Multifunctional colored radiation refrigeration material as well as preparation method and application thereof

By using cellulose nanocrystals and nanofibers combined with long-afterglow luminescent powder, a multi-functional color radiation refrigeration material solves the problems of single color and function and high cost of traditional materials, achieving both efficient radiation refrigeration and beautiful effects, cooling The effect is remarkable.

CN118704233APending Publication Date: 2024-09-27CHENGDU YILUOWEIXING NEW MATERIAL TECH CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410705368.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-03
Publication Date
2024-09-27

AI Technical Summary

Technical Problem

Traditional radiant refrigeration materials have problems such as single color, single function and high cost. Moreover, the use of traditional colorants to prepare colored materials will absorb sunlight and cause heating, which offsets the radiant refrigeration effect, making it difficult to meet the needs of both aesthetics and functionality.

Method used

A multi-functional color radiation refrigeration material composed of a cellulose nanocrystal layer, a long afterglow luminescent layer and a non-woven substrate is used to prepare cellulose nanocrystals and nanofibers through the oxidation reaction of microcrystalline cellulose and pulp boards, combined with long afterglow Luminous powder that creates high reflectivity and fluorescent emission effects, reduces solar heating, and enables patterning through screen printing.

Benefits of technology

It achieves efficient radiant cooling capacity, bright color appearance and long afterglow luminescence performance. The cooling effect can reach 9℃ lower than the ambient temperature, which has huge energy saving potential and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004872319090000021
    Figure HDA0004872319090000021
  • Figure BDA0004872319080000081
    Figure BDA0004872319080000081
  • Figure HDA0004872319090000012
    Figure HDA0004872319090000012
Patent Text Reader

Abstract

The invention belongs to the field of radiation refrigeration materials, and discloses a multifunctional color radiation refrigeration material and a preparation method and application thereof. According to the invention, the cellulose nanocrystalline upper layer with bright structural color and the long-afterglow luminescent lower layer with high reflectivity are constructed, and are sequentially deposited on the non-woven fabric base material to obtain the multifunctional colored radiation refrigeration material. The material has adjustable color in a visible light range, high reflectivity, high emissivity and long afterglow luminescence performance, and can be applied to the fields of radiation refrigeration, emergency display and the like. Outdoor experiments show that the material can achieve the cooling effect which is 9 DEG C lower than the environment temperature on average, and has huge energy-saving potential.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of radiation refrigeration materials, and in particular relates to a multifunctional colored radiation refrigeration material and a preparation method and application thereof. Background Art

[0002] In recent decades, energy crisis and global warming are major challenges facing the world today. At present, refrigeration energy consumption accounts for about 10% of the world's total electricity consumption. Improving the efficiency of existing refrigeration systems and exploring new refrigeration technologies have become urgent tasks. Radiative cooling technology is a passive cooling strategy with zero energy consumption and zero environmental pollution. Radiative cooling technology currently has broad application prospects in building energy conservation, personal thermal management, photovoltaic cooling, and water collection.

[0003] According to the second law of thermodynamics, heat will always spontaneously transfer from the surface of a high-temperature object to the surface of a low-temperature object, and this process is irreversible. The temperature of outer space is only about 3K, which is much lower than the temperature of any object on Earth. Therefore, an object can spontaneously radiate its own heat to outer space in the form of thermal radiation to reduce its temperature, thereby achieving radiation cooling. The combined effect of all atmospheric components results in the lowest atmospheric radiation wavelength range of 8 to 13μm, the so-called "atmospheric window". The atmospheric window overlaps with the wavelength range of thermal radiation of terrestrial objects. Therefore, any terrestrial object can effectively radiate heat to the cold universe through thermal radiation through the atmospheric window to keep itself cool. In order to maximize the radiation cooling ability of the material, the optical properties of the material need to be precisely controlled to ensure near-zero absorptivity or high reflectivity over the entire solar spectrum of 0.3-2.5μm, as well as strong thermal radiation through the atmospheric transparent window, that is, high infrared emissivity in the mid-infrared region of 8-13μm.

[0004] However, traditional radiation cooling materials have problems such as single color, single function and high cost, which limit their application. At present, the use of traditional colorants (such as dyes, etc.) to prepare colored radiation cooling materials will inevitably absorb sunlight, causing the object to be heated, thereby offsetting the radiation cooling effect. Therefore, it is necessary to develop multifunctional, low-cost, colorful and efficient radiation cooling materials to meet the practical application needs of both aesthetics and functionality. Summary of the invention

[0005] In order to overcome the shortcomings and deficiencies in the prior art, the primary purpose of the present invention is to provide a multifunctional color radiation refrigeration material; the radiation refrigeration material is composed of an upper CNC layer that provides bright structural colors and high and medium infrared emissivity, a lower layer that provides high reflectivity and long afterglow performance, and a long afterglow powder layer and a bottom substrate that converts part of the absorbed sunlight into fluorescent light and emits it to reduce the heating of the material by sunlight. The radiation refrigeration material has efficient radiation refrigeration capacity, bright color appearance and long afterglow luminescence performance, and can also obtain fluorescent patterns and structural color patterns through screen printing.

[0006] Another object of the present invention is to provide a method for preparing the multifunctional colored radiation refrigeration material.

[0007] Another object of the present invention is to provide an application of the multifunctional colored radiation refrigeration material.

[0008] The purpose of the present invention is achieved through the following technical solutions:

[0009] A multifunctional color radiation cooling material comprises a cellulose nanocrystal layer, a long afterglow luminescent layer and a non-woven fabric substrate from top to bottom.

[0010] The cellulose nanocrystal layer provides structural color and mid-infrared emissivity up to 90%; the long afterglow luminescent layer provides solar reflectivity up to 90% and long afterglow performance, while converting part of the absorbed sunlight into fluorescent light for emission, thereby reducing the heating of the material by sunlight.

[0011] The method for preparing the above-mentioned multifunctional colored radiation refrigeration material comprises the following steps:

[0012] (1) using microcrystalline cellulose to prepare a cellulose nanocrystal (CNC) suspension with a concentration of 1 wt%;

[0013] (2) using pulp board to prepare cellulose nanofiber (CNF) suspension with a concentration of 2 wt‰;

[0014] (3) mixing the long afterglow luminescent powder and the cellulose nanofiber (CNF) suspension obtained in step (2) and depositing the mixture on a non-woven fabric substrate, and drying the mixture naturally to cover the non-woven fabric substrate with a long afterglow luminescent layer;

[0015] (4) mixing the cellulose nanocrystal (CNC) suspension obtained in step (1) with the polyethylene glycol (PEG) solution, and then continuing to deposit the mixture on the long afterglow luminescent layer, and drying the mixture naturally, thereby finally obtaining a multifunctional color radiation refrigeration material.

[0016] The cellulose nanocrystal (CNC) suspension in step (1) is prepared specifically according to the following steps: pouring microcrystalline cellulose into sulfuric acid for acid hydrolysis, pouring into deionized water after the acid hydrolysis is completed, centrifuging the obtained precipitate, washing it with water, and centrifuging and ultrasonicating it again after dialysis to obtain a cellulose nanocrystal (CNC) suspension.

[0017] The acid hydrolysis temperature is 45° C., and the acid hydrolysis time is 80 min. The sulfuric acid has a mass fraction of 64%. The dosage ratio of the microcrystalline cellulose to the sulfuric acid is 17 g:300 mL.

[0018] The cellulose nanofiber (CNF) suspension in step (2) is prepared specifically according to the following steps: using 2,2,6,6-tetramethylpiperidin-1-oxyl free radical (TEMPO), sodium bromide (NaBr), and sodium hypochlorite (NaClO) to carry out an oxidation reaction on the pulp board, using hydrochloric acid solution (HCl) and sodium hydroxide solution (NaOH) to adjust the pH value of the reaction system during the reaction, and after the reaction is completed, filtering and washing the precipitate with water, and then ultrasonicating and centrifuging to obtain a cellulose nanofiber (CNF) suspension.

[0019] The pH value of the reaction system is maintained at 10; the usage ratio of the 2,2,6,6-tetramethylpiperidin-1-oxyl free radical, sodium bromide, sodium hypochlorite and pulp board is 0.16g:1g:62mL:10g; the concentrations of the hydrochloric acid solution and the sodium hydroxide solution are both 0.1mol / L.

[0020] The long afterglow luminescent powder in step (3) is SrAl2O4:Eu 2+ ,Dy 3+ or CaAl2O4:Eu 2+ ,Dy 3+ ; The mass ratio of the long afterglow luminescent powder to the cellulose nanofibers in the cellulose nanofiber (CNF) suspension is 3:1.

[0021] The concentration of the polyethylene glycol (PEG) solution in step (4) is 1wt%; the mass ratio of the cellulose nanocrystals in the cellulose nanocrystal (CNC) suspension to the polyethylene glycol in the polyethylene glycol (PEG) solution is 9:1, 8:2 or 7:3.

[0022] The above-mentioned multifunctional colored radiation cooling material is applied in the field of radiation cooling and emergency display.

[0023] Compared with the prior art, the present invention has the following advantages and effects:

[0024] (1) The preparation method of the multifunctional colored radiation refrigeration material of the present invention is simple. The CNC and CNF used are both degradable and renewable materials. The raw materials are easily available and the cost is low.

[0025] (2) Compared with other colored radiative cooling materials, the present invention uses the Bragg reflection of the chiral nematic structure of CNC to give the material a bright color, avoiding the absorption of sunlight by traditional colorants, reducing the heating effect of the sun, and improving the radiative cooling performance.

[0026] (3) The long afterglow powder introduced in the present invention improves the reflectivity of the material and also gives the material the performance of long afterglow luminescence, which not only improves the radiation cooling effect of the material but also can realize functions such as emergency display.

[0027] (4) The multifunctional colored radiation cooling material of the present invention has high reflectivity and emissivity, and can achieve an average cooling effect of 9°C below the ambient temperature in outdoor experiments, which has huge energy-saving potential.

[0028] (5) The method for preparing the multifunctional colored radiation cooling material of the present invention has wide versatility and can be used on substrates of different materials to enhance the radiation cooling effect of the substrates. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 These are photos of radiation cooling materials in different colors;

[0030] Figure 2 is the reflectivity spectrum of the radiation cooling material of different colors;

[0031] Figure 3 is the emissivity spectrum of radiative cooling materials of different colors;

[0032] Figure 4 This is the outdoor temperature monitoring experimental data of Example 1. DETAILED DESCRIPTION

[0033] The present invention is further described below with reference to specific embodiments, but they should not be construed as limiting the present invention.

[0034] Example 1

[0035] (1) Preparation of cellulose nanocrystal (CNC) suspension: 17 g of microcrystalline cellulose was weighed and added to 300 mL of 64% sulfuric acid, stirred in a 45°C water bath for 80 min for acid hydrolysis, then poured into 2.6 L of deionized water to terminate the reaction and allowed to stand overnight; the supernatant was poured out, and the precipitate was centrifuged and washed three times (3000 rpm, 8 min / time); the obtained suspension was placed in a dialysis bag and dialyzed with deionized water for one week; the dialyzed suspension was then centrifuged (10000 rpm, 15 min) and sonicated in an ice water bath (300 W, 15 min) to obtain a cellulose nanocrystal (CNC) suspension with a mass fraction of 1%.

[0036] (2) Preparation of cellulose nanofiber (CNF) suspension: Weigh 10 g of crushed pulp board and add it to 1 L of distilled water to obtain a suspension; add 0.16 g of TEMPO, 1 g of NaBr and 62 mL of NaClO to the obtained suspension respectively; place a pH meter in the suspension to monitor its pH value, and adjust the pH value of the system with 0.1 mol / L HCl solution under constant stirring to keep it at around 10; as the reaction proceeds, the pH value of the solution gradually decreases, and to maintain the pH value of the system, 0.1 mol / L NaOH solution is slowly added; when the pH value of the system does not change for at least 30 minutes, the reaction is terminated and CNF slurry is obtained; the CNF slurry is thoroughly washed to neutrality, and then ultrasonicated in an ice-water bath (300 W, 2 h) and centrifuged (10000 rpm, 15 min) to obtain a cellulose nanofiber (CNF) suspension with a mass fraction of 2‰.

[0037] (3) Preparation of SrAl2O4:Eu 2+ ,Dy 3+ -CNF@nonwoven fabric: 0.06g SrAl2O4:Eu 2+ ,Dy 3+ The powder was added to 10 mL of the cellulose nanofiber (CNF) suspension obtained in step (2), mixed and stirred evenly, and deposited on a non-woven fabric substrate. The non-woven fabric substrate was naturally dried at room temperature. The non-woven fabric substrate was covered with a long afterglow luminescent layer, namely SrAl2O4:Eu 2+ ,Dy 3+ -CNF@nonwoven fabric;

[0038] (4) Preparation of SrAl2O4:Eu 2+ ,Dy 3+ -CNF / CNC@nonwoven fabric: 2 mL of 1% PEG solution and 18 mL of cellulose nanocrystal (CNC) suspension obtained in step (1) were mixed and stirred evenly, and then the SrAl2O4:Eu2O4 obtained in step (3) was deposited on the 2+ ,Dy 3+ -CNF@ non-woven fabric forms a cellulose nanocrystal layer, which is naturally dried at room temperature to obtain a colorful radiative cooling material.

[0039] Example 2

[0040] The colored radiation refrigeration material was prepared by the same method as in Example 1, except that: in step (4), 4 mL of 1% PEG solution and 16 mL of the cellulose nanocrystal (CNC) suspension obtained in step (1) were mixed and stirred evenly, and the SrAl2O4:Eu2O4 obtained in step (3) was further deposited. 2+ ,Dy 3+-CNF@ non-woven fabric, and dried naturally at room temperature. The other process steps are the same as those in Example 1.

[0041] Example 3

[0042] The colored radiation refrigeration material was prepared by the same method as in Example 1, except that: in step (4), 6 mL of PEG solution with a mass fraction of 1% and 14 mL of cellulose nanocrystal (CNC) suspension obtained in step (1) were mixed and stirred evenly, and then the SrAl2O4:Eu2O4 obtained in step (3) was continuously deposited. 2+ ,Dy 3+ -CNF@ non-woven fabric, and dried naturally at room temperature. The other process steps are the same as those in Example 1.

[0043] Example 4

[0044] (1) Preparation of cellulose nanocrystal (CNC) suspension: 17 g of microcrystalline cellulose was weighed and added to 300 mL of 64% sulfuric acid, stirred in a 45°C water bath for 80 min for acid hydrolysis, then poured into 2.6 L of deionized water to terminate the reaction and allowed to stand overnight; the supernatant was poured out, and the precipitate was centrifuged and washed three times (3000 rpm, 8 min / time); the obtained suspension was placed in a dialysis bag and dialyzed with deionized water for one week; the dialyzed suspension was then centrifuged (10000 rpm, 15 min) and sonicated in an ice water bath (300 W, 15 min) to obtain a cellulose nanocrystal (CNC) suspension with a mass fraction of 1%.

[0045] (2) Preparation of cellulose nanofiber (CNF) suspension: Weigh 10 g of crushed pulp board and add it to 1 L of distilled water to obtain a suspension; add 0.16 g of TEMPO, 1 g of NaBr and 62 mL of NaClO to the obtained suspension respectively; place a pH meter in the suspension to monitor its pH value, and adjust the pH value of the system with a 0.1 mol / L HCl solution under constant stirring to keep it at about 10. As the reaction proceeds, the pH value of the solution gradually decreases; to maintain the pH value of the system, slowly add 0.1 mol / L NaOH solution; when the pH value of the system does not change for at least 30 minutes, the reaction is terminated to obtain CNF slurry; the CNF slurry is thoroughly washed to neutrality, and then ultrasonicated (300 W, 2 h) and centrifuged (10000 rpm, 15 min) in an ice water bath to obtain cellulose nanofiber (CNF) suspensions with mass fractions of 2‰ and 5‰, respectively.

[0046] (3) Preparation of fluorescent patterned long afterglow powder-CNF@non-woven fabric: 0.06g SrAl2O4:Eu 2+ ,Dy 3+The powder was added to 10 mL of the cellulose nanofiber (CNF) suspension with a mass fraction of 2‰ obtained in step (2), mixed and stirred evenly, deposited on the non-woven fabric substrate, and dried naturally at room temperature to obtain long afterglow powder-CNF@non-woven fabric. 2+ ,Dy 3+ The powder was added into 10 mL of cellulose nanofiber (CNF) suspension with a mass fraction of 5‰ obtained in step (2), and stirred to mix evenly to obtain CaAl2O4:Eu 2+ ,Dy 3+ -CNF ink. Using the obtained CaAl2O4:Eu 2+ ,Dy 3+ -CNF ink was screen-printed on the surface of the long afterglow powder-CNF@nonwoven fabric obtained above to obtain a long afterglow powder-CNF@nonwoven fabric with a fluorescent pattern.

[0047] (4) Preparation of structural color patterned long afterglow powder-CNF / CNC@non-woven fabric: 2 mL of 1% PEG solution and 18 mL of cellulose nanocrystal (CNC) suspension obtained in step (1) were mixed and stirred evenly, and then deposited on the long afterglow powder-CNF@non-woven fabric with a fluorescent pattern obtained in step (3), dried naturally at room temperature, and then screen-printed on the surface with 10% glucose solution as ink to obtain a multifunctional color radiation refrigeration material.

[0048] Comparative Example 1

[0049] The color radiation cooling material was prepared by the same method as in Example 1, except that step (3) was omitted, and the long afterglow luminescent layer was not deposited, but a mixture of the PEG solution and the cellulose nanocrystal suspension was directly deposited on the non-woven fabric substrate to form a cellulose nanocrystal layer. The other process steps were the same as in Example 1.

[0050] Comparative Example 2

[0051] The colored radiation cooling material was prepared by the same method as in Example 1, except that step (4) was omitted and the cellulose nanocrystal layer (CNC layer) was not deposited. The other process steps were the same as in Example 1.

[0052] Comparative Example 3

[0053] The same method as in Example 1 is used to prepare the colored radiation cooling material, except that: the SrAl2O4:Eu in step (3) 2+ ,Dy 3+ The amount of powder used was 0.08 g, and the other process steps were the same as in Example 1.

[0054] Comparative Example 4

[0055] The same method as in Example 1 is used to prepare the colored radiation cooling material, except that: the SrAl2O4:Eu in step (3) 2+ ,Dy 3+ The amount of powder used was 0.02 g, and the other process steps were the same as in Example 1.

[0056] The performance test data of the radiation refrigeration materials obtained in Examples 1-4 and Comparative Examples 1-4 are shown in Table 1 below:

[0057] Table 1 Performance test data of radiation cooling materials

[0058]

[0059] It can be seen from the data in Table 1 that the multifunctional colored radiation cooling material prepared by the method of the present invention has excellent radiation cooling performance, and can achieve an average cooling effect of 9°C lower than the outdoor ambient temperature even in the hot summer. In addition, patterning the material by screen printing not only improves the aesthetics of the material and broadens its application field, but also ensures excellent radiation cooling effect, with high reflectivity and obvious outdoor cooling ability.

[0060] In Comparative Example 1, no long afterglow luminescent layer is added. It can be seen that the reflectivity of the material is significantly reduced to only 31.5%. At the same time, its outdoor cooling effect is also significantly worse, and the temperature difference with the outdoor environment is reduced to 5.7°C. In Comparative Example 2, no CNC layer is added. Although the material still has a high reflectivity of 91%, the appearance is white, and the temperature difference with the outdoor environment in the outdoor test is reduced to 5.4°C. It can be seen that the synergistic effect of the long afterglow powder and CNC in the present invention ensures that the prepared material has excellent radiation cooling performance with a colorful appearance, and also gives the material multifunctionality such as patterning and long afterglow luminescence.

[0061] In addition, in Comparative Example 3, the content of long afterglow powder was increased, and the adhesion between long afterglow powder-CNF / CNC and non-woven fabric substrate was significantly reduced, and it was very easy to fall off during use, while its radiative cooling performance was not significantly improved. In Comparative Example 4, the content of long afterglow powder was reduced, and the reflectivity of the material dropped to 78.3%, and the temperature difference with the outdoor environment was reduced to 4.2 degrees Celsius. Therefore, the long afterglow powder content defined in this invention is more conducive to obtaining a material with excellent radiative cooling performance.

[0062] The above embodiments are relatively suitable implementation modes of the present invention. The implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations and simplifications made without departing from the spirit and principle of the present invention shall be equivalent replacement modes and shall be included in the protection scope of the present invention.

Claims

1. A multifunctional color radiation cooling material, characterized in that: The material includes a cellulose nanocrystal layer, a long afterglow luminescent layer and a non-woven fabric substrate from top to bottom.

2. The multifunctional color radiation refrigeration material according to claim 1, characterized in that: The cellulose nanocrystal layer provides structural color and mid-infrared emissivity up to 90%; the long afterglow luminescent layer provides solar reflectivity up to 90% and long afterglow performance, while converting part of the absorbed sunlight into fluorescent light for emission, thereby reducing the heating of the material by sunlight.

3. The method for preparing a multifunctional color radiation refrigeration material according to claim 1, characterized in that The following steps are involved: (1) using microcrystalline cellulose to prepare a cellulose nanocrystal suspension with a concentration of 1 wt%; (2) using a pulp board to prepare a cellulose nanofiber suspension with a concentration of 2 wt‰; (3) mixing the long afterglow luminescent powder and the cellulose nanofiber suspension obtained in step (2) and depositing the mixture on a non-woven fabric substrate, and drying the mixture naturally to cover the non-woven fabric substrate with a long afterglow luminescent layer; (4) The cellulose nanocrystal suspension obtained in step (1) and the polyethylene glycol solution are mixed and then deposited on the long afterglow luminescent layer, and dried naturally to finally obtain a multifunctional color radiation refrigeration material.

4. The preparation method according to claim 3, characterized in that: The cellulose nanocrystal suspension in step (1) is prepared specifically according to the following steps: pouring microcrystalline cellulose into sulfuric acid for acid hydrolysis, pouring into deionized water after the acid hydrolysis is completed, centrifuging the obtained precipitate, washing it with water, dialyzing it, centrifuging it again and sonicating it to obtain a cellulose nanocrystal suspension.

5. The preparation method according to claim 4, characterized in that: The acid hydrolysis temperature is 45° C., and the acid hydrolysis time is 80 min. The sulfuric acid has a mass fraction of 64%. The dosage ratio of the microcrystalline cellulose to the sulfuric acid is 17 g:300 mL.

6. The preparation method according to claim 3, characterized in that: The cellulose nanofiber suspension in step (2) is prepared specifically according to the following steps: using 2,2,6,6-tetramethylpiperidin-1-oxyl free radical, sodium bromide and sodium hypochlorite to oxidize the pulp board, using hydrochloric acid solution and sodium hydroxide solution to adjust the pH value of the reaction system during the reaction, and after the reaction, filtering and washing the precipitate with water, and then ultrasonicating and centrifuging to obtain the cellulose nanofiber suspension.

7. The preparation method according to claim 6, characterized in that: The pH value of the reaction system is maintained at 10; the usage ratio of the 2,2,6,6-tetramethylpiperidin-1-oxyl free radical, sodium bromide, sodium hypochlorite and pulp board is 0.16g:1g:62mL:10g; the concentrations of the hydrochloric acid solution and the sodium hydroxide solution are both 0.1mol / L.

8. The preparation method according to claim 3, characterized in that: The long afterglow luminescent powder in step (3) is SrAl2O4:Eu 2+ ,Dy 3+ or CaAl2O4:Eu 2+ ,Dy 3+ ; The mass ratio of the long afterglow luminescent powder to the cellulose nanofibers in the cellulose nanofiber suspension is 3:

1.

9. The preparation method according to claim 3, characterized in that: The concentration of the polyethylene glycol solution in step (4) is 1 wt %; the mass ratio of the cellulose nanocrystals in the cellulose nanocrystal suspension to the polyethylene glycol in the polyethylene glycol solution is 9:1, 8:2 or 7:

3.

10. Application of the multifunctional color radiation cooling material according to claim 1 in the field of radiation cooling and emergency display.

Citation Information

Cited By

  • Humidity response color-changing radiation refrigeration material and preparation method and application thereof

    CN120722472A

  • Humidity-responsive color-changing radiation refrigeration material, preparation method and application thereof

    CN120722472B