Magnesia-iron spinel brick and preparation method thereof
By adding iron powder, iron red and nickel oxide powder to the preparation of mafic spinel bricks, the divalent iron oxidation is prevented and nickel iron spinel and mafic spinel are formed, which solves the high-temperature burning of mafic spinel bricks. The problem of the transformation of divalent iron in Chengzhong has improved the performance of kiln skin and high-temperature strength.
Patent Information
- Application Number
- CN202411254859.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-09
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-09-09
AI Technical Summary
During the high-temperature firing process of existing mafic spinel bricks, divalent ferrous oxide transforms into trivalent iron, resulting in reduced performance and toughness of the kiln skin and insufficient high-temperature strength performance.
Iron powder, iron red and nickel oxide powder are added to the preparation of mafic spinel bricks. Through the sintering and conversion of nickel oxide, the oxidation of divalent iron is prevented and nickel iron spinel and magnesium are formed. Iron spinel improves the high-temperature strength properties of the material.
It effectively improves the kiln-hanging performance and high-temperature strength properties of mafic spinel bricks, avoids the formation of the liquid phase of iron powder, and enhances the density and high-temperature stability of the material.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of refractory materials, and in particular relates to a magnesia-iron spinel brick and a preparation method thereof. Background Art
[0002] The lining material of the high temperature zone of the cement rotary kiln is the key to ensure the stable operation of the kiln. In order to ensure the stable operation of the cement rotary kiln, its lining material needs to have good high temperature resistance, chemical stability, mechanical strength, wear resistance and thermal shock stability. Magnesia-chrome bricks are commonly used as lining materials for cement rotary kilns. Magnesia-chrome bricks are inert to alkaline cement components and have good kiln skin bonding ability. However, used magnesia-chrome bricks will produce highly toxic hexavalent chromium, which can be dissolved in water and cause serious environmental pollution.
[0003] In order to reduce environmental pollution, it is necessary to gradually replace chromium-containing refractory materials with chromium-free alkaline refractory materials. At present, magnesia-iron-aluminum spinel materials are considered to be the best materials to replace magnesia-chrome bricks. Magnesia-iron-aluminum spinel not only has the excellent performance of magnesia-chrome bricks, but also has good structural toughness and lower thermal conductivity, which can meet the demand for refractory materials in cement rotary kiln linings.
[0004] The Chinese patent document with publication number CN115124359A discloses a high-stability magnesia-iron spinel brick for cement kilns and a preparation method thereof. The magnesia-iron spinel brick is prepared by using high-iron magnesia sand, high-purity magnesia sand, magnesia-iron-aluminum spinel particles, and a resin binder. The obtained magnesia-iron spinel brick has outstanding acid and alkali corrosion resistance and can be used stably for a long time. Under the working condition of the cement rotary kiln, the presence of ferrous oxide in the magnesia-iron spinel brick can promote the stability of the cement rotary kiln skin. However, the magnesia-iron spinel brick in the above patent, during the high-temperature firing process, the divalent ferrous oxide in the magnesia-iron-aluminum spinel in the brick body will be converted into trivalent iron at high temperature, resulting in the reduction of the kiln skin performance and toughness of the brick body. Summary of the invention
[0005] The technical problem solved by the present invention is to provide a magnesia-iron spinel brick and a preparation method thereof, wherein iron powder is added to prevent the oxidation of divalent ferrous oxide in the ferroalumina spinel, thereby improving its kiln skin performance; and iron red and nickel oxide powder are added, wherein the nickel oxide converts iron and iron red into nickel-iron spinel, which covers the surface of the material, protects the divalent iron in the ferroalumina spinel from being destroyed, and avoids the formation of an iron powder liquid phase; excess iron red liquid phase forms magnesia-iron spinel with magnesium oxide, and excess nickel oxide forms a solid solution with magnesium oxide, thereby improving the high-temperature strength performance of the material.
[0006] In order to solve the above problems, one aspect of the present invention provides a magnesia-iron spinel brick, the raw materials for preparing the brick include the following components in mass percentage:
[0007] Magnesia 65%~81%, magnesia waste bricks 8%~17%, ferroalumina spinel 6%~12%, iron powder 0.5%~3%, nickel oxide powder 0.3%~3% and iron red 0.3%~3%; external binder 1%~5%.
[0008] Preferably, the raw materials for its preparation include the following components in percentage by mass:
[0009] Magnesia 71%~77%, magnesia waste bricks 12%~15%, ferroalumina spinel 8%~10%, iron powder 1%~2%, nickel oxide powder 0.5%~2% and iron red 0.5%~2%; external binder 2%~4%.
[0010] Preferably, the raw materials for its preparation include the following components in percentage by mass:
[0011] Magnesia 71%~74%, magnesia waste bricks 14%~15%, ferroalumina spinel 8%~10%, iron powder 2%, nickel oxide powder 1% and iron red 1%; external binder 3%.
[0012] Preferably, the mass ratio of iron powder, nickel oxide powder and iron oxide red is 1:0.25~1:0.25~1.
[0013] Preferably, the mass ratio of the total mass of magnesia sand and magnesia waste bricks to ferroaluminum spinel, nickel oxide powder and iron oxide red is 100:8.8~11.8:0.5~2.5:0.5~2.5.
[0014] Preferably, the magnesia includes magnesia particles with a particle size of >3mm and ≤5mm, magnesia particles with a particle size of >1mm and ≤3mm, magnesia particles with a particle size of >0mm and ≤1mm, and magnesia fine powder with a particle size of 200 mesh; the mass ratio of magnesia particles with a particle size of >3mm and ≤5mm, magnesia particles with a particle size of >1mm and ≤3mm, magnesia particles with a particle size of >0mm and ≤1mm, and magnesia fine powder with a particle size of 200 mesh is 2~8:20~28:15~22:24~27;
[0015] The iron-aluminum spinel includes iron-aluminum spinel with a particle size of >1mm and ≤3mm and iron-aluminum spinel with a particle size of >0mm and ≤1mm; the mass ratio of the iron-aluminum spinel with a particle size of >1mm and ≤3mm and the iron-aluminum spinel with a particle size of >0mm and ≤1mm is 3-8:3-5.
[0016] Preferably, the particle size of the iron powder is 200 mesh; the particle size of the nickel oxide powder is 200 mesh; and the particle size of the iron oxide red is 200 mesh.
[0017] Preferably, the magnesia is high-purity magnesia; in the high-purity magnesia, MgO>96.5wt%, SiO2<0.8wt%, Fe2O3<0.8wt%, Al2O3<0.15wt%, CaO<1.5wt%, ignition loss<0.1wt%;
[0018] In the magnesia waste brick, MgO>97wt%, SiO2<1wt%, Al2O3<1wt%, CaO<1wt%;
[0019] In the iron-aluminum spinel, Al2O3>55wt%, Fe2O3>40wt%, SiO2<0.15wt%, CaO<1.5wt%, ignition loss<3.5wt%, and bulk density>3.9g / cm 3 ;
[0020] Another object of the present invention is to provide a method for preparing the above-mentioned magnesia-iron spinel brick, comprising the following steps:
[0021] The raw materials for preparing the magnesia-iron spinel brick are mixed, then molded, and then the molded product is fired to obtain the magnesia-iron spinel brick.
[0022] Preferably, the sintering temperature is 1500-1530° C., and the sintering time is 2-10 hours.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] The magnesia-iron spinel brick of the present invention is added with iron powder to prevent the divalent ferrous oxide in the ferroalumina spinel from being converted into trivalent iron, thereby improving its kiln skin performance. Iron red and nickel oxide powder are further added. First of all, for the iron red itself, iron red (ferrous oxide) is a good sintering agent for refractory materials. In the initial stage of sintering, the iron red in the brick will produce a certain liquid phase. Due to the surface tension of the liquid phase, capillary force is generated. Under the action of the capillary force, the solid phase particles flow more greatly, so that the particles are close to each other and rearranged, which improves the stacking condition of the particles, promotes the densification process, and improves the density of the sample block. Secondly, and more importantly, during the heating process of firing, the iron powder can first prevent the divalent iron in the iron-aluminum spinel from being oxidized. As the firing continues, nickel oxide converts iron and iron red into divalent iron, namely nickel-iron spinel NiFe2O4. On the one hand, it covers the surface of the material and protects the divalent iron in the iron-aluminum spinel from being destroyed by isolating oxygen or the divalent iron in the nickel-iron spinel. On the other hand, it converts the iron powder into nickel-iron spinel to avoid the formation of liquid phase of iron powder at working temperature. Thirdly, as the firing continues, the excess iron red liquid phase in the system will be reabsorbed by the magnesium oxide in the system to form magnesium iron spinel, avoiding the existence of liquid iron red at the working temperature; since the molecular structure of nickel oxide is similar to that of magnesium oxide, the excess nickel oxide can form a solid solution with part of the magnesium oxide, and the molecules are intertwined with each other, which greatly improves the high-temperature strength performance of the material. However, due to the formation of the solid solution, the material has higher strength, higher density, and stronger rigidity, which will reduce the thermal shock performance of the material, and cracks will appear during use and the strength will deteriorate. Therefore, magnesium waste bricks are further added to improve the thermal shock stability of the material through the relatively high porosity in the magnesium waste bricks. DETAILED DESCRIPTION
[0025] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solution of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] One aspect of an embodiment of the present invention provides a magnesia-iron spinel brick, wherein the raw materials for preparing the brick include the following components in percentage by mass:
[0027] Magnesia 65%~81%, magnesia waste bricks 8%~17%, ferroalumina spinel 6%~12%, iron powder 0.5%~3%, nickel oxide powder 0.3%~3% and iron red 0.3%~3%; external binder 1%~5%.
[0028] During the high-temperature firing process of magnesia-iron spinel bricks, the divalent ferrous oxide in the ferroaluminum spinel in the raw material will be converted into trivalent iron at high temperature, which will reduce the kiln skin performance and toughness of the brick body. For this reason, in the magnesia-iron spinel bricks of the embodiment of the present invention, iron powder is added to the raw materials for preparation. The iron powder can be oxidized before the divalent iron in the ferroaluminum spinel, thereby preventing the divalent ferrous oxide in the ferroaluminum spinel from being converted into trivalent iron. However, due to the low melting point of iron powder, the unoxidized iron powder will form a liquid phase at the working temperature of the magnesia-iron spinel brick, which will reduce the high-temperature strength of the material. For this reason, iron red and nickel oxide powder are further added to the magnesia-iron spinel bricks of the embodiment of the present invention. First of all, for iron red itself, iron red (ferric oxide) is a good sintering agent for refractory materials. In the initial stage of sintering, iron red in bricks will produce a certain liquid phase. Due to the surface tension of the liquid phase, capillary force is generated. Under the action of capillary force, the solid phase particles flow more and the particles are close to each other and rearranged, which improves the accumulation of particles, promotes the densification process, and improves the density of the sample. Secondly, and more importantly, during the heating process of sintering, iron powder can first prevent the divalent iron in the iron-aluminum spinel from being oxidized. As the sintering continues, nickel oxide converts iron and iron red into divalent iron, that is, nickel-iron spinel NiFe2O4. On the one hand, it covers the surface of the material and protects the divalent iron in the iron-aluminum spinel from being destroyed by isolating oxygen or the divalent iron in the nickel-iron spinel. On the other hand, it converts iron powder into nickel-iron spinel to avoid the formation of iron powder liquid phase at working temperature. Thirdly, as the firing continues, the excess iron red liquid phase in the system will be reabsorbed by the magnesium oxide in the system to form magnesium iron spinel, avoiding the existence of liquid iron red at the working temperature; since the molecular structure of nickel oxide is similar to that of magnesium oxide, the excess nickel oxide can form a solid solution with part of the magnesium oxide, and the molecules are intertwined with each other, which greatly improves the high-temperature strength performance of the material. However, due to the formation of the solid solution, the material has higher strength, higher density, and stronger rigidity, which will reduce the thermal shock performance of the material, and cracks will appear during use and the strength will deteriorate. Therefore, magnesium waste bricks are further added to improve the thermal shock stability of the material through the relatively high porosity in the magnesium waste bricks.
[0029] In some embodiments, the raw materials for preparing the magnesia-iron spinel brick include the following components in percentage by mass:
[0030] Magnesia sand 71%~77%, magnesia waste brick 12%~15%, ferroalumina spinel 8%~10%, iron powder 1%~2%, nickel oxide powder 0.5%~2% and iron red 0.5%~2%; external binder 2%~4%. Within the above mass percentage range, the comprehensive performance of the magnesia-iron spinel brick can be better.
[0031] Further preferably, the raw materials for preparing the magnesia-iron spinel brick include the following components in percentage by mass:
[0032] Magnesia 71%~74%, magnesia waste bricks 14%~15%, ferroalumina spinel 8%~10%, iron powder 2%, nickel oxide powder 1% and iron red 1%; external binder 3%.
[0033] Since iron powder, nickel oxide powder and iron red can only generate nickel-iron spinel at a certain ratio, in addition to considering the reaction between iron powder, nickel oxide powder and iron red, iron powder also needs to prevent the oxidation of divalent iron in ferroaluminum spinel, iron red also needs to act as a sintering agent to improve material properties, and nickel oxide powder will also form a solid solution with magnesium oxide to improve material properties. Therefore, the ratio of iron powder, nickel oxide powder and iron red cannot only consider the ratio required for the reaction to generate nickel-iron spinel, but also needs to consider the other functions of each component. Preferably, the mass ratio of iron powder, nickel oxide powder and iron red is 1:0.25~1:0.25~1. At this mass ratio, the strength performance, thermal shock resistance and kiln skin performance of magnesium-iron spinel bricks can be better.
[0034] During the firing process, magnesium oxide in magnesia sand and magnesia waste bricks reacts with ferroaluminum spinel and iron red to form magnesia-iron spinel on the one hand, and forms a solid solution with nickel oxide powder on the other hand, so that the high-temperature strength of the material is improved. Taking into account the amount of different reactions, it is found through experimental attempts that preferably, the mass ratio of the total mass of magnesia sand and magnesia waste bricks to ferroaluminum spinel, nickel oxide powder, and iron red is 100:8.8~11.8:0.5~2.5:0.5~2.5. When the mass fraction within this ratio is used, the strength performance, thermal shock resistance, and kiln skin performance of magnesia-iron spinel bricks can be improved.
[0035] In some embodiments, the magnesia includes magnesia particles with a particle size of >3mm and ≤5mm, magnesia particles with a particle size of >1mm and ≤3mm, magnesia particles with a particle size of >0mm and ≤1mm, and magnesia fine powder with a particle size of 200 mesh; the mass ratio of magnesia particles with a particle size of >3mm and ≤5mm, magnesia particles with a particle size of >1mm and ≤3mm, magnesia particles with a particle size of >0mm and ≤1mm, and magnesia fine powder with a particle size of 200 mesh is 2~8:20~28:15~22:24~27.
[0036] In some embodiments, the iron-aluminum spinel includes iron-aluminum spinel with a particle size of >1 mm and ≤3 mm and iron-aluminum spinel with a particle size of >0 mm and ≤1 mm; the mass ratio of the iron-aluminum spinel with a particle size of >1 mm and ≤3 mm and the iron-aluminum spinel with a particle size of >0 mm and ≤1 mm is 3~8:3~5.
[0037] In some embodiments, the magnesia waste bricks are mainly derived from waste bricks removed from submerged arc furnaces, which are furnaces for smelting ferronickel, ferrosilicon, ferromanganese, and titanium slag. Preferably, in the magnesia waste bricks, MgO>97wt%, SiO2<1wt%, Al2O3<1wt%, and CaO<1wt%. Preferably, the particle size of the magnesia waste bricks is 200 mesh.
[0038] In some embodiments, the particle size of the iron powder is 200 mesh; the particle size of the nickel oxide powder is 200 mesh; and the particle size of the iron oxide red is 200 mesh.
[0039] In some embodiments, the magnesia is high-purity magnesia; in the high-purity magnesia, MgO>96.5wt%, SiO2<0.8wt%, Fe2O3<0.8wt%, Al2O3<0.15wt%, CaO<1.5wt%, and loss on ignition<0.1wt%.
[0040] In some embodiments, in the iron-aluminum spinel, Al2O3>55wt%, Fe2O3>40wt%, SiO2<0.15wt%, CaO<1.5wt%, ignition loss<3.5wt%, and bulk density>3.9g / cm 3 .
[0041] In some embodiments, the binding agent is pulp.
[0042] Another object of the embodiment of the present invention is to provide a method for preparing the above-mentioned magnesia-iron spinel brick, comprising the following steps:
[0043] The raw materials for preparing the magnesia-iron spinel brick are mixed, then molded, and then the molded product is fired to obtain the magnesia-iron spinel brick.
[0044] Preferably, the sintering temperature is 1500-1530° C., and the sintering time is 2-10 hours.
[0045] In the following embodiments, in high-purity magnesia, MgO>96.5wt%, SiO2<0.8wt%, Fe2O3<0.8wt%, Al2O3<0.15wt%, CaO<1.5wt%, loss on ignition<0.1wt%; in ferroaluminum spinel, Al2O3>55wt%, Fe2O3>40wt%, SiO2<0.15wt%, CaO<1.5wt%, loss on ignition<3.5wt%, bulk density>3.9g / cm 3 . Example 1
[0046] The raw materials for preparing the magnesia-iron spinel brick of this embodiment include the following components in percentage by mass:
[0047] 3% of high-purity magnesia particles with a particle size of >3mm and ≤5mm, 26% of high-purity magnesia particles with a particle size of >1mm and ≤3mm, 21% of high-purity magnesia particles with a particle size of >0mm and ≤1mm, 27% of high-purity magnesia fine powder with a particle size of 200 mesh, 12% of magnesia waste bricks with a particle size of 200 mesh, 4% of iron-aluminum spinel with a particle size of >1mm and ≤3mm, 4% of iron-aluminum spinel with a particle size of >0mm and ≤1mm, 2% of iron powder with a particle size of 200 mesh, 0.5% of nickel oxide powder with a particle size of 200 mesh, and 0.5% of iron red with a particle size of 200 mesh; 3% of pulp binder is added. Example 2
[0048] The raw materials for preparing the magnesia-iron spinel brick of this embodiment include the following components in percentage by mass:
[0049] 7% of high-purity magnesia particles with a particle size of >3mm and ≤5mm, 26% of high-purity magnesia particles with a particle size of >1mm and ≤3mm, 16% of high-purity magnesia particles with a particle size of >0mm and ≤1mm, 26.5% of high-purity magnesia fine powder with a particle size of 200 mesh, 13% of magnesia waste bricks with a particle size of 200 mesh, 4% of iron-aluminum spinel with a particle size of >1mm and ≤3mm, 4% of iron-aluminum spinel with a particle size of >0mm and ≤1mm, 2% of iron powder with a particle size of 200 mesh, 1% of nickel oxide powder with a particle size of 200 mesh, and 0.5% of iron red with a particle size of 200 mesh; 3% of pulp binder was added. Example 3
[0050] The raw materials for preparing the magnesia-iron spinel brick of this embodiment include the following components in percentage by mass:
[0051] 7% of high-purity magnesia particles with a particle size of >3mm and ≤5mm, 26% of high-purity magnesia particles with a particle size of >1mm and ≤3mm, 16% of high-purity magnesia particles with a particle size of >0mm and ≤1mm, 26.5% of high-purity magnesia fine powder with a particle size of 200 mesh, 13% of magnesia waste bricks with a particle size of 200 mesh, 4% of iron-aluminum spinel with a particle size of >1mm and ≤3mm, 4% of iron-aluminum spinel with a particle size of >0mm and ≤1mm, 2% of iron powder with a particle size of 200 mesh, 0.5% of nickel oxide powder with a particle size of 200 mesh, 1% of iron red with a particle size of 200 mesh; and 3% of additional pulp binder. Example 4
[0052] The raw materials for preparing the magnesia-iron spinel brick of this embodiment include the following components in percentage by mass:
[0053] 7% of high-purity magnesia particles with a particle size of >3mm and ≤5mm, 25% of high-purity magnesia particles with a particle size of >1mm and ≤3mm, 16% of high-purity magnesia particles with a particle size of >0mm and ≤1mm, 26% of high-purity magnesia fine powder with a particle size of 200 mesh, 14% of magnesia waste bricks with a particle size of 200 mesh, 4% of iron-aluminum spinel with a particle size of >1mm and ≤3mm, 4% of iron-aluminum spinel with a particle size of >0mm and ≤1mm, 2% of iron powder with a particle size of 200 mesh, 1% of nickel oxide powder with a particle size of 200 mesh, and 1% of iron red with a particle size of 200 mesh; and 3% of additional pulp binder. Example 5
[0054] The raw materials for preparing the magnesia-iron spinel brick of this embodiment include the following components in percentage by mass:
[0055] 7% of high-purity magnesia particles with a particle size of >3mm and ≤5mm, 24% of high-purity magnesia particles with a particle size of >1mm and ≤3mm, 16% of high-purity magnesia particles with a particle size of >0mm and ≤1mm, 26% of high-purity magnesia fine powder with a particle size of 200 mesh, 14% of magnesia waste bricks with a particle size of 200 mesh, 5% of iron-aluminum spinel with a particle size of >1mm and ≤3mm, 4% of iron-aluminum spinel with a particle size of >0mm and ≤1mm, 2% of iron powder with a particle size of 200 mesh, 1% of nickel oxide powder with a particle size of 200 mesh, and 1% of iron red with a particle size of 200 mesh; and 3% of additional pulp binder. Example 6
[0056] The raw materials for preparing the magnesia-iron spinel brick of this embodiment include the following components in percentage by mass:
[0057] 7% of high-purity magnesia particles with a particle size of >3mm and ≤5mm, 23% of high-purity magnesia particles with a particle size of >1mm and ≤3mm, 15% of high-purity magnesia particles with a particle size of >0mm and ≤1mm, 26% of high-purity magnesia fine powder with a particle size of 200 mesh, 15% of magnesia waste bricks with a particle size of 200 mesh, 6% of iron-aluminum spinel with a particle size of >1mm and ≤3mm, 4% of iron-aluminum spinel with a particle size of >0mm and ≤1mm, 2% of iron powder with a particle size of 200 mesh, 1% of nickel oxide powder with a particle size of 200 mesh, and 1% of iron red with a particle size of 200 mesh; and 3% of additional pulp binder. Example 7
[0058] The raw materials for preparing the magnesia-iron spinel brick of this embodiment include the following components in percentage by mass:
[0059] 7% of high-purity magnesia particles with a particle size of >3mm and ≤5mm, 25% of high-purity magnesia particles with a particle size of >1mm and ≤3mm, 15% of high-purity magnesia particles with a particle size of >0mm and ≤1mm, 25.5% of high-purity magnesia fine powder with a particle size of 200 mesh, 15% of magnesia waste bricks with a particle size of 200 mesh, 4% of iron-aluminum spinel with a particle size of >1mm and ≤3mm, 4% of iron-aluminum spinel with a particle size of >0mm and ≤1mm, 2% of iron powder with a particle size of 200 mesh, 1.5% of nickel oxide powder with a particle size of 200 mesh, 1% of iron red with a particle size of 200 mesh; and 3% of pulp binder. Example 8
[0060] The raw materials for preparing the magnesia-iron spinel brick of this embodiment include the following components in percentage by mass:
[0061] 7% of high-purity magnesia particles with a particle size of >3mm and ≤5mm, 25% of high-purity magnesia particles with a particle size of >1mm and ≤3mm, 16% of high-purity magnesia particles with a particle size of >0mm and ≤1mm, 25.5% of high-purity magnesia fine powder with a particle size of 200 mesh, 14% of magnesia waste bricks with a particle size of 200 mesh, 4% of iron-aluminum spinel with a particle size of >1mm and ≤3mm, 4% of iron-aluminum spinel with a particle size of >0mm and ≤1mm, 2% of iron powder with a particle size of 200 mesh, 1% of nickel oxide powder with a particle size of 200 mesh, and 1.5% of iron red with a particle size of 200 mesh; plus 3% of pulp binder. Example 9
[0062] The raw materials for preparing the magnesia-iron spinel brick of this embodiment include the following components in percentage by mass:
[0063] 7% of high-purity magnesia particles with a particle size of >3mm and ≤5mm, 25% of high-purity magnesia particles with a particle size of >1mm and ≤3mm, 16% of high-purity magnesia particles with a particle size of >0mm and ≤1mm, 24% of high-purity magnesia fine powder with a particle size of 200 mesh, 14% of magnesia waste bricks with a particle size of 200 mesh, 4% of iron-aluminum spinel with a particle size of >1mm and ≤3mm, 4% of iron-aluminum spinel with a particle size of >0mm and ≤1mm, 2% of iron powder with a particle size of 200 mesh, 2% of nickel oxide powder with a particle size of 200 mesh, and 2% of iron red with a particle size of 200 mesh; 3% of additional pulp binder. Example 10
[0064] The raw materials for preparing the magnesia-iron spinel brick of this embodiment include the following components in percentage by mass:
[0065] 5% high-purity magnesia particles with a particle size of >3mm and ≤5mm, 23% high-purity magnesia particles with a particle size of >1mm and ≤3mm, 16% high-purity magnesia particles with a particle size of >0mm and ≤1mm, 23.2% high-purity magnesia fine powder with a particle size of 200 mesh, 17% magnesia waste bricks with a particle size of 200 mesh, 6% iron-aluminum spinel with a particle size of >1mm and ≤3mm, 6% iron-aluminum spinel with a particle size of >0mm and ≤1mm, 0.5% iron powder with a particle size of 200 mesh, 3% nickel oxide powder with a particle size of 200 mesh, 0.3% iron red with a particle size of 200 mesh; and 3% additional pulp binder. Embodiment 11
[0066] The raw materials for preparing the magnesia-iron spinel brick of this embodiment include the following components in percentage by mass:
[0067] 8% high-purity magnesia particles with a particle size of >3mm and ≤5mm, 25% high-purity magnesia particles with a particle size of >1mm and ≤3mm, 22% high-purity magnesia particles with a particle size of >0mm and ≤1mm, 25% high-purity magnesia fine powder with a particle size of 200 mesh, 8% magnesia waste bricks with a particle size of 200 mesh, 3% iron-aluminum spinel with a particle size of >1mm and ≤3mm, 3% iron-aluminum spinel with a particle size of >0mm and ≤1mm, 3% iron powder with a particle size of 200 mesh, 0.3% nickel oxide powder with a particle size of 200 mesh, 3% iron red with a particle size of 200 mesh; and 3% additional pulp binder. Example 12
[0068] The magnesia-iron spinel brick of this embodiment has a different mass ratio of iron powder, nickel oxide powder and red iron compared with that of embodiment 5. The mass ratio of iron powder, nickel oxide powder and red iron is 1:1:1. The raw materials for its preparation include the following components in mass percentage:
[0069] 7% of high-purity magnesia particles with a particle size of >3mm and ≤5mm, 24% of high-purity magnesia particles with a particle size of >1mm and ≤3mm, 16% of high-purity magnesia particles with a particle size of >0mm and ≤1mm, 26% of high-purity magnesia fine powder with a particle size of 200 mesh, 13% of magnesia waste bricks with a particle size of 200 mesh, 4% of iron-aluminum spinel with a particle size of >1mm and ≤3mm, 4% of iron-aluminum spinel with a particle size of >0mm and ≤1mm, 2% of iron powder with a particle size of 200 mesh, 2% of nickel oxide powder with a particle size of 200 mesh, and 2% of iron red with a particle size of 200 mesh; and 3% of additional pulp binder. Example 13
[0070] The magnesia-iron spinel brick of this embodiment has a different mass ratio of iron powder, nickel oxide powder and iron red compared with that of Example 5. The mass ratio of iron powder, nickel oxide powder and iron red is 1:0.25:0.25. The raw materials for its preparation include the following components in mass percentage:
[0071] 8% high-purity magnesia particles with a particle size of >3mm and ≤5mm, 24% high-purity magnesia particles with a particle size of >1mm and ≤3mm, 16% high-purity magnesia particles with a particle size of >0mm and ≤1mm, 26% high-purity magnesia fine powder with a particle size of 200 mesh, 14% magnesia waste bricks with a particle size of 200 mesh, 5% iron-aluminum spinel with a particle size of >1mm and ≤3mm, 4% iron-aluminum spinel with a particle size of >0mm and ≤1mm, 2% iron powder with a particle size of 200 mesh, 0.5% nickel oxide powder with a particle size of 200 mesh, and 0.5% iron red with a particle size of 200 mesh; 3% additional pulp binder. Embodiment 14
[0072] The magnesia-iron spinel brick of this embodiment has a different mass ratio of iron powder, nickel oxide powder and iron red compared with that of embodiment 5. The mass ratio of iron powder, nickel oxide powder and iron red is 1:1.17:1.17. The raw materials for its preparation include the following components in mass percentage:
[0073] 8% high-purity magnesia particles with a particle size of >3mm and ≤5mm, 24% high-purity magnesia particles with a particle size of >1mm and ≤3mm, 16% high-purity magnesia particles with a particle size of >0mm and ≤1mm, 26% high-purity magnesia fine powder with a particle size of 200 mesh, 13% magnesia waste bricks with a particle size of 200 mesh, 4% iron-aluminum spinel with a particle size of >1mm and ≤3mm, 4% iron-aluminum spinel with a particle size of >0mm and ≤1mm, 1.5% iron powder with a particle size of 200 mesh, 1.75% nickel oxide powder with a particle size of 200 mesh, 1.75% iron red with a particle size of 200 mesh; 3% additional pulp binder. Embodiment 15
[0074] The magnesia-iron spinel brick of this embodiment has a different mass ratio of iron powder, nickel oxide powder and iron red compared with that of embodiment 5. The mass ratio of iron powder, nickel oxide powder and iron red is 1:0.2:0.2. The raw materials for its preparation include the following components in mass percentage:
[0075] 7% of high-purity magnesia particles with a particle size of >3mm and ≤5mm, 24% of high-purity magnesia particles with a particle size of >1mm and ≤3mm, 16% of high-purity magnesia particles with a particle size of >0mm and ≤1mm, 26% of high-purity magnesia fine powder with a particle size of 200 mesh, 14.2% of magnesia waste bricks with a particle size of 200 mesh, 5% of iron-aluminum spinel with a particle size of >1mm and ≤3mm, 5% of iron-aluminum spinel with a particle size of >0mm and ≤1mm, 2% of iron powder with a particle size of 200 mesh, 0.4% of nickel oxide powder with a particle size of 200 mesh, and 0.4% of iron red with a particle size of 200 mesh; 3% of pulp binder was added. Example 16
[0076] The magnesia-iron spinel brick of this embodiment is different from that of Example 5 in that the mass ratio of the total mass of magnesia sand and magnesia waste bricks to ferroaluminum spinel, nickel oxide powder and iron red is 100:8.9:0.56:0.56, and the raw materials for its preparation include the following components in mass percentage:
[0077] 9% of high-purity magnesia particles with a particle size of >3mm and ≤5mm, 24% of high-purity magnesia particles with a particle size of >1mm and ≤3mm, 16% of high-purity magnesia particles with a particle size of >0mm and ≤1mm, 26% of high-purity magnesia fine powder with a particle size of 200 mesh, 15% of magnesia waste bricks with a particle size of 200 mesh, 4% of iron-aluminum spinel with a particle size of >1mm and ≤3mm, 4% of iron-aluminum spinel with a particle size of >0mm and ≤1mm, 1% of iron powder with a particle size of 200 mesh, 0.5% of nickel oxide powder with a particle size of 200 mesh, and 0.5% of iron red with a particle size of 200 mesh; plus 3% of pulp binder. Embodiment 17
[0078] The magnesia-iron spinel brick of this embodiment, compared with Example 5, has a different mass ratio of the total mass of magnesia sand and magnesia waste bricks to ferroaluminum spinel, nickel oxide powder, and iron red. The mass ratio of the total mass of magnesia sand and magnesia waste bricks to ferroaluminum spinel, nickel oxide powder, and iron red is 100:11.6:1.16:1.16, and its preparation raw materials include the following components in mass percentage:
[0079] 7% of high-purity magnesia particles with a particle size of >3mm and ≤5mm, 24% of high-purity magnesia particles with a particle size of >1mm and ≤3mm, 16% of high-purity magnesia particles with a particle size of >0mm and ≤1mm, 26% of high-purity magnesia fine powder with a particle size of 200 mesh, 13% of magnesia waste bricks with a particle size of 200 mesh, 5% of iron-aluminum spinel with a particle size of >1mm and ≤3mm, 5% of iron-aluminum spinel with a particle size of >0mm and ≤1mm, 2% of iron powder with a particle size of 200 mesh, 1% of nickel oxide powder with a particle size of 200 mesh, and 1% of iron red with a particle size of 200 mesh; and 3% of additional pulp binder. Embodiment 18
[0080] The magnesia-iron spinel brick of this embodiment is different from that of Example 5 in that the mass ratio of the total mass of magnesia sand and magnesia waste bricks to ferroaluminum spinel, nickel oxide powder and iron red is 100:6.9:3:3, and the raw materials for its preparation include the following components in mass percentage:
[0081] 7% of high-purity magnesia particles with a particle size of >3mm and ≤5mm, 24% of high-purity magnesia particles with a particle size of >1mm and ≤3mm, 16% of high-purity magnesia particles with a particle size of >0mm and ≤1mm, 26% of high-purity magnesia fine powder with a particle size of 200 mesh, 14% of magnesia waste bricks with a particle size of 200 mesh, 3% of iron-aluminum spinel with a particle size of >1mm and ≤3mm, 3% of iron-aluminum spinel with a particle size of >0mm and ≤1mm, 1.8% of iron powder with a particle size of 200 mesh, 2.6% of nickel oxide powder with a particle size of 200 mesh, and 2.6% of iron red with a particle size of 200 mesh; plus 3% of pulp binder. Embodiment 19
[0082] The magnesia-iron spinel brick of this embodiment, compared with Example 5, has a different mass ratio of the total mass of magnesia sand and magnesia waste bricks to ferroaluminum spinel, nickel oxide powder, and iron red. The mass ratio of the total mass of magnesia sand and magnesia waste bricks to ferroaluminum spinel, nickel oxide powder, and iron red is 100:13.8:0.34:0.34, and its preparation raw materials include the following components in mass percentage:
[0083] 7% of high-purity magnesia particles with a particle size of >3mm and ≤5mm, 24% of high-purity magnesia particles with a particle size of >1mm and ≤3mm, 16% of high-purity magnesia particles with a particle size of >0mm and ≤1mm, 26% of high-purity magnesia fine powder with a particle size of 200 mesh, 14% of magnesia waste bricks with a particle size of 200 mesh, 6% of iron-aluminum spinel with a particle size of >1mm and ≤3mm, 6% of iron-aluminum spinel with a particle size of >0mm and ≤1mm, 0.4% of iron powder with a particle size of 200 mesh, 0.3% of nickel oxide powder with a particle size of 200 mesh, and 0.3% of iron red with a particle size of 200 mesh; 3% of pulp binder was added.
[0084] Comparative Example 1
[0085] The magnesia-iron spinel brick of this comparative example is different from that of Example 5 in that iron powder, nickel oxide powder and red iron are not added, and the relative proportions of the other components remain unchanged.
[0086] Comparative Example 2
[0087] The magnesia-iron spinel brick of this comparative example is different from that of Example 5 in that nickel oxide powder and iron red are not added, and the iron powder is 4%.
[0088] The raw materials for preparing the ferromagnesian spinel bricks of the above-mentioned embodiments and comparative examples, except for the pulp, are configured into a mixture, stirred for 5 minutes, and then stirred for another 25 minutes after adding the pulp, and formed by a 1200-ton electric screw press, with a molding size of 230mm×114mm×75mm, dried in a drying kiln for 24 hours, and then fired in a firing kiln, with a firing temperature of 1500℃, a cart speed of 120 minutes per cart, and a 6-hour heat preservation in the firing section, to obtain ferromagnesian spinel brick samples, and each sample is tested, and the test sample preparation is carried out according to GB / T7321. The test results are shown in Table 1 below.
[0089] Kiln lining performance: Cement raw materials are sandwiched between two refractory brick samples, and heated in an electric furnace at 1500℃*3h. After cooling, three-point bending test is performed. (Sample shape: 62.5mm*25mm*25mm, cement raw materials: 95% ordinary silicate rock + 3% potassium sulfate + 2% potassium chloride). The test results are shown in Table 2 below.
[0090] It can be seen from the data in Table 1 below that iron powder, nickel oxide powder and iron red are not added to the raw materials of the ferromagnesian spinel brick of Comparative Example 1. As the lining material of the cement kiln, the ferromagnesian spinel brick has poor kiln skin performance and poor toughness; iron powder is added to the raw materials of the ferromagnesian spinel brick of Comparative Example 2, but nickel oxide powder and iron red are not added. Although the kiln skin performance is good, the high temperature strength performance of the ferromagnesian spinel brick is significantly reduced due to the melting of the remaining iron powder to produce a liquid phase. In contrast, the ferromagnesian spinel bricks of each embodiment of the present invention have good kiln skin performance and high temperature strength performance.
[0091] In each embodiment of the present invention, in Embodiment 1-11, the mass percentage of each component of the raw material is different, among which, compared with Embodiments 10 and 11, the mass percentage of each component in Embodiment 1-9 is in a preferred range, and the kiln lining performance, high temperature strength performance, and thermal shock stability of the magnesia-iron spinel brick are better. Furthermore, compared with Embodiments 1-3 and 7-9, the kiln lining performance and high temperature strength performance of Embodiments 4-6 are better, and the mass percentage of each component is in a further preferred range.
[0092] Compared with Example 5, Examples 12-15 differ in that the mass ratios of the added iron powder, nickel oxide powder and iron red are different. Among them, the mass ratios of iron powder, nickel oxide powder and iron red in Examples 5, 12 and 13 are more optimal, and the obtained magnesia-iron spinel bricks have significantly better kiln skin performance and high temperature strength performance.
[0093] Compared with Example 5, Examples 16-19 differ in that the total mass of the added magnesia sand and magnesia waste bricks has a different mass ratio to ferroaluminum spinel, nickel oxide powder, and iron red. Among them, the mass ratio of the total mass of magnesia sand and magnesia waste bricks to ferroaluminum spinel, nickel oxide powder, and iron red in Examples 5, 16, and 17 is better, and the obtained magnesia-iron spinel bricks have significantly better kiln skin performance and high temperature strength performance.
[0094] Table 1
[0095] <![CDATA[Bulk density after firing / g / cm 3 > Porosity after firing / % Compressive strength after burning / MPa Example 1 2.96 16 60 Example 2 2.97 15 65 Example 3 2.97 15 68 Example 4 2.98 14 86 Example 5 2.98 14 88 Example 6 2.97 14 85 Example 7 2.97 15 70 Example 8 2.97 15 74 Example 9 2.96 16 68 Example 10 2.94 17 54 Embodiment 11 2.94 17 52 Example 12 2.98 14 83 Example 13 2.98 14 84 Embodiment 14 2.97 15 76 Embodiment 15 2.97 15 72 Example 16 2.98 14 82 Embodiment 17 2.98 14 85 Embodiment 18 2.96 15 70 Embodiment 19 2.96 15 69 Comparative Example 1 2.98 15 75 Comparative Example 2 2.98 18 45
[0096] Table 2
[0097] Flexural strength / Mpa Example 1 1.3 Example 2 1.2 Example 3 1.4 Example 4 1.6 Example 5 1.7 Example 6 1.6 Example 7 1.2 Example 8 1.3 Example 9 1.3 Example 10 1.1 Embodiment 11 1.1 Example 12 1.6 Example 13 1.6 Embodiment 14 1.3 Embodiment 15 1.2 Example 16 1.5 Embodiment 17 1.4 Embodiment 18 1.2 Embodiment 19 1.1 Comparative Example 1 0.7 Comparative Example 2 1.4
[0098] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.
Claims
1. A magnesia-iron spinel brick, It is characterized in that The raw materials for its preparation include the following components in percentage by mass: Magnesia 65%~81%, magnesia waste bricks 8%~17%, ferroalumina spinel 6%~12%, iron powder 0.5%~3%, nickel oxide powder 0.3%~3% and iron red 0.3%~3%; external binder 1%~5%.
2. The ferromagnesian spinel brick according to claim 1, It is characterized in that The raw materials for its preparation include the following components in percentage by mass: Magnesia 71%~77%, magnesia waste bricks 12%~15%, ferroalumina spinel 8%~10%, iron powder 1%~2%, nickel oxide powder 0.5%~2% and iron red 0.5%~2%; external binder 2%~4%.
3. The ferromagnesian spinel brick according to claim 2, It is characterized in that The raw materials for its preparation include the following components in percentage by mass: Magnesia 71%~74%, magnesia waste bricks 14%~15%, ferroalumina spinel 8%~10%, iron powder 2%, nickel oxide powder 1% and iron red 1%; external binder 3%.
4. The ferromagnesian spinel brick according to claim 1, Features: The mass ratio of iron powder, nickel oxide powder and iron red is 1:0.25~1:0.25~1.
5. The ferromagnesian spinel brick according to claim 1, Features: The mass ratio of the total mass of magnesia sand and magnesia waste bricks to ferroaluminum spinel, nickel oxide powder and iron red is 100:8.8~11.8:0.5~2.5:0.5~2.
5.
6. The ferromagnesian spinel brick according to claim 1, Features: The magnesia includes magnesia particles with a particle size of >3mm and ≤5mm, magnesia particles with a particle size of >1mm and ≤3mm, magnesia particles with a particle size of >0mm and ≤1mm, and magnesia fine powder with a particle size of 200 mesh; the mass ratio of magnesia particles with a particle size of >3mm and ≤5mm, magnesia particles with a particle size of >1mm and ≤3mm, magnesia particles with a particle size of >0mm and ≤1mm, and magnesia fine powder with a particle size of 200 mesh is 2-8:20-28:15-22:24-27; The iron-aluminum spinel includes iron-aluminum spinel with a particle size of >1mm and ≤3mm and iron-aluminum spinel with a particle size of >0mm and ≤1mm; the mass ratio of the iron-aluminum spinel with a particle size of >1mm and ≤3mm and the iron-aluminum spinel with a particle size of >0mm and ≤1mm is 3-8:3-5.
7. The ferromagnesian spinel brick according to claim 1, Features: The particle size of the iron powder is 200 mesh; the particle size of the nickel oxide powder is 200 mesh; and the particle size of the iron oxide red is 200 mesh.
8. The ferromagnesian spinel brick according to claim 1, Features: The magnesia sand is high-purity magnesia sand; in the high-purity magnesia sand, MgO>96.5wt%, SiO 2 <0.8wt%Fe 2 O 3 <0.8wt%Al 2 O 3 <0.15wt%,CaO<1.5wt%,ignition loss<0.1wt%; In the magnesium waste brick, MgO>97wt%, SiO 2 <1wt%Al 2 O 3 <1wt%,CaO<1wt%; In the iron-aluminum spinel, Al 2 O 3 >55wt%Fe 2 O 3 >40wt%SiO 2 <0.15wt%, CaO<1.5wt%, ignition loss<3.5wt%, bulk density>3.9g / cm 3 .
9. A method for preparing a magnesia-iron spinel brick as claimed in any one of claims 1 to 8, It is characterized in that The following steps are involved: The raw materials for preparing the magnesia-iron spinel brick are mixed, then molded, and then the molded product is fired to obtain the magnesia-iron spinel brick.
10. The preparation method according to claim 9, Features: The sintering temperature is 1500-1530° C. and the sintering time is 2-10 hours.