Pole piece, preparation method of pole piece, solid-state battery and preparation method of solid-state battery

By using ultrasonic spraying technology to introduce a mixed conductive layer of nano conductive agent and organic polymer solid electrolyte on the surface of the solid-state battery pole piece, the problem of insufficient interface contact between the composite solid electrolyte layer and the pole piece is solved, and the cycle stability of the solid-state battery is improved. and production efficiency.

CN118738271AInactive Publication Date: 2024-10-01CHONGQING TALENT NEW ENERGY CO LTD

Patent Information

Application Number
CN202411072753.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-08-10
Filing Date
2024-08-06
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the existing solid-state battery pole piece structural design, the interface contact between the composite solid electrolyte layer and the pole piece is insufficient, resulting in high interface impedance, affecting the cycle stability of the battery, and batch preparation is difficult, limiting the solid-state battery industry. development.

Method used

Ultrasonic spraying technology is used to introduce a mixed conductive layer on the surface of the pole piece, including nano conductive agents and organic polymer solid electrolytes, and through the construction of multi-layer solid electrolyte layers, the interface contact and compatibility are improved, and the interface impedance is reduced.

Benefits of technology

It achieves close interface contact with the solid-state battery pole pieces, reduces the interface impedance, improves the cycle stability and structural stability of the battery, and simplifies the mass production process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738271A_ABST
    Figure CN118738271A_ABST
Patent Text Reader

Abstract

The invention relates to a pole piece and a preparation method thereof, and a solid-state battery and a preparation method thereof. The mixed conductive layer comprising the nano conductive agent and the organic polymer solid electrolyte is introduced into the surface of the pole piece, the contact area between the mixed conductive layer and the pole piece is effectively increased by using the nano conductive agent, the organic polymer solid electrolyte can construct flexible interface contact, ion conduction is improved, interface impedance is reduced, and the performance of the lithium ion battery is improved. And the cycling stability of the solid-state battery is improved. The slurry mixed with the conductive layer and the solid electrolyte are compounded with the pole piece by using an ultrasonic spraying method, so that slurry particles can be fully refined, the stability of the coating can be improved, a uniform layered structure with controllable thickness can be realized, the structural stability and the interface compatibility of the solid battery can be improved, and the diaphragm-free solid battery can be prepared.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of solid-state batteries and relates to a pole piece and a preparation method thereof and a solid-state battery and a preparation method thereof. Background Art

[0002] Solid-state batteries have attracted widespread attention due to their reliable safety and high energy density. The thermal stability and chemical stability of solid-state electrolyte materials improve the safety of solid-state batteries, while the structural design of solid-state battery electrodes and the effective interface contact between active substances are the key to improving the safety and energy density of solid-state batteries.

[0003] The existing solid-state battery structures can be divided into systems with diaphragms and systems without diaphragms. In the system with diaphragms, the currently widely used diaphragm materials are all organic polymer materials, which have the following two problems: on the one hand, they will shrink and melt when the battery is abnormally heated, causing large-area contact between the positive and negative pole pieces, resulting in short circuits or even explosions; on the other hand, impurities and burrs in the battery may also pierce the diaphragm, causing direct contact between the positive and negative pole pieces, resulting in short circuits and safety issues. For an ideal system without diaphragms, the solid-state battery structure can adopt a stacked structure of positive active material, solid electrolyte layer, and negative active material to form a battery core, but the existing solid-state battery structure and related processes have problems such as easy detachment of the active material coating and poor solid interface contact, which leads to battery performance degradation, and the process of mass preparation of solid electrolyte pole pieces is difficult, which restricts the current development of solid-state battery industrialization.

[0004] Therefore, in order to solve the above-mentioned problems mentioned in the membrane-free system, it is necessary to rationally design the structure of the solid-state battery electrode and select appropriate process methods to effectively solve the problems of interface contact and interface compatibility between the solid electrolyte and the positive and negative electrode active materials.

[0005] In the prior art, there are solid-state lithium batteries with multifunctional layered composite solid electrolytes. The multifunctional layered solid electrolyte layer is formed by coating a solution containing a composite solid electrolyte on the surface of the positive electrode plate as a buffer solid electrolyte layer, and a solid electrolyte layer is arranged between the positive electrode and the negative electrode to improve the interface contact between the solid electrolyte layer and the battery plate. However, the interface contact between the composite solid electrolyte layer and the battery plate is still point contact, and the coating thickness is uneven, which cannot achieve the effect of reducing the interface impedance, affecting the cycle stability of the battery. Summary of the invention

[0006] Problem that the invention aims to solve

[0007] In view of the problem that the interface contact between the above-mentioned composite solid electrolyte layer and the electrode is insufficient and the interface impedance still needs to be reduced, there is an urgent need for a electrode and a solid-state battery with a reasonable electrode structure design and suitable interlayer composition, which can improve the interface contact between the solid electrolyte and the battery electrode and enhance the cycle stability of the solid-state battery, as well as a preparation method that can improve the process effect of solid-state electrolyte introduction and solve the problem of mass production of solid-state battery electrodes.

[0008] Solutions for solving problems

[0009] In view of the above problems, the present invention provides a pole piece, which can effectively solve the interface contact problem between the solid electrolyte and the battery pole piece through the pole piece composite technology, realize the close contact between the solid electrolyte and the positive and negative active material particles, and reduce the thickness of the solid electrolyte layer, realize a uniform and stable interlayer structure, reduce the interface impedance and relieve the interface stress through interface softening, and improve the cycle stability of the solid-state battery. In addition, the present invention also provides a method for preparing the pole piece, which uses an ultrasonic spraying method to fully refine the slurry particles, improve the stability of the coating, and realize a uniform layered structure with controllable thickness, improve the structural stability and interface compatibility of the solid-state battery, prepare a diaphragm-free battery, and solve the problem of mass production of solid-state battery pole pieces.

[0010] Specifically, the present invention provides a pole piece, which includes a mixed conductive layer on a positive pole piece or a negative pole piece, wherein the mixed conductive layer includes a nano conductive agent and an organic polymer solid electrolyte.

[0011] According to the pole piece described above, in the mixed conductive layer, the mass ratio of the nano conductive agent to the organic polymer solid electrolyte is (85-20): (15-80), preferably the mass ratio of the nano conductive agent to the organic polymer solid electrolyte is (80-25): (20-75).

[0012] According to the pole piece described above, the particle size of the nano-conductive agent is 5-500 nm, and preferably the particle size of the nano-conductive agent is 10-300 nm.

[0013] According to the pole piece described above, the thickness of the mixed conductive layer is 100nm-1000nm, preferably the thickness of the mixed conductive layer is 150-800nm;

[0014] Preferably, the mixed conductive layer further comprises a binder;

[0015] Preferably, the binder is selected from one or more of polyvinylidene fluoride, polyvinyl alcohol, polytetrafluoroethylene, sodium hydroxymethyl cellulose, styrene-butadiene rubber, nitrile rubber, styrene-butadiene-styrene copolymer, polyacrylic acid, and lithium polyacrylate.

[0016] According to the pole piece described above, the nano conductive agent is selected from one or more of conductive graphite, conductive carbon black, acetylene black, carbon nanotubes, Ketjen black, graphene, carbon molecular sieve, carbon nanofiber, polystyrene sulfonic acid, lithium polystyrene sulfonate and polyethylene dioxythiophene;

[0017] Preferably, the organic polymer solid electrolyte is selected from one or more of polyethylene oxide, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polyvinylidene fluoride-chlorotrifluoroethylene, polyacrylonitrile, polymethyl methacrylate, polypropylene carbonate, polyphenylene sulfide, polyethyl cyanoacrylate, polypentylene succinate, polyvinyl chloride, polyvinyl carbonate, polyvinyl pyrrolidone, chitosan, polyimide, polyacrylate, polyurethane, aramid, polyetherimide, polyamide, polysulfone, aromatic sulfone, polyaromatic sulfone, polyether sulfone, epoxy resin and polyphenylene sulfone resin.

[0018] According to the pole piece described above, the pole piece further comprises a first composite solid electrolyte layer on the mixed conductive layer;

[0019] Preferably, the thickness of the first composite solid electrolyte layer is 200-3000 nm, preferably the thickness of the first composite solid electrolyte layer is 250-2000 nm;

[0020] Preferably, the first composite solid electrolyte layer comprises an inorganic ceramic material, an organic polymer solid electrolyte, and a lithium salt.

[0021] According to the pole piece described above, the inorganic ceramic material used for the first composite solid electrolyte layer is selected from one or more of nitrides, carbides, metal oxides, and non-metal oxides;

[0022] Preferably, the inorganic ceramic material can be selected from one or more combinations of oxides, nitrides, borides, halides, carbides, dielectric ceramics, ferroelectric ceramics, piezoelectric ceramics, diatomaceous earth, mullite, montmorillonite and kaolin;

[0023] The oxides include, but are not limited to, one or more combinations of silicon oxide, boron oxide, magnesium oxide, copper oxide, nickel oxide, calcium oxide, aluminum oxide, titanium oxide, zirconium oxide, vanadium oxide, lanthanum oxide, beryllium oxide, yttrium oxide, cerium oxide, and lead zirconium titanate;

[0024] The nitride includes but is not limited to one or more combinations of silicon nitride, titanium nitride, aluminum nitride, boron nitride, magnesium nitride, zirconium nitride and silicon oxynitride;

[0025] The carbide is selected from one or more of silicon carbide, boron carbide, tantalum carbide, vanadium carbide, zirconium carbide, tungsten carbide, molybdenum carbide, manganese carbide, iron carbide, titanium carbide and niobium carbide;

[0026] The dielectric ceramics, ferroelectric ceramics and piezoelectric ceramics respectively include BaTiO3, MgTiO3, CaTiO3, PbTiO3, SrTiO3, BaO·TiO2, BaO-Nd2O3-TiO2, LiNbO3, LiTaO3, Cd2Ta2O7, Pb2Nb2O7, Cd2Nb2O7, PbNb2O6, Sr 1-x Ba x Nb2O6 and Ba2NaNb5O 15 One or more of;

[0027] According to the pole piece described above, the pole piece further comprises a second solid electrolyte layer on the first composite solid electrolyte layer;

[0028] Preferably, the thickness of the second solid electrolyte layer is 2 μm-50 μm, preferably the thickness of the second solid electrolyte layer is 5 μm-40 μm;

[0029] Preferably, the second solid electrolyte layer further comprises a lithium salt and / or a binder.

[0030] According to the pole piece described above, the solid electrolyte used for the second solid electrolyte layer includes one or more of an inorganic solid electrolyte and an organic polymer solid electrolyte;

[0031] Preferably, the inorganic solid electrolyte is selected from one or more of an oxide solid electrolyte, a sulfide solid electrolyte, a halide solid electrolyte, a borate solid electrolyte, a nitride solid electrolyte and a hydride solid electrolyte.

[0032] According to the pole piece described above, the oxide solid electrolyte is selected from one or more of a garnet solid electrolyte, a perovskite solid electrolyte, a NASICON solid electrolyte and a LISICON solid electrolyte;

[0033] The garnet-type solid electrolyte includes Li x Ln3Z y A z O 12 and / or Li x La 3-y B y Zr z O 12 ; Wherein, A is one or more of Ta, Nb, Mg, Ti, Te, and W, and B is one or more of Ca, Rb, Al, and Ga;

[0034] The perovskite solid electrolyte includes Li 3.3 La 0.53 TiO3、Li 3xLa 2 / 3-x TiO3 and Li x Sr y M z One or more of TaO3; wherein M is one or more of Zr and Nb;

[0035] The NASICON-type solid electrolyte includes Li x Al y M z (PO4)3、Li x Y y Zr z (PO4)3, LiTi2(PO4)3, LiGe2(PO4)3 and LiGeTi(PO4)3; wherein M is one or more of Ti, Ge, Hf, Zn, Zr and Si;

[0036] The LISICON type solid electrolyte includes Li 3+x (P 1-x Si x )O4 and / or Li 3+x Ge x V 1-x O4;

[0037] The sulfide solid electrolyte is selected from Argyrodite solid electrolyte LiPSMX, Thio-LiSICON solid electrolyte Li 4-x A 1-x B x S4 and one or more of glassy sulfides; wherein M is one or more of O, Cu, Zn, Bi, Sn, Al, Mn, Ce and In, X is one or more of F, Cl, Br and I; A is one or more of Si, Sn, Ge and Zr, and B is one or more of O, P, Al, Zn and Ga;

[0038] The glassy sulfide includes one or more of Li2S-P2S5, Li2S-GeS2, Li2S-SiS2, Li2S-SiS2-Li4SiO4, Li2S-B2S3, and Li2S-B2S3-LiI;

[0039] The halide solid electrolyte includes LiX, Li2MX 4、 Li3M′X6、Li x M″ y Ln z Cl 3、 LiM″′Cl5X″ and Li 3- y Zr y M″″1-y Cl6; wherein X is one or more of F, Cl, Br, I, M is one or more of Mg, Mn, Fe, Zn and Cd, M' is one or more of O, In, Y, Yb, Sc, Ho, Er, M "is one or more of Ta, Zr, Ca and Al, Ln is one or more of La, Ce, Pr, Nd, Sm, M "' is selected from one or more of La, Ta, Nb, X "is selected from O, Cl, F or OH, M " " is selected from one or more of Y, Er, Yb, Ho, Lu;

[0040] Among them, 0 <x<1,0<y<1,0<z<1;

[0041] The borate solid electrolyte is selected from one or more of Li2B4O7, Li2O-B2O3-P2O5;

[0042] The nitride solid electrolyte is selected from one or more of LiPON, Li3N, Li7PN4, and LiSi2N3;

[0043] The hydride solid electrolyte includes but is not limited to one or more of Li3AlH6, LiBH4, LiNH2, Li2NH, LiBH4-LiNH2, LiBH4-LiX; wherein X is one or more of Cl, Br and I;

[0044] Preferably, the perovskite-type oxide solid electrolyte is selected from lithium lanthanum titanium oxide;

[0045] The garnet-type oxide solid electrolyte is selected from one or more of lithium lanthanum zirconium oxide, niobium-doped lithium lanthanum zirconium oxide, tantalum-doped lithium lanthanum zirconium oxide, and niobium-tantalum dual-doped lithium lanthanum zirconium oxide;

[0046] The NASICON type oxide solid electrolyte is selected from one or more of lithium aluminum titanium phosphate, lithium yttrium titanium phosphate, and lithium aluminum germanium phosphate.

[0047] According to the pole piece described above, the binder is selected from one or more of polyvinylidene fluoride, polyvinyl alcohol, polytetrafluoroethylene, sodium hydroxymethyl cellulose, styrene-butadiene rubber, nitrile rubber, styrene-butadiene-styrene copolymer, polyacrylic acid, and lithium polyacrylate;

[0048] Preferably, the lithium salt is selected from one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium bis(trifluoromethanesulfonyl imide), lithium bis(fluorosulfonyl imide) and lithium difluorooxalatoborate.

[0049] The present invention provides a method for preparing a pole piece, which comprises the following steps:

[0050] Step S2: spraying a conductive slurry containing a nano conductive agent and an organic polymer solid electrolyte onto the surface of the positive electrode sheet or the negative electrode sheet by ultrasonic spraying, and then optionally heating and curing to obtain a positive electrode sheet or a negative electrode sheet with a mixed conductive layer.

[0051] According to the above preparation method, the preparation method further comprises the following steps:

[0052] Step S4: spraying the slurry containing the inorganic ceramic material onto the surface of the mixed conductive layer obtained in step S2 by ultrasonic spraying, thereby obtaining a positive electrode sheet or a negative electrode sheet having the mixed conductive layer and the first composite solid electrolyte layer in sequence.

[0053] According to the above preparation method, the preparation method further comprises the following steps:

[0054] Step S6: spraying the second solid electrolyte slurry onto the surface of the first composite solid electrolyte layer obtained in step S4 by ultrasonic spraying, thereby obtaining a positive electrode sheet or a negative electrode sheet having a mixed conductive layer, a first composite solid electrolyte layer and a second solid electrolyte layer in sequence.

[0055] According to the above preparation method, the preparation method further comprises the following steps:

[0056] Step Sx: hot pressing the finally prepared positive electrode sheet or negative electrode sheet;

[0057] Preferably, the hot pressing temperature is 40-60° C., the pressure is 0.1-0.5 MPa, and the hot pressing time is 5-20 minutes.

[0058] According to the preparation method described above, the solid content of the conductive paste is 5 to 40% by mass;

[0059] Preferably, the solid content of the slurry containing the inorganic ceramic material is 5 to 30% by mass;

[0060] Preferably, the second solid electrolyte slurry has a solid content of 5 to 40% by mass.

[0061] According to the preparation method described above, in the conductive paste of step S2, the mass ratio of the nano conductive agent to the organic polymer solid electrolyte is (85-20): (15-80), preferably the mass ratio of the nano conductive agent to the organic polymer solid electrolyte is (80-25): (20-75);

[0062] Preferably, the particle size of the nano conductive agent is 5-500 nm, more preferably the particle size of the nano conductive agent is 10-300 nm.

[0063] According to the preparation method described above, in the ultrasonic spraying in step S2, step S4 and step S6, the spraying conditions are as follows: ultrasonic power is 10-100W, ultrasonic frequency is 20-200kHz, continuous spraying amount is 0-3000ml / h, preferably 800-1700ml / h, spraying distance is 10-100mm, air guide pressure is 0.1-0.3MPa, spray width is 50-400mm, spraying angle is 85-90°, and the temperature of the positive electrode sheet or the negative electrode sheet is 30-80°C;

[0064] Preferably, the spraying conditions in step S2, step S4 and step S6 are the same or different.

[0065] According to the preparation method described above, in step S2, the temperature of heating and curing is 60-120°C, preferably the temperature of heating and curing is 80-100°C.

[0066] According to the preparation method described above, the nano-conductive agent used in step S2 is selected from one or more of conductive graphite, conductive carbon black, acetylene black, carbon nanotubes, Ketjen black, graphene, carbon molecular sieves, carbon nanofibers, polystyrene sulfonic acid, lithium polystyrene sulfonate and polyethylene dioxythiophene;

[0067] Preferably, the organic polymer solid electrolyte used in step S2 is selected from one or more of polyethylene oxide, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polyvinylidene fluoride-chlorotrifluoroethylene, polyacrylonitrile, polymethyl methacrylate, polypropylene carbonate, polyphenylene sulfide, polyethyl cyanoacrylate, polypentylene succinate, polyvinyl chloride, polyvinyl carbonate, polyvinyl pyrrolidone, chitosan, polyimide, polyacrylate, polyurethane, aramid, polyetherimide, polyamide, polysulfone, aromatic sulfone, polyaromatic sulfone, polyether sulfone, epoxy resin and polyphenylene sulfone resin.

[0068] According to the preparation method described above, the slurry containing the inorganic ceramic material used in step S4 further contains an organic polymer solid electrolyte and a lithium salt;

[0069] The inorganic ceramic material used in step S4 is selected from one or more of nitrides, carbides, metal oxides, and non-metal oxides;

[0070] Preferably, the inorganic ceramic material can be selected from one or more combinations of oxides, nitrides, borides, halides, carbides, dielectric ceramics, ferroelectric ceramics, piezoelectric ceramics, diatomaceous earth, mullite, montmorillonite and kaolin;

[0071] The oxides include, but are not limited to, one or more combinations of silicon oxide, boron oxide, magnesium oxide, copper oxide, nickel oxide, calcium oxide, aluminum oxide, titanium oxide, zirconium oxide, vanadium oxide, lanthanum oxide, beryllium oxide, yttrium oxide, cerium oxide, and lead zirconium titanate;

[0072] The nitride includes but is not limited to one or more combinations of silicon nitride, titanium nitride, aluminum nitride, boron nitride, magnesium nitride, zirconium nitride and silicon oxynitride;

[0073] The carbide is selected from one or more of silicon carbide, boron carbide, tantalum carbide, vanadium carbide, zirconium carbide, tungsten carbide, molybdenum carbide, manganese carbide, iron carbide, titanium carbide, and niobium carbide;

[0074] The dielectric ceramics, ferroelectric ceramics and piezoelectric ceramics respectively include BaTiO3, MgTiO3, CaTiO3, PbTiO3, SrTiO3, BaO·TiO2, BaO-Nd2O3-TiO2, LiNbO3, LiTaO3, Cd2Ta2O7, Pb2Nb2O7, Cd2Nb2O7, PbNb2O6, Sr 1-x Ba x Nb2O6、Ba2NaNb5O 15 One or more of;

[0075] Preferably, the organic polymer solid electrolyte is selected from one or more of polyethylene oxide, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polyvinylidene fluoride-chlorotrifluoroethylene, polyacrylonitrile, polymethyl methacrylate, polypropylene carbonate, polyphenylene sulfide, polyethyl cyanoacrylate, polypentylene succinate, polyvinyl chloride, polyvinylene carbonate, polyvinyl pyrrolidone, chitosan, polyimide, polyacrylate, polyurethane, aramid, polyetherimide, polyamide, polysulfone, aromatic sulfone, polyaromatic sulfone, polyether sulfone, epoxy resin and polyphenylene sulfone resin;

[0076] Preferably, the lithium salt is selected from one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium bis(trifluoromethanesulfonyl imide), lithium bis(fluorosulfonyl imide), and lithium difluorooxalatoborate.

[0077] According to the preparation method described above, the second solid electrolyte used in step S6 is selected from one or more of an inorganic solid electrolyte and an organic polymer solid electrolyte;

[0078] Preferably, the inorganic solid electrolyte is selected from one or more of an oxide solid electrolyte, a sulfide solid electrolyte, a halide solid electrolyte, a borate solid electrolyte, and a nitride solid electrolyte;

[0079] Preferably, the oxide solid electrolyte is selected from one or more of a garnet-type solid electrolyte, a perovskite-type solid electrolyte, a NASICON-type solid electrolyte and a LISICON-type solid electrolyte;

[0080] The garnet-type solid electrolyte includes Li x Ln3Z y A z O 12 and / or Li x La 3-y B y Zr z O 12 ; Wherein, A is one or more of Ta, Nb, Mg, Ti, Te, and W, and B is one or more of Ca, Rb, Al, and Ga;

[0081] The perovskite solid electrolyte includes Li 3.3 La 0.53 TiO3、Li 3x La 2 / 3-x TiO3 and Li x Sr y M z One or more of TaO3; wherein M is one or more of Zr and Nb;

[0082] The NASICON-type solid electrolyte includes Li x Al y M z (PO4)3、Li x Y y Zr z (PO4)3, LiTi2(PO4)3, LiGe2(PO4)3 and LiGeTi(PO4)3; wherein M is one or more of Ti, Ge, Hf, Zn, Zr and Si;

[0083] The LISICON type solid electrolyte includes Li 3+x (P 1-x Si x )O4 and / or Li 3+x Ge x V 1-x O4;

[0084] The sulfide solid electrolyte is selected from Argyrodite solid electrolyte LiPSMX, Thio-LiSICON solid electrolyte Li 4-x A 1-x B xS4 and one or more of glassy sulfides; wherein M is one or more of O, Cu, Zn, Bi, Sn, Al, Mn, Ce and In, X is one or more of F, Cl, Br and I; A is one or more of Si, Sn, Ge and Zr, and B is one or more of O, P, Al, Zn and Ga;

[0085] The glassy sulfide includes one or more of Li2S-P2S5, Li2S-GeS2, Li2S-SiS2, Li2S-SiS2-Li4SiO4, Li2S-B2S3, and Li2S-B2S3-LiI;

[0086] The halide solid electrolyte includes LiX, Li2MX 4、 Li3M′X6、Li x M″ y Ln z Cl 3、 LiM″′Cl5X″ and Li 3- y Zr y M″″ 1-y Cl6; wherein X is one or more of F, Cl, Br, I, M is one or more of Mg, Mn, Fe, Zn and Cd, M' is one or more of O, In, Y, Yb, Sc, Ho, Er, M "is one or more of Ta, Zr, Ca and Al, Ln is one or more of La, Ce, Pr, Nd, Sm, M "' is selected from one or more of La, Ta, Nb, X "is selected from O, Cl, F or OH, M " " is selected from one or more of Y, Er, Yb, Ho, Lu;

[0087] Among them, 0 <x<1,0<y<1,0<z<1;

[0088] The borate solid electrolyte is selected from one or more of Li2B4O7, Li2O-B2O3-P2O5;

[0089] The nitride solid electrolyte is selected from one or more of LiPON, Li3N, Li7PN4, and LiSi2N3;

[0090] The hydride solid electrolyte includes but is not limited to one or more of Li3AlH6, LiBH4, LiNH2, Li2NH, LiBH4-LiNH2, LiBH4-LiX; wherein X is one or more of Cl, Br and I;

[0091] The organic polymer solid electrolyte is selected from one or more of polyethylene oxide, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polyvinylidene fluoride-chlorotrifluoroethylene, polyacrylonitrile, polymethyl methacrylate, polypropylene carbonate, polyphenylene sulfide, polyethyl cyanoacrylate, polypentylene succinate, polyvinyl chloride, polyvinylene carbonate, polyvinyl pyrrolidone, chitosan, polyimide, polyacrylate, polyurethane, aramid, polyetherimide, polyamide, polysulfone, aromatic sulfone, polyaromatic sulfone, polyether sulfone, epoxy resin and polyphenylene sulfone resin;

[0092] Preferably, the perovskite-type oxide solid electrolyte is selected from lithium lanthanum titanium oxide;

[0093] The garnet-type oxide solid electrolyte is selected from one or more of lithium lanthanum zirconium oxide, niobium-doped lithium lanthanum zirconium oxide, tantalum-doped lithium lanthanum zirconium oxide, and niobium-tantalum dual-doped lithium lanthanum zirconium oxide;

[0094] The NASICON type oxide solid electrolyte is selected from one or more of lithium aluminum titanium phosphate, lithium yttrium titanium phosphate, and lithium aluminum germanium phosphate.

[0095] According to the preparation method described above, the slurry in step S2 further includes a binder;

[0096] Preferably, the slurry in step S6 further includes a lithium salt and / or a binder.

[0097] According to the preparation method described above, the binder is selected from one or more of polyvinylidene fluoride, polyvinyl alcohol, polytetrafluoroethylene, sodium hydroxymethyl cellulose, styrene-butadiene rubber, nitrile rubber, styrene-butadiene-styrene copolymer, polyacrylic acid, and lithium polyacrylate;

[0098] The lithium salt is selected from one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium bis(trifluoromethanesulfonyl imide), lithium bis(fluorosulfonyl imide), and lithium difluorooxalatoborate;

[0099] Preferably, the binder used in the slurry in step S2 and the binder used in the slurry in step S6 are the same as or different from each other.

[0100] The present invention also provides a solid-state battery, which includes the pole piece described above or the positive pole piece or negative pole piece obtained by the preparation method described above.

[0101] The present invention further provides a method for preparing a solid-state battery, which comprises: a step of preparing a positive electrode sheet or a negative electrode sheet by the preparation method described above.

[0102] According to the preparation method described above, it also includes the steps of rolling, drying, and then hot-pressing the positive electrode sheet and / or the negative electrode sheet for integration.

[0103] According to the preparation method described above, in the hot pressing integration, the hot pressing temperature is 50-85° C., the pressure is 0.2-0.9 MPa, and the hot pressing time is 20-40 minutes.

[0104] Effects of the Invention

[0105] The above technical solution of the present invention has the following beneficial effects:

[0106] 1. A mixed conductive layer including a nano-conductive agent and an organic polymer solid electrolyte is introduced on the surface of the positive electrode and the negative electrode. The nano-conductive agent can effectively increase the contact area between the positive electrode active material and the negative electrode active material, and the organic polymer solid electrolyte is combined with the ultrasonic spraying process to achieve interface softening, which can effectively reduce the interface impedance, increase the ion / electron transmission rate, further reduce the surface porosity of the electrode, and realize the preparation of ultra-thin and dense solid-state battery electrodes, thereby improving the electrochemical performance and safety of the battery;

[0107] 2. The present invention utilizes an ultrasonic spraying method to prepare the pole piece, which can fully disperse the slurry and prepare an ultra-thin coating containing a solid electrolyte on the surface of the pole piece, thereby improving the uniformity of the pole piece composite and the stability of the coating, and realizing a uniform layered structure with controllable thickness, thereby improving the structural stability of the solid-state battery, solving the solid-solid contact problem through pole piece composite, improving interface compatibility, and reducing the internal resistance of the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0108] Figure 1 This is a scanning electron microscope characterization of the composite solid-state battery electrode obtained in Example 1. DETAILED DESCRIPTION

[0109] The following describes the embodiments of the present invention, but the present invention is not limited thereto. The present invention is not limited to the various structures described below, and various changes can be made within the scope of the invention claim, and the embodiments obtained by appropriately combining different embodiments and appropriately combining the technical means disclosed in the embodiments are also included in the technical scope of the present invention. In addition, all the documents recorded in this specification are cited in this specification as references.

[0110] Unless defined otherwise, technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention belongs.

[0111] In this specification, the numerical range expressed using "a numerical value A to a numerical value B" means a range including the endpoints numerical values ​​A and B.

[0112] In this specification, unless otherwise specified, the word "multiple" in "multiple", "multiple", "plurality", etc. means a numerical value of 2 or more.

[0113] In the present specification, the term “substantially”, “substantially” or “essentially” means that the error is less than 5%, or less than 3%, or less than 1% compared with a relevant perfect standard or theoretical standard.

[0114] In this specification, unless otherwise specified, "%" means mass percentage.

[0115] In this specification, if "room temperature", "normal temperature" or the like appears, the temperature may generally be 10 to 37°C, or 15 to 35°C.

[0116] In this specification, the meanings of “may” or “can” include both existence and non-existence, and both performing a certain process and not performing a certain process.

[0117] In the present specification, “optionally”, “optionally” and “optionally” mean that the event or situation described below may or may not occur, and the description includes cases where the event occurs and cases where the event does not occur.

[0118] The term "comprising" and any variations thereof in the specification and claims of the present invention and the above drawings are intended to cover non-exclusive inclusions. For example, a process, method or system, product or device comprising a series of steps or units is not limited to the listed steps or units, but may optionally include steps or units not listed, or may optionally include other steps or units inherent to these processes, methods, products or devices.

[0119] In this specification, the references to "some / certain / preferred embodiments", "embodiments", etc., mean that the specific elements (e.g., features, structures, properties and / or characteristics) described in connection with the embodiments are included in at least one embodiment described herein, and may or may not exist in other embodiments. In addition, it should be understood that the elements may be combined in various embodiments in any suitable manner.

[0120] <First aspect>

[0121] A first aspect of the present invention relates to a pole piece, which includes a mixed conductive layer on a positive pole piece or a negative pole piece, wherein the mixed conductive layer includes a nano conductive agent and an organic polymer solid electrolyte.

[0122] In the present invention, a mixed conductive layer including a nano-conductive agent and an organic polymer solid electrolyte is introduced on the surface of the positive electrode sheet or the negative electrode sheet. The nano-conductive agent can effectively increase the contact area between the mixed conductive layer and the positive electrode sheet or the negative electrode sheet, and the organic polymer solid electrolyte in the mixed conductive layer can effectively reduce the interface impedance and improve the cycle stability of the solid-state battery.

[0123] In some preferred embodiments of the present invention, the mass ratio of the nano-conductive agent to the organic polymer solid electrolyte is (85-20): (15-80), preferably the mass ratio of the nano-conductive agent to the organic polymer solid electrolyte is (80-25): (20-75), for example, it can be 85:15, 80:20, 75:25, 70:30, 65:35, 60:40, 55:45, 50:50, 45:55, 40:60, 35:65, 30:70, 25:75, 20:80, etc. The mass ratio of the nano-conductive agent to the organic polymer solid electrolyte within the above range is conducive to improving the dispersibility of the conductive particles and the uniformity of the entire slurry during preparation, and can improve the close contact with the positive or negative electrode interface; if the proportion of the nano-conductive agent is too high, the particles are easily agglomerated, which is not conducive to dispersion and affects the uniformity of the mixed conductive layer prepared by ultrasonic spraying, affecting the cycle stability of the battery.

[0124] In some preferred embodiments of the present invention, the particle size of the nano-conductive agent may be 5-500 nm, preferably 10-300 nm, for example, 5 nm, 10 nm, 15 nm, 20 nm, 25 nm, 30 nm, 50 nm, 75 nm, 100 nm, 150 nm, 200 nm, 250 nm, 300 nm, 350 nm, 400 nm, 450 nm, 500 nm, etc. The nano-scale conductive agent can effectively increase the contact area with the positive electrode active material or the negative electrode active material, solve the problem of poor interface contact between the active material and the solid electrolyte, and reduce the interface impedance.

[0125] In the present invention, the nano-conductive agent used for the mixed conductive layer can be selected from one or more of conductive graphite, conductive carbon black, acetylene black, carbon nanotubes, Ketjen black, graphene, carbon molecular sieves, carbon nanofibers, polystyrene sulfonic acid, lithium polystyrene sulfonate and polyethylene dioxythiophene. In the present invention, the organic polymer solid electrolyte used for the mixed conductive layer can be selected from one or more of polyethylene oxide, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polyvinylidene fluoride-chlorotrifluoroethylene, polyacrylonitrile, polymethyl methacrylate, polypropylene carbonate, polyphenylene sulfide, polycyanoethyl acrylate, polypentylene succinate, polyvinyl chloride, polyvinylene carbonate, polyvinyl pyrrolidone, chitosan, polyimide, polyacrylate, polyurethane, aramid, polyetherimide, polyamide, polysulfone, aromatic sulfone, polyaromatic sulfone, polyether sulfone, epoxy resin and polyphenylene sulfone resin.

[0126] In some preferred embodiments of the present invention, the thickness of the mixed conductive layer may be 100nm-1000nm, preferably 150-800nm, for example, 100nm, 150nm, 200nm, 250nm, 300nm, 350nm, 400nm, 450nm, 500nm, 550nm, 600nm, 650nm, 700nm, 750nm, 800nm, 850nm, 900nm, 950nm, 1000nm, etc. The thickness of the mixed conductive layer within the above range can effectively increase the structural stability of the solid-state battery pole piece,

[0127] In some preferred embodiments of the present invention, the mixed conductive layer further comprises a binder. The present invention has no particular limitation on the binder, and those commonly used in the art can be used. For example, the binder can be selected from one or more of polyvinylidene fluoride, polyvinyl alcohol, polytetrafluoroethylene, sodium hydroxymethyl cellulose, styrene-butadiene rubber, nitrile rubber, styrene-butadiene-styrene copolymer, polyacrylic acid, and lithium polyacrylate.

[0128] There is no particular limitation on the content of the binder, and it can be adjusted according to actual needs. For example, it can be 1-10% by mass of the mixed conductive layer.

[0129] It should be noted that the mixed conductive layer of the present invention preferably does not contain an inorganic solid electrolyte, because the inorganic solid electrolyte has a large particle size, usually in the micron level, which may have an adverse effect on the electrode of the present invention.

[0130] In some preferred embodiments of the present invention, the pole piece further comprises a first composite solid electrolyte layer on the mixed conductive layer, wherein the first composite solid electrolyte layer comprises an inorganic ceramic material, an organic polymer solid electrolyte, and a lithium salt.

[0131] Introducing the first composite solid electrolyte layer on the mixed conductive layer can fill the interface gap in the solid-state battery, improve the interfacial contact between layers, reduce the interface impedance, increase the transmission rate of lithium ions between interfaces, prevent the occurrence of interface side reactions, and improve the cycle stability and thermal stability of the solid-state battery. In addition, by setting the first composite solid electrolyte layer, the solid-solid contact area can be increased to provide a transmission channel for lithium ions.

[0132] In some preferred embodiments of the present invention, the thickness of the first composite solid electrolyte layer is 200-3000nm, preferably the thickness of the first composite solid electrolyte layer is 250-2000nm, for example, it can be 200nm, 250nm, 300nm, 400nm, 500nm, 600nm, 700nm, 800nm, 900nm, 1000nm, 1500nm, 2000nm, 2500nm, 3000nm, etc. The thickness of the first composite solid electrolyte layer within the above range can effectively enhance the conduction of ions between interfaces and improve interface stability. Too high a thickness will increase the interface impedance and affect the rate performance of the battery.

[0133] In the present invention, the inorganic ceramic material used for the first composite solid electrolyte layer can be selected from one or more combinations of oxides, nitrides, borides, halides, carbides, dielectric ceramics, ferroelectric ceramics, piezoelectric ceramics, diatomaceous earth, mullite, montmorillonite and kaolin.

[0134] Specifically, the oxides include, but are not limited to, one or more combinations of silicon oxide, boron oxide, magnesium oxide, copper oxide, nickel oxide, calcium oxide, aluminum oxide, titanium oxide, zirconium oxide, vanadium oxide, lanthanum oxide, beryllium oxide, yttrium oxide, cerium oxide, and lead zirconium titanate;

[0135] The nitride includes but is not limited to one or more combinations of silicon nitride, titanium nitride, aluminum nitride, boron nitride, magnesium nitride, zirconium nitride and silicon oxynitride;

[0136] The carbide is selected from one or more of silicon carbide, boron carbide, tantalum carbide, vanadium carbide, zirconium carbide, tungsten carbide, molybdenum carbide, manganese carbide, iron carbide, titanium carbide and niobium carbide;

[0137] The dielectric ceramics, ferroelectric ceramics and piezoelectric ceramics respectively include BaTiO3, MgTiO3, CaTiO3, PbTiO3, SrTiO3, BaO·TiO2, BaO-Nd2O3-TiO2, LiNbO3, LiTaO3, Cd2Ta2O7, Pb2Nb2O7, Cd2Nb2O7, PbNb2O6, Sr 1-x Ba x Nb2O6、Ba2NaNb5O 15 One or more of;

[0138] The organic polymer solid electrolyte for the first composite solid electrolyte layer can be selected from one or more of polyethylene oxide, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polyvinylidene fluoride-chlorotrifluoroethylene, polyacrylonitrile, polymethyl methacrylate, polypropylene carbonate, polyphenylene sulfide, polycyanoethyl acrylate, polypentylene succinate, polyvinyl chloride, polyvinylene carbonate, polyvinyl pyrrolidone, chitosan, polyimide, polyacrylate, polyurethane, aramid, polyetherimide, polyamide, polysulfone, aromatic sulfone, polyaromatic sulfone, polyether sulfone, epoxy resin and polyphenylene sulfone resin. The lithium salt for the first composite solid electrolyte layer can be selected from one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium bistrifluoromethanesulfonyl imide (LiTFSI), lithium bisfluorosulfonyl imide and lithium difluoro oxalate borate.

[0139] In some preferred embodiments of the present invention, the pole piece further comprises a second solid electrolyte layer on the first composite solid electrolyte layer.

[0140] In some preferred embodiments of the present invention, the thickness of the second solid electrolyte layer is 2 μm-50 μm, preferably the thickness of the second solid electrolyte layer is 5 μm-40 μm, for example, 2 μm, 5 μm, 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm, etc. The thickness of the second solid electrolyte layer within the above range can improve the cycle stability of the solid-state battery and increase the safety of the battery. If the thickness is too low, it is easy to cause a short circuit, which is not conducive to improving the cycle stability of the battery.

[0141] In some preferred embodiments of the present invention, the second solid electrolyte used in the second solid electrolyte layer includes one or more of an inorganic solid electrolyte and an organic polymer solid electrolyte.

[0142] Specifically, the inorganic solid electrolyte may be selected from one or more of an oxide solid electrolyte, a sulfide solid electrolyte, a halide solid electrolyte, a borate solid electrolyte, a nitride solid electrolyte and a hydride solid electrolyte.

[0143] More specifically, the oxide solid electrolyte is selected from one or more of a garnet-type solid electrolyte, a perovskite-type solid electrolyte, a NASICON-type solid electrolyte, and a LISICON-type solid electrolyte;

[0144] Garnet-type solid electrolytes include Li x Ln3Z y A z O 12 and / or Li x La 3-y B y Zr z O12 ; Wherein, A is one or more of Ta, Nb, Mg, Ti, Te, and W, and B is one or more of Ca, Rb, Al, and Ga;

[0145] Perovskite solid electrolytes include Li 3.3 La 0.53 TiO3、Li 3x La 2 / 3-x TiO3 and Li x Sr y M z One or more of TaO3; wherein M is one or more of Zr and Nb;

[0146] NASICON-type solid electrolytes include Li x Al y M z (PO4)3、Li x Y y Zr z (PO4)3, LiTi2(PO4)3, LiGe2(PO4)3 and LiGeTi(PO4)3; wherein M is one or more of Ti, Ge, Hf, Zn, Zr and Si;

[0147] LISICON type solid electrolyte includes Li 3+x (P 1-x Si x )O4 and / or Li 3+x Ge x V 1-x O4;

[0148] The sulfide solid electrolyte is selected from Argyrodite-type solid electrolyte LiPSMX, Thio-LiSICON-type solid electrolyte Li 4-x A 1-x B x S4 and one or more of glassy sulfides; wherein M is one or more of O, Cu, Zn, Bi, Sn, Al, Mn, Ce and In, X is one or more of F, Cl, Br and I; A is one or more of Si, Sn, Ge and Zr, and B is one or more of O, P, Al, Zn and Ga;

[0149] The glassy sulfide includes one or more of Li2S–P2S5, Li2S–GeS2, Li2S-SiS2, Li2S-SiS2-Li4SiO4, Li2S-B2S3, Li2S-B2S3-LiI;

[0150] Halide solid electrolytes include LiX, Li2MX4、 Li3M′X6、Li x M″ y Ln z Cl 3、 LiM″′Cl5X″ and Li 3- y Zr y M″″ 1-y Cl6; wherein X is one or more of F, Cl, Br, I, M is one or more of Mg, Mn, Fe, Zn and Cd, M' is one or more of O, In, Y, Yb, Sc, Ho, Er, M "is one or more of Ta, Zr, Ca and Al, Ln is one or more of La, Ce, Pr, Nd, Sm, M "' is selected from one or more of La, Ta, Nb, X "is selected from O, Cl, F or OH, M " " is selected from one or more of Y, Er, Yb, Ho, Lu;

[0151] Among them, 0 <x<1,0<y<1,0<z<1;

[0152] The borate solid electrolyte is selected from one or more of Li2B4O7, Li2O-B2O3-P2O5;

[0153] The nitride solid electrolyte is selected from one or more of LiPON, Li3N, Li7PN4, and LiSi2N3;

[0154] The hydride solid electrolyte includes, but is not limited to, one or more of Li3AlH6, LiBH4, LiNH2, Li2NH, LiBH4-LiNH2, LiBH4-LiX; wherein X is one or more of Cl, Br and I;

[0155] Preferably, the perovskite oxide solid electrolyte is selected from lithium lanthanum titanium oxide;

[0156] The garnet-type oxide solid electrolyte is selected from one or more of lithium lanthanum zirconium oxide, niobium-doped lithium lanthanum zirconium oxide, tantalum-doped lithium lanthanum zirconium oxide, and niobium-tantalum dual-doped lithium lanthanum zirconium oxide;

[0157] The NASICON type oxide solid electrolyte is selected from one or more of lithium aluminum titanium phosphate, lithium yttrium titanium phosphate, and lithium aluminum germanium phosphate.

[0158] In the present invention, the organic polymer solid electrolyte can be selected from polyethylene oxide, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polyvinylidene fluoride-trifluorochloroethylene, polyacrylonitrile, polymethyl methacrylate, polypropylene carbonate, polyphenylene sulfide, polycyanoethyl acrylate, polypentanediol succinate, polyvinyl chloride, polyvinylene carbonate, polyvinyl pyrrolidone, chitosan, polyimide, polyacrylate, polyurethane, aramid, polyetherimide, polyamide, polysulfone, aromatic sulfone, polyaryl sulfone, polyether sulfone, epoxy resin and polyphenylene sulfone resin. In some preferred embodiments of the present invention, the second solid electrolyte layer also includes a lithium salt and / or a binder. In the present invention, there is no particular limitation on lithium salts and binders, and those commonly used in the art can be used. Examples of lithium salts may be the same as those listed above for the first composite solid electrolyte layer. Examples of binders may be the same as those listed above for the mixed conductive layer.

[0159] In a specific embodiment, the lithium salt optionally used in the second solid electrolyte layer can be the same as or different from the lithium salt used in the first composite solid electrolyte layer; the binder optionally used in the second solid electrolyte layer can be the same as or different from the binder optionally used in the mixed conductive layer.

[0160] The content of the lithium salt and the binder in the second solid electrolyte layer is not particularly limited and can be adjusted according to actual needs. For example, each of them can be 1-20% by mass of the mass of the second solid electrolyte layer.

[0161] <Second Aspect>

[0162] The second aspect of the present invention relates to a method for preparing the pole piece described in the first aspect, which comprises the following steps:

[0163] Step S2: spraying a conductive slurry containing a nano conductive agent and an organic polymer solid electrolyte onto the surface of the positive electrode sheet or the negative electrode sheet by ultrasonic spraying, and then optionally heating and curing to obtain a positive electrode sheet or a negative electrode sheet with a mixed conductive layer.

[0164] In some preferred embodiments of the present invention, the preparation method further comprises the following steps:

[0165] Step S4: spraying the slurry containing the inorganic ceramic material onto the surface of the mixed conductive layer obtained in step S2 by ultrasonic spraying, thereby obtaining a positive electrode sheet or a negative electrode sheet having the mixed conductive layer and the first composite solid electrolyte layer in sequence.

[0166] In some preferred embodiments of the present invention, the preparation method further comprises the following steps:

[0167] Step S6: spraying the second solid electrolyte slurry onto the surface of the first composite solid electrolyte layer obtained in step S4 by ultrasonic spraying, thereby obtaining a positive electrode sheet or a negative electrode sheet having a mixed conductive layer, a first composite solid electrolyte layer and a second solid electrolyte layer in sequence.

[0168] In addition, in some specific embodiments of the present invention, the preparation method may further include the following slurry preparation steps:

[0169] Step S1: homogenizing a composition containing a nano conductive agent and an organic polymer solid electrolyte in a solvent to prepare a conductive paste; and / or

[0170] Step S3: slurrying the composition containing the inorganic ceramic material in a solvent to prepare a slurry containing the inorganic ceramic material; and / or

[0171] Step S5: slurrying the composition containing the second solid electrolyte in a solvent to prepare a second solid electrolyte slurry.

[0172] In some preferred embodiments, the preparation method of the present invention may further include step Sx: hot pressing the finally prepared positive electrode sheet or negative electrode sheet.

[0173] In the present invention, there is no particular limitation on the method for preparing the positive electrode sheet or the negative electrode sheet before spraying the conductive slurry, and the positive electrode sheet or the negative electrode sheet may be prepared by a common method in the art such as a conventional coating method, an electrostatic spraying method, etc.

[0174] There is no particular limitation on the positive electrode active material or negative electrode active material used for the positive electrode sheet or negative electrode sheet, and those commonly used in the art can be used. Preferably, the positive electrode active material of the present invention includes but is not limited to one or more combinations of nickel-cobalt-manganese ternary materials, nickel-cobalt-aluminum ternary materials, lithium iron phosphate, lithium cobalt oxide, lithium manganese oxide, and lithium vanadium phosphate.

[0175] Preferably, the negative electrode active material described in the present invention includes but is not limited to one or more of graphite, graphene, carbon nanotubes, silicon-based alloys, silicon-oxygen negative electrodes, silicon-carbon negative electrodes, lithium metal negative electrodes, lithium alloy negative electrodes, lithium titanium oxides, transition metal oxides and transition metal sulfides.

[0176] Each step is described in detail below.

[0177] Step S1

[0178] In step S1 , a composition containing a nano-conductive agent and an organic polymer solid electrolyte is slurried in a solvent to prepare a conductive paste.

[0179] Examples of the nano-conductive agent and the organic polymer solid electrolyte used in step S1 are the same as those listed in the above <First Aspect>, and are not described in detail here.

[0180] In the present invention, the solid content of the conductive paste may be 5 to 40% by mass, for example, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40% by mass, etc.

[0181] In the conductive slurry of step S1, the mass ratio of the nano-conductive agent to the organic polymer solid electrolyte is (85-20): (15-80), preferably (80-25): (20-75), for example, it can be 85:15, 80:20, 75:25, 70:30, 65:35, 60:40, 55:45, 50:50, 45:55, 40:60, 35:65, 30:70, 25:75, 20:80, etc. The mass ratio of the nano-conductive agent to the organic polymer solid electrolyte within the above range is conducive to improving the dispersibility of the conductive particles and the uniformity of the slurry as a whole during preparation, and can improve the close contact with the positive electrode interface; if the proportion of the nano-conductive agent is too high, the particles will agglomerate, which is not conducive to dispersion and affects the uniformity of the mixed conductive layer prepared by ultrasonic spraying, affecting the cycle stability of the battery.

[0182] In step S1, the organic solvent used for homogenization can be selected from one or more of N-methylpyrrolidone (NMP), dimethylformamide (DMF), dimethylacetamide, butyrate, toluene, xylene, anisole, hexane, heptane, dibromomethane, dichloroethane, ethanol and glycol ether.

[0183] In some preferred embodiments, the composition containing the nano-conductive agent and the organic polymer solid electrolyte in step S1 further comprises a binder, and examples of the binder are the same as those listed in the above <First Aspect>.

[0184] Step S2

[0185] In step S2, the conductive slurry prepared in step S1 is sprayed onto the surface of the positive electrode sheet or the negative electrode sheet by ultrasonic spraying, and then optionally heated and cured to obtain a positive electrode sheet or a negative electrode sheet having a mixed conductive layer.

[0186] In the present invention, in the ultrasonic spraying of step S2, the spraying conditions are as follows:

[0187] The ultrasonic power is 10-100W, for example, 10W, 20W, 30W, 40W, 50W, 60W, 70W, 80W, 90W, 100W, etc.;

[0188] The ultrasonic frequency is 20-200kHz, for example, 20kHz, 30kHz, 40kHz, 50kHz, 80kHz, 100kHz, 120kHz, 150kHz, 200kHz, etc.;

[0189] The continuous spraying rate is 0-3000ml / h (greater than 0ml / h and less than 3000ml / h), preferably 100-1700ml / h, more preferably 200-1200ml / h, for example, 10ml / h, 50ml / h, 100ml / h, 200ml / h, 300ml / h, 400ml / h, 500ml / h, 600ml / h, 800ml / h, 1000ml / h, 1100ml / h, 1200ml / h, 1300ml / h, 1400ml / h, 1500ml / h, 1600ml / h, 1700ml / h, 1800ml / h, 1900ml / h, 2000ml / h, 2100ml / h, 2200ml / h, 2300ml / h, 2400ml / h, 2500ml / h, 2600ml / h, 2700ml / h, 2800ml / h, 2900ml / h, 3000ml / h, 3100ml / h, 3100ml / h, 3200ml / h, 3300ml / h, 3500ml / h, 3600ml / h, 3700ml / h, 3800ml / h, 3900ml / h, 4000ml / h When the spraying amount is within the above range, the slurry particles can be refined and the slurry can be evenly sprayed on the surface of the battery pole piece, which is beneficial to control the thickness of the obtained solid electrolyte layer, achieve close contact between the layers, avoid the problem of electrolyte particles agglomerating due to too fast spraying speed, causing clogging of equipment and waste of slurry, and improve the efficiency of preparing solid-state battery pole pieces;

[0190] The spraying distance is 10-100 mm, for example, it can be 10 mm, 20 mm, 30 mm, 40 mm, 50 mm, 60 mm, 70 mm, 80 mm, 90 mm, 100 mm, etc.;

[0191] The air guide pressure is 0.1-0.3 MPa, for example, 0.1 MPa, 0.15 MPa, 0.2 MPa, 0.25 MPa, 0.3 MPa, etc., so as to prevent material splashing;

[0192] The spray width is 50 to 400 mm, for example, 50 mm, 80 mm, 100 mm, 150 mm, 200 mm, 250 mm, 300 mm, 350 mm, 400 mm, etc.

[0193] The spraying distance is 20 to 100 mm, for example, 20 mm, 30 mm, 40 mm, 50 mm, 60 mm, 70 mm, 80 mm, 90 mm, 100 mm, etc.;

[0194] The spraying angle is 85-90°, for example, 85°, 86°, 87°, 88°, 89°, 90°, etc.;

[0195] In some preferred embodiments of the present invention, the positive electrode sheet or the negative electrode sheet may be heated during spraying. The heating temperature may be 30-80°C, for example, 30°C, 40°C, 50°C, 60°C, 70°C, 80°C, etc. By heating the electrode sheet, the slurry can be evenly distributed on the surface of the electrode sheet, reducing particle agglomeration during the mixing process and improving the cycle stability of the battery.

[0196] In some specific embodiments, after spraying, heating and curing may be performed. Preferably, heating and curing is performed so that the interface between the mixed conductive layer and the pole piece is more stable, which is beneficial to reduce the interface impedance. The heating and curing temperature is 70 to 120°C, for example, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, etc.

[0197] In some embodiments, the positive electrode sheet or the negative electrode sheet is placed on a work plate during spraying. Thus, the heating of the positive electrode sheet or the negative electrode sheet and the drying after spraying can be achieved through the work plate, thereby reducing the process flow and achieving mass production.

[0198] In some specific embodiments, when spraying the slurry, the positive electrode sheet or the negative electrode sheet is placed on a working plate, then heated and the spraying conditions are set, the slurry is sprayed onto the surface of the sheet to a desired thickness, the static coating equipment is turned off after standing for a period of time, and then dried and naturally cooled, thereby obtaining a positive electrode sheet or a negative electrode sheet with a mixed conductive layer.

[0199] In some embodiments, during the standing period, the temperature of the working plate may be raised to a temperature slightly higher than the heating temperature during spraying, for example, 10 to 30° C. higher. The standing period may be, for example, 20 to 120 minutes.

[0200] Step S3

[0201] In some preferred embodiments of the present invention, the method for preparing a pole piece may further include step S3: slurrying the composition containing the inorganic ceramic material in a solvent to prepare a slurry containing the inorganic ceramic material.

[0202] In the present invention, the composition containing the inorganic ceramic material further comprises an organic polymer solid electrolyte and a lithium salt.

[0203] Examples of the inorganic ceramic material, organic polymer solid electrolyte and lithium salt used in step S3 are the same as those listed in the above <First Aspect>, and will not be repeated here.

[0204] In the present invention, the solid content of the slurry containing the inorganic ceramic material may be 5 to 30% by mass, for example, 5%, 10%, 15%, 20%, 25%, 30% by mass, etc.

[0205] In step S3, examples of the organic solvent used in the homogenization are the same as those in step S1 above. In a specific embodiment, the organic solvent used in step S3 may be the same as or different from that in step S1.

[0206] Step S4

[0207] In step S4, the slurry containing the inorganic ceramic material prepared in step S3 is sprayed onto the surface of the mixed conductive layer obtained in step S2 by ultrasonic spraying, thereby obtaining a positive electrode sheet or a negative electrode sheet having a mixed conductive layer and a first composite solid electrolyte layer in sequence.

[0208] The range of each condition of ultrasonic spraying in step S4 is the same as that in step S2 above, and will not be repeated here. In a specific embodiment, the conditions of ultrasonic spraying adopted in step S4 may be the same as or different from those in step S2.

[0209] Step S5

[0210] In some preferred embodiments of the present invention, the method for preparing a pole piece may further include step S5: slurrying the composition containing the second solid electrolyte in a solvent to prepare a second solid electrolyte slurry.

[0211] In the present invention, there is no particular limitation on the second solid electrolyte, and those commonly used in the art can be used.

[0212] In some embodiments of the present invention, the second solid electrolyte may be selected from one or more of an inorganic solid electrolyte and an organic polymer solid electrolyte. Examples of the inorganic solid electrolyte and the organic polymer solid electrolyte are the same as those listed in the above <First Aspect>.

[0213] In step S5, examples of the organic solvent used in homogenization are the same as those in step S1. In a specific embodiment, the organic solvent used in step S5 may be the same as or different from those in step S1 and step S3.

[0214] In the present invention, the solid content of the second solid electrolyte slurry may be 5 to 40% by mass, for example, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40% by mass, etc.

[0215] In some preferred embodiments, the composition containing the second solid electrolyte in step S5 further contains a lithium salt and / or a binder.

[0216] There is no particular limitation on the lithium salt, and those commonly used in the art can be used. In some embodiments of the present invention, the lithium salt can be selected from one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium bis(trifluoromethanesulfonyl imide), lithium bis(fluorosulfonyl imide) and lithium difluorooxalate borate. Examples of the binder are the same as those listed in <First Aspect> above, and in a specific embodiment, the binder used in step S5 can be the same or different from that in step S1.

[0217] Step S6

[0218] In step S6, the second solid electrolyte slurry prepared in step S5 is sprayed onto the surface of the first composite solid electrolyte layer obtained in step S4 by ultrasonic spraying, thereby obtaining a positive electrode sheet or a negative electrode sheet having a mixed conductive layer, a first composite solid electrolyte layer and a second solid electrolyte layer in sequence.

[0219] The range of each condition of ultrasonic spraying in step S6 is the same as that in step S2, and will not be repeated here. In a specific embodiment, the conditions of ultrasonic spraying adopted in step S6 may be the same as or different from those in step S2 and step S4.

[0220] In the preparation method of the present invention, a mixed conductive layer is introduced on the surface of the positive electrode active material and the negative electrode active material by ultrasonic spraying, so that the interface contact between the active material and the solid electrolyte is increased and the interface impedance is reduced. In addition, a multi-layer solid electrolyte layer can be introduced on the positive electrode plate or the negative electrode plate by ultrasonic spraying, thereby preparing a plate with uniform coating thickness and uniform and stable interlayer structure, and can effectively increase the structural stability of the solid-state battery plate and improve the cycle stability of the solid-state battery.

[0221] Step Sx

[0222] In some preferred embodiments, the preparation method of the present invention may further include step Sx: hot pressing the finally prepared positive electrode sheet or negative electrode sheet.

[0223] In the hot pressing of the present invention, the hot pressing temperature is 40 to 60°C, for example, 40°C, 45°C, 50°C, 55°C, 60°C, etc., the pressure can be 0.1 to 0.5 MPa, for example, 0.1 MPa, 0.2 MPa, 0.3 MPa, 0.4 MPa, 0.5 MPa, etc., and the hot pressing time can be 5 to 20 minutes, for example, 5 minutes, 10 minutes, 15 minutes, 20 minutes, etc.

[0224] During the hot pressing process, the interface contact between the positive electrode sheet or the negative electrode sheet, the mixed conductive layer, and the optional first composite solid electrolyte layer and the second solid electrolyte layer is increased, the crystallization area of ​​the polymer is reduced, ion transport behavior is induced and a new ion transport interface is formed, the electrochemical stability window of the solid electrolyte is improved, the ionic conductivity between the multilayer structure is improved, and the compatibility of the electrode and the solid electrolyte interface is increased.

[0225] <Third Aspect>

[0226] The third aspect of the present invention relates to a solid-state battery, which includes the pole piece in the above <first aspect> or the pole piece obtained by the preparation method described in the above <second aspect>.

[0227] <Fourth Aspect>

[0228] The fourth aspect of the present invention relates to a method for preparing a solid-state battery, comprising: the steps of preparing a positive electrode sheet and / or a negative electrode sheet by the preparation method described in the above <Second Aspect>; and

[0229] The steps of rolling and drying the positive electrode sheets and / or negative electrode sheets and then hot pressing them for integration.

[0230] The "hot pressing integration" here refers to integrating the positive and negative electrode sheets by hot pressing. The "hot pressing" in the above step Sx refers to hot pressing the positive electrode sheet or hot pressing the negative electrode sheet.

[0231] In the hot pressing integration of the present invention, the hot pressing temperature is 50-85°C, for example, it can be 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, etc., the pressure can be 0.2-0.9Mpa, for example, it can be 0.2MPa, 0.3MPa, 0.4MPa, 0.5MPa, 0.6MPa, 0.7MPa, 0.8MPa, 0.9MPa, etc., and the hot pressing time can be 20-40 minutes, for example, it can be 20 minutes, 25 minutes, 30 minutes, 35 minutes, 40 minutes, etc.

[0232] Example

[0233] The present invention will be described in detail below by way of examples. The examples of the embodiments are intended to explain the present invention and should not be construed as limiting the present invention. If no specific techniques or conditions are specified in the embodiments, the techniques or conditions described in the literature in this area or the product instructions are used. If no manufacturer is specified for the reagents or instruments used, they are all conventional products that can be obtained commercially.

[0234] Example 1

[0235] The present invention provides a pole piece and a preparation method thereof, and a solid-state battery and a preparation method thereof. Ultrathin mixed conductive layers are introduced on the surface of positive electrode active material and negative electrode active material by ultrasonic spraying, thereby increasing the interface contact between active material and solid electrolyte, reducing interface impedance, and introducing multiple layers of solid electrolyte layer on the positive electrode piece or negative electrode piece to improve the cycle stability of solid-state battery. The specific steps are as follows:

[0236] (1) Mix nano-conductive carbon black (particle size 200 nm) and polyimide at a mass percentage of 70%:

[0237] 30% of the mixture was mixed evenly, dissolved in DMF solvent and stirred thoroughly, and a binder, polyvinylidene fluoride, was added to prepare a slurry with a solid content of 35% by mass;

[0238] (2) In the lithium iron phosphate positive electrode sheet (positive electrode active material lithium iron phosphate (LiFePO4), conductive carbon black (SP), adhesive polyvinylidene fluoride (PVDF) are dispersed in the solvent N-methylpyrrolidone (NMP) and mixed evenly to obtain a positive electrode slurry, wherein the mass ratio of lithium iron phosphate, PVDF and conductive carbon black is 94:3:3, and the positive electrode slurry is coated on aluminum foil, and after drying and rolling, a positive electrode sheet is obtained, and the same applies below.) The above slurry is introduced into the surface and gaps of the positive active material by ultrasonic spraying, wherein the ultrasonic power is 40W, the ultrasonic frequency is controlled at 100kHz, the spray width is 50mm, the spray angle is 88°, the continuous spraying amount is controlled at 500ml / h, the spraying distance is 35mm, and the air pressure is controlled at 0.2MPa to obtain a mixed conductive layer with a thickness of 1μm, and heated and cured at 60°C for 1 hour;

[0239] (3) Boron nitride, polyvinylidene fluoride, and LiTFSI were dissolved in a DMF solvent in a mass ratio of 5:3:2 and stirred thoroughly to prepare a slurry with a solid content of 55 mass%, and the slurry was sprayed on the surface of the mixed conductive layer by ultrasonic spraying, wherein the ultrasonic power was 40 W, the ultrasonic frequency was controlled at 80 kHz, the spray width was 50 mm, the spray angle was 88°, the continuous spraying amount was controlled at 500 ml / h, the spraying distance was 35 mm, and the gas pressure was controlled at 0.1 MPa to obtain a first composite solid electrolyte layer with a thickness of 2 μm;

[0240] (4) Tantalum-doped lithium lanthanum zirconium oxide, polypentanediol succinate, and LiTFSI were mixed and stirred in DMF at a mass ratio of 7:2:1 to prepare a slurry with a solid content of 40% by mass, and the slurry was sprayed on the surface of the first composite solid electrolyte layer by ultrasonic spraying, wherein the ultrasonic frequency was controlled at 90kHz, the continuous spraying amount was controlled at 800ml / h, the spraying distance was 35mm, and the air pressure was controlled at 0.2MPa to obtain a composite electrode containing a second solid electrolyte, the thickness of the second solid electrolyte layer was 30μm, and the slurry was heated and cured at 60°C for 1 hour;

[0241] (5) The composite battery positive electrode sheet and the lithium metal negative electrode stack obtained in the above steps are assembled into a solid-state battery by hot pressing at a temperature of 65° C. and a pressure of 0.4 MPa.

[0242] Example 2

[0243] This embodiment provides a pole piece and a method for preparing the same, and a solid-state battery and a method for preparing the same. A multi-layer solid electrolyte is introduced on the pole piece by ultrasonic spraying. The specific steps are as follows:

[0244] (1) Mix nano-conductive carbon black (particle size 200 nm) and PVDF-HFP at a mass percentage of 60%:

[0245] 40% of the mixture was mixed evenly, dissolved in DMF solvent and stirred thoroughly, and a binder, polyvinylidene fluoride, was added to prepare a slurry with a solid content of 35% by mass;

[0246] (2) The slurry is introduced onto the surface and gap of the positive active material by ultrasonic spraying on the surface of the lithium iron phosphate positive electrode sheet, wherein the ultrasonic power is 60W and the ultrasonic frequency is controlled at 110

[0247] kHz, spray width 50mm, spray angle 88°, continuous spraying volume controlled at 500ml / h, spraying distance 30mm, air guide pressure controlled at 0.2MPa, a mixed conductive layer with a thickness of 1μm was obtained, and heated and cured at 60℃ for 1 hour;

[0248] (3) dissolving boron oxide, polyvinylidene fluoride, and LiTFSI in a DMF solvent at a mass ratio of 3:5:2 and stirring the mixture to prepare a slurry with a solid content of 60% by mass, and spraying the slurry on the surface of the mixed conductive layer by ultrasonic spraying, wherein the ultrasonic frequency is controlled at 80 kHz, the continuous spraying amount is controlled at 500 ml / h, the spraying distance is 35 mm, and the gas pressure is controlled at 0.1 MPa to obtain a first composite solid electrolyte layer with a thickness of 2 μm;

[0249] (4) Tantalum-doped lithium lanthanum zirconium oxide, polypentanediol succinate, and LiTFSI were mixed and stirred in DMF at a mass ratio of 7:2:1 to prepare a slurry with a solid content of 40% by mass, and the slurry was sprayed on the surface of the first composite solid electrolyte layer by ultrasonic spraying, wherein the ultrasonic power was 60W, the ultrasonic frequency was controlled at 80kHz, the spray width was 50mm, the spray angle was 90°, the continuous spraying amount was controlled at 800ml / h, the spraying distance was 35mm, and the air guide pressure was controlled at 0.2MPa to obtain a composite electrode containing a second solid electrolyte, the thickness of the second solid electrolyte layer was 30μm, and the slurry was heated and cured at 60°C for 1 hour;

[0250] (5) The composite battery positive electrode sheet and the lithium metal negative electrode stack obtained in the above steps are assembled into a solid-state battery by hot pressing at a temperature of 65° C. and a pressure of 0.4 MPa.

[0251] Example 3

[0252] This embodiment provides a pole piece and a method for preparing the same, and a solid-state battery and a method for preparing the same. A multi-layer solid electrolyte is introduced on the pole piece by ultrasonic spraying. The specific steps are as follows:

[0253] (1) carbon nanotubes (particle size 100 nm) and polyimide were uniformly mixed in a ratio of 60%:40% by mass, dissolved in DMF solvent and stirred thoroughly, and a binder polyvinylidene fluoride was added to prepare a slurry with a solid content of 35% by mass;

[0254] (2) The slurry is introduced onto the surface and gap of the positive active material by ultrasonic spraying on the surface of the lithium iron phosphate positive electrode sheet, wherein the ultrasonic power is 60W and the ultrasonic frequency is controlled at 110

[0255] kHz, spray width 50mm, spray angle 88°, continuous spraying volume controlled at 500ml / h, spraying distance 30mm, air guide pressure controlled at 0.2MPa, a mixed conductive layer with a thickness of 1μm was obtained, and heated and cured at 60℃ for 1 hour;

[0256] (3) dissolving boron oxide, polyvinylidene fluoride, and LiTFSI in a DMF solvent at a mass ratio of 5:3:2 and stirring the mixture to prepare a slurry with a solid content of 50% by mass, and spraying the slurry on the surface of the mixed conductive layer by ultrasonic spraying, wherein the ultrasonic power is 60 W, the ultrasonic frequency is controlled at 80 kHz, the spray width is 50 mm, the spray angle is 90°, the continuous spraying amount is controlled at 500 ml / h, the spraying distance is 35 mm, and the gas pressure is controlled at 0.1 MPa to obtain a first composite solid electrolyte layer with a thickness of 2 μm;

[0257] (4) Tantalum-doped lithium lanthanum zirconium oxide, polypentanediol succinate, and LiTFSI were mixed and stirred in DMF at a mass ratio of 7:2:1 to prepare a slurry with a solid content of 40% by mass, and the slurry was sprayed on the surface of the first composite solid electrolyte layer by ultrasonic spraying, wherein the ultrasonic frequency was controlled at 90kHz, the continuous spraying amount was controlled at 800ml / h, the spraying distance was 35mm, and the air pressure was controlled at 0.2MPa to obtain a composite electrode containing a second solid electrolyte, the thickness of the second solid electrolyte layer was 30μm, and the slurry was heated and cured at 60°C for 1 hour;

[0258] (5) The composite battery positive electrode sheet and the lithium metal negative electrode stack obtained in the above steps are assembled into a solid-state battery by hot pressing at a temperature of 65° C. and a pressure of 0.4 MPa.

[0259] Example 4

[0260] This embodiment provides a pole piece and a method for preparing the same, and a solid-state battery and a method for preparing the same. A multi-layer solid electrolyte is introduced on the pole piece by ultrasonic spraying. The specific steps are as follows:

[0261] (1) carbon nanotubes (particle size 100 nm) and PVDF-HFP were uniformly mixed in a ratio of 65%:35% by mass, dissolved in DMF solvent and stirred thoroughly, and a binder polyvinylidene fluoride was added to prepare a slurry with a solid content of 35% by mass;

[0262] (2) The slurry is introduced onto the surface and gap of the positive active material by ultrasonic spraying on the surface of the lithium iron phosphate positive electrode sheet, wherein the ultrasonic power is 70W and the ultrasonic frequency is controlled at 110

[0263] kHz, spray width 50mm, spray angle 88°, continuous spraying volume controlled at 500ml / h, spraying distance 30mm, air guide pressure controlled at 0.2MPa, a mixed conductive layer with a thickness of 1μm was obtained, and heated and cured at 60℃ for 1 hour;

[0264] (3) dissolving boron oxide, polyvinylidene fluoride, and LiTFSI in a DMF solvent in a mass ratio of 5:3:2 and stirring the mixture to prepare a slurry with a solid content of 40% by mass, and spraying the slurry on the surface of the mixed conductive layer by ultrasonic spraying, wherein the ultrasonic power is 60 W, the ultrasonic frequency is controlled at 80 kHz, the spray width is 50 mm, the spray angle is 90°, the continuous spraying amount is controlled at 500 ml / h, the spraying distance is 35 mm, and the gas pressure is controlled at 0.1 MPa to obtain a first composite solid electrolyte layer with a thickness of 2 μm;

[0265] (4) Tantalum-doped lithium lanthanum zirconium oxide, polypentanediol succinate, and LiTFSI were mixed and stirred in DMF at a mass ratio of 7:2:1 to prepare a slurry with a solid content of 40% by mass, and the slurry was sprayed on the surface of the first composite solid electrolyte layer by ultrasonic spraying, wherein the ultrasonic frequency was controlled at 90kHz, the continuous spraying amount was controlled at 800ml / h, the spraying distance was 35mm, and the air pressure was controlled at 0.2MPa to obtain a composite electrode containing a second solid electrolyte, the thickness of the second solid electrolyte layer was 30μm, and the slurry was heated and cured at 60°C for 1 hour;

[0266] (5) The composite battery positive electrode sheet and the lithium metal negative electrode stack obtained in the above steps are assembled into a solid-state battery by hot pressing at a temperature of 65° C. and a pressure of 0.4 MPa.

[0267] Example 5

[0268] This embodiment provides a pole piece and a method for preparing the same, and a solid-state battery and a method for preparing the same. A multi-layer solid electrolyte is introduced on the pole piece by ultrasonic spraying. The specific steps are as follows:

[0269] (1) carbon nanotubes (particle size 100 nm) and PVDF-HFP were uniformly mixed in a ratio of 65%:35% by mass, dissolved in DMF solvent and stirred thoroughly, and a binder polyvinylidene fluoride was added to prepare a slurry with a solid content of 35% by mass;

[0270] (2) The slurry was introduced onto the surface and gap of the positive active material by ultrasonic spraying on the surface of the NCM622 (C-96500) positive electrode sheet, wherein the ultrasonic power was 30 W, the ultrasonic frequency was controlled at 110 kHz, the spray width was 50 mm, the spray angle was 87°, and the continuous spraying amount was controlled at 500

[0271] ml / h, the spraying distance was 30 mm, the air pressure was controlled at 0.2 MPa, and a mixed conductive layer with a thickness of 1 μm was obtained, which was heated and cured at 60 °C for 1 hour;

[0272] (3) dissolving boron oxide, polyvinylidene fluoride, and LiTFSI in a DMF solvent in a mass ratio of 3:5:2 and stirring the mixture to prepare a slurry with a solid content of 45 mass%, and spraying the slurry on the surface of the mixed conductive layer by ultrasonic spraying, wherein the ultrasonic power is 60 W, the ultrasonic frequency is controlled at 80 kHz, the spray width is 50 mm, the spray angle is 90°, the continuous spraying amount is controlled at 500 ml / h, the spraying distance is 35 mm, and the gas pressure is controlled at 0.1 MPa to obtain a first composite solid electrolyte layer with a thickness of 2 μm;

[0273] (4) Li7La3Zr2O 12The solid electrolyte, polypentane succinate, and LiTFSI were mixed and stirred in DMF at a mass ratio of 7:2:1 to prepare a slurry with a solid content of 40% by mass, which was sprayed on the surface of the first composite solid electrolyte layer by ultrasonic spraying, wherein the ultrasonic frequency was controlled at 90 kHz, the continuous spraying amount was controlled at 800 ml / h, and the spraying distance was 35

[0274] mm, the gas pressure is controlled at 0.2 MPa, and a composite electrode containing a second solid electrolyte is obtained. The thickness of the second solid electrolyte layer is 30 μm, and it is heated and cured at 60°C for 1 hour;

[0275] (5) The composite battery positive electrode sheet and the lithium metal negative electrode stack obtained in the above steps are assembled into a solid-state battery by hot pressing at a temperature of 65° C. and a pressure of 0.4 MPa.

[0276] Example 6

[0277] This embodiment provides a pole piece and a method for preparing the same, and a solid-state battery and a method for preparing the same. A multi-layer solid electrolyte is introduced on the pole piece by ultrasonic spraying. The specific steps are as follows:

[0278] (1) Mix nano-conductive carbon black (particle size 200 nm) and PVDF-HFP at a mass percentage of 55%:

[0279] 45% ratio is mixed evenly, dissolved in DMF solvent and stirred thoroughly, and a binder polyvinylidene fluoride is added to prepare a slurry with a solid content of 35% by mass;

[0280] (2) The slurry was introduced onto the surface and gap of the positive active material by ultrasonic spraying on the surface of the NCM622 (C-96500) positive electrode sheet, wherein the ultrasonic power was 60 W, the ultrasonic frequency was controlled at 110 kHz, the spray width was 50 mm, the spray angle was 87°, and the continuous spraying amount was controlled at 500

[0281] ml / h, the spraying distance was 30 mm, the air pressure was controlled at 0.2 MPa, and a mixed conductive layer with a thickness of 1 μm was obtained, which was heated and cured at 60 °C for 1 hour;

[0282] (3) dissolving boron oxide, polyvinylidene fluoride, and LiTFSI in a DMF solvent at a mass ratio of 3:5:2 and stirring the mixture to prepare a slurry with a solid content of 50 mass%, and spraying the slurry on the surface of the mixed conductive layer by ultrasonic spraying, wherein the ultrasonic power is 50 W, the ultrasonic frequency is controlled at 80 kHz, the spray width is 50 mm, the spray angle is 90°, the continuous spraying amount is controlled at 500 ml / h, the spraying distance is 35 mm, and the gas pressure is controlled at 0.1 MPa to obtain a first composite solid electrolyte layer with a thickness of 2 μm;

[0283] (4) Li7La3Zr2O 12 The solid electrolyte, polypentane succinate, and LiTFSI were mixed and stirred in DMF at a mass ratio of 7:2:1 to prepare a slurry with a solid content of 40% by mass, which was sprayed on the surface of the first composite solid electrolyte layer by ultrasonic spraying, wherein the ultrasonic frequency was controlled at 90 kHz, the continuous spraying amount was controlled at 800 ml / h, and the spraying distance was 35

[0284] mm, the gas pressure is controlled at 0.2 MPa, and a composite electrode containing a second solid electrolyte is obtained. The thickness of the second solid electrolyte layer is 30 μm, and it is heated and cured at 60°C for 1 hour;

[0285] (5) The composite battery positive electrode sheet and the lithium metal negative electrode stack obtained in the above steps are assembled into a solid-state battery by hot pressing at a temperature of 65° C. and a pressure of 0.4 MPa.

[0286] Example 7

[0287] This embodiment provides a pole piece and a method for preparing the same, and a solid-state battery and a method for preparing the same. A multi-layer solid electrolyte is introduced on the pole piece by ultrasonic spraying. The specific steps are as follows:

[0288] (1) Mix nano-conductive carbon black (particle size 200 nm) and styrene-butadiene rubber in a ratio of 85% by mass:

[0289] 15% ratio is mixed evenly, dissolved in DMF solvent and stirred thoroughly, and sodium hydroxymethyl cellulose is added to prepare a slurry with a solid content of 40% by mass;

[0290] (2) The slurry was introduced onto the surface and gap of the negative electrode active material by ultrasonic spraying on the surface of the silicon-carbon negative electrode plate, wherein the ultrasonic power was 60 W, the ultrasonic frequency was controlled at 60 kHz, the spray width was 50 mm, the spray angle was 90°, the continuous spraying amount was controlled at 700 ml / h, the spraying distance was 20 mm, and the air pressure was controlled at 0.2 MPa to obtain a mixed conductive layer with a thickness of 1 μm, and heated and cured at 60° C. for 1 hour;

[0291] (3) Boron nitride, styrene-butadiene rubber, and LiTFSI were dissolved in DMF solvent in a mass ratio of 3:5:2 and stirred thoroughly to prepare a slurry with a solid content of 50 mass%, which was sprayed on the surface of the mixed conductive layer by ultrasonic spraying, wherein the ultrasonic power was 30 W, the ultrasonic frequency was controlled at 80 kHz, the spray width was 50 mm, the spray angle was 90°, and the continuous spraying amount was controlled at 700

[0292] ml / h, the spraying distance was 20 mm, and the gas pressure was controlled at 0.1 MPa to obtain the first composite solid electrolyte layer with a thickness of 2 μm;

[0293] (4) Li7La3Zr2O 12 The solid electrolyte, styrene-butadiene rubber and LiTFSI are mixed and stirred in DMF in a mass ratio of 7:2:1 to prepare a slurry with a solid content of 40% by mass, which is sprayed on the surface of the first composite solid electrolyte layer by ultrasonic spraying, wherein the ultrasonic frequency is controlled at 90kHz, the continuous spraying amount is controlled at 800ml / h, the spraying distance is 35mm, and the air pressure is controlled at 0.2MPa to obtain a composite electrode containing a second solid electrolyte, the thickness of the second solid electrolyte layer is 30μm, and the slurry is heated and cured at 60°C for 1 hour;

[0294] (5) The composite negative electrode sheet and the lithium iron phosphate positive electrode stack obtained in the above steps are assembled into a solid-state battery by hot pressing at a temperature of 65° C. and a pressure of 0.4 MPa.

[0295] Example 8

[0296] This embodiment provides a pole piece and a method for preparing the same, and a solid-state battery and a method for preparing the same. A multi-layer solid electrolyte is introduced on the pole piece by ultrasonic spraying. The specific steps are as follows:

[0297] (1) carbon nanotubes (particle size 50 nm) and styrene-butadiene rubber were uniformly mixed in a ratio of 70%:30% by mass, dissolved in DMF solvent and stirred thoroughly, and sodium hydroxymethyl cellulose was added to prepare a slurry with a solid content of 40% by mass;

[0298] (2) The slurry was introduced onto the surface and gap of the negative electrode active material by ultrasonic spraying on the surface of the silicon-carbon negative electrode plate, wherein the ultrasonic power was 60 W, the ultrasonic frequency was controlled at 60 kHz, the spray width was 50 mm, the spray angle was 90°, the continuous spraying amount was controlled at 700 ml / h, the spraying distance was 20 mm, and the air pressure was controlled at 0.2 MPa to obtain a mixed conductive layer with a thickness of 1 μm, and heated and cured at 60° C. for 1 hour;

[0299] (3) Boron oxide, styrene-butadiene rubber, and LiTFSI were dissolved in DMF solvent in a mass ratio of 3:5:2 and stirred thoroughly to prepare a slurry with a solid content of 50 mass%, which was sprayed on the surface of the mixed conductive layer by ultrasonic spraying, wherein the ultrasonic power was 30 W, the ultrasonic frequency was controlled at 80 kHz, the spray width was 50 mm, the spray angle was 90°, and the continuous spraying amount was controlled at 700

[0300] ml / h, the spraying distance was 20 mm, and the gas pressure was controlled at 0.1 MPa to obtain the first composite solid electrolyte layer with a thickness of 2 μm;

[0301] (4) Li7La3Zr2O 12The solid electrolyte, styrene-butadiene rubber and LiTFSI are mixed and stirred in DMF in a mass ratio of 7:2:1 to prepare a slurry with a solid content of 40% by mass, which is sprayed on the surface of the first composite solid electrolyte layer by ultrasonic spraying, wherein the ultrasonic frequency is controlled at 90kHz, the continuous spraying amount is controlled at 800ml / h, the spraying distance is 35mm, and the air pressure is controlled at 0.2MPa to obtain a composite electrode containing a second solid electrolyte, the thickness of the second solid electrolyte layer is 30μm, and the slurry is heated and cured at 60°C for 1 hour;

[0302] (5) The composite negative electrode sheet and the lithium iron phosphate positive electrode stack obtained in the above steps are assembled into a solid-state battery by hot pressing at a temperature of 65° C. and a pressure of 0.4 MPa.

[0303] Example 9

[0304] This embodiment provides a pole piece and a method for preparing the same, and a solid-state battery and a method for preparing the same. A multi-layer solid electrolyte is introduced on the pole piece by ultrasonic spraying. The specific steps are as follows:

[0305] (1) Nano-conductive carbon black (particle size 300 nm) and styrene-butadiene rubber are mixed at a mass percentage of 70%:

[0306] 30% of the mixture was mixed evenly, dissolved in DMF solvent and stirred thoroughly, and sodium hydroxymethyl cellulose was added to prepare a slurry with a solid content of 40% by mass;

[0307] (2) The slurry was introduced onto the surface and gap of the negative electrode active material by ultrasonic spraying on the surface of the silicon-carbon negative electrode plate, wherein the ultrasonic power was 60 W, the ultrasonic frequency was controlled at 60 kHz, the spray width was 50 mm, the spray angle was 90°, the continuous spraying amount was controlled at 700 ml / h, the spraying distance was 20 mm, and the air pressure was controlled at 0.2 MPa to obtain a mixed conductive layer with a thickness of 1 μm, and heated and cured at 60° C. for 1 hour;

[0308] (3) Boron oxide, styrene-butadiene rubber, and LiTFSI were dissolved in DMF solvent in a mass ratio of 3:5:2 and stirred thoroughly to prepare a slurry with a solid content of 35 mass%, which was sprayed on the surface of the mixed conductive layer by ultrasonic spraying, wherein the ultrasonic power was 30 W, the ultrasonic frequency was controlled at 80 kHz, the spray width was 50 mm, the spray angle was 90°, and the continuous spraying amount was controlled at 700

[0309] ml / h, the spraying distance was 20 mm, and the gas pressure was controlled at 0.1 MPa to obtain the first composite solid electrolyte layer with a thickness of 2 μm;

[0310] (4) Tantalum-doped lithium lanthanum zirconium oxide, styrene-butadiene rubber, and LiTFSI were mixed and stirred in DMF at a mass ratio of 7:2:1 to prepare a slurry with a solid content of 40 mass%, and the slurry was sprayed on the surface of the first composite solid electrolyte layer by ultrasonic spraying, wherein the ultrasonic frequency was controlled at 90 kHz, the continuous spraying amount was controlled at 800 ml / h, the spraying distance was 35 mm, and the air pressure was controlled at 0.2 MPa to obtain a composite electrode containing a second solid electrolyte, the thickness of the second solid electrolyte layer was 30 μm, and the slurry was heated and cured at 60° C. for 1 hour;

[0311] (5) The composite negative electrode sheet and the lithium iron phosphate positive electrode stack obtained in the above steps are assembled into a solid-state battery by hot pressing at a temperature of 65° C. and a pressure of 0.4 MPa.

[0312] Example 10

[0313] This embodiment provides a pole piece and a method for preparing the same, and a solid-state battery and a method for preparing the same. A multi-layer solid electrolyte is introduced on the pole piece by ultrasonic spraying. The specific steps are as follows:

[0314] (1) carbon nanotubes (particle size 50 nm) and styrene-butadiene rubber were uniformly mixed in a ratio of 8%:20% by mass, dissolved in DMF solvent and stirred thoroughly, and sodium hydroxymethyl cellulose was added to prepare a slurry with a solid content of 40% by mass;

[0315] (2) The slurry was introduced onto the surface and gap of the negative electrode active material by ultrasonic spraying on the surface of the silicon-carbon negative electrode plate, wherein the ultrasonic power was 60 W, the ultrasonic frequency was controlled at 60 kHz, the spray width was 50 mm, the spray angle was 90°, the continuous spraying amount was controlled at 700 ml / h, the spraying distance was 20 mm, and the air pressure was controlled at 0.2 MPa to obtain a mixed conductive layer with a thickness of 1 μm, and heated and cured at 60° C. for 1 hour;

[0316] (3) Boron nitride, styrene-butadiene rubber, and LiTFSI were dissolved in DMF solvent in a mass ratio of 3:5:2 and stirred thoroughly to prepare a slurry with a solid content of 40 mass%, which was sprayed on the surface of the mixed conductive layer by ultrasonic spraying, wherein the ultrasonic power was 30 W, the ultrasonic frequency was controlled at 80 kHz, the spray width was 50 mm, the spray angle was 90°, and the continuous spraying amount was controlled at 700

[0317] ml / h, the spraying distance was 20 mm, and the gas pressure was controlled at 0.1 MPa to obtain the first composite solid electrolyte layer with a thickness of 2 μm;

[0318] (4) Tantalum-doped lithium lanthanum zirconium oxide, styrene-butadiene rubber, and LiTFSI were mixed and stirred in DMF at a mass ratio of 7:2:1 to prepare a slurry with a solid content of 40 mass%, and the slurry was sprayed on the surface of the first composite solid electrolyte layer by ultrasonic spraying, wherein the ultrasonic frequency was controlled at 90 kHz, the continuous spraying amount was controlled at 800 ml / h, the spraying distance was 35 mm, and the air pressure was controlled at 0.2 MPa to obtain a composite electrode containing a second solid electrolyte, the thickness of the second solid electrolyte layer was 30 μm, and the slurry was heated and cured at 60° C. for 1 hour;

[0319] (5) The composite negative electrode sheet and the lithium iron phosphate positive electrode stack obtained in the above steps are assembled into a solid-state battery by hot pressing at a temperature of 65° C. and a pressure of 0.4 MPa.

[0320] Embodiment 11

[0321] This embodiment provides a pole piece and a method for preparing the same, and a solid-state battery and a method for preparing the same, wherein a multi-layer solid electrolyte is introduced by ultrasonic spraying, and the difference from Embodiment 1 is that a first composite solid electrolyte layer is not provided;

[0322] Example 12

[0323] This embodiment provides a pole piece and a preparation method thereof, and a solid-state battery and a preparation method thereof, wherein a multi-layer solid electrolyte is introduced by ultrasonic spraying, and the difference from Embodiment 1 is that the ultrasonic frequency is different, which is 10kHz;

[0324] Embodiment 13

[0325] This embodiment provides a pole piece and a method for preparing the same, and a solid-state battery and a method for preparing the same, wherein a multi-layer solid electrolyte is introduced by ultrasonic spraying. The difference from Embodiment 1 is that the solid content of the slurry is different, which is 80% by mass.

[0326] Embodiment 14

[0327] This embodiment provides a pole piece and a preparation method thereof, and a solid-state battery and a preparation method thereof, wherein a multi-layer solid electrolyte is introduced by ultrasonic spraying. The difference from Embodiment 1 is that no nano conductive agent is selected, and the particle size of the conductive agent used is 3.5 μm.

[0328] Embodiment 15

[0329] This embodiment provides a pole piece and a preparation method thereof, and a solid-state battery and a preparation method thereof, wherein a multi-layer solid electrolyte is introduced by ultrasonic spraying. The difference from Embodiment 1 is that the thickness of the mixed conductive layer is different, and the thickness is 1.5 μm;

[0330] Example 16

[0331] This embodiment provides a pole piece and a method for preparing the same, and a solid-state battery and a method for preparing the same. Multilayer solid electrolytes are introduced using an ultrasonic spraying method. The difference from Embodiment 1 is that the mass ratio of the nano-conductive agent to the organic polymer solid electrolyte is 95:5.

[0332] Embodiment 17

[0333] This comparative example provides a pole piece and a preparation method thereof and a solid-state battery and a preparation method thereof, and uses an ultrasonic spraying method to introduce a multilayer solid electrolyte. The difference from Example 1 is that the continuous spraying amount used is 3100 mL / h.

[0334] Comparative Example 1

[0335] This comparative example provides a pole piece and a preparation method thereof, and a solid-state battery and a preparation method thereof, wherein a multi-layer solid electrolyte is introduced by ultrasonic spraying, and the difference from Example 1 is that no mixed conductive layer is provided;

[0336] Performance Test:

[0337] Peel strength test: It is carried out in a peel force tester. At room temperature of 25°C and air humidity of -35°C dew point environment, one side of the prepared battery electrode collector is adhered to the working panel with a test double-sided tape, and the active material surface and the peel force tester are connected with a test tape. The peeling speed is 60mm / min and the peeling angle is 180°. The peeling force is tested and recorded.

[0338] Interface impedance test: The prepared composite electrode and lithium metal sheet were assembled into a button cell, and the AC impedance was tested in an electrochemical workstation using the AC impedance method. The voltage amplitude was set to 5 mV and the frequency range was 0.1 Hz to 1 MHz for testing.

[0339] Cycle stability test: The positive electrode sheet and the negative electrode sheet, the positive electrode sheet containing a solid electrolyte or the negative electrode sheet are cut and assembled into button batteries, and charged and discharged at a rate of 0.3C at 25°C. Each embodiment is cycled 200 times, and the battery capacity before and after the cycle is recorded 200 times, and the first charge and discharge capacity is recorded, and the first coulombic efficiency is calculated.

[0340] Table 1

[0341]

[0342]

[0343] By comparing and analyzing the test results of Examples 1-17 and Comparative Example 1, when the applied process conditions are within the preferred range of ultrasonic spraying, the battery pole pieces prepared in Examples 1-17 have higher peel strength, the adhesion between the active substances of the composite pole pieces containing solid electrolytes is stronger, and the contact with the current collector is closer, which effectively reduces the interface impedance. Ultrasonic spraying of organic polymer solid electrolytes can reduce the interface impedance, maintain the stability and close contact of the interlayer interface, and effectively improve the cycle stability of the solid-state battery. The cycle capacity retention rate of the solid-state battery in Examples 1-17 is much higher than that in Comparative Example 1, and it can be stably cycled for more than 200 times at a rate of 0.3C, showing good cycle stability.

[0344] Figure 1 This is a scanning electron microscope characterization of the composite solid-state battery pole piece obtained in Example 1. The surface particles of the pole piece prepared by ultrasonic spraying are fully refined and no agglomeration of the solid electrolyte particles is found. The solid electrolyte is evenly dispersed on the surface of the pole piece to construct a continuous and dense solid electrolyte layer.

[0345] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and variations will be apparent to those of ordinary skill in the art without departing from the scope and spirit of the described embodiments. The selection of terms used herein is intended to best explain the principles of the embodiments, practical applications, or technical improvements in the market, or to enable other persons of ordinary skill in the art to understand the embodiments disclosed herein.

[0346] Industrial Applicability

[0347] In the present invention, a mixed conductive layer including a nano-conductive agent and an organic polymer solid electrolyte is introduced on the surface of the pole piece. The use of the nano-conductive agent effectively increases the contact area between the mixed conductive layer and the pole piece, and the organic polymer solid electrolyte can reduce the interface impedance and improve the cycle stability of the solid-state battery. The present invention uses an ultrasonic spraying method to spray the slurry used to form the mixed conductive layer, which can fully refine the slurry particles, improve the stability of the coating, and achieve a uniform layered structure with controllable thickness, thereby improving the structural stability of the solid-state battery.

Claims

1. A pole piece, characterized in that: The invention comprises a mixed conductive layer on a positive electrode sheet or a negative electrode sheet, wherein the mixed conductive layer comprises a nano conductive agent and an organic polymer solid electrolyte.

2. The pole piece according to claim 1, characterized in that: In the mixed conductive layer, the mass ratio of the nano conductive agent to the organic polymer solid electrolyte is (85-20):(15-80), preferably the mass ratio of the nano conductive agent to the organic polymer solid electrolyte is (80-25):(20-75).

3. The pole piece according to claim 1, characterized in that: The particle size of the nano-conductive agent is 5-500 nm, and preferably the particle size of the nano-conductive agent is 10-300 nm.

4. The pole piece according to claim 1, characterized in that: The thickness of the mixed conductive layer is 100nm-1000nm, preferably the thickness of the mixed conductive layer is 150-800nm; Preferably, the mixed conductive layer further comprises a binder; Preferably, the binder is selected from one or more of polyvinylidene fluoride, polyvinyl alcohol, polytetrafluoroethylene, sodium hydroxymethyl cellulose, styrene-butadiene rubber, nitrile rubber, styrene-butadiene-styrene copolymer, polyacrylic acid, and lithium polyacrylate.

5. The pole piece according to any one of claims 1 to 4, characterized in that: The nano conductive agent is selected from one or more of conductive graphite, conductive carbon black, acetylene black, carbon nanotubes, Ketjen black, graphene, carbon molecular sieves, carbon nanofibers, polystyrene sulfonic acid, lithium polystyrene sulfonate and polyethylene dioxythiophene; Preferably, the organic polymer solid electrolyte is selected from one or more of polyethylene oxide, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polyvinylidene fluoride-chlorotrifluoroethylene, polyacrylonitrile, polymethyl methacrylate, polypropylene carbonate, polyphenylene sulfide, polyethyl cyanoacrylate, polypentylene succinate, polyvinyl chloride, polyvinyl carbonate, polyvinyl pyrrolidone, chitosan, polyimide, polyacrylate, polyurethane, aramid, polyetherimide, polyamide, polysulfone, aromatic sulfone, polyaromatic sulfone, polyether sulfone, epoxy resin and polyphenylene sulfone resin.

6. The pole piece according to any one of claims 1 to 4, characterized in that: The pole piece also includes a first composite solid electrolyte layer on the mixed conductive layer; Preferably, the thickness of the first composite solid electrolyte layer is 200-3000 nm, preferably the thickness of the first composite solid electrolyte layer is 250-2000 nm; Preferably, the first composite solid electrolyte layer comprises an inorganic ceramic material, an organic polymer solid electrolyte, and a lithium salt.

7. The pole piece according to claim 6, characterized in that: The inorganic ceramic material used for the first composite solid electrolyte layer is selected from one or more of nitrides, carbides, metal oxides, and non-metal oxides; Preferably, the inorganic ceramic material is selected from one or more combinations of oxides, nitrides, borides, halides, carbides, dielectric ceramics, ferroelectric ceramics, piezoelectric ceramics, diatomaceous earth, mullite, montmorillonite and kaolin; Wherein, the oxide includes one or more combinations of silicon oxide, boron oxide, magnesium oxide, copper oxide, nickel oxide, calcium oxide, aluminum oxide, titanium oxide, zirconium oxide, vanadium oxide, lanthanum oxide, beryllium oxide, yttrium oxide, cerium oxide and lead zirconium titanate; Wherein, the nitride includes one or more combinations of silicon nitride, titanium nitride, aluminum nitride, boron nitride, magnesium nitride, zirconium nitride and silicon oxynitride; The carbide is selected from one or more of silicon carbide, boron carbide, tantalum carbide, vanadium carbide, zirconium carbide, tungsten carbide, molybdenum carbide, manganese carbide, iron carbide, titanium carbide and niobium carbide; The dielectric ceramic, the ferroelectric ceramic, and the piezoelectric ceramic each contain BaTiO3, MgTiO3, CaTiO3PbTiO3, SrTiO3, BaO·TiO2, BaO-Nd2O3-TiO2, LiNbO3, LiTaO3, Cd2Ta2O7, Pb2Nb2O7, Cd2Nb2O7, PbNb2O6, Sr 1-x Ba x Nb2O6 and Ba2NaNb5O 15 One or more of .

8. The pole piece according to claim 6, characterized in that: The pole piece further includes a second solid electrolyte layer on the first composite solid electrolyte layer; Preferably, the thickness of the second solid electrolyte layer is 2 μm-50 μm, preferably the thickness of the second solid electrolyte layer is 5 μm-40 μm; Preferably, the second solid electrolyte layer further comprises a lithium salt and / or a binder.

9. The pole piece according to claim 8, characterized in that: The solid electrolyte used for the second solid electrolyte layer includes one or more of an inorganic solid electrolyte and an organic polymer solid electrolyte; Preferably, the inorganic solid electrolyte is selected from one or more of an oxide solid electrolyte, a sulfide solid electrolyte, a halide solid electrolyte, a borate solid electrolyte, a nitride solid electrolyte and a hydride solid electrolyte.

10. The pole piece according to claim 9, characterized in that: The oxide solid electrolyte is selected from one or more of a garnet-type solid electrolyte, a perovskite-type solid electrolyte, a NASICON-type solid electrolyte and a LISICON-type solid electrolyte; The garnet-type solid electrolyte includes Li x Ln3Z y A z O 12 and / or Li x La 3-y B y Zr z O 12 ; Wherein, A is one or more of Ta, Nb, Mg, Ti, Te, and W, and B is one or more of Ca, Rb, Al, and Ga; The perovskite solid electrolyte includes Li 3.3 La 0.53 TiO3、Li 3x La 2 / 3-x TiO3 and Li x Sr y M z One or more of TaO3; wherein M is one or more of Zr and Nb; The NASICON-type solid electrolyte includes Li x Al y M z (PO4)3、Li x Y y Zr z (PO4)3, LiTi2(PO4)3, LiGe2(PO4)3 and LiGeTi(PO4)3; wherein M is one or more of Ti, Ge, Hf, Zn, Zr and Si; The LISICON type solid electrolyte includes Li 3+x (P 1-x Si x )O4 and / or Li 3+x Ge x V 1-x O4; The sulfide solid electrolyte is selected from Argyrodite solid electrolyte LiPSMX, Thio-LiSICON solid electrolyte Li 4-x A 1-x B x S4 and one or more of glassy sulfides; wherein M is one or more of O, Cu, Zn, Bi, Sn, Al, Mn, Ce and In, X is one or more of F, Cl, Br and I; A is one or more of Si, Sn, Ge and Zr, and B is one or more of O, P, Al, Zn and Ga; The glassy sulfide includes one or more of Li2S-P2S5, Li2S-GeS2, Li2S-SiS2, Li2S-SiS2-Li4SiO4, Li2S-B2S3, and Li2S-B2S3-LiI; The halide solid electrolyte includes LiX, Li2MX 4、 Li3M′X6、Li x M″ y Ln z Cl 3、 LiM″′Cl5X″ and Li 3- y Zr y M″″ 1-y Cl6; wherein X is one or more of F, Cl, Br, I, M is one or more of Mg, Mn, Fe, Zn and Cd, M' is one or more of O, In, Y, Yb, Sc, Ho, Er, M "is one or more of Ta, Zr, Ca and Al, Ln is one or more of La, Ce, Pr, Nd, Sm, M "' is selected from one or more of La, Ta, Nb, X "is selected from O, Cl, F or OH, M " " is selected from one or more of Y, Er, Yb, Ho, Lu; Among them, 0 <x<1,0<y<1,0<z<1; The borate solid electrolyte is selected from one or more of Li2B4O7, Li2O-B2O3-P2O5; The nitride solid electrolyte is selected from one or more of LiPON, Li3N, Li7PN4, and LiSi2N3; The hydride solid electrolyte includes but is not limited to one or more of Li3AlH6, LiBH4, LiNH2, Li2NH, LiBH4-LiNH2, LiBH4-LiX; wherein X is one or more of Cl, Br and I; Preferably, the perovskite-type oxide solid electrolyte is selected from lithium lanthanum titanium oxide; The garnet-type oxide solid electrolyte is selected from one or more of lithium lanthanum zirconium oxide, niobium-doped lithium lanthanum zirconium oxide, tantalum-doped lithium lanthanum zirconium oxide, and niobium-tantalum dual-doped lithium lanthanum zirconium oxide; The NASICON type oxide solid electrolyte is selected from one or more of lithium aluminum titanium phosphate, lithium yttrium titanium phosphate, and lithium aluminum germanium phosphate.

11. The pole piece according to claim 8, characterized in that: The binder is selected from one or more of polyvinylidene fluoride, polyvinyl alcohol, polytetrafluoroethylene, sodium hydroxymethyl cellulose, styrene-butadiene rubber, nitrile rubber, styrene-butadiene-styrene copolymer, polyacrylic acid, and lithium polyacrylate; Preferably, the lithium salt is selected from one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium bis(trifluoromethanesulfonyl imide), lithium bis(fluorosulfonyl imide) and lithium difluorooxalatoborate.

12. A method for preparing a pole piece, characterized in that: It includes the following steps: Step S2: spraying a conductive slurry containing a nano conductive agent and an organic polymer solid electrolyte onto the surface of the positive electrode sheet or the negative electrode sheet by ultrasonic spraying, and then optionally heating and curing to obtain a positive electrode sheet or a negative electrode sheet with a mixed conductive layer.

13. The preparation method according to claim 12, characterized in that: The preparation method further comprises the following steps: Step S4: spraying the slurry containing the inorganic ceramic material onto the surface of the mixed conductive layer obtained in step S2 by ultrasonic spraying, thereby obtaining a positive electrode sheet or a negative electrode sheet having the mixed conductive layer and the first composite solid electrolyte layer in sequence.

14. The preparation method according to claim 13, characterized in that: The preparation method further comprises the following steps: Step S6: spraying the second solid electrolyte slurry onto the surface of the first composite solid electrolyte layer obtained in step S4 by ultrasonic spraying, thereby obtaining a positive electrode sheet or a negative electrode sheet having a mixed conductive layer, a first composite solid electrolyte layer and a second solid electrolyte layer in sequence.

15. The preparation method according to any one of claims 12 to 14, characterized in that: The preparation method further comprises the following steps: Step Sx: hot pressing the finally prepared positive electrode sheet or negative electrode sheet; Preferably, the hot pressing temperature is 40-60° C., the pressure is 0.1-0.5 MPa, and the hot pressing time is 5-20 minutes.

16. The preparation method according to any one of claims 12 to 14, characterized in that: The solid content of the conductive paste is 5 to 40% by mass; Preferably, the solid content of the slurry containing the inorganic ceramic material is 5 to 30% by mass; Preferably, the second solid electrolyte slurry has a solid content of 5 to 40% by mass.

17. The preparation method according to any one of claims 12 to 14, characterized in that: In the conductive paste of step S2, the mass ratio of the nano conductive agent to the organic polymer solid electrolyte is (85-20): (15-80), preferably the mass ratio of the nano conductive agent to the organic polymer solid electrolyte is (80-25): (20-75); Preferably, the particle size of the nano conductive agent is 5-500 nm, more preferably the particle size of the nano conductive agent is 10-300 nm.

18. The preparation method according to claim 14, characterized in that: In the ultrasonic spraying in step S2, step S4 and step S6, the spraying conditions are as follows: ultrasonic power is 10-100W, ultrasonic frequency is 20-200kHz, continuous spraying amount is 0-3000ml / h, preferably 800-1700ml / h, spraying distance is 10-100mm, air pressure is 0.1-0.3MPa, spray width is 50-400mm, spraying angle is 85-90°, and temperature of positive electrode sheet or negative electrode sheet is 30-80°C; Preferably, the spraying conditions in step S2, step S4 and step S6 are the same or different.

19. The preparation method according to any one of claims 12 to 14, characterized in that: In the step S2, the temperature of heating and curing is 60-120°C, preferably 80-100°C.

20. The preparation method according to any one of claims 12 to 14, characterized in that: The nano-conductive agent used in step S2 is selected from one or more of conductive graphite, conductive carbon black, acetylene black, carbon nanotubes, Ketjen black, graphene, carbon molecular sieves, carbon nanofibers, polystyrene sulfonic acid, lithium polystyrene sulfonate and polyethylene dioxythiophene; Preferably, the organic polymer solid electrolyte used in step S2 is selected from one or more of polyethylene oxide, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polyvinylidene fluoride-chlorotrifluoroethylene, polyacrylonitrile, polymethyl methacrylate, polypropylene carbonate, polyphenylene sulfide, polyethyl cyanoacrylate, polypentylene succinate, polyvinyl chloride, polyvinyl carbonate, polyvinyl pyrrolidone, chitosan, polyimide, polyacrylate, polyurethane, aramid, polyetherimide, polyamide, polysulfone, aromatic sulfone, polyaromatic sulfone, polyether sulfone, epoxy resin and polyphenylene sulfone resin.

21. The preparation method according to claim 13, characterized in that: The slurry containing the inorganic ceramic material used in step S4 further contains an organic polymer solid electrolyte and a lithium salt; The inorganic ceramic material used in step S4 is selected from one or more of nitrides, carbides, metal oxides, and non-metal oxides; Preferably, the oxide includes but is not limited to one or more combinations of silicon oxide, boron oxide, magnesium oxide, copper oxide, nickel oxide, calcium oxide, aluminum oxide, titanium oxide, zirconium oxide, vanadium oxide, lanthanum oxide, beryllium oxide, yttrium oxide, cerium oxide, and lead zirconium titanate; Preferably, the nitride includes but is not limited to one or more combinations of silicon nitride, titanium nitride, aluminum nitride, boron nitride, magnesium nitride, zirconium nitride and silicon oxynitride; Preferably, the carbide is selected from one or more of silicon carbide, boron carbide, tantalum carbide, vanadium carbide, zirconium carbide, tungsten carbide, molybdenum carbide, manganese carbide, iron carbide, titanium carbide, and niobium carbide; The dielectric ceramics, ferroelectric ceramics and piezoelectric ceramics respectively include BaTiO3, MgTiO3, CaTiO3, PbTiO3, SrTiO3, BaO·TiO2, BaO-Nd2O3-TiO2, LiNbO3, LiTaO3, Cd2Ta2O7, Pb2Nb2O7, Cd2Nb2O7, PbNb2O6, Sr 1- x Ba x Nb2O6、Ba2NaNb5O 15 One or more of; Preferably, the organic polymer solid electrolyte is selected from one or more of polyethylene oxide, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polyvinylidene fluoride-chlorotrifluoroethylene, polyacrylonitrile, polymethyl methacrylate, polypropylene carbonate, polyphenylene sulfide, polyethyl cyanoacrylate, polypentylene succinate, polyvinyl chloride, polyvinylene carbonate, polyvinyl pyrrolidone, chitosan, polyimide, polyacrylate, polyurethane, aramid, polyetherimide, polyamide, polysulfone, aromatic sulfone, polyaromatic sulfone, polyether sulfone, epoxy resin and polyphenylene sulfone resin; Preferably, the lithium salt is selected from one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium bis(trifluoromethanesulfonyl imide), lithium bis(fluorosulfonyl imide), and lithium difluorooxalatoborate.

22. The preparation method according to claim 14, characterized in that: The second solid electrolyte used in step S6 is selected from one or more of an inorganic solid electrolyte and an organic polymer solid electrolyte; Preferably, the inorganic solid electrolyte is selected from one or more of an oxide solid electrolyte, a sulfide solid electrolyte, a halide solid electrolyte, a borate solid electrolyte, a nitride solid electrolyte and a hydride solid electrolyte; Preferably, the oxide solid electrolyte is selected from one or more of a garnet-type solid electrolyte, a perovskite-type solid electrolyte, a NASICON-type solid electrolyte and a LISICON-type solid electrolyte; The garnet-type solid electrolyte includes Li x Ln3Z y A z O 12 and / or Li x La 3-y B y Zr z O 12 ; Wherein, A is one or more of Ta, Nb, Mg, Ti, Te, and W, and B is one or more of Ca, Rb, Al, and Ga; The perovskite solid electrolyte includes Li 3.3 La 0.53 TiO3、Li 3x La 2 / 3-x TiO3 and Li x Sr y M z One or more of TaO3; wherein M is one or more of Zr and Nb; The NASICON-type solid electrolyte includes Li x Al y M z (PO4)3、Li x Y y Zr z (PO4)3, LiTi2(PO4)3, LiGe2(PO4)3 and LiGeTi(PO4)3; wherein M is one or more of Ti, Ge, Hf, Zn, Zr and Si; The LISICON type solid electrolyte includes Li 3+x (P 1-x Si x )O4 and / or Li 3+x Ge x V 1-x O4; The sulfide solid electrolyte is selected from Argyrodite solid electrolyte LiPSMX, Thio-LiSICON solid electrolyte Li 4-x A 1-x B x S4 and one or more of glassy sulfides; wherein M is one or more of O, Cu, Zn, Bi, Sn, Al, Mn, Ce and In, X is one or more of F, Cl, Br and I; A is one or more of Si, Sn, Ge and Zr, and B is one or more of O, P, Al, Zn and Ga; The glassy sulfide includes one or more of Li2S-P2S5, Li2S-GeS2, Li2S-SiS2, Li2S-SiS2-Li4SiO4, Li2S-B2S3, and Li2S-B2S3-LiI; The halide solid electrolyte includes LiX, Li2MX 4、 Li3M′X6、Li x M″ y Ln z Cl 3、 LiM″′Cl5X″ and Li 3- y Zr y M″″ 1-y Cl6; wherein X is one or more of F, Cl, Br, I, M is one or more of Mg, Mn, Fe, Zn and Cd, M' is one or more of O, In, Y, Yb, Sc, Ho, Er, M "is one or more of Ta, Zr, Ca and Al, Ln is one or more of La, Ce, Pr, Nd, Sm, M "' is selected from one or more of La, Ta, Nb, X "is selected from O, Cl, F or OH, M " " is selected from one or more of Y, Er, Yb, Ho, Lu; Among them, 0 <x<1,0<y<1,0<z<1; The borate solid electrolyte is selected from one or more of Li2B4O7, Li2O-B2O3-P2O5; The nitride solid electrolyte is selected from one or more of LiPON, Li3N, Li7PN4, and LiSi2N3; The hydride solid electrolyte includes but is not limited to one or more of Li3AlH6, LiBH4, LiNH2, Li2NH, LiBH4-LiNH2, LiBH4-LiX; wherein X is one or more of Cl, Br and I; The organic polymer solid electrolyte is selected from one or more of polyethylene oxide, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polyvinylidene fluoride-chlorotrifluoroethylene, polyacrylonitrile, polymethyl methacrylate, polypropylene carbonate, polyphenylene sulfide, polyethyl cyanoacrylate, polypentylene succinate, polyvinyl chloride, polyvinylene carbonate, polyvinyl pyrrolidone, chitosan, polyimide, polyacrylate, polyurethane, aramid, polyetherimide, polyamide, polysulfone, aromatic sulfone, polyaromatic sulfone, polyether sulfone, epoxy resin and polyphenylene sulfone resin; Preferably, the perovskite-type oxide solid electrolyte is selected from lithium lanthanum titanium oxide; The garnet-type oxide solid electrolyte is selected from one or more of lithium lanthanum zirconium oxide, niobium-doped lithium lanthanum zirconium oxide, tantalum-doped lithium lanthanum zirconium oxide, and niobium-tantalum dual-doped lithium lanthanum zirconium oxide; The NASICON type oxide solid electrolyte is selected from one or more of lithium aluminum titanium phosphate, lithium yttrium titanium phosphate, and lithium aluminum germanium phosphate.

23. The preparation method according to claim 14, characterized in that: The slurry in step S2 also includes a binder; Preferably, the slurry in step S6 further includes a lithium salt and / or a binder.

24. The preparation method according to claim 23, characterized in that: The binder is selected from one or more of polyvinylidene fluoride, polyvinyl alcohol, polytetrafluoroethylene, sodium hydroxymethyl cellulose, styrene-butadiene rubber, nitrile rubber, styrene-butadiene-styrene copolymer, polyacrylic acid, and lithium polyacrylate; The lithium salt is selected from one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium bis(trifluoromethanesulfonyl imide), lithium bis(fluorosulfonyl imide), and lithium difluorooxalatoborate; Preferably, the binder used in the slurry in step S2 and the binder used in the slurry in step S6 are the same as or different from each other.

25. A solid-state battery, characterized in that: It comprises the electrode sheet according to any one of claims 1 to 11 or the positive electrode sheet or negative electrode sheet obtained by the preparation method according to any one of claims 12 to 24.

26. A method for preparing a solid-state battery, characterized in that: include: The step of preparing a positive electrode sheet or a negative electrode sheet by the preparation method according to any one of claims 12 to 24.

27. The preparation method according to claim 26, characterized in that: The method also includes the steps of rolling and drying the positive electrode sheet and / or the negative electrode sheet and then hot pressing them for integration.

28. The preparation method according to claim 27, characterized in that: In the hot pressing integration, the hot pressing temperature is 50-85° C., the pressure is 0.2-0.9 MPa, and the hot pressing time is 20-40 minutes.

Citation Information

Patent Citations

  • Positive plate and preparation method thereof, and solid-state chemical power supply

    CN110993953A

  • Preparation method of positive plate or negative plate for solid-state battery, positive plate or negative plate for solid-state battery and solid-state battery

    CN111799514A

  • Lithium metal solid-state battery capable of operating at room temperature and preparation method of lithium metal solid-state battery

    CN114665150A

Cited By

  • Negative electrode structure and all-solid-state battery comprising same

    CN119447179A

  • Battery pole piece for solid-state battery, preparation method of battery pole piece and solid-state battery

    CN121282103A

  • A battery pole for a solid-state battery, a method for manufacturing the same, and a solid-state battery

    CN121282103B

  • Gradient composite pole piece, preparation method and secondary battery

    CN121565788A

  • Gradient composite electrode plate and preparation method, secondary battery

    CN121565788B