS in steel, which become the starting point of cracks and deteriorate the processing performance. Therefore, the lower the content, the better. Taking the production cost into consideration, the upper limit of the S content in the present invention is set to 0.003%.

[0030] Al: Aluminum plays a role in deoxidation and nitrogen determination during the smelting process, but too much aluminum will lead to a large number of aluminum inclusions. In the present invention, the Al content is controlled at 0.03% to 0.05%.

[0031] Nb: Niobium in a solid solution state can inhibit static and dynamic recrystallization during hot deformation, increase the recrystallization termination temperature, increase the strain accumulation of the rear part of the rack during continuous rolling, promote the transformation of austenite to ferrite, and refine the ferrite grains. Niobium carbonitride can also delay recrystallization, prevent the growth of austenite grains, and have a significant grain refinement strengthening effect. However, excessive Nb content will increase the yield strength ratio of the steel plate, so the present invention controls the niobium content to 0.01% to 0.02%.

[0032] Cr: It is a medium-strong carbide-forming element, which can significantly improve the hardenability of steel and strongly delay the transformation of pearlite and bainite. Although Cr is a weak solid solution strengthening element, it can increase the supercooling ability of austenite, thereby refining the structure and obtaining a strengthening effect. In addition, Cr can also promote the diffusion of carbon into austenite and reduce the yield strength of ferrite, which is more conducive to obtaining a steel plate with low yield strength. The present invention controls the Cr content to be below 0.30%.

[0033] The invention discloses a hot-rolled steel plate with high surface quality and low yield ratio for automobiles, wherein the metallographic structure of the finished steel plate consists of a large amount of ferrite, a small amount of martensite and bainite, wherein the volume fraction of ferrite is 80% to 90%, the volume fraction of martensite is 10% to 17%, and the volume fraction of bainite is 0 to 3%; the ferrite grain size is less than 4 μm, and the banded structure grade is ≤1.5.

[0034] The tensile strength of the finished steel plate is 650-700MPa, the yield strength ratio is 0.55-0.58, the elongation is ≥28.0%, and the n value is ≥0.20.

[0035] The thickness of the finished steel plate is 4 to 10 mm, with good surface quality, free of defects such as iron oxide stripes, color difference and cracks. The surface roughness Ra of the steel plate is 1.5 to 2.5 μm, and the surface cleanliness reaches Sa ≤ 3.0.

[0036] The manufacturing process of a hot-rolled steel plate with high surface quality and low yield strength ratio for automobiles of the present invention comprises the processes of smelting, continuous casting, heating, rolling, cooling, coiling, wet sandblasting and descaling, and specifically comprises the following steps:

[0037] (1) Smelting and continuous casting: RH+LF double process is adopted for refining, and the H and O contents are strictly controlled, [H]≤0.0002%, [O]≤0.0015%; calcium treatment is carried out in the refining process, and the amount of silicon calcium wire is fed>2.2m / ton of steel; electromagnetic stirring and light pressure reduction technology are used in the continuous casting process to prevent defects such as center segregation and looseness of the ingot, and reduce the occurrence of banded structure defects in the steel plate;

[0038] (2) Heating: Heat the 200-230 mm thick ingot to 1150-1180°C, with a soaking time of 100-130 minutes. Appropriate heating temperature and soaking time can not only make the composition of the ingot fully uniform, but also ensure that the original austenite grains are fine;

[0039] (3) Rolling, cooling and coiling: The reduction ratio of the steel plate in the non-recrystallization zone is greater than 90%, the final rolling temperature is 800-840°C, constant speed rolling is adopted, and the steel throwing speed is 4-8 m / s; after the final rolling, the cooling mode of air cooling + ultra-fast cooling is adopted, air cooling to 630°C-660°C and then ultra-fast cooling is carried out, the cooling rate is greater than 100°C / s, the steel plate is cooled to below 180°C, then coiled and air cooled to room temperature, and the thickness of the finished steel plate is 4-10 mm.

[0040] (4) Wet sandblasting descaling: After the steel coil is cooled to room temperature, it is unrolled for wet sandblasting descaling. The steel plate travel speed is 15-25 m / min, the steel sand hardness is HRC>60, and the sandblasting motor speed is 2100-2300 rpm.

[0041] In order to more intuitively embody the present invention, the embodiments of the present invention are further described in conjunction with examples. The following examples are only preferred specific embodiments of the present invention, but the protection scope of the present invention is not limited thereto. Any technical solution that can be obviously obtained by a person skilled in the art within the technical scope disclosed in the present invention, including simple changes or equivalent replacements, is within the protection scope of the present invention.

[0042] [Example]

[0043] In this embodiment, the slab is smelted by RH+LF double process, and the H and O contents are strictly controlled (H≤0.0002%, O≤0.0015%). At the same time, calcium treatment is performed in the refining process, and the amount of silicon calcium wire is>2.2m / ton steel. Electromagnetic stirring and light pressure reduction technology are used in the continuous casting process, and the thickness of the slab is 200mm-230mm. The slab is heated to 1150-1180℃, and rolled after soaking for 100-130 minutes. The rolling reduction rate of the steel plate in the non-recrystallization zone is>90%, the final rolling temperature is 800-840℃, and constant speed rolling is adopted, and the steel throwing speed is 4-8m / s; after the final rolling, the cooling mode of air cooling + ultra-fast cooling is adopted, and ultra-fast cooling is performed after air cooling to 630℃-660℃, and the cooling rate is>100℃ / s. After the steel plate is cooled to ≤180℃, it is coiled and air-cooled to room temperature. After the steel coil is cooled to room temperature, it is unrolled for sandblasting and descaling. The steel plate travel speed is 15-25m / min, the steel sand hardness is HRC>60, and the sandblasting motor speed is 2100-2300rpm. The finished steel plate thickness is 4-10mm.

[0044] The chemical composition of the steel in each embodiment is shown in Table 1, the heating, rolling and coiling process parameters are shown in Table 2, the wet sandblasting dephosphorization process parameters are shown in Table 3, the microstructure and mechanical properties of the finished steel plate are shown in Table 4, and the microstructure, grain size, banded structure, roughness and smoothness of the finished steel plate are shown in Table 5.

[0045] Table 1 Chemical composition of steel (wt, %)

[0046]

[0047] Table 2 Heating, rolling and coiling process parameters

[0048]

[0049] Table 3 Wet sandblasting phosphorus removal process parameters

[0050]

[0051] Table 4 Microstructure and mechanical properties of finished steel plates

[0052]

[0053] Table 5 Organization, grain size, banded structure, roughness and finish of finished steel plates

[0054]

[0055] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A hot-rolled steel plate with high surface quality and low yield strength ratio for automobiles. It is characterized in that The chemical composition of the steel plate is, by mass percentage, C: 0.05% to 0.08%, Si: 0.05% to 0.10%, Mn: 0.8% to 1.0%, P: 0.030% to 0.050%, S≤0.003%, Al: 0.03% to 0.05%, Cr≤0.30%, Nb: 0.010% to 0.020%, and the balance is Fe and unavoidable impurities.

2. The hot-rolled steel sheet with high surface quality and low yield strength ratio for automobiles according to claim 1, It is characterized in that The structure of the steel plate consists of ferrite, martensite and bainite, wherein the volume fraction of ferrite is 80% to 90%, the volume fraction of martensite is 10% to 17%, and the volume fraction of bainite is 0 to 3%; the grain size of ferrite is less than 4 μm, and the banded structure grade is ≤1.

5.

3. The hot-rolled steel sheet with high surface quality and low yield strength ratio for automobiles according to claim 1, It is characterized in that The steel plate has a tensile strength of 650-700 MPa, a yield strength ratio of 0.55-0.58, an elongation of ≥28.0%, and an n value of ≥0.

20.

4. The method for producing a hot-rolled steel sheet with high surface quality and low yield strength ratio for automobiles according to any one of claims 1 to 3, It is characterized in that The steps include: (1) Smelting and continuous casting: Refining adopts RH+LF double process, and the smelting end point is controlled to be [H]≤0.0002%, [O]≤0.0015%; calcium treatment is carried out in the refining process, and the amount of silicon calcium wire is fed>2.2m / ton of steel; electromagnetic stirring and soft pressure are used in the continuous casting process; (2) Heating: The heating temperature is 1150-1180°C and the soaking time is 100-130 min; (3) Rolling, cooling and coiling: The rolling reduction ratio of the steel plate in the non-recrystallization zone is greater than 90%, the final rolling temperature is 800-840°C, constant speed rolling is adopted, and the steel throwing speed is 4-8 m / s; after the final rolling, the cooling mode of air cooling + ultra-fast cooling is adopted, and the air cooling to 630°C-660°C is followed by ultra-fast cooling, and the cooling rate is greater than 100°C / s; the steel plate is cooled to below 180°C, then coiled and air cooled to room temperature; (4) Wet sandblasting descaling: After the steel coil is cooled to room temperature, it is unrolled and wet sandblasting descaling is performed. The steel plate travel speed is 15-25 m / min, the steel sand hardness is HRC>60, and the speed of the sandblasting motor is 2100-2300 rpm.

5. A method for manufacturing a hot-rolled steel sheet with high surface quality and low yield strength ratio for automobiles according to claim 4, It is characterized in that The thickness of the ingot is 200-230 mm, and the thickness of the finished steel plate is 4-10 mm.

6. A method for manufacturing a hot-rolled steel sheet with high surface quality and low yield ratio for automobiles according to claim 4, It is characterized in that The surface roughness Ra of the finished steel plate is 1.5~2.5μm, and the surface cleanliness Sa≤3.0.

Citation Information

Patent Citations

  • Ultrafine grained hot rolled dual-phase steel with tensile strength of above 750MPa and manufacturing method of plate thereof

    CN101880825A

  • Non-quenched and tempered steel plate with low yield ratio and super high strength and producing method thereof

    CN103882330A

  • 800MPa level hot-rolling high broaching steel plate and manufacturing method thereof

    CN105483545A

  • Hot rolled dual-phase steel with tensile strength being 600 MPa and manufacturing method of steel

    CN107881430A

  • Steel for 690MPa grade hot rolled thick low-yield-ratio automobile spoke and preparation method thereof

    CN108504958A

Cited By

  • 1180MPa-grade high-surface-quality hot-rolled TRIP steel with excellent reaming performance and manufacturing method thereof

    CN120519777A

  • 1180mpa grade high surface quality hot-rolled trip steel having excellent hole expansion performance and method of manufacturing the same

    CN120519777B

  • 980MPa-grade high-surface-quality hot-rolled TRIP steel with excellent reaming performance and manufacturing method thereof

    CN120519778A

  • 780MPa-grade high-surface-quality hot-rolled TRIP steel with excellent reaming performance and manufacturing method thereof

    CN120519780A

  • 780mpa grade high surface quality hot-rolled trip steel having excellent hole expansion performance and method of manufacturing the same

    CN120519780B