A method for preparing high-viscosity ACR resin for foaming soft products
By modifying the emulsion of silica and specific monomers, a high viscosity ACR resin is formed, which solves the problem of low viscosity of the existing ACR resin, and achieves the effect of preparing PVC soft bubbles with low density and uniform cell.
Patent Information
- Application Number
- CN202411299019.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-18
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-09-18
AI Technical Summary
The existing ACR resin has a low molecular weight and low viscosity, making it difficult to effectively improve the viscosity and strength of PVC melt, resulting in bubble cells collapse and making it difficult to obtain soft PVC foam with delicate and uniform cells.
By preparing the modified silica and emulsion, the seed emulsion is formed and core polymerized and shell polymerized, and finally a high viscosity ACR resin is obtained by spray drying. This method improves the viscosity and strength of the ACR resin by surface modification of nanosilica and addition of allyl pyruvate and ethylene glycol monoallyl ether.
A high viscosity ACR resin with an intrinsic viscosity of 18.8~20.3dL/g was achieved, and was used to prepare PVC soft bubbles with a density of 1.93~2.14g/m3, which solved the problem of bubble cell and bubble collapse. The obtained foam density is low and bubbles are bubbled. The pore structure is uniform and small.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a high-viscosity ACR resin for foaming soft products, and belongs to the technical field of polyacrylate foaming regulators. Background Art
[0002] There are many types of soft foam plastic materials, among which soft polyvinyl chloride foam is widely used in home furnishing, medical treatment, clothing and shoe sole materials due to its light weight, softness, insulation, shock absorption, durability and low cost. Especially in the field of shoe sole materials, soft foam PVC has a tendency to replace EVA and PU in the midsole of shoes because of its high cost performance. However, since PVC has low melt viscosity and poor stability at high temperature, and the pores are easily broken, it is difficult to obtain high-quality soft foam materials with low density, good softness and fine pores.
[0003] Generally, when preparing high-density soft PVC foaming materials, soft foam can be obtained without adding chemical crosslinking agents to the formula for modification. This is mainly because when preparing high-density soft PVC foaming materials, the amount of gas in the PVC melt is small, and the melt viscosity of the PVC polymer can be relatively maintained at a high state, so it is easier to obtain high-density soft PVC foam. However, in the preparation of low- and medium-density PVC foaming materials, the foaming ratio is very large, so the amount of gas in the PVC polymer melt is relatively large. In this case, it is difficult to maintain a high viscosity of the PVC melt, which leads to the appearance of bubble and bubble collapse. Using a crosslinking agent to increase the viscosity of the PVC melt during the foaming process will lead to a decrease in the toughness and elasticity of the final foam. In order to obtain a soft PVC foam with a high foaming ratio, an effective method is to add a polyacrylate foaming regulator, that is, an ACR resin polymer, to the formula, which can promote PVC melting and plasticization, improve the strength and elongation of the foaming melt, and make the foaming process stable and controllable, thereby obtaining a PVC soft foam with uniform and fine pore structure, good independence, and low density. Most of the ACR resin foaming regulators currently available on the market can only be used to adjust the cell pores of PVC rigid foams, and are not suitable for the foaming of soft PVC foams, especially low-density soft PVC foams, where it is even more difficult to find a suitable ACR resin foaming regulator. The main reason for this is that the molecular weight of the ACR resins currently available on the market is low and the viscosity is not high. After being added to the PVC foaming formula, the ACR resins with very low viscosity are difficult to effectively improve the viscosity and strength of the PVC melt, resulting in cell fusion and collapse, and ultimately it is difficult to obtain soft PVC foams with fine and uniform cells.
[0004] Chinese patent CN105254817A discloses a method for preparing a core-shell structured acrylic ester foaming regulator, wherein the specific preparation method comprises the following steps: reacting deionized water, an emulsifier, an acrylic ester monomer, and an initiator to obtain a core-layer acrylic ester seed latex; reacting the core-layer acrylic ester seed latex, deionized water, an emulsifier, an acrylic ester monomer, and an initiator to obtain a core-shell structured acrylic ester copolymer emulsion; and spray drying the emulsion to obtain a core-shell structured acrylic ester foaming regulator. The acrylic ester foaming regulator obtained in the patent has a low intrinsic viscosity and is difficult to significantly increase the viscosity of the polyvinyl chloride melt, so it is difficult to be used in the field of soft PVC foaming.
[0005] Chinese patent CN118440235A discloses a foaming regulator for polyvinyl chloride and its preparation method and application. The raw materials for its preparation include at least a polymerized monomer, a crosslinking agent, an emulsifier, an initiator, and water. The polymerized monomer includes at least methyl methacrylate, butyl acrylate, styrene, and acrylonitrile. By optimizing the crosslinking agent system, the provided foaming regulator has an excellent foam stabilizing effect, which effectively solves the defect that the polyacrylate foaming regulator has insufficient melt strength in PVC foam products and cannot obtain a uniform and dense foamed board. The acrylic foaming regulator obtained in this patent is mainly used for the foaming of PVC hard boards, and is not suitable for the foaming regulation of low-density PVC soft foams.
[0006] As can be seen from the above, there are currently few high-viscosity ACR resins suitable for foaming regulation of soft PVC foam. Therefore, developing a method for preparing a high-viscosity ACR resin for foaming soft products for foaming regulation of low-density PVC soft foam is a research work with great application prospects. Summary of the invention
[0007] In view of the above-mentioned deficiencies in the prior art, the present invention provides a method for preparing a high-viscosity ACR resin for foaming soft products, thereby achieving the following invention objectives: preparing an ACR resin with high viscosity suitable for foaming soft low-density PVC foam.
[0008] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solutions:
[0009] A method for preparing a high-viscosity ACR resin for foaming soft products, the method comprising six steps of preparing modified silica, preparing an emulsion, preparing a seed emulsion, core polymerization, shell polymerization, and spray drying;
[0010] The following are further improvements to the above technical solution:
[0011] Step 1: Preparation of modified silica
[0012] Add nano silicon dioxide and anhydrous ethanol into a high-speed dispersion kettle, disperse vigorously at a speed of 8000-12000 rpm for 5-11 hours, reduce the dispersion speed to 1000-3000 rpm, increase the temperature and keep the temperature constant at 40-60° C., add γ-methacryloxypropyltrimethoxysilane, react at the constant temperature for 5-9 hours, centrifuge, wash the separated solid with anhydrous ethanol for 2-4 times, put it into a vacuum drying oven at 40-60° C. and dry it for 4-8 hours to obtain modified silicon dioxide;
[0013] The particle size of the nano silicon dioxide is 10-60 nm;
[0014] The mass ratio of the nano silicon dioxide, anhydrous ethanol and gamma-methacryloxypropyltrimethoxysilane is 20-50:120-180:5-10.
[0015] Step 2: Prepare emulsion
[0016] Sodium dodecyl sulfate, sodium polyoxyethylene ether sulfate and deionized water are added into a reaction kettle, and after being stirred and dissolved completely, α-methylacrylic acid, butyl acrylate and modified silicon dioxide are added, and the stirring rate is controlled at 1500-3500 rpm, and after stirring and emulsifying for 9-13 hours, stirring is stopped to obtain a uniform and stable emulsion;
[0017] The mass ratio of sodium dodecyl sulfate, sodium polyoxyethylene ether sulfate, deionized water, α-methylacrylic acid, butyl acrylate and modified silicon dioxide is 2-5:1-3:130-190:10-20:4-9:1-4.
[0018] Step 3: Prepare seed emulsion
[0019] The emulsion obtained in step 2 is added to a polymerization kettle with a total mass of 50 wt %, and the pressure in the polymerization kettle is evacuated to -0.09~-0.08 MPa, and then nitrogen is introduced to a positive pressure, and then the vacuum is evacuated and nitrogen is introduced again. After three cycles, the temperature in the kettle is raised and kept constant at 50~65° C. under nitrogen protection, and the stirring rate is controlled at 300~800 rpm, and potassium persulfate of 0.1~0.2 wt % of the total mass of the emulsion in the polymerization kettle is added, and the reaction is stirred at a constant temperature for 4~7 hours to obtain a seed emulsion.
[0020] Step 4: Nuclear fusion
[0021] The temperature of the seed emulsion in the polymerization kettle is maintained at 50-65° C., the stirring rate is controlled at 400-800 rpm, and under nitrogen protection, the other half of the emulsion remaining in step 2 is added dropwise to the seed emulsion at a rate of 0.2-1.3 g / sec, and at the same time, a potassium persulfate aqueous solution with a mass concentration of 5-8wt% is added dropwise to the seed emulsion at a rate of 0.01-0.06 g / sec, and the added mass of the potassium persulfate aqueous solution is 4-7% of the mass of the seed emulsion. After the emulsion and the potassium persulfate aqueous solution are added dropwise, the reaction is continued with stirring for 3-6 hours to obtain a core polymerization emulsion.
[0022] Step 5: Shell polymerization
[0023] The core polymerization emulsion obtained in step 4 is kept at a constant temperature of 50-65° C., and the stirring rate is controlled at 400-800 rpm. Under nitrogen protection, the shell monomer emulsion is added dropwise to the core polymerization emulsion at a rate of 0.4-1.5 g / sec. At the same time, a potassium persulfate aqueous solution with a mass concentration of 5-8 wt% is added dropwise to the seed emulsion at a rate of 0.02-0.09 g / sec. The mass of the potassium persulfate aqueous solution added is 6-9% of the mass of the core polymerization emulsion. After the shell monomer emulsion and the potassium persulfate aqueous solution are added dropwise, the reaction is continued with stirring for 4-8 hours to obtain a shell polymerization emulsion;
[0024] The added mass of the shell monomer emulsion is 75-97wt% of the total mass of the core polymerization emulsion;
[0025] The shell monomer emulsion is prepared by: adding sodium dodecyl sulfate, sodium polyoxyethylene ether sulfate, and deionized water into a reaction kettle, stirring and dissolving them completely, then adding allyl pyruvate, ethylene glycol monoallyl ether, and methyl methacrylate, controlling the stirring rate to 1700-3600 rpm, stirring and emulsifying for 6-11 hours, and stopping stirring to obtain a uniform and stable shell monomer emulsion;
[0026] The mass ratio of sodium lauryl sulfate, sodium polyoxyethylene ether sulfate, deionized water, allyl pyruvate, ethylene glycol monoallyl ether and methyl methacrylate is 1-4:2-5:150-210:11-19:3-8:15-25.
[0027] Step 6: Spray drying
[0028] The shell polymerization emulsion is sent to a spray dryer, and the temperature of the drying hot air is controlled to be 160-180°C. After spray drying, a white powder with a particle size of 1-2.5 μm is obtained, which is a high-viscosity ACR resin for foaming soft products.
[0029] Compared with the prior art, the present invention achieves the following beneficial effects:
[0030] 1. The present invention uses γ-methacryloxypropyltrimethoxysilane to modify the surface of nano-silicon dioxide, so that the surface of nano-silicon dioxide has functional groups containing carbon-carbon double bonds. After these nano-silicon dioxides with carbon-carbon double bonds bonded on the surface are prepared into emulsions, they are dispersed in emulsion droplets as nano-scale particles. In the step of preparing seed emulsions, these nano-scale particles rich in carbon-carbon double bonds on the surface react quickly with α-methacrylic acid and butyl acrylate to form a seed emulsion with nano-scale particles as the central core. The seed emulsion formed by this method not only refines the particle size of the ACR resin seed core but also increases the The strength of the core is improved. The above two effects can be achieved because, firstly, the particle size of nano-silica is mostly in the range of tens to tens of nanometers and it is easy to disperse to the nanoscale. Secondly, nano-silica has a huge specific surface area and a large number of functional groups containing carbon-carbon double bonds bonded thereon. It can form a certain degree of cross-linking with two acrylic substances, α-methacrylic acid and butyl acrylate. This cross-linking structure gives the seed core a higher strength. In addition, this cross-linking structure can also contribute to a very high melt viscosity in the subsequent thermal processing of ACR resin for PVC soft foaming.
[0031] 2. In the present invention, allyl pyruvate and ethylene glycol monoallyl ether are added to the shell monomer emulsion. Compared with adding only a single methyl methacrylate monomer, the shell layer formed after adding the two monomers of allyl pyruvate and ethylene glycol monoallyl ether has carboxyl and hydroxyl groups at the ends. The polarity of the polymer chain segments formed by these two monomers is greater, and it is easier to have a polar adsorption effect with the chlorine atoms on the polyvinyl chloride, thereby more easily enhancing the strength of the PVC melt. Moreover, the carboxyl and hydroxyl groups at the ends of these two monomers themselves have a relatively strong hydrogen bonding effect, so they can enhance the end force and entanglement of the ACR resin body molecular chain, which greatly increases the viscosity of the ACR resin, thereby enhancing its intrinsic viscosity, and is more conducive to the foam stabilization effect of the ACR resin in the PVC foaming process;
[0032] 3. The high viscosity ACR resin for foaming soft products obtained by the present invention has an intrinsic viscosity of 18.8-20.3 dL / g. The PVC soft foam obtained by using the high viscosity ACR resin for foaming soft products has a density of 1.93-2.14 g / m 3 . DETAILED DESCRIPTION
[0033] The preferred embodiments of the present invention are described below. It should be understood that the preferred embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0034] Example 1: A method for preparing a high viscosity ACR resin for foaming soft products
[0035] Step 1: Preparation of modified silica
[0036] Add nano-silicon dioxide and anhydrous ethanol into a high-speed dispersing kettle, disperse vigorously at a speed of 11000 rpm for 9 hours, reduce the dispersing speed to 2500 rpm, increase the temperature and keep the temperature constant at 55°C, add γ-methacryloxypropyltrimethoxysilane, react at the constant temperature for 6 hours, centrifuge, wash the separated solid with anhydrous ethanol for 3 times, put it into a vacuum drying oven at 46°C and dry it for 7 hours to obtain modified silicon dioxide;
[0037] The particle size of the nano silicon dioxide is 50 nm;
[0038] The mass ratio of the nano silicon dioxide, anhydrous ethanol and gamma-methacryloxypropyltrimethoxysilane is 40:160:8.
[0039] Step 2: Prepare emulsion
[0040] Sodium lauryl sulfate, sodium polyoxyethylene ether sulfate and deionized water were added into a reaction kettle, and after being stirred and dissolved completely, α-methylacrylic acid, butyl acrylate and modified silicon dioxide were added, and the stirring rate was controlled at 3200 rpm, and after stirring and emulsifying for 10 hours, stirring was stopped to obtain a uniform and stable emulsion;
[0041] The mass ratio of sodium dodecyl sulfate, sodium polyoxyethylene ether sulfate, deionized water, α-methylacrylic acid, butyl acrylate and modified silicon dioxide is 4:2:170:16:7:3.
[0042] Step 3: Prepare seed emulsion
[0043] The emulsion obtained in step 2 is added to a polymerization kettle with a total mass of 50 wt% thereof, and the pressure in the polymerization kettle is evacuated to -0.086 MPa, and then nitrogen is introduced to a positive pressure, and then the pressure is evacuated again and nitrogen is introduced. After three cycles, the temperature in the kettle is raised and kept constant at 60° C. under nitrogen protection, and the stirring rate is controlled at 650 rpm, and potassium persulfate of 0.13 wt% of the total mass of the emulsion in the polymerization kettle is added. After the reaction is stirred at a constant temperature for 5 hours, a seed emulsion is obtained.
[0044] Step 4: Nuclear fusion
[0045] The temperature of the seed emulsion in the polymerization kettle was maintained at 59° C., the stirring rate was controlled at 490 rpm, and under nitrogen protection, the other half of the emulsion remaining in step 2 was added dropwise to the seed emulsion at a rate of 0.8 g / sec, and at the same time, a potassium persulfate aqueous solution with a mass concentration of 7wt% was added dropwise to the seed emulsion at a rate of 0.04 g / sec, and the added mass of the potassium persulfate aqueous solution was 6% of the mass of the seed emulsion. After the emulsion and the potassium persulfate aqueous solution were added dropwise, the reaction was continued with stirring for 5 hours to obtain a core polymerization emulsion.
[0046] Step 5: Shell polymerization
[0047] The core polymerization emulsion obtained in step 4 was kept at a constant temperature of 62° C. and the stirring rate was controlled to be 560 rpm. Under nitrogen protection, the shell monomer emulsion was added dropwise to the core polymerization emulsion at a rate of 0.9 g / sec. At the same time, a 7wt% potassium persulfate aqueous solution was added dropwise to the seed emulsion at a rate of 0.07 g / sec. The added mass of the potassium persulfate aqueous solution was 8% of the mass of the core polymerization emulsion. After the shell monomer emulsion and the potassium persulfate aqueous solution were added dropwise, the reaction was continued with stirring for 5 hours to obtain a shell polymerization emulsion.
[0048] The added mass of the shell monomer emulsion is 92wt% of the total mass of the core polymerization emulsion;
[0049] The shell monomer emulsion is prepared by: adding sodium dodecyl sulfate, sodium polyoxyethylene ether sulfate, and deionized water into a reaction kettle, stirring and dissolving them completely, then adding allyl pyruvate, ethylene glycol monoallyl ether, and methyl methacrylate, stirring and emulsifying at a stirring rate of 3300 rpm for 9 hours, and then stopping stirring to obtain a uniform and stable shell monomer emulsion;
[0050] The mass ratio of sodium dodecyl sulfate, sodium polyoxyethylene ether sulfate, deionized water, allyl pyruvate, ethylene glycol monoallyl ether, and methyl methacrylate is 3:4:190:16:5:19.
[0051] Step 6: Spray drying
[0052] The shell polymerization emulsion is sent to a spray dryer, and the temperature of the drying hot air is controlled to be 175°C. After spray drying, a white powder with a particle size of 2 μm is obtained, which is a high-viscosity ACR resin for foaming soft products.
[0053] Example 2: Preparation method of high viscosity ACR resin for foaming soft products
[0054] Step 1: Preparation of modified silica
[0055] Add nano-silicon dioxide and anhydrous ethanol into a high-speed dispersing kettle, disperse vigorously at a speed of 8000 rpm for 5 hours, reduce the dispersing speed to 1000 rpm, increase the temperature and keep the temperature constant at 40°C, add γ-methacryloxypropyltrimethoxysilane, react at the constant temperature for 5 hours, centrifuge, wash the separated solid with anhydrous ethanol twice, put it into a vacuum drying oven at 40°C and dry it for 4 hours to obtain modified silicon dioxide;
[0056] The particle size of the nano silicon dioxide is 10 nm;
[0057] The mass ratio of the nano silicon dioxide, anhydrous ethanol and gamma-methacryloxypropyltrimethoxysilane is 20:120:5.
[0058] Step 2: Prepare emulsion
[0059] Sodium lauryl sulfate, sodium polyoxyethylene ether sulfate and deionized water were added into a reaction kettle, and after being stirred and dissolved completely, α-methylacrylic acid, butyl acrylate and modified silicon dioxide were added, and the stirring rate was controlled at 1500 rpm. After stirring and emulsifying for 9 hours, stirring was stopped to obtain a uniform and stable emulsion;
[0060] The mass ratio of sodium dodecyl sulfate, sodium polyoxyethylene ether sulfate, deionized water, α-methylacrylic acid, butyl acrylate and modified silicon dioxide is 2:1:130:10:4:1.
[0061] Step 3: Prepare seed emulsion
[0062] The emulsion obtained in step 2 is added to a polymerization kettle with a total mass of 50 wt %. The pressure in the polymerization kettle is evacuated to -0.09 MPa, and then nitrogen is introduced to a positive pressure, and then the pressure is evacuated again and nitrogen is introduced. After three cycles, the temperature in the kettle is raised and kept constant at 50° C. under nitrogen protection, and the stirring rate is controlled at 300 rpm. Potassium persulfate in an amount of 0.1 wt % of the total mass of the emulsion in the polymerization kettle is added, and the reaction is stirred at a constant temperature for 4 hours to obtain a seed emulsion.
[0063] Step 4: Nuclear fusion
[0064] The temperature of the seed emulsion in the polymerization kettle was maintained at 50° C., the stirring rate was controlled at 400 rpm, and under nitrogen protection, the other half of the emulsion remaining in step 2 was added dropwise to the seed emulsion at a rate of 0.2 g / sec, and at the same time, a potassium persulfate aqueous solution with a mass concentration of 5 wt% was added dropwise to the seed emulsion at a rate of 0.01 g / sec, and the added mass of the potassium persulfate aqueous solution was 4% of the mass of the seed emulsion. After the emulsion and the potassium persulfate aqueous solution were added dropwise, the reaction was continued with stirring for 3 hours to obtain a core polymerization emulsion.
[0065] Step 5: Shell polymerization
[0066] The core polymerization emulsion obtained in step 4 was kept at a constant temperature of 50° C. and the stirring rate was controlled to be 400 rpm. Under nitrogen protection, the shell monomer emulsion was added dropwise to the core polymerization emulsion at a rate of 0.4 g / s. At the same time, a 5 wt% potassium persulfate aqueous solution was added dropwise to the seed emulsion at a rate of 0.02 g / s. The mass of the potassium persulfate aqueous solution added was 6% of the mass of the core polymerization emulsion. After the shell monomer emulsion and the potassium persulfate aqueous solution were added dropwise, the reaction was continued with stirring for 4 hours to obtain a shell polymerization emulsion.
[0067] The added mass of the shell monomer emulsion is 75wt% of the total mass of the core polymerization emulsion;
[0068] The shell monomer emulsion is prepared by: adding sodium dodecyl sulfate, sodium polyoxyethylene ether sulfate, and deionized water into a reaction kettle, stirring and dissolving them completely, then adding allyl pyruvate, ethylene glycol monoallyl ether, and methyl methacrylate, stirring and emulsifying at a stirring rate of 1700 rpm for 6 hours, and then stopping stirring to obtain a uniform and stable shell monomer emulsion;
[0069] The mass ratio of sodium dodecyl sulfate, sodium polyoxyethylene ether sulfate, deionized water, allyl pyruvate, ethylene glycol monoallyl ether, and methyl methacrylate is 1:2:150:11:3:15.
[0070] Step 6: Spray drying
[0071] The shell polymerization emulsion is sent to a spray dryer, and the temperature of the drying hot air is controlled to be 160°C. After spray drying, a white powder with a particle size of 1 μm is obtained, which is a high-viscosity ACR resin for foaming soft products.
[0072] Example 3: Preparation method of high viscosity ACR resin for foaming soft products
[0073] Step 1: Preparation of modified silica
[0074] Add nano-silicon dioxide and anhydrous ethanol into a high-speed dispersing kettle, disperse vigorously at a speed of 12000 rpm for 11 hours, reduce the dispersing speed to 3000 rpm, increase the temperature and keep the temperature constant at 60°C, add γ-methacryloxypropyltrimethoxysilane, react at the constant temperature for 9 hours, centrifuge, wash the separated solid with anhydrous ethanol for 4 times, put it into a vacuum drying oven at 60°C and dry it for 8 hours to obtain modified silicon dioxide;
[0075] The particle size of the nano silicon dioxide is 60nm;
[0076] The mass ratio of the nano silicon dioxide, anhydrous ethanol and gamma-methacryloxypropyltrimethoxysilane is 50:180:10.
[0077] Step 2: Prepare emulsion
[0078] Sodium lauryl sulfate, sodium polyoxyethylene ether sulfate and deionized water were added into a reaction kettle, and after being stirred and dissolved completely, α-methylacrylic acid, butyl acrylate and modified silicon dioxide were added, and the stirring rate was controlled at 3500 rpm. After stirring and emulsifying for 13 hours, stirring was stopped to obtain a uniform and stable emulsion;
[0079] The mass ratio of sodium dodecyl sulfate, sodium polyoxyethylene ether sulfate, deionized water, α-methylacrylic acid, butyl acrylate and modified silicon dioxide is 5:3:190:20:9:4.
[0080] Step 3: Prepare seed emulsion
[0081] The emulsion obtained in step 2 is added to a polymerization kettle with a total mass of 50 wt% thereof, and the pressure in the polymerization kettle is evacuated to -0.08 MPa, and then nitrogen is introduced to a positive pressure, and then the pressure is evacuated again and nitrogen is introduced. After three cycles, the temperature in the kettle is raised and kept constant at 65° C. under nitrogen protection, and the stirring rate is controlled at 800 rpm, and potassium persulfate of 0.2 wt% of the total mass of the emulsion in the polymerization kettle is added. After the reaction is stirred at a constant temperature for 7 hours, a seed emulsion is obtained.
[0082] Step 4: Nuclear fusion
[0083] The temperature of the seed emulsion in the polymerization kettle was maintained at 65° C., the stirring rate was controlled at 800 rpm, and under nitrogen protection, the other half of the emulsion remaining in step 2 was added dropwise to the seed emulsion at a rate of 1.3 g / sec, and at the same time, an aqueous potassium persulfate solution with a mass concentration of 8wt% was added dropwise to the seed emulsion at a rate of 0.06 g / sec, and the added mass of the aqueous potassium persulfate solution was 7% of the mass of the seed emulsion. After the emulsion and the aqueous potassium persulfate solution were added dropwise, the reaction was continued with stirring for 6 hours to obtain a core polymerization emulsion.
[0084] Step 5: Shell polymerization
[0085] The core polymerization emulsion obtained in step 4 was kept at a constant temperature of 65° C. and the stirring rate was controlled to 800 rpm. Under nitrogen protection, the shell monomer emulsion was added dropwise to the core polymerization emulsion at a rate of 1.5 g / s. At the same time, an aqueous potassium persulfate solution with a mass concentration of 8wt% was added dropwise to the seed emulsion at a rate of 0.09 g / s. The mass of the potassium persulfate solution added was 9% of the mass of the core polymerization emulsion. After the shell monomer emulsion and the aqueous potassium persulfate solution were added dropwise, the reaction was continued with stirring for 8 hours to obtain a shell polymerization emulsion.
[0086] The added mass of the shell monomer emulsion is 97wt% of the total mass of the core polymerization emulsion;
[0087] The shell monomer emulsion is prepared by: adding sodium dodecyl sulfate, sodium polyoxyethylene ether sulfate, and deionized water into a reaction kettle, stirring and dissolving them completely, then adding allyl pyruvate, ethylene glycol monoallyl ether, and methyl methacrylate, stirring and emulsifying at a stirring rate of 3600 rpm for 11 hours, and then stopping stirring to obtain a uniform and stable shell monomer emulsion;
[0088] The mass ratio of sodium dodecyl sulfate, sodium polyoxyethylene ether sulfate, deionized water, allyl pyruvate, ethylene glycol monoallyl ether and methyl methacrylate is 4:5:210:19:8:25.
[0089] Step 6: Spray drying
[0090] The shell polymerization emulsion is sent to a spray dryer, the temperature of the drying hot air is controlled to be 180°C, and a white powder with a particle size of 2.5 μm is obtained by spray drying, which is a high-viscosity ACR resin for foaming soft products.
[0091] Comparative Example 1: Based on Example 1, step 1, preparing modified silica, is not performed. In step 2, in preparing the emulsion, 3 parts of modified silica are replaced by 3 parts of butyl acrylate. The specific operation is as follows:
[0092] Step 1, preparing modified silicon dioxide is not performed;
[0093] Step 2: Prepare emulsion
[0094] The 3 parts of modified silica were replaced by 3 parts of butyl acrylate, and the other operations were the same as in Example 1;
[0095] The operations of steps 3, 4, 5 and 6 are the same as those of Example 1.
[0096] Comparative Example 2: Based on Example 1, in step 5, shell polymerization, no allyl pyruvate and ethylene glycol monoallyl ether were added to the shell monomer emulsion, and 16 parts of allyl pyruvate and 5 parts of ethylene glycol monoallyl ether were replaced by 21 parts of methyl methacrylate in equal amounts. The specific operation was as follows:
[0097] The operations of steps 1, 2, 3, and 4 are the same as those of Example 1;
[0098] Step 5: Shell polymerization
[0099] The core polymerization emulsion obtained in step 4 was kept at a constant temperature of 62° C. and the stirring rate was controlled to be 560 rpm. Under nitrogen protection, the shell monomer emulsion was added dropwise to the core polymerization emulsion at a rate of 0.9 g / sec. At the same time, a 7wt% potassium persulfate aqueous solution was added dropwise to the seed emulsion at a rate of 0.07 g / sec. The added mass of the potassium persulfate aqueous solution was 8% of the mass of the core polymerization emulsion. After the shell monomer emulsion and the potassium persulfate aqueous solution were added dropwise, the reaction was continued with stirring for 5 hours to obtain a shell polymerization emulsion.
[0100] The added mass of the shell monomer emulsion is 92wt% of the total mass of the core polymerization emulsion;
[0101] The shell monomer emulsion is prepared by adding sodium dodecyl sulfate, sodium polyoxyethylene ether sulfate and deionized water into a reaction kettle, stirring and dissolving completely, then adding methyl methacrylate, stirring and emulsifying at a stirring rate of 3300 rpm for 9 hours, and then stopping stirring to obtain a uniform and stable shell monomer emulsion;
[0102] The mass ratio of sodium lauryl sulfate, sodium polyoxyethylene ether sulfate, deionized water and methyl methacrylate is 3:4:190:40;
[0103] The operation of step 6 is the same as that of embodiment 1.
[0104] Performance Test:
[0105] The high viscosity ACR resin for foaming soft products obtained in Examples 1, 2, 3 and Comparative Examples 1 and 2 was used to measure the intrinsic viscosity using an Ubbelohde viscometer. According to the PVC soft foam formula: 100 parts of PVC, 10 parts of azodicarbonamide foaming agent, 35 parts of dioctyl phthalate plasticizer, 5 parts of high viscosity ACR resin for foaming soft products, and 7 parts of calcium zinc stabilizer, the corresponding soft foam was prepared and the foam density was tested. The test results are shown in Table 1:
[0106] Table 1
[0107]
[0108] From the data in Table 1, it can be seen that in Comparative Example 1 without adding modified silica, the intrinsic viscosity is reduced to the lowest value of all the embodiments and comparative examples, and the foam density is also increased to the highest value of all the embodiments and comparative examples, which shows that modified silica plays a vital role in improving the intrinsic viscosity of high-viscosity ACR resin for foaming soft products, and the intrinsic viscosity has a significant negative correlation with the density of PVC soft foam, that is, the higher the intrinsic viscosity, the lower the density of the obtained PVC soft foam; in Comparative Example 2, allyl pyruvate and ethylene glycol monoallyl ether are not added to the shell monomer emulsion, and the intrinsic viscosity of Comparative Example 2 is also significantly lower than that of Example 1, and the soft foam density is 1.8 g / cm greater than that of Example 1. 3 This indicates that allyl pyruvate and ethylene glycol monoallyl ether also contribute greatly to improving the intrinsic viscosity of ACR resin, which in turn significantly affects the density of soft foam.
[0109] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A method for preparing a high-viscosity ACR resin for foaming soft products, characterized in that: The preparation method of the high-viscosity ACR resin for foaming soft products comprises six steps of preparing modified silica, preparing emulsion, preparing seed emulsion, core polymerization, shell polymerization, and spray drying; The modified silicon dioxide is prepared by adding nano silicon dioxide and anhydrous ethanol into a high-speed dispersion kettle, dispersing vigorously at a speed of 8000-12000 rpm for 5-11 hours, reducing the dispersion speed to 1000-3000 rpm, heating and maintaining the temperature at 40-60° C., adding γ-methacryloxypropyltrimethoxysilane, reacting at the constant temperature for 5-9 hours, centrifuging, washing the separated solid with anhydrous ethanol for 2-4 times, and drying it in a vacuum drying oven at 40-60° C. for 4-8 hours to obtain the modified silicon dioxide; The emulsion is prepared by adding sodium lauryl sulfate, sodium polyoxyethylene ether sulfate and deionized water into a reaction kettle, stirring and dissolving completely, then adding α-methylacrylic acid, butyl acrylate and modified silicon dioxide, controlling the stirring rate to 1500-3500 rpm, stirring and emulsifying for 9-13 hours, and then stopping the stirring to obtain a uniform and stable emulsion; The emulsion obtained in the step of preparing the seed emulsion and preparing the emulsion is added into a polymerization kettle with 50wt% of the total mass, and the pressure in the polymerization kettle is evacuated to -0.09-0.08MPa, and then nitrogen is introduced to a positive pressure, and then the vacuum is evacuated and nitrogen is introduced again. After three cycles, the temperature in the kettle is raised and kept constant at 50-65°C under nitrogen protection, and the stirring rate is controlled at 300-800 rpm, and potassium persulfate is added with an amount of 0.1-0.2wt% of the total mass of the emulsion in the polymerization kettle, and the reaction is stirred at a constant temperature for 4-7 hours to obtain a seed emulsion; The nuclear polymerization is carried out by maintaining the temperature of the seed emulsion in the polymerization kettle at 50-65° C., controlling the stirring rate at 400-800 rpm, and dripping the other half of the emulsion remaining in the step of preparing the emulsion into the seed emulsion at a rate of 0.2-1.3 g / sec under nitrogen protection, and simultaneously dripping a potassium persulfate aqueous solution with a mass concentration of 5-8 wt % into the seed emulsion at a rate of 0.01-0.06 g / sec, wherein the mass of the potassium persulfate aqueous solution added is 4-7% of the mass of the seed emulsion, and after the emulsion and the potassium persulfate aqueous solution are dripped, continuing the stirring reaction for 3-6 hours to obtain a nuclear polymerization emulsion; The shell polymerization comprises the following steps: the core polymerization emulsion obtained in the core polymerization step is kept at a constant temperature of 50-65° C., the stirring rate is controlled at 400-800 rpm, and the shell monomer emulsion is added dropwise to the core polymerization emulsion at a rate of 0.4-1.5 g / sec under nitrogen protection, and at the same time, a potassium persulfate aqueous solution with a mass concentration of 5-8 wt% is added dropwise to the seed emulsion at a rate of 0.02-0.09 g / sec, wherein the mass of the potassium persulfate aqueous solution added is 6-9% of the mass of the core polymerization emulsion, and after the shell monomer emulsion and the potassium persulfate aqueous solution are both added dropwise, the reaction is continued with stirring for 4-8 hours to obtain a shell polymerization emulsion; The added mass of the shell monomer emulsion is 75-97wt% of the total mass of the core polymerization emulsion; The shell monomer emulsion is prepared by: adding sodium dodecyl sulfate, sodium polyoxyethylene ether sulfate, and deionized water into a reaction kettle, stirring and dissolving them completely, then adding allyl pyruvate, ethylene glycol monoallyl ether, and methyl methacrylate, controlling the stirring rate to 1700-3600 rpm, stirring and emulsifying for 6-11 hours, and stopping stirring to obtain a uniform and stable shell monomer emulsion; The mass ratio of sodium lauryl sulfate, sodium polyoxyethylene ether sulfate, deionized water, allyl pyruvate, ethylene glycol monoallyl ether, and methyl methacrylate is 1-4:2-5:150-210:11-19:3-8:15-25; In the spray drying, the shell polymerized emulsion is fed into a spray dryer, the temperature of the drying hot air is controlled to be 160-180° C., and a white powder with a particle size of 1-2.5 μm is obtained by spray drying, which is a high-viscosity ACR resin for foaming soft products.
2. The method for preparing a high-viscosity ACR resin for foaming soft products according to claim 1, characterized in that: The particle size of the nano silicon dioxide is 10-60 nm; The mass ratio of the nano silicon dioxide, anhydrous ethanol and gamma-methacryloxypropyltrimethoxysilane is 20-50:120-180:5-10.
3. The method for preparing a high-viscosity ACR resin for foaming soft products according to claim 1, characterized in that: In the step of preparing the emulsion, the mass ratio of sodium dodecyl sulfate, sodium polyoxyethylene ether sulfate, deionized water, α-methylacrylic acid, butyl acrylate, and modified silicon dioxide is 2-5:1-3:130-190:10-20:4-9:1-4.
Citation Information
Patent Citations
Preparation method of acrylate foaming regulator with core-shell structure
CN105254817A
Foaming regulator for polyvinyl chloride as well as preparation method and application of foaming regulator
CN118440235A
Synthetic method of high-impact-strength ACR
CN111234115A
Preparation method of modified material for PVC
CN114292478A