Diffractive element
By optimizing the liquid crystal orientation pattern and surfactant distribution in the optically anisotropic layer, the problem of poor orientation of liquid crystal compounds is solved, the diffraction efficiency is improved, and the performance of optical devices is enhanced.
Patent Information
- Application Number
- CN202380023329.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-01
- Filing Date
- 2023-02-28
- Publication Date
- 2024-10-01
AI Technical Summary
In the prior art, the poor orientation of liquid crystal compounds leads to poor diffraction efficiency. Especially in thinner and miniaturized optical devices, it is difficult to achieve efficient light direction control.
An optically anisotropic layer with a liquid crystal alignment pattern derived from a liquid crystal compound whose optical axis continuously rotates in-plane, combined with the secondary ion intensity distribution of the surfactant, is analyzed by time-of-flight secondary ion mass spectrometry to ensure the consistency of the liquid crystal alignment pattern. Smoothness and orientation, forming a multi-layer coating structure to improve diffraction efficiency.
It achieves good orientation of liquid crystal compounds, improves diffraction efficiency, and by optimizing the distribution of surfactants and the structure of the liquid crystal immobilization layer, orientation defects and shrinkage holes are avoided, and the performance of the optical anisotropic layer is enhanced.
Smart Images

Figure CN118742831A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a diffraction element. Background Art
[0002] Diffractive elements that control the direction of light are used in many optical devices or systems. Diffractive elements that control the direction of light are used in various optical devices such as backlights of liquid crystal display devices, head mounted displays (HMDs) such as AR (Augmented Reality) glasses and VR (Virtual Reality) that overlay virtual images and various information on the actual scene, projectors, beam deflectors, and sensors for detecting objects and measuring the distance to objects.
[0003] In such optical devices, since the devices are being made thinner and smaller, it is desired to make the diffraction elements used thinner and smaller. As a thin and small diffraction element, it is proposed to use an optically anisotropic layer composed of a liquid crystal composition containing a liquid crystal compound.
[0004] For example, Patent Document 1 describes a polarization diffraction grating, which includes a polarization-sensitive photo-alignment layer and a liquid crystal composition disposed on the photo-alignment layer, wherein an anisotropic orientation pattern corresponding to a polarization hologram is disposed in the photo-alignment layer, so that the liquid crystal composition is oriented into the orientation pattern. The orientation pattern of the polarization diffraction grating changes periodically along at least one straight line in a plane, and by using an optical anisotropic layer that changes the orientation pattern in such a plane, a diffraction element that is thin and controls the transmission direction of incident light can be realized.
[0005] In addition, non-patent document 1 describes a method for producing a diffraction element, which comprises spin-coating a thin film of a photo-orientation material on a glass substrate and then exposing it to the light by interference of a circularly polarized light beam to generate a polarization hologram (orientation pattern), thereby orienting the liquid crystal molecules to the orientation pattern of the orientation film.
[0006] Previous technical literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Application No. 2008-532085
[0009] Non-patent literature
[0010] Non-patent literature 1: Tao Zhan et al., Fabrication of Pancharatnam-Berry phase optical elements with highly stable polarization holography, Optics Express, Vol. 27, No. 3 / 4 February 2020, pp2632-2642 Summary of the invention
[0011] Technical issues to be solved by the invention
[0012] According to the research conducted by the present inventors, it has been found that in a diffraction element including an optically anisotropic layer in which a liquid crystal compound is arranged in a predetermined orientation pattern, there is a problem that the diffraction efficiency deteriorates when the orientation of the liquid crystal compound is poor.
[0013] An object of the present invention is to solve the problems of the prior art and to provide a diffraction element having a good orientation of a liquid crystal compound.
[0014] Means for solving technical problems
[0015] In order to solve the problem, the present invention has the following structure.
[0016] [1] A diffraction element comprising an optically anisotropic layer having a liquid crystal orientation pattern in which the direction of an optical axis derived from a liquid crystal compound changes while continuously rotating in at least one direction in a plane, wherein:
[0017] The birefringence Δn of the optically anisotropic layer is 0.20 or more,
[0018] The optically anisotropic layer contains a surfactant,
[0019] The depth distribution of the secondary ion intensity derived from the surfactant was obtained by analyzing the components in the depth direction of the optically anisotropic layer by time-of-flight secondary ion mass spectrometry while irradiating the optical anisotropic layer from one surface to the other surface, and when the depth position of 20% of the thickness from one surface to the other surface of the optically anisotropic layer was set as position D20 and the depth position of 80% of the thickness from one surface to the other surface was set as position D80, the average value of the secondary ion intensity derived from the surfactant between position D20 and position D80 was calculated, and in the region from position D20 to position D80, a peak of secondary ion intensity greater than 1.1 times the average value was observed, and no peak of secondary ion intensity greater than 5 times the average value was observed.
[0020] [2] The diffraction element according to [1], wherein:
[0021] There are two or more peaks with secondary ion intensities that are 1.1 times or more of the average value, and the distance between adjacent peaks is defined as T.
[0022] In the liquid crystal alignment pattern, when the length of the direction of the optical axis derived from the liquid crystal compound rotated 180° in the plane is set as one period Λ,
[0023] The peak-to-peak distance T and one period Λ of the liquid crystal orientation pattern satisfy:
[0024] 0.05≤T / Λ≤0.25.
[0025] [3] The diffraction element according to [1] or [2], wherein:
[0026] The optically anisotropic layer has a region where the optical axis of the liquid crystal compound is twisted in the thickness direction, and the twist angle in the thickness direction of the optically anisotropic layer is 10° to 360°.
[0027] [4] The diffraction element according to any one of [1] to [3], wherein:
[0028] The surfactant is a surfactant containing a fluorine atom and having a molecular weight of 800 to 2,000.
[0029] [5] The diffraction element according to any one of [1] to [4], wherein:
[0030] The birefringence Δn of the optically anisotropic layer is 0.40 or less.
[0031] Effects of the Invention
[0032] According to the present invention, a diffraction element having a good orientation of a liquid crystal compound can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 It is a schematic diagram showing an example of the diffraction element of the present invention.
[0034] Figure 2 It is conceptually expressed Figure 1 The diagram shows the structure of the optically anisotropic layer of the diffraction element shown.
[0035] Figure 3 yes Figure 2 A top view of the optically anisotropic layer is shown.
[0036] Figure 4 This is a diagram for explaining the function of the diffraction element.
[0037] Figure 5This is a diagram for explaining the function of the diffraction element.
[0038] Figure 6 This is a graph showing the relationship between sputtering time and secondary ion intensity.
[0039] Figure 7 This is a diagram showing an example of an exposure apparatus for forming an alignment pattern.
[0040] Figure 8 This is a conceptual diagram showing another example of the optically anisotropic layer included in the diffraction element of the present invention.
[0041] Fig. 9 This is a conceptual diagram showing another example of the optically anisotropic layer included in the diffraction element of the present invention.
[0042] Fig.10 It is conceptually expressed Fig. 9 A diagram showing the structure of the optically anisotropic layer.
[0043] Fig.11 It is a plan view conceptually showing another example of the optically anisotropic layer included in the diffraction element of the present invention.
[0044] Fig.12 This is a diagram showing another example of an exposure apparatus for forming an alignment pattern.
[0045] Fig.13 This is a diagram conceptually showing a method for evaluating diffraction efficiency in Examples. DETAILED DESCRIPTION
[0046] Hereinafter, the present invention will be described in detail. In addition, in the present specification, the numerical range expressed using "to" means a range including the numerical values described before and after "to" as the lower limit and the upper limit.
[0047] In the present specification, “(meth)acrylate” is a symbol indicating both acrylic acid and methacrylate, “(meth)acryloyl” is a symbol indicating both acryloyl and methacryloyl, and “(meth)acrylic acid” is a symbol indicating both acrylic acid and methacrylic acid.
[0048] In the present invention, visible light is light of wavelength observed by human eyes among electromagnetic waves, and is light in the wavelength range of 380 to 780 nm. Ultraviolet light is light in the wavelength range of 10 nm or more and less than 380 nm, and infrared light is light in the wavelength range of more than 780 nm.
[0049] Furthermore, among visible light, light in the wavelength region of 420 to 490 nm is blue (B) light, light in the wavelength region of 495 to 570 nm is green (G) light, and light in the wavelength region of 620 to 750 nm is red (R) light.
[0050] [Diffractive element]
[0051] The diffraction element of the present invention,
[0052] The optical anisotropic layer includes a liquid crystal alignment pattern in which the direction of the optical axis of the liquid crystal compound changes while continuously rotating in at least one direction in a plane, wherein:
[0053] The birefringence Δn of the optically anisotropic layer is 0.20 or more,
[0054] The optically anisotropic layer contains a surfactant,
[0055] The depth distribution of the secondary ion intensity derived from the surfactant was obtained by analyzing the components in the depth direction of the optically anisotropic layer by time-of-flight secondary ion mass spectrometry while irradiating the optical anisotropic layer from one surface to the other surface, and when the depth position of 20% of the thickness from one surface to the other surface of the optically anisotropic layer was set as position D20 and the depth position of 80% of the thickness from one surface to the other surface was set as position D80, the average value of the secondary ion intensity derived from the surfactant between position D20 and position D80 was calculated, and in the region from position D20 to position D80, a peak of secondary ion intensity greater than 1.1 times the average value was observed, and no peak of secondary ion intensity greater than 5 times the average value was observed.
[0056] exist Figure 1 , an example of the diffraction element of the present invention is conceptually shown.
[0057] Figure 1 The diffraction element 10 shown includes an optically anisotropic layer 12 , an alignment film 32 , and a support 30 .
[0058] The optically anisotropic layer 12 is an optically anisotropic layer formed of a liquid crystal composition containing a liquid crystal compound. Figure 2 and Figure 3 As shown, the optically anisotropic layer 12 has a liquid crystal orientation pattern in which the direction of the optical axis of the liquid crystal compound is continuously rotated in one direction in the plane. Although it will be described in detail later, the optically anisotropic layer having a liquid crystal orientation pattern in which the direction of the optical axis of the liquid crystal compound is continuously rotated in one direction in the plane acts as a diffraction element that diffracts the transmitted light. That is, the diffraction element of the present invention acts as a diffraction element that diffracts the transmitted light.
[0059] <Optically anisotropic layer>
[0060] use Figure 2 and Figure 3 The optically anisotropic layer will be described.
[0061] Figure 2 and Figure 3 The example shown is an optically anisotropic layer having a fixed liquid crystal phase of an aligned liquid crystal compound and having a liquid crystal alignment pattern in which the direction of the optical axis derived from the liquid crystal compound changes while continuously rotating in at least one direction in the plane.
[0062] As in Figure 2 2 conceptually shows that, in the optically anisotropic layer, the liquid crystal compound 40 is not twisted in a spiral shape in the thickness direction, and the liquid crystal compound 40 located at the same position in the plane direction is oriented so that the optical axis 40A is oriented in the same direction.
[0063] <<Liquid crystal orientation pattern of optically anisotropic layer>>
[0064] The optically anisotropic layer has a liquid crystal alignment pattern in which the direction of the optical axis 40A derived from the liquid crystal compound 40 changes while continuously rotating in one direction within the plane of the optically anisotropic layer.
[0065] In addition, the optical axis 40A derived from the liquid crystal compound 40 is an axis having the highest refractive index in the liquid crystal compound 40, which is a so-called slow axis. For example, when the liquid crystal compound 40 is a rod-shaped liquid crystal compound, the optical axis 40A is along the long axis direction of the rod shape. In the following description, the optical axis 40A derived from the liquid crystal compound 40 is also referred to as "optical axis 40A of the liquid crystal compound 40" or "optical axis 40A".
[0066] Figure 3 2 is a conceptual top view of an optically anisotropic layer.
[0067] In addition, the top view refers to the Figure 2 The figure in which the optically anisotropic layer is observed from above is a figure in which the optically anisotropic layer is observed from the thickness direction (=the lamination direction of each layer (film)).
[0068] And, in Figure 3 In FIG. 1 , in order to clearly show the structure of the optically anisotropic layer, only the surface of the liquid crystal compound 40 is shown.
[0069] like Figure 3As shown, on the surface, the liquid crystal compound 40 constituting the optical anisotropic layer has a liquid crystal orientation pattern in which the direction of the optical axis 40A changes while continuously rotating in a predetermined direction indicated by an arrow D (hereinafter referred to as the arrangement axis D) in the plane of the optical anisotropic layer. In the example shown in the figure, the liquid crystal orientation pattern has a liquid crystal compound 40 having an optical axis 40A that changes while continuously rotating in a clockwise direction along the arrangement axis D direction.
[0070] The liquid crystal compound 40 constituting the optically anisotropic layer is in a state of being two-dimensionally aligned in the alignment axis D and in a direction orthogonal to the one direction (the alignment axis D direction).
[0071] In the following description, for convenience, the direction perpendicular to the arrangement axis D is referred to as the Y direction. That is, the arrow Y direction is a direction perpendicular to a direction in which the orientation of the optical axis 40A of the liquid crystal compound 40 changes while continuously rotating within the plane of the optical anisotropic layer. Figure 1-2 and the following Figure 4-5 , Figure 8 to Figure 10 In the figure, the Y direction is perpendicular to the paper surface.
[0072] The orientation of the optical axis 40A of the liquid crystal compound 40 changes while continuously rotating along the arrangement axis D direction (a predetermined direction). Specifically, it means that the angle formed by the optical axis 40A of the liquid crystal compound 40 arranged along the arrangement axis D direction and the arrangement axis D direction is different depending on the position in the arrangement axis D direction. Along the arrangement axis D direction, the angle formed by the optical axis 40A and the arrangement axis D direction changes from θ to θ+180° or θ-180° in sequence.
[0073] The difference in angle between the optical axes 40A of the liquid crystal compounds 40 adjacent to each other in the arrangement axis D direction is preferably 45° or less, more preferably 15° or less, and still more preferably a smaller angle.
[0074] Furthermore, in the present invention, it is assumed that the rotation direction of the optical axis 40A of the liquid crystal compound in the direction of the arrangement axis D is the direction in which the liquid crystal compound 40 (optical axis 40A) rotates in a direction in which the angle formed by the optical axes 40A of the liquid crystal compounds 40 adjacent to each other in the direction of the arrangement axis D becomes smaller. Figure 2 and Figure 3 In the optically anisotropic layer shown, the optical axis 40A of the liquid crystal compound 40 is rotated rightward (clockwise) along the arrow direction of the alignment axis D.
[0075] On the other hand, the liquid crystal compound 40 forming the optically anisotropic layer is oriented in the same direction as the optical axis 40A in the Y direction orthogonal to the arrangement axis D direction (ie, the Y direction orthogonal to one direction in which the optical axis 40A rotates continuously).
[0076] In other words, in the Y direction of the liquid crystal compound 40 forming the optically anisotropic layer, the angles formed between the optical axis 40A of the liquid crystal compound 40 and the direction of the alignment axis D are equal.
[0077] In the optically anisotropic layer, the angles formed by the optical axis 40A and the direction of the arrangement axis D (a direction in which the direction of the optical axis of the liquid crystal compound 40 is rotated) of the liquid crystal compound arranged in the Y direction are equal. The region in which the liquid crystal compound 40 in the Y direction, in which the angles formed by the optical axis 40A and the direction of the arrangement axis D are equal, is defined as region R.
[0078] At this time, the value of the in-plane retardation (Re) in each region R is preferably half a wavelength, that is, λ / 2. These in-plane retardations are calculated by the product of the refractive index difference Δn associated with the refractive index anisotropy of the region R and the thickness of the optical anisotropic layer. Here, the refractive index difference associated with the refractive index anisotropy of the region R in the optical anisotropic layer is a refractive index difference defined by the difference between the refractive index in the slow axis direction in the plane of the region R and the refractive index in the direction perpendicular to the slow axis direction. That is, the refractive index difference Δn associated with the refractive index anisotropy of the region R is equal to the difference between the refractive index of the liquid crystal compound 40 in the direction of the optical axis 40A and the refractive index of the liquid crystal compound 40 in the direction perpendicular to the optical axis 40A in the plane of the region R. That is, the refractive index difference Δn is equal to the refractive index difference of the liquid crystal compound 40.
[0079] In the optically anisotropic layer, in the liquid crystal orientation pattern of this liquid crystal compound 40, in the direction of the arrangement axis D where the in-plane optical axis 40A continuously rotates and changes, the length (distance) of rotating the optical axis 40A of the liquid crystal compound 40 by 180° is set as the length Λ of one period in the liquid crystal orientation pattern.
[0080] That is, the distance between the centers of the two liquid crystal compounds 40 in the direction of the arrangement axis D, which have the same angle with respect to the direction of the arrangement axis D, is set to the length Λ of one period. Figure 3 As shown, the distance between the centers of the two liquid crystal compounds 40 whose arrangement axis D direction coincides with the direction of the optical axis 40A is defined as the length of one period Λ. In the following description, the length of one period Λ is also referred to as "one period Λ".
[0081] The liquid crystal alignment pattern of the optically anisotropic layer repeats this one period Λ in the direction of the arrangement axis D (that is, one direction in which the orientation of the optical axis 40A changes by continuous rotation).
[0082] If circularly polarized light is incident on such an optically anisotropic layer, the light is refracted and the direction of the circularly polarized light is converted.
[0083] exist Figure 4 and Figure 5 This effect is conceptually shown in . In the optically anisotropic layer, the value of the product of the refractive index difference of the liquid crystal compound and the thickness of the optically anisotropic layer is set to λ / 2.
[0084] like Figure 4 As shown, when the value of the product of the refractive index difference of the liquid crystal compound of the optical anisotropic layer and the thickness of the optical anisotropic layer is λ / 2, if the incident light L as left-handed circularly polarized light 1 When incident on the optical anisotropic layer, the incident light L 1 The optical anisotropic layer imparts a phase difference of 180°, thereby transmitting light L 2 is converted into right-handed circularly polarized light.
[0085] Furthermore, the liquid crystal alignment pattern formed on the optically anisotropic layer is a periodic pattern in the direction of the arrangement axis D, so the transmitted light L 2 Towards the incident light L 1 In this way, the incident light L of left-handed circularly polarized light 1 The transmitted light L is converted into right-handed circularly polarized light that is tilted by a predetermined angle in the direction of the arrangement axis D relative to the incident direction. 2 .exist Figure 4 In the example shown, the transmitted light L 2 is diffracted to travel to the lower right.
[0086] On the other hand, Figure 5 As shown, when the product of the refractive index difference of the liquid crystal compound in the optical anisotropic layer and the thickness of the optical anisotropic layer is λ / 2, if the incident light L of right-handed circularly polarized light 4 When incident on the optical anisotropic layer, the incident light L 4 The optically anisotropic layer imparts a phase difference of 180°, thereby converting the transmitted light L into left-handed circularly polarized light. 5 .
[0087] Furthermore, the liquid crystal alignment pattern formed on the optically anisotropic layer is a periodic pattern in the direction of the arrangement axis D, so the transmitted light L 5 Towards the incident light L 4 At this time, the transmitted light L 5 Directed and transmitted light L 2 The different direction is the direction opposite to the arrow direction of the arrangement axis D relative to the incident direction. 4 The transmitted light L is converted into left-handed circularly polarized light that is tilted by a predetermined angle in the direction opposite to the direction of the arrangement axis D relative to the incident direction. 5 .exist Figure 5 In the example shown, the transmitted light L 5is diffracted to travel to the lower left.
[0088] As described above, the optical anisotropic layer can adjust the transmission light L according to the length of one period Λ of the formed liquid crystal alignment pattern. 2 and L 5 Specifically, regarding the optical anisotropic layer, the shorter the period Λ of the liquid crystal alignment pattern, the stronger the interference between the light passing through the adjacent liquid crystal compounds 40, so that the transmitted light L 2 and L 5 Refraction is greater.
[0089] Furthermore, by setting the rotation direction of the optical axis 40A of the liquid crystal compound 40 rotating along the arrangement axis D to the opposite direction, the direction of refraction of the transmitted light can be set to the opposite direction. Figure 4-5 In the example shown, the rotation direction of the optical axis 40A toward the arrangement axis D is clockwise, but by setting the rotation direction to counterclockwise, the direction of refraction of the transmitted light can be set to the opposite direction. Figure 4 and Figure 5 In the figure, when the rotation direction of the optical axis 40A toward the arrangement axis D is counterclockwise, the left-handed circularly polarized light incident on the optical anisotropic layer from the upper side in the figure is converted into right-handed circularly polarized light by the optical anisotropic layer, and diffracted to travel in the lower left direction in the figure. Also, the right-handed circularly polarized light incident on the optical anisotropic layer from the upper side in the figure is converted into left-handed circularly polarized light by the optical anisotropic layer, and diffracted to travel in the lower right direction in the figure.
[0090] Here, in the present invention, the birefringence (refractive index difference) Δn of the optically anisotropic layer 12 is greater than or equal to 0.20, and the optically anisotropic layer 12 contains a surfactant. The components in the depth direction of the optically anisotropic layer 12 are analyzed by time-of-flight secondary ion mass spectrometry from one surface of the optically anisotropic layer toward the other surface while irradiating an ion beam, thereby obtaining a depth-direction distribution of secondary ion intensity derived from the surfactant. When a depth position of 20% of the thickness from one surface toward the other surface of the optically anisotropic layer 12 is set as position D20 and a depth position of 80% of the thickness from one surface toward the other surface is set as position D80, an average value (hereinafter also simply referred to as the average value) of the secondary ion intensity derived from the surfactant between position D20 and position D80 is calculated. In the region from position D20 to position D80, a peak (hereinafter also simply referred to as the peak) indicating a secondary ion intensity greater than or equal to 1.1 times the average value is observed, and a peak indicating a secondary ion intensity greater than or equal to 5 times the average value is not observed.
[0091] As described later, the optically anisotropic layer 12 is formed on the alignment film 32 that orients the liquid crystal compound 40 in a predetermined pattern, thereby forming a liquid crystal alignment pattern in which the direction of the optical axis 40A derived from the liquid crystal compound 40 changes while continuously rotating in at least one direction in the plane. As described above, in order for the optically anisotropic layer 12 to obtain the function of transmitting and diffracting light, the value of the product of the birefringence Δn of the liquid crystal compound 40 in the optically anisotropic layer 12 and the thickness of the optically anisotropic layer 12 needs to be λ / 2. That is, the optically anisotropic layer 12 needs to be set to a predetermined thickness according to the birefringence Δn of the liquid crystal compound 40.
[0092] However, when the optically anisotropic layer becomes thicker, the alignment regulating force of the alignment film becomes less effective at a position away from the alignment film, and the alignment of the liquid crystal compound in the optically anisotropic layer deteriorates, which causes a problem of deteriorating the diffraction efficiency.
[0093] In contrast, an optically anisotropic layer is formed by performing multi-layer coating by repeating coating and curing. An optically anisotropic layer of a desired thickness is formed by forming multiple thin liquid crystal fixing layers that become optically anisotropic layers, so that the liquid crystal orientation pattern of the bottom liquid crystal fixing layer acts as an orientation film for the liquid crystal fixing layer formed thereon, so that the liquid crystal compound is properly oriented in each liquid crystal fixing layer, and the orientation of the optically anisotropic layer as a whole is improved, thereby being able to improve the diffraction efficiency.
[0094] However, according to the research of the present inventors, it is found that even if the optical anisotropic layer is formed by multilayer coating, the orientation is not sufficient, and the diffraction efficiency is sometimes reduced. In this regard, the present inventors have conducted research and found that when the optical anisotropic layer is formed by multilayer coating, the surfactant is biased near the interface between the liquid crystal fixing layers formed by multilayer coating.
[0095] At this point, it can be seen that if the amount of surfactant biased on the interface between the liquid crystal fixing layers is too much, when the next liquid crystal fixing layer is formed on the underlying liquid crystal fixing layer, cissing will occur and a smooth liquid crystal fixing layer cannot be formed, thereby causing the orientation of the liquid crystal compound to deteriorate.
[0096] On the other hand, when the amount of surfactant on the interface between the liquid crystal fixing layers is too small, smoothness and orientation cannot be ensured. In addition, the above-mentioned situation of too small amount of surfactant may occur when the amount of surfactant added is insufficient, when the partiality on the coating surface is low, or when the surfactant is designed in such a way that the surfactant is removed by the solvent contained in the liquid crystal composition that becomes the upper liquid crystal fixing layer.
[0097] In contrast, the diffraction element of the present invention is a diffraction element as follows: from one surface of the optically anisotropic layer 12 toward the other surface, the components in the depth direction of the optically anisotropic layer 12 are analyzed by time-of-flight secondary ion mass spectrometry while irradiating an ion beam, thereby obtaining the depth-direction distribution of the secondary ion intensity originating from the surfactant; when the depth position of 20% of the thickness from one surface to the other surface of the optically anisotropic layer 12 is set as position D20 and the depth position of 80% of the thickness from one surface to the other surface is set as position D80, the average value of the secondary ion intensity originating from the surfactant between position D20 and position D80 is calculated; in the region from position D20 to position D80, a peak of secondary ion intensity of a magnitude greater than 1.1 times the average value is observed, and no peak of secondary ion intensity of a magnitude greater than 5 times the average value is observed.
[0098] In this regard, use Figure 6 Provide explanation.
[0099] First, if Figure 1 As shown, the optical anisotropic layer 12 of the diffraction element 10 of the present invention is formed by multilayer coating and has a plurality of layers (in Figure 1 In the example shown, there are five layers of liquid crystal fixing layers 13a to 13e. Figure 1 In FIG. 1 , the dotted line in the optically anisotropic layer 12 represents the interface between the liquid crystal fixing layers.
[0100] In addition, each liquid crystal fixing layer has the same liquid crystal alignment pattern, and the optical axes of the liquid crystal compounds 40 existing at the same position in the plane direction are oriented in the same direction.
[0101] When the composition in the depth direction of the layer is analyzed by TOF-SIMS (Time-of-Flight Secondary Ion Mass Spectrometry) while ion sputtering is performed from the surface of the optically anisotropic layer 12 on the side opposite to the support 30 toward the surface on the support 30 side, the following can be obtained: Figure 6 The depth distribution of the secondary ion intensity originating from the surfactant is shown in FIG. Figure 6 In the graph, the vertical axis represents the secondary ion intensity derived from the surfactant, and the horizontal axis represents the sputtering time, that is, the depth from a surface. Figure 6 In FIG. 1 , the distribution indicated by the solid line corresponds to the distribution of the present invention, and the distribution indicated by the dashed line corresponds to the distribution of the conventional example.
[0102] The TOF-SIMS method is specifically described in "Surface Analysis Technology Series Secondary Ion Mass Spectrometry" compiled by the Surface Science Society of Japan, Maruzen Co., Ltd. (published in 1999).
[0103] Figure 6 The distribution in is equivalent to Figure 1 The results shown are obtained by analyzing the components in the depth direction of each layer by TOF-SIMS while performing ion sputtering from one surface (the surface on the opposite side of the support 30) toward the other surface (the surface on the support 30 side) of the optically anisotropic layer 12 arranged on the support 30.
[0104] In addition, as mentioned above, Figure 1 The optically anisotropic layer 12 shown corresponds to an example of a method in which a composition for forming an optically anisotropic layer including predetermined components (liquid crystal compound and surfactant) is applied in multiple layers on a support 30 having an alignment film 32 .
[0105] Figure 6 The position where the horizontal axis is 0 corresponds to the surface of the optically anisotropic layer 12 on the opposite side to the support 30, and the position indicated by the dotted line on the horizontal axis corresponds to the surface on the support 30 side of the optically anisotropic layer 12. That is, from the horizontal axis 0 to the position indicated by the dotted line corresponds to one surface to the other surface of the optically anisotropic layer 12.
[0106] In addition, when analyzing the components in the depth direction of a specific optical anisotropic layer by TOF-SIMS while irradiating an ion beam, the following series of operations are repeated: after performing component analysis in a surface depth region of 1 to 2 nm, further digging in the depth direction from 1 nm to several hundred nm and performing component analysis in the next surface depth region of 1 to 2 nm.
[0107] exist Figure 6 The distribution in the depth direction shown shows the result of the secondary ion intensity derived from the surfactant.
[0108] In addition, in this specification, the "secondary ion intensity derived from the surfactant" obtained by analyzing the components in the depth direction of the optical anisotropic layer using TOF-SIMS and detecting the distribution in the depth direction refers to the intensity of the fragment ions derived from the surfactant. For example, although it depends on the type of surfactant, in the case of a surfactant containing elements or structures such as F, Si, Na, K and SOx, the intensity of the secondary ions derived from these elements or structures contained in the surfactant can be cited.
[0109] like Figure 6As shown in FIG. 1 , when an ion beam is irradiated from one surface of the optically anisotropic layer toward the other surface, the components in the depth direction of the optically anisotropic layer are analyzed by the TOF-SIMS method. As shown in FIG. Figure 6 As shown by the arrows in the figure, multiple peaks of secondary ion intensity originating from the surfactant are observed. The peaks of secondary ion intensity correspond to Figure 1 The depth of the interface between the liquid crystal fixing layers 13a to 13e in the optically anisotropic layer 12 shown in FIG. Figure 6 The distribution shown in FIG. 1 includes a peak (indicated by arrow P) observed at a depth position of the interface between the first liquid crystal fixing layer 13a on the support 30 side and the second liquid crystal fixing layer 13b formed thereon. 1 ), a peak (arrow P) observed at a depth position of the interface between the second liquid crystal fixing layer 13b and the third liquid crystal fixing layer 13c formed thereon. 2 ), a peak (arrow P) observed at a depth position of the interface between the third liquid crystal fixing layer 13c and the fourth liquid crystal fixing layer 13d formed thereon. 3 ) and a peak (arrow P) observed at a depth position of the interface between the fourth liquid crystal fixing layer 13d and the fifth liquid crystal fixing layer 13e formed thereon. 4 ).
[0110] Here, the surfactant tends to be biased toward the air interface side and the support interface side (particularly the air interface side). Therefore, the secondary ion intensity derived from the surfactant tends to be high near one surface and near the other surface. In order to eliminate this influence, in the obtained distribution, the depth position corresponding to 2 / 10 (20%) of the thickness of the entire optical anisotropic layer 12 from one surface toward the other surface is set as position D20 (reference Figure 1 , Figure 6 ), the depth position corresponding to 8 / 10 (80%) of the total thickness of the optically anisotropic layer 12 is defined as position D80 (reference Figure 1 , Figure 6 ), the average value of the secondary ion intensity derived from the surfactant between position D20 and position D80 is calculated, and the baseline is drawn with the average value. That is, the average value of the secondary ion intensity derived from the surfactant in the area between position D20 and position D80 is calculated, and a straight line representing the average value is drawn along the horizontal axis, and the straight line is used as the baseline.
[0111] Next, in the region between position D20 and position D80 of the above distribution, the maximum value of the secondary ion intensity representing a magnitude greater than 1.1 times the average value obtained above is regarded as a peak. In the present invention, in the above distribution, more than one peak representing a secondary ion intensity greater than 1.1 times the average value is observed, and the values of all peaks are less than 5 times the average value.
[0112] In the above distribution, a peak having a value of 1.1 times or more of the average value indicates that the optically anisotropic layer 12 is formed by multi-layer coating. As described above, the optically anisotropic layer 12 is formed by forming multiple liquid crystal fixing layers, so that the liquid crystal orientation pattern of the bottom liquid crystal fixing layer acts as an orientation film for the liquid crystal fixing layer formed thereon, so that the liquid crystal compound is properly oriented in each liquid crystal fixing layer, and the orientation of the optically anisotropic layer as a whole is improved. And, as described above, when the amount of surfactant partial distribution on the interface between the liquid crystal fixing layers is too small, that is, in the above distribution, when the value of the peak is less than 1.1 times the average value, smoothness and orientation cannot be ensured.
[0113] Furthermore, in the above distribution, the peak value is more than 5 times the average value, which means that the amount of surfactant on the interface between the liquid crystal fixing layers is too much. As mentioned above, if the amount of surfactant on the interface between the liquid crystal fixing layers is too much, when the next liquid crystal fixing layer is formed on the bottom liquid crystal fixing layer, it will cause shrinkage holes and it will not be possible to form a smooth liquid crystal fixing layer, which will cause the orientation of the liquid crystal compound to deteriorate. In contrast, in the present invention, in the above distribution, the values of all peaks are less than 5 times the average value, so that when the next liquid crystal fixing layer is formed on the bottom liquid crystal fixing layer, shrinkage holes can be suppressed and a smooth liquid crystal fixing layer can be formed, thereby improving the orientation of the liquid crystal compound.
[0114] exist Figure 6 In the graph shown, in the distribution of the embodiment represented by the solid line, the value of any peak is less than 5 times the average value. On the other hand, in the distribution of the conventional example represented by the single-dot chain line, the value of any peak is more than 5 times the average value.
[0115] In order to observe a peak with a value greater than 1.1 times the average value and not observe a peak with a value greater than 5 times the average value in the region from position D20 to position D80 of the distribution of the secondary ion intensity originating from the surfactant in the optically anisotropic layer 12, it is sufficient to appropriately adjust the type, addition amount, type, ratio, drying speed, hardness of the coating film, etc. of the surfactant in the liquid crystal composition used to form the optically anisotropic layer.
[0116] Here, in the present invention, the birefringence Δn of the optically anisotropic layer is 0.20 or more.
[0117] As described above, in order for the optical anisotropic layer 12 to obtain the effect of transmitting and diffracting light, it is necessary to make the value of the product of the birefringence Δn of the liquid crystal compound 40 of the optical anisotropic layer 12 and the thickness of the optical anisotropic layer 12 to be λ / 2. Therefore, the thickness of the optical anisotropic layer 12 can be made thinner by increasing the birefringence Δn to more than 0.20. If the thickness of the optical anisotropic layer 12 can be made thinner, the number of layers of the liquid crystal fixing layer can be reduced when the optical anisotropic layer 12 is formed by multilayer coating. As described above, in the distribution of the secondary ion intensity derived from the surfactant of the optical anisotropic layer 12, the peak of the secondary ion intensity is observed at the position of the interface between the liquid crystal fixing layers. Therefore, if the number of layers of the liquid crystal fixing layer is small, the number of peaks of the secondary ion intensity in the above distribution becomes small. If the number of layers of the liquid crystal fixing layer is small, the number of coating times in the multilayer coating can be reduced, so the orientation and productivity can be improved.
[0118] <<Measurement method of Δn>>
[0119] Δn in this specification can be measured as follows.
[0120] The Δn×d of the optically anisotropic layer can be obtained by using a birefringence measuring device. Δn can also be calculated by measuring the thickness d of a cross section using a cross-section cutting method or an interference film thickness meter.
[0121] Here, if Δn is too high, the coloring and light resistance of the coating film tend to deteriorate. Therefore, Δn is preferably 0.40 or less.
[0122] Furthermore, from the viewpoint of orientation, the peak value of the secondary ion intensity in the above distribution is preferably 1.1 to 4.5 times the average value, and more preferably 1.1 to 1.8 times.
[0123] Furthermore, in the region between the position D20 and the position D80, if the distance between adjacent peaks (distance in the depth direction) indicating a secondary ion intensity of 1.1 times or more of the average value is set to T (nm), in other words, if the thickness of one liquid crystal fixing layer of the optically anisotropic layer 12 formed by multilayer coating is set to T (nm), then it is preferred that the distance between the peaks T and one period Λ (nm) of the liquid crystal orientation pattern of the optically anisotropic layer 12 satisfy:
[0124] 0.05≤T / Λ≤0.25.
[0125] The shorter the period Λ of the liquid crystal orientation pattern, the worse the orientation is. Therefore, it is preferred to make the peak-to-peak distance T, i.e., the thickness of the liquid crystal fixing layer formed once, thinner. Therefore, from the viewpoint of orientation, T / Λ is preferably 0.25 or less, more preferably 0.23 or less, and further preferably 0.20 or less.
[0126] On the other hand, if the peak-to-peak distance T, i.e., the thickness of the liquid crystal fixing layer formed once, is too thin, the number of layers of the liquid crystal fixing layer needs to be increased. Therefore, from the perspective of productivity, T / Λ is preferably 0.05 or more, more preferably 0.08 or more, and further preferably 0.10 or more.
[0127] From the viewpoint of alignment and productivity, the number of secondary ion intensity peaks, i.e., the number of liquid crystal fixing layers, in the region between position D20 and position D80 of the above distribution is preferably 2-30, more preferably 4-25, and even more preferably 6-20.
[0128] And, in Figure 1 In the example shown, the thickness of the liquid crystal fixing layer is set to be constant, but it is not limited to this, and the thickness of each liquid crystal fixing layer may be different from each other. When the thickness of each liquid crystal fixing layer is different from each other, that is, when there are different peak-to-peak distances in the above distribution, it is preferred that all peak-to-peak distances satisfy 0.05≤T / Λ≤0.25.
[0129] <<Method for forming optically anisotropic layer>>
[0130] The optically anisotropic layer can be formed as follows: a liquid crystal composition containing a liquid crystal compound is coated on an orientation film for orienting the liquid crystal compound in a predetermined liquid crystal orientation pattern, and a liquid crystal phase is formed in which the orientation is a liquid crystal orientation pattern in which the direction of the optical axis of the liquid crystal compound changes while continuously rotating in at least one direction within the plane, and the liquid crystal phase is fixed in a layered form.
[0131] As described above, in the present invention, the optically anisotropic layer is formed by multilayer coating. Multilayer coating refers to a method in which the first layer of liquid crystal composition is first coated on the alignment film, and then heated, cooled, and then ultraviolet curing is performed to form a liquid crystal fixing layer, and then the second layer and the subsequent layers are overlapped and coated on the liquid crystal fixing layer, and then heated, cooled, and then ultraviolet curing is performed, and the process is repeated until the desired thickness is reached to form an optically anisotropic layer.
[0132] (Support)
[0133] As a support for supporting the alignment film and the optically anisotropic layer, various sheet-like objects (films, plates) can be used as long as they can support the alignment film and the optically anisotropic layer.
[0134] The transmittance of the support with respect to diffracted light is preferably 50% or more, more preferably 70% or more, and even more preferably 85% or more.
[0135] The thickness of the support is not limited, and may be appropriately set to a thickness capable of supporting the alignment film and the optically anisotropic layer, depending on the application of the diffraction element and the material of the support.
[0136] The thickness of the support is preferably 1 to 1000 μm, more preferably 3 to 250 μm, and even more preferably 5 to 150 μm.
[0137] The support may be a single layer or a multi-layer.
[0138] As a single-layer support, there can be exemplified a support made of glass, triacetyl cellulose (TAC), polyethylene terephthalate (PET), polycarbonate, polyvinyl chloride, acrylic acid, polyolefin, etc. As an example of a multi-layer support, there can be exemplified a support including any of the above-mentioned single-layer supports as a substrate, and a support having other layers disposed on the surface of the substrate.
[0139] (Oriented Film)
[0140] An alignment film is formed on the surface of the support.
[0141] The alignment film is an alignment film for aligning the liquid crystal compound 40 in a predetermined liquid crystal alignment pattern when forming the optically anisotropic layer.
[0142] As described above, in the present invention, the optically anisotropic layer has an optical axis 40A derived from the liquid crystal compound 40 (refer to Figure 3 ) is a liquid crystal orientation pattern in which the orientation of the liquid crystal changes while continuously rotating in one direction in the plane. Therefore, the orientation film is formed so that the optically anisotropic layer can form the liquid crystal orientation pattern.
[0143] In the following description, “the rotation of the direction of the optical axis 40A” is also simply referred to as “the rotation of the optical axis 40A”.
[0144] As the alignment film, various known alignment films can be used.
[0145] For example, there can be cited friction-treated films composed of organic compounds such as polymers, oblique vapor-deposited films of inorganic compounds, films having microgrooves, and films formed by accumulating LB (Langmuir-Blodgett) films based on the Langmuir-Blodgett method of organic compounds such as ω-tricosanoic acid, dioctadecylmethylammonium chloride, and methyl stearate.
[0146] The alignment film formed by rubbing treatment can be formed by rubbing the surface of the polymer layer with paper or cloth a plurality of times in a predetermined direction.
[0147] Preferred materials for the alignment film include polyimide, polyvinyl alcohol, polymers having polymerizable groups described in Japanese Patent Application Laid-Open No. 9-152509, and materials used for forming the alignment film 32 described in Japanese Patent Application Laid-Open Nos. 2005-97377, 2005-99228, and 2005-128503.
[0148] The alignment film is preferably a so-called photo-alignment film formed by irradiating a photo-alignment material with polarized light or non-polarized light. That is, the alignment film is preferably a photo-alignment film formed by coating a photo-alignment material on a support.
[0149] Irradiation with polarized light can be performed from a vertical direction or an oblique direction with respect to the photo-alignment film, and irradiation with unpolarized light can be performed from an oblique direction with respect to the photo-alignment film.
[0150] Examples of the photo-alignment material that can be used in the alignment film of the present invention include Japanese Patent Application Publication No. 2006-285197, Japanese Patent Application Publication No. 2007-76839, Japanese Patent Application Publication No. 2007-138138, Japanese Patent Application Publication No. 2007-94071, Japanese Patent Application Publication No. 2007-121721, Japanese Patent Application Publication No. 2007-140465, Japanese Patent Application Publication No. 2007-15643 Azo compounds described in Japanese Patent Publication No. 9, Japanese Patent Publication No. 2007-133184, Japanese Patent Publication No. 2009-109831, Japanese Patent No. 3883848 and Japanese Patent No. 4151746, aromatic ester compounds described in Japanese Patent Publication No. 2002-229039, and aromatic ester compounds described in Japanese Patent Publication No. 2002-265541 and Japanese Patent Publication No. 2002-317013. Maleimide and / or alkenyl-substituted nadic imide compounds having photo-alignment units, photo-crosslinkable silane derivatives described in Japanese Patent Nos. 4205195 and 4205198, photo-crosslinkable polyimides, photo-crosslinkable polyamides and photo-crosslinkable polyesters described in Japanese Patent Publication No. 2003-520878, Japanese Patent Publication No. 2004-529220 and Japanese Patent No. 4162850 Preferred examples include compounds capable of photodimerization described in JP-A-9-118717, JP-A-10-506420, JP-A-2003-505561, International Publication No. 2010 / 150748, JP-A-2013-177561, and JP-A-2014-12823, particularly cinnamate compounds, chalcone compounds, and coumarin compounds.
[0151] Among them, it is preferable to use an azo compound, a photo-crosslinkable polyimide, a photo-crosslinkable polyamide, a photo-crosslinkable polyester, a cinnamate compound, and a chalcone compound.
[0152] The thickness of the alignment film is not limited, and may be appropriately set according to the material forming the alignment film so as to obtain a desired alignment function.
[0153] The thickness of the alignment film is preferably 0.01 to 5 μm, more preferably 0.05 to 2 μm.
[0154] The method for forming the alignment film is not limited, and various known methods corresponding to the materials for forming the alignment film can be used. As an example, a method of forming an alignment pattern by coating the alignment film on the surface of a support and drying it, and then exposing the alignment film with a laser beam can be exemplified.
[0155] Figure 7 An example of an exposure device for exposing an alignment film to light to form an alignment pattern is conceptually shown in FIG.
[0156] Figure 7 The exposure device 60 shown includes: a light source 64 provided with a laser 62; a λ / 2 plate 65 for changing the polarization direction of the laser beam M emitted by the laser 62; a beam splitter 68 for separating the laser beam M emitted by the laser 62 into two light beams, namely, light beams MA and MB; reflectors 70A and 70B respectively arranged on the optical paths of the two separated light beams MA and MB; and λ / 4 plates 72A and 72B.
[0157] In addition, the light source 64 emits linearly polarized light P 0 The λ / 4 plate 72A converts the linearly polarized light P 0 (Light MA) is converted into right-handed circularly polarized light P R , the λ / 4 plate 72B converts the linearly polarized light P 0 (Light MB) is converted into left-handed circularly polarized light P L .
[0158] The support 30 having the alignment film 32 before the alignment pattern is formed is placed in the exposure section, and two light beams MA and MB are made to intersect and interfere on the alignment film 32, and then the interference light is irradiated onto the alignment film 32 for exposure.
[0159] Due to the interference at this time, the polarization state of the light irradiated on the alignment film 32 changes periodically in the form of interference fringes. Thus, an alignment film having an alignment pattern in which the alignment state changes periodically (hereinafter also referred to as a pattern alignment film) can be obtained.
[0160] In the exposure device 60, the period of the alignment pattern can be adjusted by changing the cross angle α of the two light beams MA and MB. That is, in the exposure device 60, by adjusting the cross angle α, in the alignment pattern in which the optical axis 40A originating from the liquid crystal compound 40 rotates continuously in one direction, the length of one period in which the optical axis 40A is rotated 180° in one direction can be adjusted.
[0161] By forming an optically anisotropic layer on the alignment film 32 having such an alignment pattern in which the alignment state changes periodically, it is possible to form an optically anisotropic layer having a liquid crystal alignment pattern in which the optical axis 40A derived from the liquid crystal compound 40 continuously rotates in one direction.
[0162] Furthermore, the rotation direction of the optical axis 40A can be reversed by rotating the optical axes of the λ / 4 plates 72A and 72B by 90° respectively.
[0163] As described above, the patterned orientation film has the following orientation pattern: the liquid crystal compound is oriented so that the direction of the optical axis of the liquid crystal compound in the optically anisotropic layer formed on the patterned orientation film changes while rotating continuously in at least one direction in the plane. If the axis of the patterned orientation film along the direction in which the liquid crystal compound is oriented is set as the orientation axis, it can be said that the patterned orientation film has an orientation pattern in which the direction of the orientation axis changes while rotating continuously in at least one direction in the plane. The orientation axis of the patterned orientation film can be detected by measuring the absorption anisotropy. For example, when linearly polarized light is irradiated onto the patterned orientation film while rotating and the amount of light transmitted through the patterned orientation film is measured, it is observed that the direction in which the amount of light becomes maximum or minimum gradually changes along one direction in the plane.
[0164] In the present invention, the alignment film is provided in a preferred embodiment and is not an essential constituent element.
[0165] For example, an orientation pattern can be formed on the support by rubbing the support, processing the support with a laser beam, etc., so that the optically anisotropic layer can have a structure in which the orientation of the optical axis 40A of the liquid crystal compound 40 changes while continuously rotating in at least one direction in the plane. That is, in the present invention, the support can also function as an orientation film.
[0166] (Formation of Optically Anisotropic Layer)
[0167] The optically anisotropic layer can be formed of a lamellar fixed liquid crystal phase having a liquid crystal orientation pattern in which the direction of the optical axis derived from the liquid crystal compound changes while continuously rotating in at least one direction in the plane.
[0168] The structure formed by fixing the liquid crystal phase can be any structure that maintains the orientation of the liquid crystal compound in the liquid crystal phase. The following structure is typically preferred: on the basis of setting the polymerizable liquid crystal compound to an orientation state along the liquid crystal orientation pattern, it is polymerized and cured by ultraviolet irradiation, heating, etc. to form a layer without fluidity, and at the same time, it is changed to a state in which the orientation morphology will not change due to an external field or external force.
[0169] In the structure in which the liquid crystal phase is fixed, the liquid crystal compound 40 may not exhibit liquid crystallinity in the optically anisotropic layer as long as the optical properties of the liquid crystal phase are maintained. For example, a polymerizable liquid crystal compound may lose its liquid crystallinity by increasing its molecular weight through a curing reaction.
[0170] As a material used for forming the optically anisotropic layer having a fixed liquid crystal phase, a liquid crystal composition containing a liquid crystal compound is mentioned as an example. The liquid crystal compound is preferably a polymerizable liquid crystal compound.
[0171] Furthermore, the liquid crystal composition used for forming the optically anisotropic layer may further contain a surfactant, a polymerization initiator, and the like.
[0172] --Polymerizable Liquid Crystalline Compounds--
[0173] The polymerizable liquid crystal compound may be a rod-like liquid crystal compound or a disc-like liquid crystal compound.
[0174] Examples of rod-shaped polymerizable liquid crystal compounds that form an optically anisotropic layer include rod-shaped nematic liquid crystal compounds. As rod-shaped nematic liquid crystal compounds, preferably used are azomethines, azoxyls, cyanobiphenyls, cyanophenyl esters, benzoates, cyclohexanecarboxylic acid phenyl esters, cyanophenylcyclohexanes, cyano-substituted phenylpyrimidines, alkoxy-substituted phenylpyrimidines, phenyldioxanes, tolans, and alkenylcyclohexylbenzonitriles. Not only low molecular weight liquid crystal compounds but also high molecular weight liquid crystal compounds can be used.
[0175] The polymerizable liquid crystal compound is obtained by introducing a polymerizable group into a liquid crystal compound. Examples of the polymerizable group include an unsaturated polymerizable group, an epoxy group, and an aziridine group, preferably an unsaturated polymerizable group, and more preferably an ethylenically unsaturated polymerizable group. The polymerizable group can be introduced into the molecule of the liquid crystal compound by various methods. The number of polymerizable groups possessed by the polymerizable liquid crystal compound is preferably 1 to 6, and more preferably 1 to 3.
[0176] Examples of polymerizable liquid crystal compounds include compounds described in Makromol.Chem., Vol. 190, p. 2255 (1989), Advanced Materials, Vol. 5, p. 107 (1993), U.S. Pat. No. 4,683,327, U.S. Pat. No. 5,622,648, U.S. Pat. No. 5,770,107, International Publication No. 95 / 22586, International Publication No. 95 / 24455, International Publication No. 97 / 00600, International Publication No. 98 / 23580, International Publication No. 98 / 52905, Japanese Patent Application Publication No. 1-272551, Japanese Patent Application Publication No. 6-16616, Japanese Patent Application Publication No. 7-110469, Japanese Patent Application Publication No. 11-80081 and Japanese Patent Application Publication No. 2001-328973. Two or more polymerizable liquid crystal compounds may be used simultaneously. When two or more polymerizable liquid crystal compounds are used simultaneously, the alignment temperature can be lowered.
[0177] Furthermore, as polymerizable liquid crystal compounds other than the above, cyclic organopolysiloxane compounds having a cholesteric phase as disclosed in Japanese Patent Laid-Open No. 57-165480 can be used. In addition, as the above-mentioned polymer liquid crystal compounds, polymers having a mesogen group showing liquid crystal introduced into the main chain, the side chain, or both the main chain and the side chain, polymer cholesteric liquid crystals having a cholesteric group introduced into the side chain, liquid crystal polymers as disclosed in Japanese Patent Laid-Open No. 9-133810, and liquid crystal polymers as disclosed in Japanese Patent Laid-Open No. 11-293252 can be used.
[0178] --Disc-like Liquid Crystalline Compounds--
[0179] As the discotic liquid crystal compound, for example, the discotic liquid crystal compounds described in Japanese Patent Application Laid-Open No. 2007-108732 or Japanese Patent Application Laid-Open No. 2010-244038 can be preferably used.
[0180] The amount of the polymerizable liquid crystal compound added to the liquid crystal composition is preferably 75 to 99.9% by mass, more preferably 80 to 99% by mass, and even more preferably 85 to 90% by mass, relative to the solid content mass of the liquid crystal composition (mass after removing the solvent).
[0181] The type of liquid crystal compound is not particularly limited as long as it can be oriented in a pattern that changes while the direction of the optical axis of the liquid crystal compound is continuously rotated in at least one direction in the plane and can be set to a structure that satisfies the range of Δn specified in the present invention, but from the viewpoint of high Δn and reduced coloration, diphenylacetylene liquid crystal compounds and thiolane liquid crystal compounds can be preferably used. As diphenylacetylene liquid crystal compounds, preferably the compounds described in WO2019 / 182129A1.
[0182] Furthermore, in order to achieve a higher Δn, a compound represented by the following general formula (I) is preferred.
[0183] [Chemical formula 1]
[0184]
[0185] In the general formula (I),
[0186] P 1 and P 2 Each independently represents a hydrogen atom, -CN, -NCS or a polymerizable group.
[0187] Sp 1 and Sp 2 Each independently represents a single bond or a divalent linking group. 1 and Sp 2 It does not mean a divalent linking group containing at least one group selected from the group consisting of an aromatic hydrocarbon ring group, an aromatic heterocyclic group, and an aliphatic hydrocarbon ring group. Examples of the divalent linking group include alkylene, -O-, -S-, -SO- 2 -, -CO-, -NH-, and groups formed by combining these (e.g., -alkylene-O-).
[0188] Z 1 , Z 2 and Z 3 each independently represents a single bond, -O-, -S-, -CHR-, -CHRCHR-, -OCHR-, -CHRO-, -SO-, -SO 2 -, -COO-, -OCO-, -CO-S-, -S-CO-, -O-CO-O-, -CO-NR-, -NR-CO-, -SCHR-, -CHRS-, -SO-CHR-, -CHR-SO-, -SO 2 -CHR-, -CHR-SO 2 -、-CF 2 O-、-OCF 2 -、-CF 2 S-, -SCF 2-, -OCHRCHRO-, -SCHRCHRS-, -SO-CHRCHR-SO-, -SO 2 -CHRCHR-SO 2 -, -CH=CH-COO-, -CH=CH-OCO-, -COO-CH=CH-, -OCO-CH=CH-, -COO-CHRCHR-, -OCO-CHRCHR-, -CHRCHR-COO-, -CHRCHR-OCO-, -COO-CHR-, -OCO-CHR-, -CHR-COO-, -CHR-OCO-, -CR=CR-, -CR=N-, -N=CR-, -N=N-, -CR=NN=CR-, -CF=CF- or -C≡C-. R represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms. When there are multiple Rs, they may be the same or different. When Z 1 and Z 2 When there are multiple Z, they may be the same or different. 3 They can be the same or different. 2 Z 3 Represents a single bond.
[0189] X 1 and X 2 Each independently represents a single bond or -S-. 1 and X 2 They can be the same or different.
[0190] k represents an integer of 2 to 4.
[0191] m and n each independently represent an integer of 0 to 3. A plurality of m may be the same or different.
[0192] A 1 , A 2 , A 3 and A 4 Each independently represents a group represented by any one of the following general formulae (B-1) to (B-7) or a group formed by linking two or three groups represented by any one of the following general formulae (B-1) to (B-7). 2 and A 3 They can be the same or different. 1 and A 4 When there are plural of each, they may be the same or different.
[0193] [Chemical formula 2]
[0194]
[0195] In the general formulas (B-1) to (B-7),
[0196] W 1 ~W 18 Represent CR independently 1 or N, R 1 represents a hydrogen atom or a substituent L described below.
[0197] Y 1 ~Y 6 NR 2 , O or S, R 2 represents a hydrogen atom or a substituent L described below.
[0198] G 1 ~G 4 Represent CR independently 3 R 4 NR 5 , O or S, R 3 ~R 5 Each independently represents a hydrogen atom or a substituent L described below.
[0199] M 1 and M 2 Represent CR independently 6 or N, R 6 represents a hydrogen atom or a substituent L described below.
[0200] *Indicates bonding position.
[0201] The substituent L is an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, an alkylamino group having 1 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an alkanoyl group having 1 to 10 carbon atoms, an alkanoyloxy group having 1 to 10 carbon atoms, an alkanoylamino group having 1 to 10 carbon atoms, an alkanoylthio group having 1 to 10 carbon atoms, an alkoxycarbonyl group having 2 to 10 carbon atoms, an alkylaminocarbonyl group having 2 to 10 carbon atoms, an alkylthiocarbonyl group having 2 to 10 carbon atoms, a hydroxyl group, an amino group, a mercapto group, a carboxyl group, a sulfone group, an amide group, a cyano group, a nitro group, a halogen atom or a polymerizable group. The above-mentioned groups described as the substituent L have -CH 2 -, the -CH 2 - is substituted with -O-, -CO-, -CH=CH- or -C≡C-, which is also included in the substituent L. In addition, when the above-mentioned group described as the substituent L has a hydrogen atom, a group in which at least one of the hydrogen atoms contained in the above-mentioned group is substituted with at least one selected from the group consisting of a fluorine atom and a polymerizable group is also included in the substituent L.
[0202] --Surfactant--
[0203] In the present invention, the liquid crystal composition used when forming the optically anisotropic layer contains a surfactant.
[0204] The surfactant is preferably a compound that can function as an alignment control agent that helps the liquid crystal compound to be oriented stably or quickly. Examples of the surfactant include silicone surfactants and fluorine surfactants, and preferably fluorine surfactants are used.
[0205] Specific examples of surfactants include compounds described in paragraphs
[0082] to
[0090] of JP-A-2014-119605, compounds described in paragraphs
[0031] to
[0034] of JP-A-2012-203237, compounds exemplified in paragraphs
[0092] and
[0093] of JP-A-2005-99248, compounds exemplified in paragraphs
[0076] to
[0078] and
[0082] to
[0085] of JP-A-2002-129162, and fluoro(meth)acrylate polymers described in paragraphs
[0018] to
[0043] of JP-A-2007-272185, and the like.
[0206] The surfactant may be used alone or in combination of two or more.
[0207] As the fluorine-based surfactant, compounds described in paragraphs
[0082] to
[0090] of JP-A-2014-119605 are preferred.
[0208] The amount of the surfactant added in the liquid crystal composition is preferably 0.01 to 10% by mass, more preferably 0.01 to 5% by mass, and even more preferably 0.02 to 1% by mass, relative to the total mass of the liquid crystal compound.
[0209] Here, the surfactant is preferably a surfactant containing a fluorine atom and having a molecular weight of 800 to 2,000.
[0210] When the molecular weight of the surfactant is 800 or more, the surface activity is high, the smoothness of the formed liquid crystal fixing layer becomes good, and the orientation becomes better. In addition, when the molecular weight is 2000 or less, when the liquid crystal fixing layer is formed by multi-layer coating lamination, the surfactant is easily dissolved in the solvent, and as a result, the amount of surfactant on the surface is reduced, and the orientation becomes better. Therefore, from the viewpoint that a peak with a value of 1.1 times or more of the average value is observed in the region from position D20 to position D80 of the distribution of the secondary ion intensity derived from the surfactant in the optically anisotropic layer 12, and a peak with a value of 5 times or more of the average value is not observed, and the orientation is high, the molecular weight of the surfactant is preferably 800 to 2000.
[0211] In addition, as the surfactant, a fluorine-based surfactant having a perfluoroalkyl group which may have an oxygen atom is also preferred. As described above, the molecular weight of the fluorine-based surfactant is preferably 800 to 2,000.
[0212] The number of carbon atoms in the perfluoroalkyl group is not particularly limited, but is preferably 2-20, more preferably 3-15.
[0213] When the perfluoroalkyl group contains an oxygen atom, it is preferably contained as -O- (ether group). When the perfluoroalkyl group contains an oxygen atom, the number of oxygen atoms is not particularly limited, but 2 to 4 are preferred.
[0214] The number of the perfluoroalkyl groups in the fluorine-based surfactant is not particularly limited, but is preferably 1 to 6, and more preferably 1 to 4.
[0215] --Polymerization Initiator--
[0216] When the liquid crystal composition contains a polymerizable compound, it preferably contains a polymerization initiator. In the embodiment in which the polymerization reaction is carried out by ultraviolet irradiation, the polymerization initiator used is preferably a photopolymerization initiator that can initiate the polymerization reaction by ultraviolet irradiation.
[0217] Examples of photopolymerization initiators include α-carbonyl compounds (described in U.S. Pat. No. 2,367,661 and U.S. Pat. No. 2,367,670), acyloin ethers (described in U.S. Pat. No. 2,448,828), α-hydrocarbon-substituted aromatic acyloin compounds (described in U.S. Pat. No. 2,722,512), polynuclear quinone compounds (described in U.S. Pat. No. 3,046,127 and U.S. Pat. No. 2,951,758), a combination of a triaryl imidazole dimer and p-aminophenyl ketone (described in U.S. Pat. No. 3,549,367), acridine and phenazine compounds (described in Japanese Patent Application Laid-Open No. 60-105667 and U.S. Pat. No. 4,239,850), and oxadiazole compounds (described in U.S. Pat. No. 4,212,970).
[0218] The content of the photopolymerization initiator in the liquid crystal composition is preferably 0.1 to 20% by mass, more preferably 0.5 to 12% by mass, based on the content of the liquid crystal compound.
[0219] --Crosslinking agent--
[0220] The liquid crystal composition may contain a crosslinking agent to increase the film strength after curing and improve durability. As the crosslinking agent, a crosslinking agent that is cured by ultraviolet rays, heat, moisture, etc. can be preferably used.
[0221] As a crosslinking agent, there is no particular limitation, and it can be appropriately selected according to the purpose, for example, multifunctional acrylate compounds such as trimethylolpropane tri(meth)acrylate and pentaerythritol tri(meth)acrylate can be cited; epoxy compounds such as (meth) acrylic acid glycidyl ester and ethylene glycol diglycidyl ether; 2,2-bishydroxymethylbutanol-tri[3-(1-aziridine) propionate] and 4,4-bis(ethyleneiminocarbonylamino) diphenylmethane and other aziridine compounds; isocyanate compounds such as hexamethylene diisocyanate and biuret type isocyanate; polyoxazoline compounds having oxazoline groups on the side chain; and alkoxysilane compounds such as vinyltrimethoxysilane, N-(2-aminoethyl) 3-aminopropyltrimethoxysilane, etc. In addition, it is possible to use a known catalyst according to the reactivity of the crosslinking agent, in addition to being able to improve film strength and durability, it is also possible to improve productivity. These can be used alone or in combination of more than two.
[0222] The content of the crosslinking agent is preferably 3 to 20% by mass, more preferably 5 to 15% by mass relative to the solid content of the liquid crystal composition. As long as the content of the crosslinking agent is within the above range, the effect of increasing the crosslinking density is easily obtained, thereby further improving the stability of the liquid crystal phase.
[0223] --Other additives--
[0224] A polymerization inhibitor, an antioxidant, an ultraviolet absorber, a light stabilizer, a colorant, metal oxide fine particles, and the like may be further added to the liquid crystal composition as necessary within a range that does not deteriorate optical properties.
[0225] When forming an optically anisotropic layer (when coating on an alignment film), a liquid crystal composition is preferably used as a liquid.
[0226] The liquid crystal composition may contain a solvent. The solvent is not limited and can be appropriately selected according to the purpose, but an organic solvent is preferable.
[0227] The organic solvent is not limited and can be appropriately selected according to the purpose. For example, ketones, alkyl halides, amides, sulfoxides, heterocyclic compounds, hydrocarbons, esters and ethers can be mentioned. These can be used alone or in combination of two or more. Among these, ketones are preferred in consideration of the burden on the environment.
[0228] Here, in order to observe a peak with a value greater than 1.1 times the average value and no peak with a value greater than 5 times the average value in the region from position D20 to position D80 of the distribution of the secondary ion intensity originating from the surfactant in the optically anisotropic layer 12, and to have high orientation, ketones are preferably used as the solvent contained in the liquid crystal composition, and it is preferred to use two or more ketones at the same time.
[0229] Furthermore, if the proportion of the solvent in the liquid crystal composition is too much, it is possible to increase the drying load and reduce productivity. On the other hand, if the proportion of the solvent is too small, the uniformity of the coating deteriorates. Therefore, from the viewpoint of orientation, the proportion of the solvent in the liquid crystal composition is preferably 50% to 98%, more preferably 60% to 96%, and further preferably 70% to 94%.
[0230] When forming the optically anisotropic layer, it is preferred that a liquid crystal composition is applied onto the surface on which the optically anisotropic layer is to be formed, and after the liquid crystal compound is oriented in a liquid crystal phase state in a predetermined liquid crystal orientation pattern, the liquid crystal compound is cured to form the optically anisotropic layer (liquid crystal fixing layer).
[0231] That is, when forming an optically anisotropic layer on an alignment film, it is preferred that a liquid crystal composition is applied on the alignment film, and after the liquid crystal compound is aligned in a predetermined liquid crystal alignment pattern, the liquid crystal compound is cured to form an optically anisotropic layer having a fixed liquid crystal phase.
[0232] The liquid crystal composition can be applied by any known method that can uniformly apply a liquid to a sheet-like object, such as a printing method such as inkjet printing and roll printing, and a method such as spin coating, bar coating, and spray coating.
[0233] The applied liquid crystal composition is dried and / or heated as required, and then cured to form an optically anisotropic layer. In the drying and / or heating process, the liquid crystal compound in the liquid crystal composition is oriented to a predetermined liquid crystal orientation pattern. When heating is performed, the heating temperature is preferably 200° C. or less, and more preferably 130° C. or less.
[0234] The aligned liquid crystal compound is further polymerized as required. The polymerization may be any of thermal polymerization and photopolymerization by light irradiation, but photopolymerization is preferred. Ultraviolet rays are preferably used for light irradiation. The irradiation energy is preferably 20 mJ / cm 2 ~50J / cm 2 , more preferably 50 to 1500 mJ / cm 2 In order to promote the photopolymerization reaction, light irradiation may be performed under heating conditions or in a nitrogen atmosphere. The wavelength of the ultraviolet rays to be irradiated is preferably 250 to 430 nm.
[0235] As described above, the optically anisotropic layer is formed to a desired thickness by repeating such multilayer coating from coating to polymerization. In this case, the liquid crystal compound in the liquid crystal composition coated on the liquid crystal fixing layer is oriented in the same liquid crystal orientation pattern as the liquid crystal orientation pattern on the surface of the underlying liquid crystal fixing layer. That is, in the case of forming the optically anisotropic layer by multilayer coating, the underlying liquid crystal fixing layer functions as an orientation film of the upper liquid crystal fixing layer.
[0236] Here, in Figure 2 In the optically anisotropic layer shown, the optical axes of the liquid crystal compounds arranged in the thickness direction are aligned in the same direction, but the present invention is not limited thereto. The optically anisotropic layer may have a region in which the optical axis of the liquid crystal compound is twisted in the thickness direction. In this case, the twist angle of the region having the twist in the thickness direction is 10° to 360° in the entire region in the thickness direction.
[0237] Figure 8 This is a diagram conceptually showing another example of the optically anisotropic layer included in the diffraction element of the present invention.
[0238] Figure 8 The optically anisotropic layer 12b shown has the same properties as those of the above-mentioned layer except that the liquid crystal compound is twisted in the thickness direction. Figure 2 and Figure 3 That is, when viewed from the thickness direction, Figure 8 The optically anisotropic layer 12b shown in FIG. Figure 3Similarly to the example shown, there is a liquid crystal alignment pattern in which the direction of the optical axis 40A changes while continuously rotating along the arrangement axis D within the plane of the optically anisotropic layer 12 b .
[0239] Figure 8 The optically anisotropic layer 12 b shown has a twisted structure in which the liquid crystal compounds 40 are stacked and rotated in the thickness direction, and the total rotation angle from the liquid crystal compounds 40 present on one main surface side of the optically anisotropic layer 12 b to the liquid crystal compounds 40 present on the other main surface side is 360° or less.
[0240] In this way, if the optically anisotropic layer has a liquid crystal orientation pattern in which the direction of the optical axis 40A changes while continuously rotating along the arrangement axis D in the plane, and the liquid crystal compound 40 has a twisted structure in the thickness direction, then in a cross section parallel to the arrangement axis D, the optically anisotropic layer has a structure in which a line segment connecting the liquid crystal compound 40 oriented in the same direction in the thickness direction is inclined relative to the main surface of the optically anisotropic layer, and in an image of a cross section obtained by cutting the optically anisotropic layer in the thickness direction along the arrangement axis D observed with a scanning electron microscope (SEM), the optically anisotropic layer has a structure in which the observed stripe pattern of the bright and dark parts is inclined relative to the main surface. Thus, the diffraction efficiency of the diffraction element can be improved.
[0241] In order to make the optically anisotropic layer have a structure in which the liquid crystal compound is twisted and aligned in the thickness direction, a chiral agent may be contained in the liquid crystal composition for forming the optically anisotropic layer.
[0242] --Chiral Reagents (Optically Active Compounds)--
[0243] Chiral agents have the function of inducing a helical structure of a liquid crystal phase. Since the twisting direction and helical twisting power (HTP) of the helix induced by the compound are different, the chiral agent can be selected according to the purpose.
[0244] There are no particular restrictions on the chiral agent, and known compounds (for example, those recorded in Handbook of Liquid Crystal Devices, Chapter 3, Item 4-3, TN (twisted nematic), STN (Super Twisted Nematic) Chiral Agents, page 199, edited by the 142nd Committee of the Japan Society for the Promotion of Science, 1989), isosorbide and isomannide derivatives, etc. can be used.
[0245] Chiral agents usually contain asymmetric carbon atoms, but axial chiral compounds or planar chiral compounds without asymmetric carbon atoms can also be used as chiral agents. In the example of axial chiral compounds or planar chiral compounds, binaphthyl, helicene, p-xylene dimer and their derivatives are included. Chiral agents can also have polymerizable groups. In the case where both the chiral agent and the liquid crystal compound have polymerizable groups, a polymer having repeating units derived from the polymerizable liquid crystal compound and repeating units derived from the chiral agent can be formed by the polymerization reaction of the polymerizable chiral agent and the polymerizable liquid crystal compound. In this way, the polymerizable group possessed by the polymerizable chiral agent is preferably a group of the same type as the polymerizable group possessed by the polymerizable liquid crystal compound. Therefore, the polymerizable group of the chiral agent is also preferably an unsaturated polymerizable group, an epoxy group or an aziridine group, more preferably an unsaturated polymerizable group, and further preferably an olefinic unsaturated polymerizable group.
[0246] Furthermore, the chiral agent may also be a liquid crystal compound.
[0247] When the chiral agent has a photoisomerizable group, it is preferred because the desired twisted orientation corresponding to the emission wavelength can be formed by irradiating a photomask with activating light or the like after coating and orientation. The photoisomerizable group is preferably an isomerization site of a compound showing photochromic properties, an azo group, an oxyazolyl group, or a cinnamoyl group. As specific compounds, compounds described in JP-A-2002-80478, JP-A-2002-80851, JP-A-2002-179668, JP-A-2002-179669, JP-A-2002-179670, JP-A-2002-179681, JP-A-2002-179682, JP-A-2002-338575, JP-A-2002-338668, JP-A-2003-313189, and JP-A-2003-313292 can be used.
[0248] The content of the chiral agent in the liquid crystal composition is preferably 0.01 to 200 mol %, more preferably 1 to 30 mol %, based on the molar amount of the liquid crystal compound.
[0249] Furthermore, the optically anisotropic layer may have a structure having regions with different twist states (twist angles and twist directions) in the thickness direction. In the case of such a structure, in the optically anisotropic layer, in an image of a cross section cut in the thickness direction in a direction in which the orientation of the optical axis of the liquid crystal compound changes while continuously rotating, a bright portion and a dark portion extending from one main surface to the other main surface are observed using a scanning electron microscope, and the dark portion has one or more angle inflection points.
[0250] exist Fig. 9 An example of such an optically anisotropic layer is shown in FIG. Fig. 9 In FIG. 1 , the bright portion 42 and the dark portion 44 are overlapped with the cross section of the optical anisotropic layer 12dc. In the following description, an image of a cross section cut in the thickness direction along one direction rotated along the optical axis observed by SEM is also referred to as a "cross-sectional SEM image".
[0251] Fig. 9 In the cross-sectional SEM image of the optically anisotropic layer 12d shown, the dark portion 44 has two inflection points of angle change. That is, the optically anisotropic layer 12d can be said to have three regions, region 37a, region 37b, and region 37c, in the thickness direction according to the inflection points of the dark portion 44.
[0252] The optically anisotropic layer 12d has a liquid crystal orientation pattern at any position in the thickness direction, wherein the optical axis derived from the liquid crystal compound 40 rotates clockwise toward the left in the figure when viewed from above in the in-plane direction, and one period of the liquid crystal orientation pattern is constant in the thickness direction.
[0253] And, if Fig. 9 As shown, the liquid crystal compound 40 is twistedly aligned in the lower region 37 a in the thickness direction so as to be twisted into a spiral shape clockwise (right-handed) from the upper side to the lower side in the figure in the thickness direction.
[0254] In the middle region 37b in the thickness direction, the liquid crystal compound 40 is not twisted in the thickness direction, and the optical axes of the liquid crystal compounds 40 stacked in the thickness direction are oriented in the same direction. That is, the optical axes of the liquid crystal compounds 40 at the same position in the in-plane direction are oriented in the same direction.
[0255] In the upper region 37 c in the thickness direction, the liquid crystal compound 40 is twistedly aligned so as to be twisted in a spiral shape counterclockwise (left-handed) from the upper side toward the lower side in the figure in the thickness direction.
[0256] That is, in Fig. 9 The regions 37 a , 37 b , and 37 c of the optically anisotropic layer 12 d shown have different states of twisting of the liquid crystal compound 40 in the thickness direction.
[0257] In an optically anisotropic layer having a liquid crystal alignment pattern in which the optical axis of the liquid crystal compound rotates continuously in one direction, it is observed that the bright and dark parts in the cross-sectional SEM image of the optically anisotropic layer connect the liquid crystal compounds in the same direction.
[0258] As an example, in Fig. 9In FIG. 1 , a dark portion 44 is observed to be connected to a liquid crystal compound 40 whose optical axis is oriented in a direction perpendicular to the paper surface.
[0259] In the lowermost region 37a in the thickness direction, the dark portion 44 is inclined toward the upper left in the figure. In the middle region 37b, the dark portion 44 extends in the thickness direction. In the uppermost region 37c, the dark portion 44 is inclined toward the upper right in the figure.
[0260] Right now, Fig. 9 The optically anisotropic layer 12d shown has two angle inflection points where the angle of the dark portion 44 changes. In the uppermost region 37c, the dark portion 44 is inclined toward the upper right, and in the lowermost region 37b, the dark portion 44 is inclined toward the upper left. That is, the dark portion 44 has different inclination directions in the region 37c and the region 37a.
[0261] In addition, Fig. 9 In the optically anisotropic layer 12d shown, the dark portion 44 has one inflection point where the inclined direction turns back in the opposite direction.
[0262] Specifically, the dark portion 44 of the optically anisotropic layer 12d has an inclination direction in the region 37c that is opposite to the inclination direction in the region 37b. Therefore, the inflection point located at the interface between the region 37c and the region 37b is an inflection point where the inclination direction turns back in the opposite direction. That is, the optically anisotropic layer 12d has one inflection point where the inclination direction turns back in the opposite direction.
[0263] Furthermore, as an example, the thickness of the region 37c and the region 37a of the optically anisotropic layer 12d are equal, and as described above, the twisted states of the liquid crystal compound 40 in the thickness direction are different. Figure 1 As shown, the bright portion 42 and the dark portion 44 in the cross-sectional SEM image are substantially C-shaped.
[0264] Therefore, in the optically anisotropic layer 12 d , the shape of the dark portion 44 is symmetrical with respect to the center line in the thickness direction.
[0265] In this optically anisotropic layer 12d, i.e., in a cross-sectional SEM image, the optically anisotropic layer 12 has a bright portion 42 and a dark portion 44 extending from one surface to the other surface, and the dark portion 44 has one or more angle inflection points, which can reduce the wavelength dependence of the diffraction efficiency and diffract light with the same diffraction efficiency without depending on the wavelength.
[0266] In addition, Fig. 9In the example shown, the dark portion 44 is configured to have two angle inflection points, but the present invention is not limited thereto. The dark portion 44 may have one angle inflection point or three or more angle inflection points. For example, when the dark portion 44 of the optically anisotropic layer has one angle inflection point, Fig. 9 Alternatively, for example, when the dark portion 44 of the optically anisotropic layer has a structure having three angle inflection points, two of the dark portions 44 may be alternately provided. Fig. 9 The structures of the regions 37c and 37a shown in the figure may be used.
[0267] In the present invention, as described above, even in the case where the optically anisotropic layer 12d has a structure having regions with different twisted states in the thickness direction, the diffraction element is as follows: from one surface of the optically anisotropic layer toward the other surface, the components in the depth direction of the optically anisotropic layer 12 are analyzed by time-of-flight secondary ion mass spectrometry while irradiating an ion beam, and the depth direction distribution of the secondary ion intensity derived from the surfactant is obtained, and when the depth position of 20% of the thickness from one surface to the other surface of the optically anisotropic layer 12 is set as position D20 and the depth position of 80% of the thickness from one surface to the other surface is set as position D80, the average value of the secondary ion intensity derived from the surfactant between position D20 and position D80 is calculated, and in the region from position D20 to position D80, a peak indicating a secondary ion intensity of a magnitude greater than or equal to 1.1 times the average value is observed, and a peak indicating a secondary ion intensity of a magnitude greater than or equal to 5 times the average value is not observed.
[0268] like Fig.10 As shown, even in the case where the optically anisotropic layer 12d has a structure having regions with different twist states in the thickness direction, each region (37a, 37b, 37c) is formed by multilayer coating. Fig.10In the example shown, region 37a is composed of four layers of liquid crystal fixing layers 38a to 38d, region 37b is composed of four layers of liquid crystal fixing layers 38e to 38h, and region 37c is composed of four layers of liquid crystal fixing layers 38i to 38l. For example, if an alignment film is formed on a support by multi-layer coating from the region 37a side, the liquid crystal composition to be region 37a is coated on the alignment film, heated and cured to form the first layer of liquid crystal fixing layer 38a, and then the second to fourth layers of liquid crystal fixing layers 38b to 38d are formed thereon to form region 37a. Next, the liquid crystal composition to be region 37b is coated on the fourth layer of liquid crystal fixing layer 38d of region 37a, and heated and cured to form the first layer of liquid crystal fixing layer 38e of region 37b. Furthermore, the second to fourth layers of liquid crystal fixing layers 38f to 38h of region 37b are formed thereon to form region 37b. Next, the liquid crystal composition to be the region 37c is applied onto the fourth layer of the liquid crystal fixing layer 38h of the region 37b, and heated and cured to form the first layer of the liquid crystal fixing layer 38i of the region 37c. Furthermore, the second to fourth layers of the liquid crystal fixing layers 38j to 38l of the region 37c are formed thereon to form the region 37c.
[0269] In this way, even in the case where the optically anisotropic layer 12d has a structure having regions with different twisted states in the thickness direction, all liquid crystal fixing layers are formed by multilayer coating. Therefore, if the distribution of the secondary ion intensity derived from the surfactant of the optically anisotropic layer 12d is obtained, peaks of the secondary ion intensity are observed at the depth positions of the interfaces between the liquid crystal fixing layers of each region and the interfaces between regions (the interface between the liquid crystal fixing layer 38d of the region 37a and the liquid crystal fixing layer 38e of the region 37b and the interface between the liquid crystal fixing layer 38h of the region 37b and the liquid crystal fixing layer 38i of the region 37c).
[0270] In the present invention, even in the case of such a structure, the secondary ion intensity peak in the region between the position D20 and the position D80 of the above distribution is not observed to be 1.1 times or more of the average value, nor is it observed to be 5 times or more of the average value. This can improve the orientation.
[0271] exist Fig.10 In the example shown, as the peak existing in the area between position D20 and position D80, a peak from the peak at the depth position of the interface between the liquid crystal fixing layer 38c and the liquid crystal fixing layer 38d to the peak at the depth position of the interface between the liquid crystal fixing layer 38i and the liquid crystal fixing layer 38j is observed.
[0272] In addition, Fig.10In the example shown, each region is configured to have four layers of liquid crystal fixing layers, but the present invention is not limited thereto, and each region may be configured to have two, three, or five or more layers of liquid crystal fixing layers. Furthermore, the number of liquid crystal fixing layers constituting each region is the same, but the present invention is not limited thereto, and the number of liquid crystal fixing layers constituting each region may be different for each region.
[0273] And, in Figure 3 In the example shown, in the liquid crystal alignment pattern of the optically anisotropic layer, the alignment axis D exists in one direction in the plane, and the optical axis 40A of the liquid crystal compound 40 rotates continuously in one direction along the alignment axis D direction.
[0274] However, the present invention is not limited thereto, and various structures can be utilized as long as the optical axis 40A of the liquid crystal compound 40 is continuously rotated in one direction in the optically anisotropic layer.
[0275] For example, as in Fig.11 The top view of FIG. 1 conceptually shows that the optically anisotropic layer 12c may be a structure having a liquid crystal orientation pattern in a radial shape. Fig.11 In the optically anisotropic layer 12c shown, the optical axis of the liquid crystal compound 40 is oriented in a plurality of directions (for example, indicated by arrows A and B) from the center of the optically anisotropic layer 12c toward the outside. 1 Direction indicated by arrow A 2 Direction indicated by arrow A 3 The direction indicated by arrow A changes while rotating continuously. 1 , A 2 and A 3 is the arrangement axis.
[0276] And, if Fig.11 As shown, the optical axis of the liquid crystal compound 40 changes while rotating in the same direction from the center toward the outside of the optically anisotropic layer 12 c. Fig.11 The orientation shown is counterclockwise. Fig.11 Arrow A in 1 , A 2 and A 3 The rotation direction of the optical axis indicated by each arrow changes from the center to the outside, and becomes counterclockwise.
[0277] In this way, in a radial liquid crystal alignment pattern, a line connecting liquid crystal compounds whose optical axes face the same direction is a circle, and line segments of the circle form a concentric circle pattern.
[0278] Thus, the optically anisotropic layer 12c having a radial liquid crystal orientation pattern directs incident light along each alignment axis (A 1 ~A 3Alternatively, when the incident light is diffracted along each arrangement axis (A 1 ~A 3 ) When the light is diffracted in an outward direction, the transmitted light can be diffused. Whether the transmitted light is diffracted along the center side or toward the outside depends on the polarization state of the incident light and the rotation direction of the optical axis in the liquid crystal orientation pattern.
[0279] Thus, in the present invention, by setting the liquid crystal orientation pattern of the optically anisotropic layer to such a radial pattern, it is possible to use a lens that collects or diverges light.
[0280] When the diffraction element is used as a lens, it is preferable to adopt a structure in which the diffraction angle gradually increases from the center of the diffraction element toward the outside. Thereby, the diffraction element can more appropriately focus or diverge light.
[0281] And, in Fig.12 Shown as Fig.11 An example of an exposure device for a radial liquid crystal alignment pattern is shown.
[0282] Fig.12 The exposure device 80 shown has: a light source 84 provided with a laser 82, a polarization beam splitter 86 for splitting the laser beam M from the laser 82 into S-polarized light MS and P-polarized light MP, a reflector 90A arranged in the optical path of the P-polarized light MP and a reflector 90B arranged in the optical path of the S-polarized light MS, a lens 92 arranged in the optical path of the S-polarized light MS, a polarization beam splitter 94, and a λ / 4 plate 96.
[0283] The P polarized light MP split by polarization beam splitter 86 is reflected by mirror 90A and enters polarization beam splitter 94. On the other hand, the S polarized light MS split by polarization beam splitter 86 is reflected by mirror 90B, collected by lens 92 and enters polarization beam splitter 94.
[0284] The P-polarized light MP and the S-polarized light MS are combined by the polarization beam splitter 94 , pass through the λ / 4 plate 96 to become right-handed circularly polarized light and left-handed circularly polarized light corresponding to the polarization directions, and enter the alignment film 32 on the support 30 .
[0285] Here, due to the interference of right-handed circularly polarized light and left-handed circularly polarized light, the polarization state of light irradiated onto the alignment film 32 changes periodically in the form of interference fringes. Since the crossing angle of left-handed circularly polarized light and right-handed circularly polarized light changes from the inside to the outside of the concentric circles, an exposure pattern that changes periodically from the inside to the outside can be obtained. Thus, in the alignment film 32, a radial alignment pattern in which the alignment state changes periodically can be obtained.
[0286] In the exposure device 80, the length Λ of one cycle of the liquid crystal orientation pattern in which the optical axis of the liquid crystal compound 40 continuously rotates 180° can be controlled by changing the refractive power of lens 92 (F value of lens 92), the focal length of lens 92, and the distance between lens 92 and the orientation film 32.
[0287] Furthermore, by adjusting the refractive power of lens 92 (F value of lens 92), the length Λ of one cycle of the liquid crystal orientation pattern can be changed in one direction of continuous rotation of the optical axis. Specifically, by the diffusion angle of light diffused by lens 92 that interferes with parallel light, the length Λ of one cycle of the liquid crystal orientation pattern can be changed in one direction of continuous rotation of the optical axis. More specifically, if the refractive power of lens 92 is weakened, it approaches parallel light, so the length Λ of one cycle of the liquid crystal orientation pattern gradually shortens from the inside to the outside, and the F value increases. On the contrary, if the refractive power of lens 92 is strengthened, the length Λ of one cycle of the liquid crystal orientation pattern suddenly shortens from the inside to the outside, and the F value decreases.
[0288] Example
[0289] Below, enumerate embodiment and comparative example, feature of the present invention is further specifically described.As long as the material, usage amount, ratio, processing content and processing step etc. shown in the following examples do not depart from the gist of the present invention, then can be changed appropriately.Therefore, the scope of the present invention should not be interpreted restrictively by the specific example shown below.
[0290] [Example 1]
[0291] (Formation of Orientation Film)
[0292] The following alignment film forming coating liquid was continuously applied onto a glass substrate having a thickness of 1.1 mm using a #2 wire bar. The support having the coating film of the alignment film forming coating liquid formed thereon was dried on a hot plate at 60° C. for 60 seconds to form an alignment film.
[0293] Coating liquid for forming an alignment film
[0294]
[0295] Photo-Orientation Material A
[0296] [Chemical formula 3]
[0297]
[0298] (Exposure of Alignment Film)
[0299] use Figure 7 The exposure device shown exposes the alignment film to form an alignment film P-1 having an alignment pattern.
[0300] The exposure device used a laser that emitted a laser beam with a wavelength (355 nm). The exposure amount based on the interference light was set to 100 mJ / cm 2 .
[0301] (Formation of Optically Anisotropic Layer)
[0302] As the optically anisotropic layer, a Fig. 9 and Fig.10 The optically anisotropic layer shown has three regions with different twist angles.
[0303] As liquid crystal compositions forming the first region (hereinafter, also referred to as ZA layer), the second region (hereinafter, also referred to as ZB layer), and the third region (hereinafter, also referred to as ZC layer) of the optically anisotropic layer, the following compositions ZA-1, ZB-1, and ZC-1 were prepared, respectively. In addition, the compositions ZA-1, ZB-1, and ZC-1 contained 50% by mass of methyl ethyl ketone (MEK) + 50% by mass of cyclopentanone (CPO) as a solvent so that the following solid content concentration was 3% by mass.
[0304] Composition ZA-1 (solid content)
[0305]
[0306] Liquid crystal compound L-1
[0307] [Chemical formula 4]
[0308]
[0309] Liquid crystal compound L-2
[0310] [Chemical formula 5]
[0311]
[0312] Chiral reagent K-1
[0313] [Chemical formula 6]
[0314]
[0315] Surfactant T-2
[0316] [Chemical formula 7]
[0317]
[0318] In addition, the molecular weight of surfactant T-2 is 1,367.
[0319] Composition ZB-1 (solid content)
[0320]
[0321] Chiral reagent K-2
[0322] [Chemical formula 8]
[0323]
[0324] Composition ZC-1 (solid content)
[0325]
[0326] First, the composition ZA-1 is applied to the alignment film in multiple layers to form the first region (ZA layer). Multilayer coating refers to repeatedly performing the following treatment: first, the first layer of the composition ZA-1 is applied to the formation surface, and then, after heating and cooling, ultraviolet curing is performed to prepare a liquid crystal fixing layer, and then the second layer and subsequent layers are applied on the liquid crystal fixing layer in an overlapping manner, and similarly, heated and cooled, and ultraviolet curing is performed. By forming the alignment film in multiple layers, even when the total thickness of the optically anisotropic layer becomes thicker, the alignment direction of the alignment film is reflected from the lower surface to the upper surface of the optically anisotropic layer.
[0327] First, the composition ZA-1 was applied to the oriented film P-1, and the coating was heated to 80°C on a hot plate. Then, ultraviolet light with a wavelength of 365nm was irradiated onto the coating using an LED (light emitting diode)-UV (Ultra Violet) exposure machine. The coating heated to 80°C on the hot plate was then exposed to light at 300mJ / cm2 using a high-pressure mercury lamp in a nitrogen environment. 2 The coating film was irradiated with ultraviolet rays having a wavelength of 365 nm at an irradiation dose of 1000 Å to fix the alignment of the liquid crystal compound, thereby forming a first liquid crystal fixing layer of the ZA layer of the optically anisotropic layer. The thickness of the liquid crystal fixing layer was set to 0.16 μm.
[0328] The second and subsequent layers were coated on the liquid crystal fixing layer to form a liquid crystal fixing layer under the same conditions as above. In this way, the coating was repeated to form a ZA layer consisting of four layers of liquid crystal fixing layers.
[0329] Regarding the ZA layer, it was confirmed by a polarizing microscope that the liquid crystal compound had a periodic orientation state of 1.0 μm in which the optical axis was rotated by 180°. The twist angle of the ZA layer in the thickness direction was 80° (-80°) in the left direction.
[0330] Next, the ZB layer was formed by applying the composition ZB-1 in multiple layers on the ZA layer.
[0331] The composition ZB-1 was applied on the ZA layer, and the first liquid crystal fixing layer of the ZB layer was formed in the same manner except that the amount of ultraviolet rays irradiated to the coating film was changed from the step of preparing the ZA layer.
[0332] The second and subsequent layers were coated on the liquid crystal fixing layer to produce a liquid crystal fixing layer under the same conditions as above. In this way, the coating was repeated to form a ZB layer consisting of 9 layers of liquid crystal fixing layers.
[0333] The ZB layer was confirmed by a polarizing microscope to have a periodic orientation state of 1.0 μm in which the optical axis of the liquid crystal compound was rotated by 180°. The twist angle of the ZB layer in the thickness direction was right-handed 4° (+4°).
[0334] Next, the ZC layer was formed by applying the composition ZC-1 on the ZB layer in multiple layers.
[0335] The composition ZC-1 was applied on the ZB layer, and the first liquid crystal fixing layer of the ZC layer was formed in the same manner as in the preparation step of the ZA layer, except that the amount of ultraviolet rays irradiated to the coating film was changed.
[0336] The second and subsequent layers were coated on the liquid crystal fixing layer to produce a liquid crystal fixing layer under the same conditions as above. In this way, the coating was repeated to form a ZC layer consisting of four layers of liquid crystal fixing layers.
[0337] The ZC layer was confirmed by a polarizing microscope to have a periodic orientation state of 1.0 μm in which the optical axis of the liquid crystal compound was rotated by 180°. The twist angle of the ZC layer in the thickness direction was right-handed 80° (twist angle 80°).
[0338] As described above, an optically anisotropic layer having three regions having different twist angles in the thickness direction is formed.
[0339] The total thickness of the optically anisotropic layers was 2.72 μm.
[0340] Furthermore, the Δn of the optically anisotropic layer was measured by the above-mentioned method and found to be 0.24.
[0341] Furthermore, the depth-direction distribution of the secondary ion intensity derived from the surfactant of the optically anisotropic layer was measured by the above-mentioned method. Based on the obtained distribution, the average value of the secondary ion intensity derived from the surfactant between the depth position D20 of 20% of the thickness of the optically anisotropic layer and the depth position D80 of 80% of the thickness was calculated, and in the region from position D20 to position D80, the peaks of the secondary ion intensity with a magnitude of 1.1 times or more of the average value were counted, and the presence or absence of the peaks of the secondary ion intensity with a magnitude of 5 times or more of the average value was investigated.
[0342] In the optically anisotropic layer of Example 1, in the thickness direction of the optically anisotropic layer, position D20 is located in the liquid crystal fixing layer of the 4th layer of the ZA layer (0.54 μm from the support side, 3.4 layers), and position D80 is located in the liquid crystal fixing layer of the 1st layer of the ZC layer (0.54 μm from the surface side, 3.4 layers). Therefore, between position D20 and position D80, there are 10 interfaces from the interface between the 4th layer of the ZA layer and the 1st layer of the ZB layer to the interface between the 9th layer of the ZB layer and the 1st layer of the ZC layer. In contrast, there are 10 peaks with a size of more than 1.1 times the average value observed in the above distribution. That is, peaks corresponding to the positions of each interface are observed. Moreover, the size of any peak is less than 5 times the average value.
[0343] [Examples 2 to 6, Comparative Examples 1 to 3]
[0344] The diffraction elements of Examples 2 to 6 and Comparative Examples 1 to 3, in which the periodic orientation state of the liquid crystal compound rotated 180° with a period of 1.0 μm, were formed in the same manner as in Example 1, except that the liquid crystal composition forming each optically anisotropic layer and the thickness and number of liquid crystal fixing layers were changed as shown in Table 1, and the structure of each optically anisotropic layer was changed as shown in Table 2. In addition, in Example 6, the ZC layer was produced by forming a liquid crystal fixing layer with a thickness of 0.28 μm after forming two liquid crystal fixing layers with a thickness of 0.16 μm.
[0345] In Table 2, T / Λ is the ratio of the peak-to-peak distance T (that is, the thickness of the liquid crystal fixing layer) to one period Λ of the liquid crystal alignment pattern.
[0346] Tables 3 to 5 show the formulations of the liquid crystal compositions used in the examples and comparative examples.
[0347] [Table 1]
[0348]
[0349] [Table 2]
[0350]
[0351] [Table 3]
[0352]
[0353] [Table 4]
[0354]
[0355] [Table 5]
[0356]
[0357] Surfactant T-3
[0358] [Chemical formula 9]
[0359]
[0360] Molecular weight: 989
[0361] Surfactant T-4
[0362] [Chemical formula 10]
[0363]
[0364] Molecular weight: 635
[0365] Surfactant T-5
[0366] [Chemical formula 11]
[0367]
[0368] Molecular weight: 2465
[0369] [evaluate]
[0370] <Orientation>
[0371] The orientation of each of the produced diffraction elements (optically anisotropic layers) was evaluated by the following method.
[0372] The liquid crystal orientation pattern of the produced diffraction element was observed using a polarizing microscope, and the orientation state of the liquid crystal compound was evaluated according to the following evaluation criteria.
[0373] AA: There is no pattern distortion in the liquid crystal alignment pattern and the alignment state is very good.
[0374] A: Although slight distortion is observed in the liquid crystal orientation pattern, the liquid crystal is in a good orientation state.
[0375] B: Distortion is observed in the liquid crystal orientation pattern, but the orientation state is maintained.
[0376] C: A slight alignment defect occurs in the liquid crystal alignment pattern.
[0377] D: A large number of alignment defects are generated in the liquid crystal alignment pattern.
[0378] <Diffraction efficiency>
[0379] pass Fig.13 The method shown measures the light intensity of diffracted light (1st-order light) and undiffracted leakage light (0th-order light).
[0380] Specifically, a laser beam LS having an output center wavelength of 530 nm was converted into circularly polarized light via a circular polarizer RA and then vertically incident on the glass substrate side of the sample S of the manufactured diffraction element. The transmitted light was captured by a screen arranged at a distance of 20 cm, and the photodetector was used to measure the 0-second light L. 0 , 1st diffracted light L 1 Then, calculate the light leakage = L 0 / (L 0 +L 1 ). In addition, the polarization state of the laser beam incident on the diffraction element was measured with right-handed circularly polarized light and left-handed circularly polarized light, and the value with the smallest light leakage was adopted. And, based on the calculated light leakage value, the diffraction efficiency was evaluated according to the following criteria.
[0381] AA: Light leakage less than 0.7%
[0382] A: Light leakage is 0.7% or more and less than 1.0%
[0383] B: Light leakage is 1.0% or more and less than 1.5%
[0384] C: Light leakage is 1.5% or more and less than 2.0%
[0385] D: Light leakage is 2.0% or more
[0386] The results are shown in Table 6.
[0387] [Table 6]
[0388]
[0389] As can be seen from Table 6, Examples 1 to 6 of the present invention have higher orientation than the comparative example, and therefore, higher diffraction efficiency can be obtained.
[0390] Regarding the surfactants (T-2 and T-3) used in Examples 1 to 6, the fluorine atoms in both groups were perfluoroalkyl groups and the number of carbon atoms was 4 or less.
[0391] In Comparative Example 1, although an optically anisotropic layer was prepared by multilayer coating, no peak was observed that was 1.1 times or more of the average value in the distribution of the secondary ion strength derived from the surfactant. That is, the amount of surfactant partiality on the interface between the liquid crystal fixing layers was too small. This is because the molecular weight of the surfactant is small and the surface partiality is reduced. In addition, the Δn of the optically anisotropic layer is less than 0.20. Therefore, it can be seen that the orientation is reduced.
[0392] Moreover, in the distribution of the secondary ion strength derived from the surfactant, Comparative Examples 2 and 3 have peaks more than 5 times the average value. That is, the partial amount of the surfactant on the interface between the liquid crystal fixed layers is too much. This is because the molecular weight is large, and when the next liquid crystal layer is formed, the surfactant on the bottom surface will not be removed by the solvent. In this case, when the next liquid crystal fixed layer is formed on the liquid crystal fixed layer of the bottom, shrinkage holes will be caused and a smooth liquid crystal fixed layer cannot be formed. Therefore, it can be known that the orientation of the liquid crystal compound deteriorates.
[0393] Furthermore, it can be seen from the comparison of Examples 1 to 5 that the size of the peak in the distribution of the secondary ion intensity derived from the surfactant can be adjusted by the amount of surfactant added and the ratio of the solvent. Furthermore, it can be seen that the ratio of the size of the peak in the above distribution to the average value is preferably 1.1 to 1.8 times.
[0394] Furthermore, it is understood that when the ratio of the peak size to the average value in the above distribution is within the range of 1.1 to 1.8 times, the orientation is further improved, and thus the diffraction efficiency is further improved.
[0395] Furthermore, from the comparison between Example 1 and Example 6, it can be seen that the ratio T / Λ of the peak-to-peak distance T to one period Λ of the liquid crystal alignment pattern is preferably 0.25 or less.
[0396] It can be seen from the above results that the effect of the present invention is obvious.
[0397] Explanation of symbols
[0398] 10-diffraction element, 12, 12b, 12c, 12d-optical anisotropic layer, 13a-first liquid crystal fixed layer, 13b-second liquid crystal fixed layer, 13c-third liquid crystal fixed layer, 13d-fourth liquid crystal fixed layer, 13e-fifth optical anisotropic layer, 30-support, 32-aligned film, 37a, 37b, 37c-region, 38a~38l-liquid crystal fixed layer, 40-liquid crystal compound, 40A-optical axis, 42-bright part, 44-dark part, 60, 80-exposure device, 62, 82-laser, 64, 84-light source, 65-λ / 2 plate, 68-beam splitter, 70A, 70B, 90A, 90B-reflecting mirror, 72A, 72B, 96-λ / 4 plate, 86, 94-polarization beam splitter, 92-lens, D, A 1 , A 2 , A 3 -arrangement axis, R-area, Λ-1 period, L 1 , L 2 -Incident light, L 4 , L 5 - emitted light, M-laser beam, MA, MB-light, P 0 -Linearly polarized light, P R -Right-handed circularly polarized light, P L -Left-handed circularly polarized light, α-crossing angle, MS-S polarized light, MP-P polarized light.
Claims
1. A diffraction element comprising an optically anisotropic layer having a liquid crystal orientation pattern in which the direction of an optical axis derived from a liquid crystal compound changes while continuously rotating in at least one direction in a plane, in, The birefringence Δn of the optically anisotropic layer is greater than 0.20, The optically anisotropic layer comprises a surfactant, The depth distribution of the secondary ion intensity originating from the surfactant is obtained by analyzing the components in the depth direction of the optically anisotropic layer by time-of-flight secondary ion mass spectrometry while irradiating an ion beam from one surface of the optically anisotropic layer to the other surface. When the depth position of 20% of the thickness from one surface to the other surface of the optically anisotropic layer is set as position D20 and the depth position of 80% of the thickness from one surface to the other surface is set as position D80, the average value of the secondary ion intensity originating from the surfactant between position D20 and position D80 is calculated. In the region from position D20 to position D80, a peak indicating a secondary ion intensity of 1.1 times or more of the average value is observed, and a peak indicating a secondary ion intensity of 5 times or more of the average value is not observed.
2. The diffraction element according to claim 1, in, There are two or more peaks showing secondary ion intensities of 1.1 times or more of the average value, and the distance between adjacent peaks is defined as T. In the liquid crystal alignment pattern, when the length of the direction of the optical axis derived from the liquid crystal compound rotated by 180° in the plane is set as one period Λ, The distance T between the peaks and one period Λ of the liquid crystal alignment pattern satisfy: 0.05≤T / Λ≤0.
25.
3. The diffraction element according to claim 1 or 2, in, The optically anisotropic layer has a region where the optical axis of the liquid crystal compound is twisted in a thickness direction, and a twist angle in the thickness direction of the optically anisotropic layer is 10° to 360°.
4. The diffraction element according to claim 1 or 2, in, The surfactant is a surfactant containing fluorine atoms and having a molecular weight of 800 to 2000.
5. The diffraction element according to claim 1 or 2, in, The optically anisotropic layer has a birefringence Δn of 0.40 or less.
Citation Information
Patent Citations
Polymerizable bifunctional acrylate monomer
JP1989272551A
Circular polarization dichromatic optical element and apparatus therefor and liquid crystal polymer
JP1997133810A
Optical compensation sheet, element having polymer layer and element having oriented film
JP1997152509A
Liquid crystal (Meth)Acrylate compound, its composition and optical isomer using the same
JP1999080081A
Cholesteric liquid crystal laminate
JP1999293252A