Back contact heterojunction solar cell and preparation method thereof, and battery assembly

The preparation process of back-contact heterojunction solar cells is simplified through laser selective doping and high-temperature annealing, solving the problem of cumbersome traditional processes, improving production efficiency and reducing costs, while maintaining battery performance.

CN118825138BActive Publication Date: 2024-11-19GOLDEN SOLAR (QUANZHOU) NEW ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411297184.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-18
Publication Date
2024-11-19
Estimated Expiration
2044-09-18

AI Technical Summary

Technical Problem

The preparation process steps of traditional back contact heterojunction solar cells are cumbersome, resulting in low production efficiency and affecting equipment cost and overall process efficiency.

Method used

Laser selective doping and high-temperature annealing are used to replace the traditional silicon nitride mask layer, simplify the process flow on the back of the silicon wafer, and open areas are formed through laser etching to reduce process steps and time.

Benefits of technology

It significantly shortens the process flow, improves production efficiency, reduces equipment costs, and ensures the performance of solar cells and improves product competitiveness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118825138B_ABST
    Figure CN118825138B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of solar cells, and in particular to a back-contact heterojunction solar cell and a preparation method and a cell assembly thereof. The preparation method of the back-contact heterojunction solar cell realizes selective doping and recrystallization by using laser instead of high-temperature annealing on the back of a silicon wafer, and at the same time utilizes the high temperature released by the laser to generate a silicon oxide mask layer in the first semiconductor region instead of a traditional silicon nitride mask layer, so that the process flow on the back of the silicon wafer is greatly shortened, which is beneficial to improving production efficiency and significantly reducing the cost of the entire process and equipment. At the same time, the thickness of the silicon oxide mask layer and the power of the laser need to satisfy a specific formula to ensure that the first semiconductor layer is at an optimal passivation level while being able to protect the first semiconductor layer from being damaged by texturing and cleaning.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of solar cells, and in particular relates to a back-contact heterojunction solar cell and a preparation method and a cell assembly thereof. Background Art

[0002] The traditional preparation process of the back side of the back contact heterojunction solar cell includes: firstly, preparing the tunneling polycrystalline layer by tubular PECVD, and then annealing; then cleaning, preparing the silicon nitride layer or silicon oxide mask layer; then removing the semiconductor film layer in the opening area by laser opening, texturing and cleaning. These processes are mainly for preparing the semiconductor layer on the back side of the silicon wafer and forming the opening area at the same time, but the process steps are somewhat cumbersome, resulting in a long process preparation time, which is not conducive to improving the production efficiency of the back contact heterojunction solar cell.

[0003] It should be noted that this part of the present invention only provides background technology related to the present invention and does not necessarily constitute prior art or known technology. Summary of the invention

[0004] The purpose of the present invention is to provide a back-contact heterojunction solar cell and a preparation method and a cell assembly, so as to overcome the technical problem of low preparation efficiency of existing back-contact heterojunction solar cells.

[0005] In order to achieve the above objectives, in a first aspect, an embodiment of the present invention provides a method for preparing a back-contact heterojunction solar cell, comprising:

[0006] S01, providing a silicon wafer;

[0007] S02, forming a first tunneling silicon oxide layer and an amorphous silicon layer on the back side of the silicon wafer in sequence to obtain a first semiconductor layer; wherein the amorphous silicon layer is composed of a first intrinsic amorphous silicon layer and a phosphorus-doped amorphous silicon layer; S03, selectively doping the surface of the amorphous silicon layer by laser to form an N-type polysilicon layer and a silicon oxide mask layer, and the area without the silicon oxide mask layer is the second semiconductor opening area; the power of the laser used for the selective doping is 10KW-18KW, and the frequency is 300KHZ-800KHZ; the phosphorus doping concentration of the doped area forming the silicon oxide mask layer is 1e20-5e20cm -3 , the thickness of the silicon oxide mask layer is 29-55nm; wherein the thickness of the silicon oxide mask layer and the power of the laser satisfy L=3P±1, L is the thickness of the silicon oxide mask layer, in nm, and P is the power of the laser, in KW;

[0008] S04, removing the first semiconductor layer in the second semiconductor opening region by texturing and cleaning, and forming a texture surface on the front side of the silicon wafer and the second semiconductor opening region, and then removing the silicon oxide mask layer outside the second semiconductor opening region on the back side of the silicon wafer by hydrofluoric acid cleaning;

[0009] S05, forming a third semiconductor layer and an anti-reflection layer in sequence on the front side of the silicon wafer, wherein the third semiconductor layer includes a second tunneling oxide layer and an aluminum oxide film layer, and the anti-reflection layer is a silicon nitride layer;

[0010] S06, depositing a second semiconductor layer on the back side of the silicon wafer, wherein the second semiconductor layer comprises a second intrinsic amorphous silicon layer and a P-type doped amorphous silicon layer or a P-type microcrystalline silicon layer.

[0011] Optionally, after step S06, the method further includes:

[0012] S07, etching an opening on the back side of the silicon wafer by laser or mask etching to form a first semiconductor opening region spaced apart from the second semiconductor opening region;

[0013] S08, cleaning and removing the second semiconductor layer remaining in the first semiconductor opening region, and then depositing a transparent conductive film layer on the back side of the obtained silicon wafer;

[0014] S09, making an opening on the transparent conductive film layer between the first semiconductor opening region and the second semiconductor opening region to form an isolation groove;

[0015] S10, forming a first electrode on the transparent conductive film layer in the first semiconductor opening region, and correspondingly forming a second electrode on the transparent conductive film layer in the second semiconductor opening region.

[0016] Optionally, in step S02, sequentially forming a tunneling silicon oxide layer and an amorphous silicon layer on the back side of the silicon wafer to obtain a first semiconductor layer specifically includes:

[0017] S201, the first semiconductor layer is formed by in-situ doping by tubular plasma enhanced chemical vapor deposition, and laughing gas is introduced in the first stage, the glow is turned on, and a tunneling silicon oxide layer is formed by chemical reaction, the reaction temperature in the first stage is 400-450° C., the reaction pressure is 100-2000 mtorr, the time is 10-60 seconds, the NO2 flow rate is 5000-8000 sccm, and the thickness of the tunneling silicon oxide layer is 1-2 nm;

[0018] S202, then enter the second stage, in which silane and hydrogen are introduced, the glow is turned on, and the first intrinsic amorphous silicon layer is formed by chemical reaction. The reaction temperature of the second stage is 400-450°C, the reaction time is 300-800 seconds, the reaction pressure is 100-2000mtorr, and the thickness of the first intrinsic amorphous silicon is 40-70nm;

[0019] S203, then enter the third stage, in which silane, phosphine and hydrogen are introduced, the glow is turned on, and a phosphorus-doped amorphous silicon layer is formed through chemical reaction. The reaction temperature of the third stage is 400-450°C, the reaction time is 400-900 seconds, the reaction pressure is 100-2000mtorr, and the thickness of the phosphorus-doped amorphous silicon layer is 60-90nm.

[0020] Optionally, the selectively doped laser is a flat-top picosecond green laser.

[0021] Optionally, in step S05, the aluminum oxide film layer is deposited by atomic energy deposition, wherein the deposition process temperature is 150-180°C and the thickness is 2-10nm, and the silicon nitride layer is formed by tubular PECVD in-situ doping, wherein the reaction temperature is 400-450°C and the thickness is 80-110m.

[0022] Optionally, in step S06, the second semiconductor layer is obtained by plasma enhanced chemical vapor deposition technology; the thickness of the second intrinsic amorphous silicon layer is 5-15nm, the thickness of the P-type doped amorphous silicon layer or the P-type microcrystalline silicon layer is 10-35nm, and the boron doping concentration in the P-type doped amorphous silicon layer or the P-type microcrystalline silicon layer is 1e19-4e20 cm -3 .

[0023] Optionally, in step S07, the width of the first semiconductor opening region is 0.1-0.3 mm, and when a laser is used to etch an opening on the back side of the silicon wafer, the laser is an ultraviolet or green laser, and the pulse width is less than 50 ns.

[0024] Optionally, in step S08, a transparent conductive film layer is deposited on the back side of the obtained silicon wafer, comprising:

[0025] A transparent conductive film is deposited on the back of a silicon wafer by physical vapor deposition technology or activated plasma deposition technology. The thickness of the transparent conductive film is 40-80 nm. The material of the transparent conductive film includes an indium oxide film doped with tin oxide, titanium oxide, zinc oxide or gallium oxide, or the material of the transparent conductive film includes a zinc oxide film doped with aluminum oxide, gallium oxide or boron oxide.

[0026] In a third aspect, an embodiment of the present invention further provides a back-contact heterojunction solar cell, which is obtained using the method for preparing a back-contact heterojunction solar cell as described in the first aspect.

[0027] In a third aspect, an embodiment of the present invention further provides a battery assembly, which includes the back-contact heterojunction solar cell as described in the second aspect.

[0028] The embodiments of the present invention have at least the following beneficial effects:

[0029] The method for preparing a back-contact heterojunction solar cell provided by an embodiment of the present invention realizes selective doping and recrystallization by using a laser on the back of a silicon wafer instead of high-temperature annealing, and at the same time utilizes the high temperature released by the laser to generate a silicon oxide mask layer in the first semiconductor region instead of a traditional silicon nitride mask layer, thereby greatly shortening the process flow on the back of the silicon wafer, which is beneficial to improving the production efficiency of solar cells, and at the same time significantly reducing the process and equipment costs of the entire solar cell; further, when using the laser method to simultaneously prepare the doping layer and the mask layer, it is necessary to match the appropriate doping concentration of the doping layer and the thickness of the mask layer, because the mask layer needs A certain thickness protects the N-type polysilicon layer from being damaged by subsequent texturing and cleaning. Therefore, a certain amount of laser energy is required to meet the growth of the mask layer. When the doping concentration of the doping layer is too high, the laser energy will cause over-doping to damage the oxide layer and affect the passivation level. When the doping concentration of the doping layer is too low, it will lead to insufficient doping and insufficient field passivation effect, which will also lead to a low passivation level. At the same time, in this process, it was found through research that the thickness of the silicon oxide mask layer and the power of the laser need to satisfy a specific formula. If this formula is met, it can ensure that the first semiconductor layer is at the optimal passivation level while protecting the first semiconductor layer from damage by texturing and cleaning. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0031] Figure 1 A process flow chart of a method for preparing a back-contact heterojunction solar cell provided by an embodiment of the present invention;

[0032] Figure 2 A process structure diagram corresponding to step S01 in a method for preparing a back-contact heterojunction solar cell provided by an embodiment of the present invention;

[0033] Figure 3 Figure 4A process structure diagram corresponding to step S02 in a method for preparing a back-contact heterojunction solar cell provided by an embodiment of the present invention;

[0034] Figure 4 A process structure diagram corresponding to step S03 in a method for preparing a back-contact heterojunction solar cell provided by an embodiment of the present invention;

[0035] Figure 5 A process structure diagram corresponding to step S05 in a method for preparing a back-contact heterojunction solar cell provided by an embodiment of the present invention;

[0036] Figure 6 A process structure diagram corresponding to steps S06 and S07 in a method for preparing a back-contact heterojunction solar cell provided by an embodiment of the present invention;

[0037] Figure 7 A process flow chart of another method for preparing a back-contact heterojunction solar cell provided by an embodiment of the present invention;

[0038] Figure 8 A process structure diagram corresponding to steps S08 and S09 in a method for preparing a back-contact heterojunction solar cell provided by an embodiment of the present invention;

[0039] Fig. 9 A process structure diagram corresponding to step S10 in a method for preparing a back-contact heterojunction solar cell provided in an embodiment of the present invention.

[0040] Description of Reference Numerals

[0041] 1. Silicon wafer, 2. First tunneling silicon oxide layer, 3. Amorphous silicon layer, 4. N-type polysilicon layer, 5. Silicon oxide mask layer, 6. Second tunneling oxide layer, 7. Aluminum oxide film layer, 8. Silicon nitride layer, 9. Second intrinsic amorphous silicon layer; 10. P-type doped amorphous silicon layer or P-type microcrystalline silicon layer; 11. Transparent conductive film layer. DETAILED DESCRIPTION

[0042] In the present invention, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.

[0043] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being "above", "above" or "above" a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" or "below" a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.

[0044] The endpoints and any values ​​of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article. Among them, the terms "optional" and "optional" all mean that they may be included or not included (or may be present or not).

[0045] The first aspect, such as Figure 1 As shown, an embodiment of the present invention provides a method for preparing a back-contact heterojunction solar cell, comprising the following steps:

[0046] S01. Provide a silicon wafer 1.

[0047] Alternatively, if Figure 2 As shown, step S01 may also include other conventional operations, such as double-sided polishing and optional cleaning of the silicon wafer 1. The silicon wafer 1 is preferably an N-type single crystal silicon wafer. The silicon wafer 1 may be a Czochralski single crystal silicon wafer or a cast single crystal silicon wafer.

[0048] S02, forming a first tunneling silicon oxide layer 2 and an amorphous silicon layer 3 in sequence on the back side of the silicon wafer 1 to obtain a first semiconductor layer; wherein the amorphous silicon layer 3 is composed of a first intrinsic amorphous silicon layer and a phosphorus-doped amorphous silicon layer.

[0049] Specifically, see Figure 3 The specific preparation process of step S02 includes:

[0050] S201, the first semiconductor layer is formed by in-situ doping by tubular PECVD, and in the first stage, laughing gas is introduced, the glow is turned on, and a tunneling silicon oxide layer is formed by chemical reaction, the reaction temperature of the first stage is 400-450°C, the reaction pressure is 100-2000mtorr, the time is 10-60 seconds, the NO2 flow rate is 5000-8000sccm, and the thickness of the tunneling silicon oxide layer is 1-2nm;

[0051] S202, then enter the second stage, in which silane and hydrogen are introduced, the glow is turned on, and the first intrinsic amorphous silicon layer is formed by chemical reaction. The reaction temperature of the second stage is 400-450°C, the reaction time is 300-800 seconds, the reaction pressure is 100-2000mtorr, and the thickness of the first intrinsic amorphous silicon is 40-70nm.

[0052] S203, then enter the third stage, in which silane, phosphine and hydrogen are introduced, the glow is turned on, and a phosphorus-doped amorphous silicon layer is formed through chemical reaction. The reaction temperature of the third stage is 400-450°C, the reaction time is 400-900 seconds, the reaction pressure is 100-2000mtorr, and the thickness of the phosphorus-doped amorphous silicon layer is 60-90nm.

[0053] S03, using laser to selectively dope the surface of the amorphous silicon layer 3 and form an N-type polysilicon layer 4 and a silicon oxide mask layer 5, the area without the silicon oxide mask layer 5 is the second semiconductor opening area S102; the power of the laser used for selective doping is 10KW-18KW, and the frequency is 300KHZ-800KHZ; the phosphorus doping concentration of the doping area forming the silicon oxide mask layer is 1e20-5e20cm -3 , the thickness of the silicon oxide mask layer 5 is 29-55nm; wherein the thickness of the silicon oxide mask layer 5 and the power of the laser satisfy L=3P±1, L is the thickness of the silicon oxide mask layer 5, in nm, and P is the power of the laser, in KW, see Figure 4 .

[0054] Specifically, the N-type polycrystalline silicon layer is formed by laser high-temperature annealing of the first intrinsic amorphous silicon layer and the phosphorus-doped amorphous silicon layer, and the silicon oxide mask layer is also a silicon oxide layer formed by laser high-temperature oxidation on the surface of the N-type polycrystalline silicon and air. The thickness of the silicon oxide has no corresponding relationship with the amorphous silicon layer. However, if the silicon oxide mask layer is too thin, it cannot play a protective role in the subsequent texturing and cleaning, and will damage the polycrystalline silicon layer and the oxide layer. If the silicon oxide mask layer is too thick, the laser energy required will be higher, and higher laser energy will cause over-deep doping and damage the oxide layer. Therefore, the embodiment of the present invention needs to control the thickness of the silicon oxide mask layer 5 within a reasonable thickness range.

[0055] Optionally, in step S03, the width of the second semiconductor opening region S102 is 0.3-0.6 mm; the selectively doped laser is a flat-top picosecond green laser with a wavelength of 532 nm; or, the selectively doped laser is a flat-top picosecond ultraviolet laser with a wavelength of 355 nm.

[0056] Optionally, the selectively doped laser is a flat-top picosecond green laser. S04, remove the first semiconductor layer in the second semiconductor opening area S102 by texturing and cleaning, and simultaneously form a texture surface on the front side of the silicon wafer 1 and the second semiconductor opening area S102, and then remove the silicon oxide mask layer 5 outside the second semiconductor opening area S102 on the back side of the silicon wafer 1 by hydrofluoric acid cleaning, see Figure 5 .

[0057] S05 , forming a third semiconductor layer and an anti-reflection layer in sequence on the front side of the silicon wafer 1 , wherein the third semiconductor layer includes a second tunneling oxide layer 6 and an aluminum oxide film layer 7 , and the anti-reflection layer is a silicon nitride layer 8 .

[0058] Alternatively, if Figure 5 As shown, in step S05, the aluminum oxide film layer 7 is deposited by atomic energy deposition, wherein the deposition process temperature is 150-180°C and the thickness is 2-10nm, and the silicon nitride layer 8 is formed by tubular PECVD in-situ doping, wherein the reaction temperature is 400-450°C and the thickness is 80-110m.

[0059] S06 , depositing a second semiconductor layer on the back side of the silicon wafer 1 , the second semiconductor layer comprising a second intrinsic amorphous silicon layer 9 and a P-type doped amorphous silicon layer or a P-type microcrystalline silicon layer 10 .

[0060] Optionally, see Figure 6 The second semiconductor layer is obtained by plasma enhanced chemical vapor deposition technology; the second intrinsic amorphous silicon layer 9 has a thickness of 5-15nm, the thickness of the P-type doped amorphous silicon layer or the P-type microcrystalline silicon layer 10 is 10-35nm, and the boron doping concentration in the P-type doped amorphous silicon layer or the P-type microcrystalline silicon layer 10 is 1e19-4e20 cm -3 .

[0061] In some embodiments, see Figure 7 , after step S06, further comprising the following steps:

[0062] S07, etching an opening on the back side of the silicon wafer 1 by laser or mask etching to form a first semiconductor opening region S101 spaced apart from the second semiconductor opening region S102.

[0063] Optionally, continue to Figure 6 , using laser or mask etching, an opening is etched on the back of the silicon wafer 1 to form a first semiconductor opening area S101 spaced apart from the second semiconductor opening area S102, and then cleaned. The width of the first semiconductor opening area S101 is 0.1-0.3mm. When the laser is used to etch the opening on the back of the silicon wafer 1, the laser is an ultraviolet or green laser, and the pulse width is less than 50ns.

[0064] S08 , cleaning and removing the remaining second semiconductor layer in the first semiconductor opening region S101 , and then depositing a transparent conductive film layer 11 on the back side of the obtained silicon wafer 1 .

[0065] Optionally, see Figure 8 A transparent conductive film is deposited on the back of the silicon wafer 1 by physical vapor deposition (PVD) or activated plasma deposition (RPD). The thickness of the transparent conductive film is 40-80 nm. The material of the transparent conductive film includes an indium oxide film doped with tin oxide, titanium oxide, zinc oxide or gallium oxide, or the material of the transparent conductive film includes a zinc oxide film doped with aluminum oxide, gallium oxide or boron oxide.

[0066] S09 , opening is performed on the transparent conductive film layer 11 between the first semiconductor opening region S101 and the second semiconductor opening region S102 to form an isolation groove.

[0067] Specifically, Figure 8 As shown, an isolation groove is formed between the first semiconductor opening region S101 and the second semiconductor region by laser or etching, and the width of the isolation groove is 30um-200um.

[0068] S10 , forming a first electrode on the transparent conductive film layer 11 in the first semiconductor opening region S101 , and correspondingly forming a second electrode on the transparent conductive film layer 11 in the second semiconductor opening region S102 .

[0069] Specifically, see Fig. 9 A first electrode is formed on the conductive film layer of the first semiconductor region, and a second electrode is correspondingly formed on the conductive film layer of the second semiconductor region. A silver gate electrode can be formed by a screen printing process and low-temperature sintering, or the electrode can be formed by electroplating. Preferably, the gate line electrode is formed by electroplating.

[0070] It should be noted that the method for preparing a back-contact heterojunction solar cell in the embodiment of the present invention may also include other conventionally required steps, which can be selected according to actual needs and will not be described in detail here.

[0071] In the second aspect, the embodiment of the present invention further provides a back-contact heterojunction solar cell, which is obtained by the preparation method of the back-contact heterojunction solar cell in the above embodiment, and includes: a silicon wafer 1, a first semiconductor layer, a second semiconductor layer, a third semiconductor layer and an anti-reflection layer. Among them, the front side refers to the light-receiving surface of the silicon wafer 1, and the back side is the opposite back side of the light-receiving surface. In the embodiment of the present invention, the side close to the silicon wafer 1 is usually considered as the inside, and the side far from the silicon wafer 1 is considered as the outside.

[0072] Specifically, the first semiconductor layer is arranged on the back side of the silicon wafer 1, and the first semiconductor layer includes a first tunneling silicon oxide layer 2 sequentially formed on the silicon wafer 1, and an N-type polysilicon layer 4 and a silicon oxide mask layer 5 formed on the first tunneling silicon oxide layer 2 by laser selective doping. The N-type polysilicon layer 4 and the silicon oxide mask layer 5 are obtained by laser selective doping of the amorphous silicon layer 3.

[0073] In order to control the thickness of the silicon oxide mask layer 5, the power of the laser used for selective doping is 10KW-18KW, and the frequency is 300KHZ-800KHZ; the phosphorus doping concentration of the doping area forming the silicon oxide mask layer is 1e20-5e20cm -3 , the thickness of the silicon oxide mask layer 5 is 29-55nm; wherein, the thickness of the silicon oxide mask layer 5 and the power of the laser satisfy L=3P±1, L is the thickness of the silicon oxide mask layer 5, the unit is nm, P is the power of the laser, the unit is KW, that is, the thickness of the silicon oxide mask layer 5 is determined by the power of the laser, thereby determining the film thickness of the silicon oxide mask layer 5 and the N-type polysilicon layer 4 respectively.

[0074] Optionally, the selectively doped laser is a flat-top picosecond green laser with a wavelength of 532 nm; or, the selectively doped laser is a flat-top picosecond ultraviolet laser with a wavelength of 355 nm.

[0075] Optionally, the selectively doped laser is a flat-top picosecond green laser.

[0076] The first semiconductor layer is separated by a plurality of second semiconductor opening regions S102, and the second semiconductor opening regions S102 and the surface of the first semiconductor layer around the second semiconductor opening regions S102 are covered with a second semiconductor layer, and the second semiconductor layer comprises a second intrinsic amorphous silicon layer 9 and a P-type doped amorphous layer or a P-type microcrystalline silicon layer. The third semiconductor layer and the anti-reflection layer are sequentially arranged on the front side of the silicon wafer 1, and the third semiconductor layer comprises a second tunneling oxide layer 6 and an aluminum oxide film layer 7, and the anti-reflection layer is a silicon nitride layer 8.

[0077] Specifically, the second semiconductor layer is obtained by plasma enhanced chemical vapor deposition technology; the thickness of the second intrinsic amorphous silicon layer 9 is 5-15nm, the thickness of the P-type doped amorphous silicon layer or the P-type microcrystalline silicon layer 10 is 10-35nm, and the boron doping concentration in the P-type doped amorphous silicon layer or the P-type microcrystalline silicon layer 10 is 1e19-4e20 cm -3 The aluminum oxide film layer 7 is deposited by atomic energy deposition, wherein the deposition process temperature is 150-180° C. and the thickness is 2-10 nm. The silicon nitride layer 8 is formed by tubular PECVD in-situ doping, wherein the reaction temperature is 400-450° C. and the thickness is 80-110 nm.

[0078] Optionally, the anti-reflection layer is mainly used to reduce the reflection of light, thereby improving the photoelectric conversion efficiency. The thickness of the anti-reflection layer is generally 80mm~100mm. If it is too thick, it is not conducive to the penetration of light, and if it is too thin, the reflection effect of the incident light is not good.

[0079] The back-contact heterojunction solar cell provided by the embodiment of the present invention realizes selective doping and recrystallization by laser high-temperature doping instead of traditional tubular furnace high-temperature annealing, and at the same time utilizes the high temperature of laser engraving to generate a silicon oxide mask layer in the first semiconductor region instead of the traditional silicon nitride mask layer. The efficiency of the back-contact solar cell prepared by the present invention is not significantly different from that of the back-contact solar cell prepared by the traditional method, but its process steps are significantly reduced, the equipment cost is greatly reduced, and the product competitiveness is greatly improved.

[0080] In some embodiments, a textured surface is formed on the front side of the silicon wafer 1 and the surface of the silicon wafer 1 located in the second semiconductor opening area S102. The second semiconductor layer and the third semiconductor layer respectively fill the textured surfaces in corresponding areas. The textured surface is formed by an acid cleaning process, which can not only remove excess film layer material, but also help to increase the bonding strength between the film layers.

[0081] In some embodiments, continue to refer to Figure 1 The back contact heterojunction solar cell further includes: an isolation groove; the isolation groove is located between the adjacent first semiconductor opening area S101 and the second semiconductor opening area S102; the first semiconductor opening area S101 and the second semiconductor layer are both covered with a transparent conductive film layer 11, and the isolation groove separates the transparent conductive film layer 11 located in the first semiconductor opening area S101 from the transparent conductive film layer 11 located on the second semiconductor layer. Optionally, the width of the isolation groove is 30um~200um.

[0082] In a third aspect, an embodiment of the present invention further provides a battery assembly, which includes the back-contact heterojunction solar cell in the aforementioned embodiment.

[0083] By preparing a battery module using the back-contact heterojunction solar cell provided by the embodiment of the present invention, the cost of the battery module is reduced by reducing the production cost of the battery, thereby improving the product competitiveness of the battery module.

[0084] The embodiments of the present invention are described in detail below, which are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention.

[0085] Example 1

[0086] A back contact heterojunction solar cell, the structure of which is as follows Fig. 9 As shown, its preparation method is as follows Figure 7 As shown, the preparation method specifically includes:

[0087] S01. Provide a silicon wafer 1.

[0088] Alternatively, if Figure 2 As shown, step S01 may also include other conventional operations, such as double-sided polishing and optional cleaning of the silicon wafer 1. The silicon wafer 1 is an N-type single crystal silicon wafer.

[0089] S02. A first tunneling silicon oxide layer 2 and an amorphous silicon layer 3 are sequentially formed on the back of the silicon wafer 1 to obtain a first semiconductor layer; wherein the amorphous silicon layer 3 is composed of a first intrinsic amorphous silicon layer and a phosphorus-doped amorphous silicon layer. The thickness of the tunneling oxide layer is 1.5 nm, the thickness of the first intrinsic amorphous silicon layer is 50 nm, the thickness of the phosphorus-doped amorphous silicon layer is 70 nm, and the total thickness of the amorphous silicon layer 3 is 120 nm.

[0090] S03, using laser to selectively dope the surface of the amorphous silicon layer 3 and form N-type polysilicon and silicon oxide mask layer 5, the area without silicon oxide mask layer 5 is the second semiconductor opening area S102; the laser used for selective doping is a flat-top picosecond green laser, the power of the laser is 10KW, and the frequency is 300KHZ; the phosphorus doping concentration of the doping area forming the silicon oxide mask layer is 1e20cm -3 , the thickness of the silicon oxide mask layer 5 is 30nm; wherein, the thickness of the silicon oxide mask layer 5 and the power of the laser satisfy L=3P±1, L is the thickness of the silicon oxide mask layer 5, the unit is nm, and P is the power of the laser, the unit is KW.

[0091] S04. Remove the first semiconductor layer in the second semiconductor opening area S102 by texturing and cleaning, and at the same time form a texture surface on the front side of the silicon wafer 1 and the second semiconductor opening area S102. Then, remove the silicon oxide mask layer 5 outside the second semiconductor opening area S102 on the back side of the silicon wafer 1 by hydrofluoric acid cleaning.

[0092] S05. A third semiconductor layer and an anti-reflection layer are sequentially formed on the front side of the silicon wafer 1. The third semiconductor layer includes a second tunneling oxide layer 6 and an aluminum oxide film layer 7. The anti-reflection layer is a silicon nitride layer 8.

[0093] Optionally, the aluminum oxide film layer 7 is deposited by atomic energy deposition, wherein the process temperature is between 160° C. and the thickness is 2 nm, and the silicon nitride layer 8 is formed by tubular PECVD in-situ doping, wherein the reaction temperature is 450° C. and the thickness is 120 nm.

[0094] S06 , depositing a second semiconductor layer on the back side of the silicon wafer 1 , wherein the second semiconductor layer comprises a second intrinsic amorphous silicon layer 9 and a P-type doped amorphous silicon layer or a P-type microcrystalline silicon layer 10 .

[0095] Optionally, the second intrinsic amorphous silicon layer 9 has a thickness of 5-15 nm, the P-type doped amorphous silicon layer or the P-type microcrystalline silicon layer 10 has a thickness of 10-35 nm, and the boron doping concentration in the P-type doped amorphous silicon layer or the P-type microcrystalline silicon layer 10 is 1e19-4e20 cm -3 .

[0096] S07 , etching an opening on the back side of the silicon wafer 1 by laser or mask etching to form a first semiconductor opening region S101 spaced apart from the second semiconductor opening region S102 .

[0097] Optionally, continue to Figure 6 , using laser or mask etching, an opening is etched on the back of the silicon wafer 1 to form a first semiconductor opening area S101 spaced apart from the second semiconductor opening area S102, and then cleaned. The width of the first semiconductor opening area S101 is 0.2 mm. When the laser is used to etch the opening on the back of the silicon wafer 1, the laser is an ultraviolet or green laser, and the pulse width is less than 50ns.

[0098] S08 , cleaning and removing the remaining second semiconductor layer in the first semiconductor opening region S101 , and then depositing a transparent conductive film layer 11 on the back side of the obtained silicon wafer 1 .

[0099] Optionally, see Figure 8 A transparent conductive film is deposited on the back of the silicon wafer 1 by physical vapor deposition (PVD) or activated plasma deposition (RPD). The thickness of the transparent conductive film is 60 nm. The material of the transparent conductive film includes an indium oxide film doped with tin oxide, titanium oxide, zinc oxide or gallium oxide, or the material of the transparent conductive film includes a zinc oxide film doped with aluminum oxide, gallium oxide or boron oxide.

[0100] S09 , opening the transparent conductive film layer 11 between the first semiconductor opening region S101 and the second semiconductor opening region S102 to form an isolation groove.

[0101] Specifically, Figure 8 As shown, an isolation groove is formed between the first semiconductor opening region S101 and the second semiconductor region by laser or etching, and the width of the isolation groove is 100 um.

[0102] S10 , forming a first electrode on the transparent conductive film layer 11 in the first semiconductor opening region S101 , and correspondingly forming a second electrode on the transparent conductive film layer 11 in the second semiconductor opening region S102 .

[0103] Continue reading Fig. 9A first electrode is formed on the conductive film layer of the first semiconductor region, and a second electrode is correspondingly formed on the conductive film layer of the second semiconductor region. A silver gate electrode can be formed by a screen printing process and low-temperature sintering, or the electrode can be formed by electroplating. Preferably, the gate line electrode is formed by electroplating.

[0104] Example 2

[0105] The method of Example 1 is referred to, except that in step S03, the power of the laser is 15KW, the frequency is 500KHZ, the thickness of the silicon oxide mask layer 5 is 45nm, but the formula L=3P±1 is still satisfied.

[0106] Example 3

[0107] The method of Example 1 is referred to, except that in step S03, the power of the laser is 18KW, the frequency is 800KHZ, the thickness of the silicon oxide mask layer 5 is 55nm, but the formula L=3P±1 is still satisfied.

[0108] Example 4

[0109] The method of Example 1 is referred to, except that the thickness of the amorphous silicon layer 3 is adjusted to 100 nm, wherein the thickness of the first intrinsic amorphous silicon layer is 40 nm, and the thickness of the phosphorus-doped amorphous silicon layer is 60 nm.

[0110] Comparative Example 1

[0111] The method of Example 1 is referred to, except that in step S03, the power of the laser is 10KW, the frequency is 100KHZ, the thickness of the silicon oxide mask layer 5 is 20nm, but the formula L=3P±1 is not satisfied.

[0112] Comparative Example 2

[0113] The method of Example 1 is referred to, except that in step S03, the power of the laser is 5KW, the frequency is 300KHZ, the thickness of the silicon oxide mask layer 5 is 10nm, but the formula L=3P±1 is not satisfied.

[0114] Comparative Example 3

[0115] The method of Example 1 is referred to, except that in step S03, the power of the laser is 2KW, the frequency is 300KHZ, the thickness of the silicon oxide mask layer 5 is 5nm, and the formula L=3P±1 is not satisfied.

[0116] Comparative Example 4

[0117] The method of Example 1 is referred to, except that in step S03, the power of the laser is 30KW, the frequency is 800KHZ, the thickness of the silicon oxide mask layer 5 is 90nm, but the formula L=3P±1 is satisfied.

[0118] Comparative Example 5

[0119] The method of Example 1 is referred to, except that the thickness of the amorphous silicon layer 3 in step S02 is adjusted to 50 nm, wherein the thickness of the first intrinsic amorphous silicon layer is 20 nm, and the thickness of the phosphorus-doped amorphous silicon layer is 30 nm.

[0120] Test Case

[0121] The comparison results of the electrical properties such as conversion effect or open circuit voltage of the back-contact heterojunction solar cells obtained in the above-mentioned embodiment and the comparative example are shown in Table 1.

[0122] Table 1 Comparison of electrical properties under different parameter conditions

[0123]

[0124] It can be seen from the above results that, compared with the comparative example, the embodiment of the present invention can significantly improve the passivation level and help improve the conversion efficiency. Further, according to Example 1 and Examples 2 to 4, it can be seen that the preferred laser power of the present invention can reasonably control the thickness of the mask layer and the doping concentration of the first semiconductor layer, which is more conducive to improving the conversion efficiency while ensuring a high passivation level.

[0125] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A method for preparing a back-contact heterojunction solar cell, characterized in that: include: S01, providing a silicon wafer; S02, sequentially forming a first tunneling silicon oxide layer and an amorphous silicon layer on the back side of the silicon wafer to obtain a first semiconductor layer; wherein the amorphous silicon layer is composed of a first intrinsic amorphous silicon layer and a phosphorus-doped amorphous silicon layer; S03, using laser to selectively dope the surface of the amorphous silicon layer and form an N-type polysilicon layer and a silicon oxide mask layer, the area without the silicon oxide mask layer is the second semiconductor opening area; the power of the laser used for the selective doping is 10KW-18KW, and the frequency is 300KHZ-800KHZ; the phosphorus doping concentration of the doping area forming the silicon oxide mask layer is 1e20-5e20cm -3 , the thickness of the silicon oxide mask layer is 29-55nm; wherein the thickness of the silicon oxide mask layer and the power of the laser satisfy L=3P±1, L is the thickness of the silicon oxide mask layer, in nm, and P is the power of the laser, in KW; S04, removing the first semiconductor layer in the second semiconductor opening region by texturing and cleaning, and forming a texture surface on the front side of the silicon wafer and the second semiconductor opening region, and then removing the silicon oxide mask layer outside the second semiconductor opening region on the back side of the silicon wafer by hydrofluoric acid cleaning; S05, forming a third semiconductor layer and an anti-reflection layer in sequence on the front side of the silicon wafer, wherein the third semiconductor layer includes a second tunneling oxide layer and an aluminum oxide film layer, and the anti-reflection layer is a silicon nitride layer; S06, depositing a second semiconductor layer on the back side of the silicon wafer, wherein the second semiconductor layer comprises a second intrinsic amorphous silicon layer and a P-type doped amorphous silicon layer or a P-type microcrystalline silicon layer.

2. The method for preparing a back-contact heterojunction solar cell according to claim 1, characterized in that: After step S06, the method further includes: S07, etching an opening on the back side of the silicon wafer by laser or mask etching to form a first semiconductor opening region spaced apart from the second semiconductor opening region; S08, cleaning and removing the second semiconductor layer remaining in the first semiconductor opening region, and then depositing a transparent conductive film layer on the back side of the obtained silicon wafer; S09, making an opening on the transparent conductive film layer between the first semiconductor opening region and the second semiconductor opening region to form an isolation groove; S10, forming a first electrode on the transparent conductive film layer in the first semiconductor opening region, and correspondingly forming a second electrode on the transparent conductive film layer in the second semiconductor opening region.

3. The method for preparing a back-contact heterojunction solar cell according to claim 1, characterized in that: In the step S02, the step of sequentially forming a tunneling silicon oxide layer and an amorphous silicon layer on the back side of the silicon wafer to obtain a first semiconductor layer specifically includes: S201, the first semiconductor layer is formed by in-situ doping by tubular plasma enhanced chemical vapor deposition, and laughing gas is introduced in the first stage, the glow is turned on, and a tunneling silicon oxide layer is formed by chemical reaction, the reaction temperature in the first stage is 400-450° C., the reaction pressure is 100-2000 mtorr, the time is 10-60 seconds, the NO2 flow rate is 5000-8000 sccm, and the thickness of the tunneling silicon oxide layer is 1-2 nm; S202, then enter the second stage, in which silane and hydrogen are introduced, the glow is turned on, and the first intrinsic amorphous silicon layer is formed by chemical reaction. The reaction temperature of the second stage is 400-450°C, the reaction time is 300-800 seconds, the reaction pressure is 100-2000mtorr, and the thickness of the first intrinsic amorphous silicon is 40-70nm; S203, then enter the third stage, in which silane, phosphine and hydrogen are introduced, the glow is turned on, and a phosphorus-doped amorphous silicon layer is formed through chemical reaction. The reaction temperature of the third stage is 400-450°C, the reaction time is 400-900 seconds, the reaction pressure is 100-2000mtorr, and the thickness of the phosphorus-doped amorphous silicon layer is 60-90nm.

4. The method for preparing a back-contact heterojunction solar cell according to claim 1, characterized in that: The selectively doped laser is a flat-top picosecond green laser.

5. The method for preparing a back-contact heterojunction solar cell according to claim 1, characterized in that: In the step S05, the aluminum oxide film layer is deposited by atomic energy deposition, wherein the deposition process temperature is 150-180°C and the thickness is 2-10nm, and the silicon nitride layer is formed by tubular PECVD in-situ doping, the reaction temperature is 400-450°C and the thickness is 80-110m.

6. The method for preparing a back-contact heterojunction solar cell according to claim 1, characterized in that: In step S06, the second semiconductor layer is obtained by plasma enhanced chemical vapor deposition technology; the thickness of the second intrinsic amorphous silicon layer is 5-15nm, the thickness of the P-type doped amorphous silicon layer or the P-type microcrystalline silicon layer is 10-35nm, and the boron doping concentration in the P-type doped amorphous silicon layer or the P-type microcrystalline silicon layer is 1e19-4e20 cm -3 .

7. The method for preparing a back-contact heterojunction solar cell according to claim 2, characterized in that: In step S07, the width of the first semiconductor opening region is 0.1-0.3 mm. When a laser is used to etch an opening on the back side of the silicon wafer, the laser is an ultraviolet or green laser with a pulse width of less than 50 ns.

8. The method for preparing a back-contact heterojunction solar cell according to claim 1, characterized in that: In step S08, a transparent conductive film layer is deposited on the back of the obtained silicon wafer, including: A transparent conductive film is deposited on the back of a silicon wafer by physical vapor deposition technology or activated plasma deposition technology. The thickness of the transparent conductive film is 40-80 nm. The material of the transparent conductive film includes an indium oxide film doped with tin oxide, titanium oxide, zinc oxide or gallium oxide, or the material of the transparent conductive film includes a zinc oxide film doped with aluminum oxide, gallium oxide or boron oxide.

9. A back contact heterojunction solar cell, characterized in that: The method for preparing a back-contact heterojunction solar cell is used as described in any one of claims 1 to 8.

10. A battery assembly, characterized in that: It includes the back-contact heterojunction solar cell as claimed in claim 9.