Resin derived carbon loaded metal-metal sulfide heterojunction particle catalyst, and preparation method and application thereof
By forming a metal-metal sulfide heterojunction particle catalyst in situ on a carbon support, the structural stability and preparation process problems of the carbon-supported catalyst are solved, and the preparation of catalysts with high activity and stability is achieved, which is suitable for industrial applications.
Patent Information
- Application Number
- CN202310356489.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-06
- Publication Date
- 2024-10-15
AI Technical Summary
Existing carbon-supported catalysts have deficiencies in structural stability and preparation processes, which lead to agglomeration and loss of metal catalysts, increase preparation costs and cause environmental pollution, and it is difficult to simultaneously prepare metals and metal oxides or metal sulfide under the same conditions. Material heterojunction particles.
A combination of sulfonic acid-based cation exchange resin and metal salt solution is used to form a resin-derived carbon-supported metal-metal sulfide heterojunction particle catalyst through carbonization treatment to achieve in-situ synthesis and improve the dispersion and binding force of metal particles. And form zero-valent metals and metal sulfides simultaneously under the same conditions.
It improves the reaction activity and stability of the catalyst, reduces the preparation cost, is suitable for large-scale production, and shows high activity and stability in different catalytic reactions.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of catalyst preparation, and specifically relates to a resin-derived carbon-supported metal-metal sulfide heterojunction particle catalyst, a preparation method and an application thereof. Background Art
[0002] Carbon materials have the characteristics of high specific surface area, excellent conductivity, chemical inertness, high temperature resistance, and high mechanical strength. They are a good catalyst carrier material. However, the structural stability of carbon materials makes the interaction between them and active metal catalysts weak, which easily causes the agglomeration and loss of metal catalysts during use, greatly reducing the stability of the catalyst. In addition, in the process of preparing carbon-supported catalysts, the carbon carrier needs to be treated with strong acid first to introduce oxygen-containing functional groups. In this process, a large amount of acid-containing wastewater will be generated, which not only greatly increases the preparation cost of the catalyst, but also pollutes the environment. Therefore, designing a green and simple synthesis method to prepare carbon-supported metal catalysts with high activity and high stability has become one of the urgent problems to be solved in the field of industrial production. Long-term studies have found that zero-valent metal particles have shown high catalytic activity in many catalytic reactions, and thus have been vigorously developed. At present, carbon-supported metal catalysts (M / C) are also the most widely used industrial catalysts. In recent years, it has been found that metal oxides (MO x ) thin layer has a great effect on improving the catalytic activity of metal particles. Li Landong et al. prepared Ni-NiO heterojunction particles to prove that in the process of catalytic hydrogenation, Ni and NiO play the role of adsorbing and dissociating H2 and adsorbing and activating reaction substrates respectively, so this Ni-NiO heterojunction particle shows super high catalytic activity in the process of catalytic hydrogenation. In addition, in the process of photocatalysis and electrocatalysis, a large number of studies have shown that in the formation of metal-metal oxide (M-MO x ) or metal-metal sulfide (M-MS x ) After forming a heterojunction, its contact interface will greatly accelerate the transfer of electrons or free radicals between the two phases of the material, so that the overall catalyst exhibits excellent photocatalytic or electrocatalytic performance. Although metal heterojunctions have shown high catalytic performance in multiple catalytic fields such as hydrogenation catalysis, photocatalysis, and electrocatalysis, the preparation of metal heterojunction particles is still very challenging. This is because different phases have different thermodynamic and chemical stabilities and are difficult to obtain simultaneously under the same preparation conditions. It is even more difficult to simultaneously form two chemical compositions, metal and metal oxide (or metal sulfide), in a monomer particle. Summary of the invention
[0003] The present invention overcomes the deficiencies of the prior art and has good application prospects.
[0004] The first aspect of the present application protects a resin-derived carbon-supported metal-metal sulfide heterojunction catalyst M-MS, where M includes one or more of Zn, Bi, Mn, Mg, Cd, Ce, La, Fe, Co, Ni, Cu, Ag, Y, Ru, Pd, Au, and Rh, and the monomer particles of the catalyst include three phases, including two material structures of metal and metal sulfide, and a heterojunction is formed at the interface of the two materials.
[0005] Preferably, the catalyst M-MS satisfies at least one of the following conditions: (1) The particle size of the metal-metal sulfide heterojunction particle catalyst is ≤100 nm; (2) The specific surface area of the catalyst is between 200 and 500 m 2 / g; (3) Graphite sheets are formed in local areas of the catalyst, and the catalyst as a whole exhibits an amorphous carbon structure; (4) More than 14% of the pore volume of the catalyst is micropores.
[0006] The second aspect of the present application protects a method for preparing a resin-derived carbon-supported metal-metal sulfide heterojunction particle catalyst, comprising the following steps: (1) Preparing a catalyst precursor: dispersing a sulfonic acid cation exchange resin in a metal salt solution. It is understood that in order to uniformly disperse the sulfonic acid cation exchange resin in the metal salt solution, the sulfonic acid cation exchange resin can be ground into resin powder, stirred at 20-80°C for not less than 6 hours, centrifuged and washed, and then dried at a temperature not exceeding 100°C to obtain a catalyst precursor; Preferably, the metal salt includes one or more of zinc acetate, zinc nitrate, bismuth nitrate, manganese nitrate, magnesium nitrate, cadmium acetate, cerium nitrate, lanthanum nitrate, yttrium nitrate, iron nitrate, cobalt acetate, nickel acetate, copper nitrate, copper acetate, silver acetate, palladium acetate, palladium chloride, platinum nitrate, gold chloride and ruthenium trichloride.
[0007] Preferably, the metal salt solution comprises an aqueous metal salt solution, an ethanol solution or a mixture of the two; Preferably, the concentration of the metal salt solution is 0.01-0.5 mol / L, and the sulfonic acid cation exchange resin and the metal salt solution are used in a solid-liquid ratio of 0.25 g: (100-200) mL.
[0008] (2) Carbonization treatment: The catalyst precursor of step (1) is carbonized under a protective atmosphere at a carbonization temperature of 600 to 1000 °C for a carbonization time of 1 to 5 h.
[0009] Preferably, the protective atmosphere of the carbonization treatment includes one or more of nitrogen, argon and hydrogen.
[0010] Preferably, the heating rate of the carbonization treatment in step (2) is 0.5-10°C / min.
[0011] A third aspect of the present application provides for the use of the catalyst in catalytic hydrogenation, catalytic oxidation, photocatalysis and electrocatalysis.
[0012] Compared with the prior art, the present invention has the following beneficial effects: (1) The raw material sulfonic acid cation exchange resin of the present invention is easily available and cheap, and the preparation method is simple. It can prepare the carbon-supported metal-metal sulfide heterojunction particle catalyst in situ, and the product yield is high, which is suitable for large-scale production; (2) The in-situ synthesis method makes the metal particles on the carbon matrix present the characteristics of small size, high dispersion and high uniformity. The in-situ effect also significantly enhances the binding force between the resin-derived carbon and the active metal component, which will facilitate the rapid transfer of electrons, reaction molecules and energy between metal and carbon, and will also help to anchor the metal particles to prevent their aggregation, thereby greatly improving the reaction activity and stability of the catalyst; (3) Under the same reaction conditions, two phases, zero-valent metal and metal sulfide, with different thermodynamic and chemical stabilities, are simultaneously obtained in the single-substance particles; (4) The method of the present invention has great universality and can prepare different carbon-supported metal-metal sulfide heterojunction catalysts using different metal salt solutions to meet the requirements of different catalytic reactions for active species; (5) The metal-metal sulfide particles obtained by the present invention have a unique heterojunction structure, adjustable ratio, and high catalytic activity and catalytic stability; (6) The resin-derived carbon carrier of the present invention has the advantages of high conductivity, stable chemical properties, and large specific surface area, which further improves the catalytic activity and catalytic stability of the supported catalyst. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] The following drawings are only used to illustrate and explain the present invention, and are not used to limit the scope of the present invention, wherein: Figure 1 This is a transmission electron microscopy image of the heterojunction Co-Co9S8 / C catalyst obtained in Example 1.
[0014] Figure 2 This is a graph showing the absorbance change of the hydrogenation reaction of p-nitrophenol catalyzed by the heterojunction Co-Co9S8 / C catalyst obtained in Example 1.
[0015] Figure 3 The heterojunction NiFe-Ni obtained in Example 2 x Fe y Transmission electron microscopy image of S / C catalyst.
[0016] Figure 4 The heterojunction NiFe-Ni obtained in Example 2 x Fe y XRD patterns of S / C catalysts.
[0017] Figure 5 This is the XRD pattern of the Cu-Cu2S / C catalyst obtained in Example 3.
[0018] Figure 6 This is a graph showing the absorbance change of the heterojunction Cu-Cu2S / C catalyst obtained in Example 3 during catalytic reduction of Cr(VI) under light irradiation. Implementation
[0019] In order to make the above-mentioned purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are described in detail below. In the following description, many specific details are set forth to facilitate a full understanding of the present application. However, the present application can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present application, so the present application is not limited by the specific embodiments disclosed below.
[0020] In the description of this application, unless otherwise defined, unspecified professional terms and professional words have the same meaning as those commonly understood by those skilled in the art and are common knowledge of those skilled in the art, and unspecified methods are conventional methods known to those skilled in the art. The term "multiple" in this application means at least two, such as two, three, etc., unless otherwise clearly and specifically defined.
[0021] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.
[0022] In the method of the present invention, the cation exchange resin with sulfonic acid groups is the 732 type strongly acidic cation exchange resin produced by Sinopharm Chemical Reagent Co., Ltd., or it may be other types of sulfonic acid cation exchange resin products, such as D001 type and Dowex 50WX8 type.
[0023] The first aspect of the present application protects a resin-derived carbon-supported metal-metal sulfide heterojunction particle catalyst M-MS, where M includes one or more of Zn, Bi, Mn, Mg, Cd, Ce, La, Fe, Co, Ni, Cu, Ag, Y, Ru, Pd, Au, and Rh. The monomer particles of the catalyst include three phases, including two material structures of metal and metal sulfide, and a heterojunction is formed at the interface of the two materials.
[0024] The catalyst M-MS satisfies at least one of the following conditions: (1) The particle size of the metal-metal sulfide heterojunction particle catalyst is ≤100 nm; (2) The specific surface area of the catalyst is between 200 and 500 m 2 / g; (3) Graphite sheets are formed in local areas of the catalyst, and the catalyst as a whole exhibits an amorphous carbon structure; (4) More than 14% of the pore volume of the catalyst is micropores.
[0025] The second aspect of the present application protects a method for preparing a resin-derived carbon-supported metal-metal sulfide heterojunction particle catalyst, comprising the following steps: (1) Preparation of catalyst precursor: Disperse sulfonic acid cation exchange resin in metal salt solution. It can be understood that in order to make the sulfonic acid cation exchange resin uniformly dispersed in the metal salt solution, the sulfonic acid cation exchange resin can be ground into resin powder, stirred at 20-80 ° C for not less than 6 hours, stirred for more than 6 hours, preferably for more than 12 hours, and most preferably for more than 24 hours, so that the metal ions in the solution and the cation exchange resin reach ion exchange equilibrium. For example, the stirring time can be 8 hours, 12 hours, 24 hours or 36 hours. After centrifugal washing, dry at a temperature not exceeding 100 ° C to obtain a catalyst precursor. The resin powder solution that has completed the ion exchange process is centrifuged, washed, and placed in an oven for drying at a temperature not exceeding 100 ° C, preferably a drying temperature not exceeding 90 ° C, and most preferably a drying temperature of 60-80 ° C, and dried for 4-48 hours. After drying, a resin powder for exchanging metal ions, i.e., a catalyst precursor, is obtained; In the method of the present invention, when the ion exchange resin is dispersed in the metal salt solution, continuous stirring is performed to improve the dispersion uniformity and ion exchange efficiency.
[0026] The metal salt solution includes an aqueous solution, an ethanol solution or a mixed solution of the two; The type of metal salt is selected according to the type of active metal required for the target catalytic reaction, such as one or more of zinc acetate, zinc nitrate, bismuth nitrate, manganese nitrate, magnesium nitrate, cadmium acetate, cerium nitrate, lanthanum nitrate, yttrium nitrate, iron nitrate, cobalt acetate, nickel acetate, copper nitrate, copper acetate, silver acetate, palladium acetate, palladium chloride, platinum nitrate, gold chloride and ruthenium trichloride.
[0027] The concentration of the metal salt solution can be 0.01 to 0.5 mol / L. The metal salt solution is generally used in excess, at a ratio of 0.25 g of sulfonic acid cation exchange resin to 100 to 200 mL of the metal salt solution. It is understood that the concentration of the metal salt solution can be 0.01 mol / L, 0.05 mol / L, 0.10 mol / L, 0.2 mol / L or 0.5 mol / L, etc.
[0028] (2) Carbonization treatment: The catalyst precursor of step (1) is carbonized under a protective atmosphere at a carbonization temperature of 600 to 1000°C for a carbonization time of 1 to 5 hours; The protective atmosphere of the carbonization treatment can be an inert gas such as nitrogen or argon that does not burn the ion exchange resin, or hydrogen with a reducing protective effect. Alternatively, a mixed gas of nitrogen, argon and hydrogen can be used according to the target ratio between metal and metal sulfide.
[0029] The heating rate is 0.5 to 10 °C / min. The heating rate of the carbonization treatment can be adjusted according to the working conditions of the equipment. It can be understood that the heating rate can be 0.5 °C / min, 2 °C / min, 4 °C / min, 6 °C / min or 10 °C / min, etc.
[0030] High-temperature carbonization treatment transforms the resin into porous carbon (resin-derived carbon). This porous carbon material does not have a large-scale regular graphite sheet structure, but only forms graphite sheets in local areas, presenting an amorphous carbon structure as a whole. The pore structure of resin-derived carbon is mainly micropores (< 2 nm), accounting for more than 14%, with a small amount of mesopores (2 nm to 50 nm), and almost no macropores (> 50 nm). The specific surface area is 200 to 500 m 2 / g. At the same time, the high-temperature carbonization treatment also drives the exchanged metal ions to be converted in situ into zero-valent metal (M) particles or metal sulfide (MS) particles or heterogeneous (M-MS) particles where the two coexist. These in-situ formed particles are uniformly loaded on the resin-derived carbon to form a new type of carbon-supported metal catalyst (M-MS / C). Since the catalyst is formed in situ, the metal particles on the carbon matrix are characterized by small size, high dispersion and high uniformity. The in-situ action also significantly enhances the binding force between the resin-derived carbon and the active metal components, which will facilitate the rapid transfer of electrons, reaction molecules and energy between metal and carbon, and will also facilitate the anchoring of metal particles to prevent their aggregation, thereby greatly improving the reaction activity and stability of the catalyst.
[0031] The experimental method of the present invention can form in situ carrier particles containing both zero-valent metal and metal sulfide chemical compositions, which belong to metal-metal sulfide heterojunction (M-MS) particles. The special heterostructure will greatly enhance the catalytic activity of the supported particles. The scheme of the present invention can obtain different carbon-supported metal heterojunction particle catalysts according to the metal species required for the target catalytic reaction by changing the type of metal ions in the ion exchange solution and appropriately adjusting and controlling the process conditions to meet the purpose of efficiently catalyzing the target reaction. At the same time, by finely controlling the experimental conditions, the ratio and bonding mode of the metal and metal sulfide in the heterojunction particles are regulated to further enhance the catalytic activity and stability of the catalyst. Example
[0032] Take 0.25 g of 732 type sulfonic acid cation exchange resin powder in 200 mL of 0.1 mol / L cobalt acetate ethanol solution, adjust the temperature to 25 °C and continue stirring for 24 hours. After the reaction is completed, the solution is naturally cooled to room temperature, and then centrifuged, washed and dried to obtain a catalyst precursor. The dried precursor is placed in a quartz boat, and the quartz boat is placed in the center of the quartz reaction tube in the tubular furnace for carbonization. The entire carbonization process is carried out under nitrogen as a protective gas. At the same time, the furnace temperature is set to heat from room temperature to a carbonization temperature of 800 °C at a rate of 5 °C / min, and then cooled to room temperature after 2 hours of constant temperature. After the carbonization reaction is completed, the carbon-loaded Co-Co9S8 heterojunction particle catalyst (Co-Co9S8 / C) is collected, such as Figure 1 As shown. It can be seen that the lattice of this loaded particle has very clear lattice stripes, proving that it has good crystallinity. At the same time, it can be seen that the lattice stripes are not uniform in direction and can be divided into three regions. After measurement, the lattice spacing in the upper half is 0.227 and 0.222nm, corresponding to the (331) and (420) crystal planes of Co9S8, and the lattice spacing in the lower left part is 0.204nm, corresponding to the (111) crystal plane of metal Co. So Figure 1 It is proved that the loaded particles are heterojunction particles composed of two phases of Co and Co9S8, in which the upper half is Co9S8, the lower left part is metal Co, and the lower right part is the coexistence area of the two phases. Example
[0033] Take 0.25 g of 732 sulfonic acid cation exchange resin powder in 200 mL of 0.09 mol / L nickel acetate ethanol solution, stir for 30 minutes until dissolved, then add 0.04 mol / L iron nitrate ethanol solution and stir for 10 minutes until dissolved. Heat from room temperature to 80 ° C and stir for 24 hours. After the reaction is completed, cool naturally to room temperature and wash the lower precipitate repeatedly with ethanol and deionized water three times. Finally, place the product in an oven at 80 ° C overnight, put the dried precursor into a quartz boat, and place the quartz boat in the center of the quartz reaction tube in the tube furnace for carbonization. The entire carbonization process is carried out under nitrogen as a protective gas. At the same time, set the furnace temperature so that it rises from room temperature to a carbonization temperature of 800 ° C at a rate of 5 ° C / min, and cools to room temperature after 2 hours of constant temperature. After the carbonization reaction is completed, the carbon-loaded NiFe-Ni x Fe y S heterojunction particle catalyst (NiFe-Ni x Fe y S / C), such as Figure 3 , as shown in 4, NiFe-Ni xFe y The S / C particle catalyst includes Ni3S2, NiS2, Ni, Ni3Fe, and NiS phases. Example
[0034] Take 0.25 g of 732 type sulfonic acid cation exchange resin powder in 200 mL of 0.13 mol / L copper nitrate ethanol solution, adjust the temperature to 80 °C and continue stirring for 24 hours. After the reaction is completed, the solution is naturally cooled to room temperature, and the catalyst precursor is obtained by centrifugation, deionized water and ethanol washing three times and drying at 75 °C overnight. The dried precursor is placed in a quartz boat, and the quartz boat is placed in the center of the quartz reaction tube in the tubular furnace for carbonization treatment. The entire carbonization process is carried out under argon as a protective gas. At the same time, the furnace temperature is set to heat from room temperature to a carbonization temperature of 800 °C at a rate of 5 °C / min, and then cool to room temperature at a constant temperature for 2 hours. After the carbonization reaction is completed, the carbon-loaded Cu-Cu2S heterojunction particle catalyst (Cu-Cu2S / C) is collected, such as Figure 5 shown. Example
[0035] Take 0.25 g of 732 sulfonic acid cation exchange resin powder in 200 mL of 0.07 mol / L nickel acetate ethanol solution, stir for 30 minutes until dissolved, then add 0.06 mol / L ferric nitrate aqueous solution and stir for 10 minutes until dissolved. Heat from room temperature to 80 ° C and stir for 24 hours. After the reaction is completed, cool naturally to room temperature and wash the lower precipitate repeatedly with ethanol and deionized water three times. Finally, place the product in an oven at 80 ° C overnight, put the dried precursor into a quartz boat, and place the quartz boat in the center of the quartz reaction tube in the tubular furnace for carbonization. The entire carbonization process is carried out under nitrogen as a protective gas. At the same time, set the furnace temperature so that it rises from room temperature to a carbonization temperature of 800 ° C at a rate of 5 ° C / min, and cools to room temperature after 3 hours of constant temperature. After the carbonization reaction is completed, the carbon-loaded NiFe-Ni x Fe y S heterojunction particle catalyst (NiFe-Ni x Fe y S / C) Example
[0036] Photocatalytic reaction The catalyst was prepared according to the method of Example 3 and used in the photocatalytic reduction of Cr(VI) in water under visible light irradiation. The catalyst was used in an amount of 0.02 g and ultrasonically dispersed in 40 mL of a 10 mg / L K2Cr2O7 aqueous solution. After being placed in the dark and magnetically stirred for 1 hour, a 300 W xenon lamp was turned on to provide visible light to start the photocatalytic reaction. During the reaction, a fan was used to cool the lamp source and the reactor so that the entire reaction system was always kept at room temperature. The reaction time was 3 hours. The experimental results are as follows: Figure 6 As shown. The peak at 540nm in the figure is [Cr2O7] 2- As the reaction time progresses, the peak value of the peak decreases continuously, proving that under visible light irradiation, [Cr2O7] 2- was successfully reduced by the catalyst. After 180 min of reaction time, [Cr2O7] 2- The conversion rate reached 92%. Example
[0037] Electrocatalytic reaction Catalysts were prepared according to the methods of Examples 2 and 4, and used to prepare the working electrodes of this experiment, Hg / HgO electrodes were used as reference electrodes, and platinum wire was used as counter electrodes. The workstation used was a CHI 760E electrochemical workstation from Shanghai Chenhua Instrument Co., Ltd., and the electrode used was a PINE rotating disk electrode. During the test, the rotating disk electrode rotated at 1600 rpm. All tests were conducted in electrolyte at room temperature.
[0038] catalyst <![CDATA[Overpotential at a current density of 10 mA·cm -2 > <![CDATA[NiFe-Ni x Fe y S / C (Example 2)]]> 323 <![CDATA[NiFe-Ni x Fe y S / C (Example 4)]]> 420 Example
[0039] Hydrogenation catalytic reaction The catalyst was prepared according to the method of Example 1 and used for the hydrogenation reaction of p-nitrophenol. The entire hydrogenation catalytic reaction was carried out in a cuvette, and the absorbance of the reaction solution was detected in real time using a UV-visible spectrophotometer. After adding NaBH4 solution to the solution, the solution changed from light yellow to bright yellow due to the generation of p-nitrophenol anions, and the maximum absorption peak of the p-nitrophenol solution shifted from 317 nm to 400 nm. After the addition of the catalyst, the reaction occurred rapidly, and the product p-aminophenol was finally generated, with a characteristic absorption peak at 298 nm. No by-products were generated during the entire reaction process. The catalytic performance tests of all catalysts were carried out at room temperature, and the reaction results are shown in Figure 2. Figure 2 The Co-Co9S8 / C catalyst exhibited excellent catalytic hydrogenation performance and achieved complete conversion of p-nitrophenol in the solution within 9 minutes.
[0040] The method of the present invention has strong universality and can be applied to different transition metal salt solutions to prepare different carbon-supported metal-metal sulfide heterojunction catalysts. The preparation method proposed by the present invention is simple, safe, has low production cost, is easy to operate and regulate, and is suitable for industrial production application.
[0041] The above embodiments are only used to help understand the method and core idea of the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.
[0042] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A resin-derived carbon-supported metal-metal sulfide heterojunction particle catalyst M-MS, characterized in that: M includes one or more of Zn, Bi, Mn, Mg, Cd, Ce, La, Fe, Co, Ni, Cu, Ag, Y, Ru, Pd, Au, and Rh. The monomer particles of the catalyst include three phases, including two material structures of metal and metal sulfide, and a heterojunction is formed at the interface of the two materials.
2. The catalyst M-MS according to claim 1, characterized in that The catalyst satisfies at least one of the following conditions: (1) The particle size of the metal-metal sulfide heterojunction particle catalyst is ≤100 nm; (2) The specific surface area of the catalyst is between 200 and 500 m 2 / g; (3) Graphite sheets are formed in local areas of the catalyst, and the catalyst as a whole exhibits an amorphous carbon structure; (4) More than 14% of the pore volume of the catalyst is micropores.
3. A method for preparing the resin-derived carbon-supported metal-metal sulfide heterojunction particle catalyst M-MS according to any one of claims 1 to 2, characterized in that: The steps include: (1) Preparing a catalyst precursor: dispersing a sulfonic acid cation exchange resin in a metal salt solution, stirring at 20 to 80 °C for not less than 6 h, centrifugally washing, and drying at no more than 100 °C to obtain a catalyst precursor; (2) Carbonization treatment: The catalyst precursor of step (1) is carbonized under a protective atmosphere at a carbonization temperature of 600 to 1000 °C for a carbonization time of 1 to 5 h.
4. The preparation method according to claim 3, characterized in that: The metal salt includes one or more of zinc acetate, zinc nitrate, bismuth nitrate, manganese nitrate, magnesium nitrate, cadmium acetate, cerium nitrate, lanthanum nitrate, yttrium nitrate, iron nitrate, cobalt acetate, nickel acetate, copper nitrate, copper acetate, silver acetate, palladium acetate, palladium chloride, platinum nitrate, gold chloride and ruthenium trichloride.
5. The preparation method according to claim 3, characterized in that: The metal salt solution includes an aqueous solution, an ethanol solution or a mixture of the two.
6. The preparation method according to claim 3, characterized in that: The concentration of the metal salt solution is 0.01-0.5 mol / L, and the sulfonic acid cation exchange resin and the metal salt solution are used in a solid-liquid ratio of 0.25 g: (100-200) mL.
7. The preparation method according to claim 3, characterized in that: The protective atmosphere of the carbonization treatment includes one or more of nitrogen, argon and hydrogen.
8. The preparation method according to claim 3, characterized in that: The heating rate of the carbonization treatment in step (2) is 0.5-10°C / min.
9. Use of the catalyst according to any one of claims 1 to 2 or the catalyst obtained by the preparation method according to any one of claims 3 to 8 in catalytic hydrogenation, catalytic oxidation, photocatalysis and electrocatalysis.
Citation Information
Patent Citations
Bimetallic sulfide Ni3S2 / FeS composite material with heterogenous interface coupling and preparation method and application thereof
CN110314690A
Preparation method and application of metal-metal sulfide heterojunction catalyst
CN114497584A
Cited By
High-mesoporosity solid waste resin-based spherical carbonaceous porous material and preparation method thereof
CN121405087A