A kind of EVA prefabricated coiled material for fitness trail and preparation method thereof
By using modified ethylene-vinyl acetate copolymer and antioxidant monomer in fitness trail rolls, combined with silicone grafted modified flame retardant particles, the problems of existing rolls are easily aging and poor impact toughness are solved. Significantly improves the mechanical properties and service life of the material.
Patent Information
- Application Number
- CN202411252043.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-09
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-09-09
AI Technical Summary
The existing fitness trail prefabricated coils are prone to aging and cracking and have poor impact toughness, which is mainly due to the insufficient interfacial compatibility during the blending of polymer and rubber particles, resulting in a decrease in the mechanical properties of the material in some areas.
Modified ethylene-vinyl acetate copolymer is used, and antioxidant monomers and hard segment chains are added to improve oxidation resistance and impact resistance, and flame retardant particles are modified through siloxane graft to enhance dispersion and material mechanical properties.
It significantly improves the material's anti-aging performance, impact toughness and environmental stress crack resistance, extends its service life, and improves the overall mechanical properties of the material.
Smart Images

Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of preparation of coiled materials for fitness trails, and in particular to an EVA prefabricated coiled material for fitness trails and a preparation method thereof. Background Art
[0002] The prefabricated coiled material of the fitness trail is an innovative product in modern urban green fitness facilities. It uses advanced prefabrication technology to carefully process environmentally friendly materials into highly wear-resistant and easy-to-lay coiled materials. This kind of trail is not only beautiful in appearance and colorful, but also can blend harmoniously with the surrounding environment and improve the quality of urban landscape. More importantly, it has excellent practical performance.
[0003] Prefabricated coiled fitness trails are quick to install and easy to maintain, greatly shortening the construction period and reducing the impact on daily life. The surface has been specially treated to provide good anti-slip and shock absorption effects, providing users with a safe and comfortable experience whether they are jogging, walking or cycling in the morning. In addition, the prefabricated coiled fitness trails also take into account environmental protection and sustainability. Most of the materials used are recyclable or biodegradable materials, reducing the consumption of natural resources and environmental pollution. It is not only a good place for urban residents to exercise, but also an important window to show the green, healthy and vibrant image of the city.
[0004] However, existing prefabricated coils all have the problems of easy aging and cracking and poor impact toughness. This is mainly because in the process of preparing the prefabricated coils by blending polymers and rubber particles, ethylene-vinyl acetate copolymer is often used as a compatibilizer to improve the interfacial compatibility between the two. However, adding too much ethylene-vinyl acetate copolymer will lead to a decrease in the impact toughness of the final material, while reducing the amount added will lead to a loose bond between the two, making the rubber particles easy to fall off. In addition, the flame retardant added directly will also cause agglomeration and uneven dispersion, resulting in a decrease in the mechanical properties of some areas of the material. Summary of the invention
[0005] The object of the present invention is to provide an EVA prefabricated coil for a fitness trail and a preparation method thereof, so as to solve the problems existing in the prior art.
[0006] In order to solve the above technical problems, the present application adopts a modified ethylene-vinyl acetate copolymer. An antioxidant monomer is added to the ethylene-vinyl acetate copolymer to improve its antioxidant ability on the one hand, and the addition of a hard segment chain can also improve the overall impact resistance on the other hand. The surface of the added flame retardant particles is grafted with siloxane to improve its dispersibility, and the outer layer of siloxane can also form intermolecular hydrogen bonds inside the material to improve the overall mechanical properties of the material. The present invention provides the following technical solutions:
[0007] A method for preparing an EVA prefabricated coil for a fitness trail comprises the following preparation steps:
[0008] S1. Weigh ethylene-vinyl acetate copolymer and antioxidant monomer in a mass ratio of 1:0.5-0.6, add the pre-irradiated ethylene-vinyl acetate copolymer and the antioxidant monomer to deionized water 10-12 times the mass of the antioxidant monomer, stir evenly, add 0.08-0.1 times the mass of the antioxidant monomer calcium hydroxyphosphate and 0.06-0.08 times the mass of the antioxidant monomer sodium dodecylbenzene sulfonate in sequence, stir evenly, add 0.003-0.005 times the mass of the antioxidant monomer benzoyl peroxide, stir evenly, react at a temperature of 60-80°C for 7-9h, filter after the reaction, wash the filtered product with deionized water 2-3 times, and vacuum dry at a temperature of 60-80°C for 8-12h to obtain a modified ethylene-vinyl acetate copolymer;
[0009] S2. Weigh 35-40 parts of polystyrene, 5-8 parts of modified ethylene-vinyl acetate copolymer, 50-55 parts of waste rubber particles, 8-10 parts of styrene-butadiene-styrene and 0.3-0.5 parts of flame retardant particles by mass fraction, melt-mix the polystyrene, modified ethylene-vinyl acetate copolymer and styrene-butadiene-styrene at a temperature of 160-170°C and a rotation speed of 75-85r / min, add the waste rubber particles after melt mixing for 3-5 minutes, continue mixing for 5-8 minutes, and then form a sheet through a cold rolling machine. After cold pressing, an EVA prefabricated coil is obtained.
[0010] As an optimization, the antioxidant monomer includes the following preparation steps: adding triethylenetetramine bridge-accepting hindered phenol to ethyl acetate at a mass ratio of 1:2~2.2, stirring evenly, and preparing a triethylenetetramine bridge-accepting hindered phenol solution; weighing hydroxyethyl acrylate and isophorone diisocyanate at a mass ratio of 1:2.45~2.5, adding dibutyltin dilaurate (0.01%~0.03% by mass of hydroxyethyl acrylate) to isophorone diisocyanate, and then adding isophorone diisocyanate to the isophorone diisocyanate under nitrogen protection at a temperature of 35~40°C within 0.5~0.6h. Hydroxyethyl acrylate is added dropwise to the cyanate ester at a uniform speed, and the reaction is carried out for 1 to 1.5 hours after the addition is completed. After the reaction is completed, a triethylenetetramine bridge-accepting hindered phenol solution in an amount of 9.6 to 9.8 times the mass of hydroxyethyl acrylate is added, and dibutyltin dilaurate in an amount of 0.01% to 0.03% of the mass of hydroxyethyl acrylate is added again. The reaction is carried out for 15 to 18 hours after the addition is completed. After the reaction is completed, the solvent is removed by rotary evaporation at a temperature of 45 to 55°C and a pressure of 130 to 135 Pa, and then the antioxidant monomer is obtained after washing with deionized water for 3 to 5 times.
[0011] As an optimization, the triethylenetetramine bridged hindered phenol comprises the following preparation steps: adding 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride to a benzene solvent at a mass ratio of 1:7-7.5, stirring evenly, and preparing a 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride solution for standby use; adding triethylenetetramine to deionized water at a mass ratio of 1:20-22, stirring evenly, and uniformly adding triethylenetetramine at a mass ratio of 85 to 100 g / cm2 over 2-2.5 h at a temperature of 0-5 °C. ~90 times of 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride solution, after the addition is completed, a 20% by mass fraction potassium carbonate aqueous solution is used to adjust the pH to 9~10; after the pH adjustment is completed, the reaction is carried out at a temperature of 25~30℃ for 22~26h, and after the reaction is completed, the solvent is removed by rotary evaporation at a temperature of 45~55℃ and a pressure of 130~135Pa, and then washed with deionized water for 3~5 times to obtain triethylenetetramine bridged hindered phenol.
[0012] As an optimization, the flame retardant particles include the following preparation steps: adding modified ammonium polyphosphate to butanol at a mass ratio of 1:8~9, adding vinyltrimethoxysilane in an amount of 1.2~1.4 times the mass of the modified ammonium polyphosphate, and then adding sodium butoxide in an amount of 0.01%~0.015% times the mass of the modified ammonium polyphosphate, reacting at a temperature of 35~45°C for 10~12h, filtering after the reaction is completed, and drying the filtered product at a temperature of 85~95°C for 4~4.5h to obtain flame retardant particles.
[0013] As an optimization, the modified ammonium polyphosphate includes the following preparation steps: adding ammonium polyphosphate to an ethanol aqueous solution with a mass fraction of 45-50% according to a mass ratio of 1:3.8-4.2, stirring evenly, and then adding 1,4-butanediamine with a mass fraction of 0.3-0.35 times the mass of the ammonium polyphosphate, stirring and condensing reflux reaction at a temperature of 75-85°C for 4-4.5 hours, filtering after the reaction is completed, and washing with deionized water 2-3 times, and drying at a temperature of 85-95°C for 4-4.5 hours to obtain the modified ammonium polyphosphate.
[0014] An EVA prefabricated coil for a fitness trail is prepared by any of the preparation methods described above.
[0015] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0016] The present application adopts polystyrene, modified ethylene-vinyl acetate copolymer, waste rubber particles, styrene-butadiene-styrene and flame retardant particles to be melt blended and then cold rolled to form; the requirements of adapting to the impact load of the fitness trail are met by adjusting the ratio of various materials, and the added ethylene-vinyl acetate copolymer makes it have good processability, and because an antioxidant is added to the modified ethylene-vinyl acetate copolymer, the anti-aging performance of the material is improved and its service life is extended;
[0017] The ethylene-vinyl acetate copolymer used therein is polymerized with an antioxidant monomer and an ethylene-vinyl acetate copolymer to prepare a modified ethylene-vinyl acetate copolymer, wherein the antioxidant monomer is triethylenetetramine bridged with a hindered phenol to construct a hindered phenol macromonomer structure, and the modified hindered phenol macromonomer structure has good processing stability and thermal oxidation stability in the polystyrene and modified ethylene-vinyl acetate copolymer system, and can effectively inhibit the thermal oxidation aging degradation of the material; and the longer bridging group makes the melt of the final material have a lower flow rate and prolongs its oxidation induction cycle and significantly improves the mechanical properties of the final material, after the triethylenetetramine bridge is accepted The antioxidant monomer with a stable synthesis effect is designed through the reaction of hydroxyl and isocyanate groups, and then it is polymerized with the ethylene-vinyl acetate copolymer through copolymerization, because the ethylene-vinyl acetate copolymer has good dispersibility during the blending process, it can be evenly distributed throughout the material, and it itself has good aging resistance, and a large amount of hard segment chains are added after the addition of the antioxidant monomer to significantly improve its strength, impact toughness and environmental stress cracking resistance;
[0018] The flame retardant particles use ammonium polyphosphate as the main body. Since ammonium polyphosphate itself has poor dispersibility, 1,4-butanediamine is first used for ion modification. On the one hand, a carbon source is constructed on its surface, and a carbon layer can be formed on its surface during the flame retardant process to improve its flame retardant effect. On the other hand, the grafted amino group can undergo Michael addition reaction with the double bond to form a wall layer constructed by siloxane on its periphery, thereby improving its dispersibility and making it less likely to agglomerate during the dispersion process. In addition, the siloxane on its periphery will also construct intermolecular hydrogen bonds with a large number of hydroxyl groups on the hindered phenol in the molten state, constructing a cross-linked network to improve the mechanical properties of the material. DETAILED DESCRIPTION
[0019] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0020] In order to more clearly illustrate the method provided by the present invention, the following examples are provided in detail. The raw materials used in the experimental part of the following examples are as follows.
[0021] Table 1: Raw materials used in the experimental part
[0022] .
[0023] Example 1
[0024] S1. Add 3,5-bis(tert-butyl)-4-hydroxybenzene propionyl chloride to benzene solvent at a mass ratio of 1:7, stir evenly, and prepare a 3,5-bis(tert-butyl)-4-hydroxybenzene propionyl chloride solution for standby use; add triethylenetetramine to deionized water at a mass ratio of 1:20, stir evenly, and evenly add 3,5-bis(tert-butyl)-4-hydroxybenzene propionyl chloride solution of 85 times the mass of triethylenetetramine within 2 hours at a temperature of 0°C. After the addition is completed, adjust the pH to 9 with a 20% potassium carbonate aqueous solution; after the pH adjustment is completed, react at a temperature of 25°C for 22 hours. After the reaction is completed, remove the solvent by rotary evaporation at a temperature of 45°C and a pressure of 130Pa, and then wash with deionized water 3 times to obtain a triethylenetetramine bridged hindered phenol;
[0025] S2, according to the mass ratio of 1:2, triethylenetetramine bridge accepting hindered phenol is added to ethyl acetate, stirred evenly, and prepared into triethylenetetramine bridge accepting hindered phenol solution; hydroxyethyl acrylate and isophorone diisocyanate are weighed according to the mass ratio of 1:2.45, and dibutyltin dilaurate is added to isophorone diisocyanate at a mass ratio of 0.01% of the mass of hydroxyethyl acrylate, and then hydroxyethyl acrylate is uniformly added to isophorone diisocyanate within 0.5h under nitrogen protection and at a temperature of 35°C. After the addition is completed, the reaction is carried out for 1h. After the reaction is completed, a triethylenetetramine bridge accepting hindered phenol solution with a mass ratio of 9.6 times that of hydroxyethyl acrylate is added, and dibutyltin dilaurate is added again at a mass ratio of 0.01% of the mass of hydroxyethyl acrylate. After the addition is completed, the reaction is terminated after 15h. After the reaction is completed, the solvent is removed by rotary evaporation at a temperature of 45°C and a pressure of 130Pa, and then washed with deionized water for 3 times to obtain an antioxidant monomer;
[0026] S3, weighing ethylene-vinyl acetate copolymer and antioxidant monomer according to a mass ratio of 1:0.5, adding the ethylene-vinyl acetate copolymer after pre-irradiation treatment and the antioxidant monomer to deionized water 10 times the mass of the antioxidant monomer, stirring evenly, adding 0.08 times the mass of the antioxidant monomer calcium hydroxyphosphate and 0.06 times the mass of the antioxidant monomer sodium dodecylbenzene sulfonate in sequence, stirring evenly, adding 0.003 times the mass of the antioxidant monomer benzoyl peroxide, stirring evenly, stirring at a temperature of 60°C for 7h, after the reaction is completed, filtering and washing the filtered product with deionized water twice, and vacuum drying at a temperature of 60°C for 8h to obtain a modified ethylene-vinyl acetate copolymer;
[0027] S4, according to the mass ratio of 1:3.8, add ammonium polyphosphate to an ethanol aqueous solution with a mass fraction of 45%, stir evenly, then add 1,4-diaminobenzene with a mass of 0.3 times of the mass of the ammonium polyphosphate, stir and reflux for 4 hours at a temperature of 75°C, filter after the reaction is completed, wash twice with deionized water, and dry at a temperature of 85°C for 4 hours to obtain modified ammonium polyphosphate;
[0028] S5. Add modified ammonium polyphosphate to butanol at a mass ratio of 1:8, then add vinyl trimethoxy silane which is 1.2 times the mass of the modified ammonium polyphosphate, and then add sodium butoxide which is 0.01% times the mass of the modified ammonium polyphosphate, and react at a temperature of 35°C for 10 hours. After the reaction is completed, filter and dry the filtered product at a temperature of 85°C for 4 hours to obtain flame retardant particles.
[0029] S6. Weigh 35 parts of polystyrene, 5 parts of modified ethylene-vinyl acetate copolymer, 50 parts of waste rubber particles, 8 parts of styrene-butadiene-styrene and 0.3 parts of flame retardant particles by mass fraction, melt-mix the polystyrene, modified ethylene-vinyl acetate copolymer and styrene-butadiene-styrene at a temperature of 160°C and a rotation speed of 75 / min, add the waste rubber particles after melt mixing for 3 minutes, continue mixing for 5 minutes, and then form a sheet through a cold rolling machine. After cold pressing, an EVA prefabricated coil is obtained.
[0030] Example 2
[0031] S1. Add 3,5-bis(tert-butyl)-4-hydroxybenzene propionyl chloride to benzene solvent at a mass ratio of 1:7.25, stir evenly, and prepare a 3,5-bis(tert-butyl)-4-hydroxybenzene propionyl chloride solution for standby use; add triethylenetetramine to deionized water at a mass ratio of 1:21, stir evenly, and evenly add 85-90 times the mass of triethylenetetramine 3,5-bis(tert-butyl)-4-hydroxybenzene propionyl chloride solution within 2.2 hours at a temperature of 3°C. After the addition is complete, adjust the pH to 9.5 with a 20% potassium carbonate aqueous solution; after the pH adjustment is completed, react at a temperature of 25-30°C for 24 hours. After the reaction is completed, remove the solvent by rotary evaporation at a temperature of 50°C and a pressure of 133Pa, and then wash 4 times with deionized water to obtain a triethylenetetramine bridged hindered phenol;
[0032] S2, according to the mass ratio of 1:2.1, triethylenetetramine bridge accepting hindered phenol is added to ethyl acetate, stirred evenly, and prepared into triethylenetetramine bridge accepting hindered phenol solution; hydroxyethyl acrylate and isophorone diisocyanate are weighed according to the mass ratio of 1:2.47, dibutyltin dilaurate is added to isophorone diisocyanate at a mass ratio of 0.02% of the mass of hydroxyethyl acrylate, and then hydroxyethyl acrylate is uniformly added to isophorone diisocyanate within 0.55h under nitrogen protection and at a temperature of 35°C. After the addition is completed, the reaction is carried out for 1.25h. After the reaction is completed, 9.7 times the mass of hydroxyethyl acrylate triethylenetetramine bridge accepting hindered phenol solution is added, and dibutyltin dilaurate is added again at a mass ratio of 0.02% of the mass of hydroxyethyl acrylate. After the addition is completed, the reaction is terminated after 16h. After the reaction is completed, the solvent is removed by rotary evaporation at a temperature of 50°C and a pressure of 135Pa, and then washed 4 times with deionized water to obtain an antioxidant monomer;
[0033] S3, weighing ethylene-vinyl acetate copolymer and antioxidant monomer according to a mass ratio of 1:0.55, adding the ethylene-vinyl acetate copolymer after pre-irradiation treatment and the antioxidant monomer to deionized water 11 times the mass of the antioxidant monomer, stirring evenly, adding 0.09 times the mass of the antioxidant monomer calcium hydroxyphosphate and 0.07 times the mass of the antioxidant monomer sodium dodecylbenzene sulfonate in sequence, stirring evenly, adding 0.004 times the mass of the antioxidant monomer benzoyl peroxide, stirring evenly, stirring at a temperature of 70°C for 8h, after the reaction is completed, filtering and washing the filtered product with deionized water 3 times, and vacuum drying at a temperature of 70°C for 10h to obtain a modified ethylene-vinyl acetate copolymer;
[0034] S4, according to the mass ratio of 1:4, add ammonium polyphosphate to a 45% ethanol aqueous solution, stir evenly, then add 1,4-diaminodiamine (0.32 times the mass of ammonium polyphosphate), stir and reflux for 4.5 hours at 80°C, filter after the reaction is completed, wash with deionized water 3 times, and dry at 90°C for 4.5 hours to obtain modified ammonium polyphosphate;
[0035] S5. Add modified ammonium polyphosphate to butanol at a mass ratio of 1:7, then add vinyl trimethoxy silane which is 1.3 times the mass of the modified ammonium polyphosphate, then add sodium butoxide which is 0.015% times the mass of the modified ammonium polyphosphate, and react at a temperature of 40°C for 11 hours. After the reaction is completed, filter and dry the filtered product at a temperature of 90°C for 4.5 hours to obtain flame retardant particles.
[0036] S6. Weigh 38 parts of polystyrene, 7 parts of modified ethylene-vinyl acetate copolymer, 54 parts of waste rubber particles, 9 parts of styrene-butadiene-styrene and 0.4 parts of flame retardant particles by mass, melt-mix the polystyrene, modified ethylene-vinyl acetate copolymer and styrene-butadiene-styrene at a temperature of 165°C and a rotation speed of 80 r / min, add the waste rubber particles after melt mixing for 4 minutes, continue mixing for 7 minutes, and then form a sheet through a cold rolling machine. After cold pressing, an EVA prefabricated coil is obtained.
[0037] Example 3
[0038] S1. Add 3,5-bis(tert-butyl)-4-hydroxybenzene propionyl chloride to benzene solvent at a mass ratio of 1:7.5, stir evenly, and prepare a 3,5-bis(tert-butyl)-4-hydroxybenzene propionyl chloride solution for standby use; add triethylenetetramine to deionized water at a mass ratio of 1:22, stir evenly, and evenly add 3,5-bis(tert-butyl)-4-hydroxybenzene propionyl chloride solution with a mass of 90 times that of triethylenetetramine at a temperature of 5°C within 2.5 hours. After the addition is completed, adjust the pH to 10 with a 20% potassium carbonate aqueous solution; after the pH adjustment is completed, react at a temperature of 30°C for 26 hours. After the reaction is completed, remove the solvent by rotary evaporation at a temperature of 55°C and a pressure of 135Pa, and then wash with deionized water 5 times to obtain a triethylenetetramine bridged hindered phenol;
[0039] S2. Add triethylenetetramine bridge-accepting hindered phenol to ethyl acetate at a mass ratio of 1:2.2, stir evenly, and prepare a triethylenetetramine bridge-accepting hindered phenol solution; weigh hydroxyethyl acrylate and isophorone diisocyanate at a mass ratio of 1:2.5, add 0.03% of dibutyltin dilaurate by mass of hydroxyethyl acrylate in isophorone diisocyanate, then add hydroxyethyl acrylate to isophorone diisocyanate at a uniform rate within 0.6h under nitrogen protection and at a temperature of 40°C, react for 1.5h after the addition is completed, add 9.8 times the mass of hydroxyethyl acrylate triethylenetetramine bridge-accepting hindered phenol solution after the reaction is completed, and add 0.03% of dibutyltin dilaurate by mass of hydroxyethyl acrylate again, and react for 18h after the addition is completed, and after the reaction is completed, remove the solvent by rotary evaporation at a temperature of 55°C and a pressure of 135Pa, and then wash with deionized water 3 to 5 times to obtain an antioxidant monomer;
[0040] S3, weighing ethylene-vinyl acetate copolymer and antioxidant monomer according to a mass ratio of 1:0.6, adding the ethylene-vinyl acetate copolymer after pre-irradiation treatment and the antioxidant monomer to deionized water 12 times the mass of the antioxidant monomer, stirring evenly, adding 0.1 times the mass of the antioxidant monomer calcium hydroxyphosphate and 0.08 times the mass of the antioxidant monomer sodium dodecylbenzene sulfonate in sequence, stirring evenly, adding 0.005 times the mass of the antioxidant monomer benzoyl peroxide, stirring evenly, stirring at a temperature of 80°C for 9h, after the reaction is completed, filtering and washing the filtered product with deionized water 3 times, and vacuum drying at a temperature of 80°C for 12h to obtain a modified ethylene-vinyl acetate copolymer;
[0041] S4. Add ammonium polyphosphate to a 50% ethanol aqueous solution at a mass ratio of 1:4.2, stir evenly, then add 1,4-butanediamine (0.35 times the mass of the ammonium polyphosphate), stir and reflux for 4.5 hours at 85°C, filter after the reaction is complete, wash with deionized water 3 times, and dry at 95°C for 4.5 hours to obtain modified ammonium polyphosphate;
[0042] S5. Add modified ammonium polyphosphate to butanol at a mass ratio of 1:9, then add vinyltrimethoxysilane which is 1.4 times the mass of the modified ammonium polyphosphate, and then add sodium butoxide which is 0.015% times the mass of the modified ammonium polyphosphate, and react at a temperature of 45°C for 12 hours. After the reaction is completed, filter the filtered product, and dry it at a temperature of 95°C for 4.5 hours to obtain flame retardant particles.
[0043] S6. Weigh 40 parts of polystyrene, 8 parts of modified ethylene-vinyl acetate copolymer, 55 parts of waste rubber particles, 10 parts of styrene-butadiene-styrene and 0.5 parts of flame retardant particles by mass fraction, melt-mix the polystyrene, modified ethylene-vinyl acetate copolymer and styrene-butadiene-styrene at a temperature of 170°C and a rotation speed of 85 r / min, add the waste rubber particles after melt mixing for 5 minutes, continue mixing for 8 minutes, and then form a sheet through a cold rolling machine. After cold pressing, an EVA prefabricated coil is obtained.
[0044] Example 4
[0045] The only difference from Example 2 is step S6: replacing the "flame retardant particles" therein with "modified ammonium polyphosphate".
[0046] Example 5
[0047] The only difference from Example 2 is that in step S6, the "flame retardant particles" are replaced with "ammonium polyphosphate".
[0048] Example 6
[0049] The only difference from Example 2 is that in step S6, "modified ethylene-vinyl acetate copolymer" is replaced by "ethylene-vinyl acetate copolymer".
[0050] Test Example 1
[0051] Mechanical properties and aging resistance tests:
[0052] The EVA prefabricated coils prepared in Examples 1 to 6 were cut into 2 mm thick and then prepared into a dumbbell shape. The tensile strength and elongation at break of the composite material samples were measured using an electronic universal testing machine. The tensile speed was set to 500 mm / min, the temperature was set to 23° C., and the relative humidity was 62% HR. The initial tensile strength was calculated.
[0053] The aging resistance test is carried out simultaneously with the mechanical properties: first, a xenon lamp is used to simulate the entire spectrum of sunlight, and the sample is placed in a xenon lamp accelerated aging test chamber. The aging time is 360 hours. The experimental conditions are air atmosphere, temperature 65°C, the light source is 25cm away from the sample, and the radiation intensity is 550W / m2. The tensile strength is tested again and counted as the tensile strength after aging.
[0054] The performance retention rate is calculated by the initial tensile strength and the tensile strength after aging; performance retention rate = tensile strength after aging / initial tensile strength.
[0055] Table 2: Mechanical properties and aging resistance test results
[0056]
[0057] From the comparison of the experimental data of Examples 1 to 3 in Table 2, it can be found that the prefabricated profiles prepared by the present invention have good mechanical properties, good performance retention rate, and excellent anti-aging performance.
[0058] In Example 4, the tensile strength and performance retention rate did not decrease too much, mainly because the modified ammonium polyphosphate used in it has been modified, and its dispersibility has been sufficiently improved. Although it is still inferior to the final flame retardant particles, its dispersion degree still maintains a good state and has little effect on the final material performance;
[0059] In Example 5, due to the direct addition of ammonium polyphosphate, it is easy to agglomerate in the material, resulting in poor final experimental results;
[0060] In Example 6, since ethylene-vinyl acetate copolymer was used, although its initial performance was good, its performance decreased significantly after aging, mainly because no antioxidant was added therein, and the initial tensile strength decreased due to the lack of antioxidant as a hard segment chain, resulting in a decrease in tensile strength.
[0061] Test Example 2
[0062] Flame retardant performance test:
[0063] Flame retardant performance test method: According to ISO2406 standard, test limit oxygen index, sample size 110×10×2mm 3 The results are shown in Table 3.
[0064] Table 3: Flame retardant performance test results
[0065]
[0066] From the comparison of the experimental data in Examples 1 to 3 in Table 3, it can be found that the prefabricated profile prepared by the present invention has good flame retardant properties.
[0067] In Example 4, since siloxane is not grafted on the surface, its flame retardant effect is still reduced, because siloxane itself also has a certain degree of flame retardant performance;
[0068] The performance in Example 5 is the same as in the above test. Since it is not easy to disperse, the content in the final material is unstable, resulting in poor final flame retardant effect;
[0069] Although there is a decrease in Example 6, it is still not much different from Examples 1 to 3, because although the ethylene-vinyl acetate copolymer is not modified, it does not affect the distribution of ammonium polyphosphate in the material and has little effect on the final flame retardant efficiency.
[0070] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.
Claims
1. A method for preparing an EVA prefabricated coil for a fitness trail, characterized in that: The method comprises the following preparation steps: S1. Weigh ethylene-vinyl acetate copolymer and antioxidant monomer in a mass ratio of 1:0.5-0.6, add the pre-irradiated ethylene-vinyl acetate copolymer and the antioxidant monomer to deionized water 10-12 times the mass of the antioxidant monomer, stir evenly, add 0.08-0.1 times the mass of the antioxidant monomer calcium hydroxyphosphate and 0.06-0.08 times the mass of the antioxidant monomer sodium dodecylbenzene sulfonate in sequence, stir evenly, add 0.003-0.005 times the mass of the antioxidant monomer benzoyl peroxide, stir evenly, react at a temperature of 60-80°C for 7-9h, filter after the reaction, wash the filtered product with deionized water 2-3 times, and vacuum dry at a temperature of 60-80°C for 8-12h to obtain a modified ethylene-vinyl acetate copolymer; S2. Weigh 35-40 parts of polystyrene, 5-8 parts of modified ethylene-vinyl acetate copolymer, 50-55 parts of waste rubber particles, 8-10 parts of styrene-butadiene-styrene and 0.3-0.5 parts of flame retardant particles by mass fraction, melt-mix the polystyrene, modified ethylene-vinyl acetate copolymer and styrene-butadiene-styrene at a temperature of 160-170°C and a rotation speed of 75-85 r / min, add the waste rubber particles after melt mixing for 3-5 minutes, continue mixing for 5-8 minutes, and form a sheet by a cold rolling machine. After cold pressing, obtain an EVA prefabricated coil; The antioxidant monomer comprises the following preparation steps: adding triethylenetetramine bridged hindered phenol to ethyl acetate at a mass ratio of 1:2-2.2, stirring evenly, and preparing a triethylenetetramine bridged hindered phenol solution; weighing hydroxyethyl acrylate and isophorone diisocyanate at a mass ratio of 1:2.45-2.5, adding dibutyltin dilaurate in an amount of 0.01%-0.03% by mass of hydroxyethyl acrylate to isophorone diisocyanate, and then adding isophorone diisocyanate to the isophorone diisocyanate under nitrogen protection at a temperature of 35-40°C within 0.5-0.6h. Hydroxyethyl acrylate is uniformly added to the acid ester, and the reaction is performed for 1 to 1.5 hours after the addition is completed. After the reaction is completed, a triethylenetetramine bridge acceptor hindered phenol solution of 9.6 to 9.8 times the mass of hydroxyethyl acrylate is added, and dibutyltin dilaurate of 0.01% to 0.03% of the mass of hydroxyethyl acrylate is added again. After the addition is completed, the reaction is completed for 15 to 18 hours. After the reaction is completed, the solvent is removed by rotary evaporation at a temperature of 45 to 55° C. and a pressure of 130 to 135 Pa, and then washed with deionized water for 3 to 5 times to obtain an antioxidant monomer; The triethylenetetramine bridged hindered phenol comprises the following preparation steps: adding 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride to a benzene solvent at a mass ratio of 1:7-7.5, stirring evenly, and preparing a 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride solution for standby use; adding triethylenetetramine to deionized water at a mass ratio of 1:20-22, stirring evenly, and uniformly dropping 85-9% triethylenetetramine at a temperature of 0-5°C within 2-2.5 hours. 0 times of 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride solution, after the addition is complete, a 20% by mass potassium carbonate aqueous solution is used to adjust the pH to 9-10; after the pH adjustment is completed, the reaction is carried out at a temperature of 25-30°C for 22-26 hours, and after the reaction is completed, the solvent is removed by rotary evaporation at a temperature of 45-55°C and a pressure of 130-135Pa, and then washed with deionized water for 3-5 times to obtain a triethylenetetramine bridged hindered phenol; The flame retardant particles include the following preparation steps: adding modified ammonium polyphosphate to butanol at a mass ratio of 1:8-9, then adding vinyl trimethoxy silane in an amount of 1.2-1.4 times the mass of the modified ammonium polyphosphate, and then adding sodium butoxide in an amount of 0.01%-0.015% times the mass of the modified ammonium polyphosphate, reacting at a temperature of 35-45°C for 10-12 hours, filtering after the reaction is completed, and drying the filtered product at a temperature of 85-95°C for 4-4.5 hours to obtain flame retardant particles; The modified ammonium polyphosphate comprises the following preparation steps: adding ammonium polyphosphate to an ethanol aqueous solution with a mass fraction of 45-50% according to a mass ratio of 1:3.8-4.2, stirring evenly, adding 1,4-butanediamine with a mass fraction of 0.3-0.35 times of the mass of the ammonium polyphosphate, stirring and condensing and refluxing for 4-4.5 hours at a temperature of 75-85°C, filtering after the reaction is completed, washing with deionized water for 2-3 times, and drying at a temperature of 85-95°C for 4-4.5 hours to obtain the modified ammonium polyphosphate.
2. An EVA prefabricated coil for a fitness trail, characterized in that: The method is prepared according to claim 1.